Resistor and its manufacturing method
A Ni-based alloy with controlled heat treatment forms a short-range ordered phase, addressing the low volume resistivity and instability of Cu-Mn alloys at high temperatures, achieving high stability and low resistance coefficient.
Patent Information
- Application Number
- JP2020115282
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-03
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-07-03
AI Technical Summary
Conventional Cu-Mn alloys exhibit low volume resistivity and instability at temperatures above 100°C, making them unsuitable for high-temperature applications.
A Ni-based alloy with specific compositions of Cr, Mo, Ti, Al, and Si, optimized to form a short-range ordered phase through controlled heat treatment, achieving high volume resistivity and low temperature coefficient of resistance.
The Ni-based alloy achieves a volume resistivity of 125 μΩcm or more and a temperature coefficient of resistance of 100 ppm/°C or less, ensuring stability and processability at high temperatures.
Smart Images

Figure 0007552104000001 
Figure 0007552104000002 
Figure 0007552104000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resistor and a manufacturing method thereof, and more particularly to a resistor having high volume resistivity, a small temperature coefficient of resistance, and excellent characteristic stability at high temperatures, and a manufacturing method thereof. [Background technology]
[0002] In recent years, with the development and improvement of the performance of power supplies, electric vehicles, etc., there is an increasing demand for precision resistance materials, especially resistance materials with high volume resistivity and low temperature coefficient of resistance. Furthermore, with the spread of SiC power devices, which have a higher operating temperature than conventional Si power devices, resistance materials are also required to have stable characteristics at 150°C or higher. Conventionally, metal thin-film resistors made of Cu-Mn alloys (Patent Document 1), which have a low temperature coefficient of resistance, have been used as precision resistance materials.
[0003] Of these, Cu-Mn alloys have an extremely low temperature coefficient of resistance at around 20 to 100°C, are easy to process, and are inexpensive. However, Cu-Mn alloys have a low volume resistivity of 35 to 50 μΩcm. In addition, above 100°C, the volume resistivity decreases and the absolute value of the temperature coefficient of resistance increases, making them unsuitable for use in high temperature ranges above 100°C. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-069724 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a resistor having a high volume resistivity, a small temperature coefficient of resistance, and excellent characteristic stability at high temperatures, and a method for producing the same. [Means for solving the problem]
[0006] In order to solve the above problems, a resistor according to the present invention has the following configuration. (1) The resistor is made of a Ni-based alloy, The Ni-based alloy is 2.5≦Cr≦25.0at%, 5.0≦Mo≦25.0at%, 0≦Ti≦1.2at%, 0≦Al≦1.8at%, 0≦Mn≦4.0at%, and 0≦Si≦7.0at% The balance is Ni and unavoidable impurities. Furthermore, the following formulas (1) and (2) are satisfied. 20.0≦Cr+Mo≦35.0at% …(1) 0.2≦Mo / Cr≦10.0 …(2) (2) The resistor is The volume resistivity at 20°C is 125 μΩcm or more, The temperature coefficient of resistance at 20 to 200°C is 100 ppm / °C or less.
[0007] The method for producing a resistor according to the present invention includes the steps of: a melting and casting step of melting and casting raw materials blended to obtain a resistor according to the present invention to obtain an ingot; a homogenization heat treatment step of performing a homogenization heat treatment on the ingot to obtain a heat-treated body; a hot working step of hot working the heat-treated body to obtain a hot-formed body; a cold working step of performing cold working on the hot-formed body to obtain a cold-formed body; a heat treatment step of subjecting the cold-formed body to a heat treatment to generate a short-range ordered phase; It is equipped with: Effect of the Invention
[0008] In a Ni-based alloy containing Cr and Mo, by optimizing the amount of Cr and Mo and performing heat treatment under appropriate conditions, a resistor with high volume resistivity, small temperature coefficient of resistance, and excellent characteristic stability at high temperatures can be obtained. This is because (a) The volume resistivity increases due to the solid solution effect of Cr and Mo, and (b) By applying appropriate heat treatment, a short-range ordered phase consisting of the three elements Ni-Cr-Mo is formed. It is thought that. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] An embodiment of the present invention will be described in detail below. [1. Ni-based alloy] [1.1. Ingredients] The resistor according to the present invention is made of a Ni-based alloy. The Ni-based alloy contains the following elements, with the balance being Ni and unavoidable impurities. The types of the added elements, their component ranges, and the reasons for their limitations are as follows:
[0010] (1) 2.5≦Cr≦25.0at%: Cr dissolves in Ni, and increases the volume resistivity due to the solid solution effect. Furthermore, it forms a short-range ordered phase, and significantly increases the volume resistivity. To obtain such an effect, the Cr content must be 2.5 at% or more. The Cr content is preferably 4.0 at% or more. On the other hand, if the Cr content is excessive, a completely ordered Ni2Cr phase is easily formed. When the Ni2Cr phase is formed, the volume resistivity drops sharply. Therefore, the Cr content must be 25.0 at% or less. The Cr content is preferably 20.0 at% or less.
[0011] (2) 5.0≦Mo≦25.0at%: Mo dissolves in Ni and increases the volume resistivity by the solid solution effect. To obtain such an effect, the Mo content must be 5.0 at% or more. The Mo content is preferably 7.5 at% or more, and more preferably 10.0 at% or more. On the other hand, if the amount of Mo is excessive, a completely ordered Ni4Mo phase or Ni3Mo phase is likely to be formed. When such an ordered phase is formed, the volume resistivity drops sharply. Therefore, the amount of Mo must be 25.0 at% or less. The amount of Mo is preferably 22.5 at% or less.
[0012] (3) 0≦Ti≦1.2at%: Ti has the effect of increasing the volume resistivity and decreasing the temperature coefficient of resistance due to the solid solution effect, and can be added as necessary. In order to obtain such effects, the Ti content is preferably 0.3 at% or more. On the other hand, if the Ti content is excessive, the temperature coefficient of resistance becomes large, so the Ti content is preferably 1.2 at % or less.
[0013] (4) 0≦Al≦1.8at%: Like Ti, Al has the effect of increasing the volume resistivity and decreasing the temperature coefficient of resistance due to the solid solution effect, and can be added as necessary. In order to obtain such effects, the Al content is preferably 0.5 at% or more. On the other hand, if the amount of Al is excessive, the temperature coefficient of resistance becomes large, so the amount of Al is preferably 1.8 at % or less.
[0014] (5) 0≦Mn≦4.0at%: Mn, like Ti and Al, has the effect of increasing the volume resistivity and decreasing the temperature coefficient of resistance due to the solid solution effect, and can be added as necessary. In order to obtain such effects, the Mn content is preferably 0.5 at% or more. On the other hand, if the Mn content is excessive, the temperature coefficient of resistance becomes large, so the Mn content is preferably 4.0 at % or less.
[0015] (6) 0≦Si≦7.0at%: Like Ti, Al and Mn, Si has the effect of increasing the volume resistivity and decreasing the temperature coefficient of resistance due to the solid solution effect, and can be added as necessary. In order to obtain such effects, the Si content is preferably 0.5 at% or more. On the other hand, if the amount of Si is excessive, the temperature coefficient of resistance becomes large, so the amount of Si is preferably 7.0 at % or less.
[0016] [1.2. Ingredient balance] In addition to each element being within the above-mentioned range, the Ni-based alloy preferably further satisfies any one or more of the following formulae (1) to (4). 20.0≦Cr+Mo≦35.0at% …(1) 0.2≦Mo / Cr≦10.0 …(2) Ti+Al+Mn+Si≦7.0at% …(3) [Cr]+[Mo]≦0.55×(Cr)+28 …(4) In the formula (4), [X] represents the atomic percentage of the element X, and (Y) represents the mass percentage of the element Y.
[0017] [1.2.1. Formula (1)] Formula (1) represents the range of the total amount of Cr and Mo (hereinafter, also referred to as "Cr+Mo amount"). The Cr+Mo amount affects the volume resistivity and temperature coefficient of resistance. When a certain amount of Cr and Mo are added to Ni, Cr and Mo are dissolved in Ni, and a short-range ordered phase consisting of the three elements Ni-Cr-Mo is formed. As a result, the volume resistivity increases and the temperature coefficient of resistance decreases.
[0018] If the amount of Cr+Mo is too small, the volume resistivity drops sharply and the temperature coefficient of resistance increases. Therefore, the amount of Cr+Mo must be 20.0 at% or more. The amount of Cr+Mo is preferably 22.5 at% or more. On the other hand, if the Cr+Mo content is excessive, intermetallic compounds are likely to be formed. If intermetallic compounds are formed, hot working becomes difficult. Therefore, the Cr+Mo content must be 35.0 at% or less. The Cr+Mo content is preferably 32.5 at% or less, and more preferably 30.0 at% or less.
[0019] [1.2.2. Formula (2)] Formula (2) represents the range of the ratio of the number of Mo atoms to the number of Cr atoms (hereinafter also referred to as the "Mo / Cr ratio"). The Mo / Cr ratio, like the amount of Cr+Mo, affects the volume resistivity and the temperature coefficient of resistance.
[0020] If the Mo / Cr ratio is too small, the volume resistivity drops sharply and the temperature coefficient of resistance increases. Therefore, the Mo / Cr ratio must be 0.2 or more. The Mo / Cr ratio is preferably 1.0 or more, and more preferably 1.5 or more. On the other hand, if the Mo / Cr ratio is excessive, intermetallic compounds are easily formed. If intermetallic compounds are formed, hot working becomes difficult. Therefore, the Mo / Cr ratio must be 10.0 or less. The Mo / Cr ratio is preferably 5.0 or less, and more preferably 4.0 or less.
[0021] [1.2.3. Formula (3)] Formula (3) represents the total amount of Ti, Al, Mn, and Si. As described above, Ti, Al, Mn, and Si all have the effect of increasing the volume resistivity and decreasing the temperature coefficient of resistance. However, if the total amount of these elements is excessive, the temperature coefficient of resistance may become large. Therefore, the total amount of these elements is preferably 7.0 at% or less.
[0022] [1.2.4. Formula (4)] Equation (4) is an empirical formula that expresses the hot workability of a Ni-based alloy containing Cr and Mo. By optimizing the Cr and Mo contents so as to satisfy equation (4), it is possible to ensure good hot workability.
[0023] [2. Resistor] The resistor according to the present invention comprises: Made of Ni-based alloy, The volume resistivity at 20°C is 125 μΩcm or more, The temperature coefficient of resistance at 20 to 200°C is 100 ppm / °C or less.
[0024] [2.1. Ni-based alloy] The resistor according to the present invention is made of a Ni-based alloy. Details of the Ni-based alloy are as described above, so a detailed description will be omitted.
[0025] [2.2. Characteristics] [2.2.1. Volume resistivity] The resistor according to the present invention is obtained by performing an appropriate heat treatment on a Ni-based alloy with optimized components. Therefore, the resistor according to the present invention has a higher volume resistivity than conventional resistors. By optimizing the components and heat treatment conditions, a resistor having a volume resistivity of 125 μΩcm or more at 20°C can be obtained. By further optimizing the components and heat treatment conditions, the volume resistivity at 20°C can be 130 μΩcm or more, or 140 μΩcm or more.
[0026] [2.2.2. Temperature coefficient of resistance] "Temperature coefficient of resistance" refers to the value expressed by the following formula (5). Temperature coefficient of resistance (ppm / ℃) = {(RR a ) / R a}×10 6 / (TT a ) …(5) however, R a is the resistance at the reference temperature, R is the resistance at any temperature. T a is the reference temperature (20°C in this invention), T is an arbitrary temperature (200° C. in this invention).
[0027] The resistor according to the present invention is obtained by performing an appropriate heat treatment on a Ni-based alloy with optimized components. Therefore, the resistor according to the present invention has a smaller temperature coefficient of resistance and a higher thermal stability of the temperature coefficient of resistance than conventional resistors. By optimizing the components and heat treatment conditions, a resistor having a temperature coefficient of resistance of 100 ppm / °C or less at 20 to 200°C can be obtained. By further optimizing the components and heat treatment conditions, the temperature coefficient of resistance at 20 to 200°C can be 70 ppm / °C or less, or 50 ppm / °C or less.
[0028] 2.2.3. Thickness The resistor according to the present invention has a high volume resistivity, a low resistance change rate, and high hot workability. Therefore, it can be easily processed into a thin ribbon shape. By optimizing the manufacturing conditions, a resistor having a thickness of 3 mm or less can be obtained. By optimizing the components and manufacturing conditions, it is possible to obtain a resistor having a minimum thickness of 0.10 mm or more, or 0.20 mm or more.
[0029] [3. Resistor manufacturing method] The method for producing a resistor according to the present invention includes the steps of: a melting and casting step of melting and casting raw materials blended to obtain a resistor according to the present invention to obtain an ingot; a homogenization heat treatment step of performing a homogenization heat treatment on the ingot to obtain a heat-treated body; a hot working step of hot working the heat-treated body to obtain a hot-formed body; a cold working step of performing cold working on the hot-formed body to obtain a cold-formed body; a heat treatment step of subjecting the cold-formed body to a heat treatment to generate a short-range ordered phase; It is equipped with:
[0030] [3.1. Melting and casting process] First, raw materials blended to obtain the resistor according to the present invention are melted and cast to obtain an ingot (melting and casting process). The method and conditions for melting and casting are not particularly limited, and well-known methods can be used.
[0031] [3.2. Homogenization heat treatment process] Next, the ingot is subjected to a homogenization heat treatment to obtain a heat-treated body (homogenization heat treatment step). The resistor according to the present invention uses a Ni-based alloy containing a relatively large amount of Cr and Mo, and therefore elements are likely to segregate in the as-cast state. The homogenization heat treatment is performed to remove such segregation of elements.
[0032] If the homogenization heat treatment temperature is too low, segregation of elements cannot be sufficiently removed. Therefore, the heat treatment temperature is preferably 1000° C. or higher. The heat treatment temperature is preferably 1100° C. or higher, and more preferably 1200° C. or higher. On the other hand, if the heat treatment temperature is too high, oxidation may progress rapidly and the oxide layer may need to be removed. Therefore, the heat treatment temperature is preferably 1250° C. or less.
[0033] If the homogenization heat treatment time is too short, segregation of elements cannot be sufficiently removed. Therefore, the heat treatment time is preferably 4 hours or more. The heat treatment time is preferably 8 hours or more, and more preferably 16 hours or more. On the other hand, if the heat treatment time is too long, it may be necessary to remove the oxide layer, so the heat treatment time is preferably 24 hours or less.
[0034] [3.3. Hot working process] Next, the heat-treated body is subjected to hot working to obtain a hot-formed body (hot working step). The hot working is performed to homogenize the structure and process it into a rough shape. The method and conditions of the hot working are not particularly limited as long as the structure can be homogenized and the shape can be processed into a rough shape. In addition, a solution treatment may be performed after the hot working and before the cold working. The solution treatment before the cold working has the advantage that the material that has been work-hardened by the hot working is softened, making it easier to perform the cold working.
[0035] [3.4. Cold working process] Next, the hot-formed body is subjected to cold working to obtain a cold-formed body (cold working step). Usually, high thickness accuracy cannot be obtained by hot working alone. Cold working is performed to process the body into a final thickness dimension. The method and conditions of cold working are not particularly limited as long as the desired dimensional accuracy can be obtained.
[0036] [3.5. Heat treatment process] Next, the cold-formed body is subjected to a heat treatment to generate a short-range ordered phase (heat treatment step), thereby obtaining a resistor according to the present invention.
[0037] In order to obtain a high volume resistivity, it is necessary to generate a short-range ordered phase in the Ni-based alloy. Such a short-range ordered phase may be generated during the cooling process after hot working. However, the short-range ordered phase is destroyed by cold working, so that in the cold-worked state, the volume resistivity is low and the temperature coefficient of resistance is unstable. Furthermore, if the distortion is not sufficiently removed by heat treatment after cold working, the distortion is gradually relaxed in a usage environment of around 200°C, and the volume resistivity and temperature coefficient of resistance change.
[0038] Therefore, it is necessary to reform the short-range ordered phase that disappeared by cold working, thereby increasing the volume resistivity and decreasing the temperature coefficient of resistance. At the same time, it is necessary to fully remove the residual strain. The method and conditions of the heat treatment are not particularly limited as long as they are capable of reforming the short-range ordered phase. Specific examples of the heat treatment method include the following.
[0039] [3.5.1. Solution treatment] The heat treatment step may be a solution treatment step. Here, the term "solution treatment" means (a) The cold-formed body is held at a relatively high solution treatment temperature for a relatively short period of time to form a solid solution in which elements are uniformly dissolved macroscopically and the ordered phase is eliminated; (b) The solid solution is then cooled from the solution treatment temperature at a predetermined average cooling rate to form a short-range ordered phase during the cooling process. It says the method. The "average cooling rate" refers to the temperature difference (ΔT) in the range from the solution treatment temperature to 400°C divided by the time (t) required for cooling (=ΔT / t).
[0040] If the temperature of the solution treatment is too low, the elements will not be sufficiently dissolved, so the treatment temperature is preferably 600° C. or higher, more preferably 800° C. or higher, and even more preferably 1000° C. or higher. On the other hand, if the temperature of the solution treatment is too high, the crystal grains may grow too rapidly, and the material strength may decrease. Therefore, the treatment temperature is preferably 1200°C or less. The treatment temperature is preferably 1100°C or less, and more preferably 1050°C or less.
[0041] If the solution treatment time is too short, the elements will not be sufficiently dissolved. Therefore, the heat treatment time is preferably 3 minutes or more. The heat treatment time is preferably 10 minutes or more, and more preferably 30 minutes or more. On the other hand, if the solution treatment time is too long, the crystal grains may grow and the material strength may decrease, so the heat treatment time is preferably 1 hour or less.
[0042] If the average cooling rate is too slow, ordering may progress excessively during cooling, resulting in a decrease in volume resistivity, so the average cooling rate is preferably 0.01° C. / s or more. On the other hand, if the average cooling rate is too fast, the formation of the short-range ordered phase becomes insufficient, and sufficient properties are not exhibited. In addition, strain is introduced during cooling, and the removal of residual strain becomes insufficient. Therefore, the average cooling rate is preferably 20°C / s or less.
[0043] 3.5.2. Annealing treatment The heat treatment step may be an annealing step, where "annealing" refers to a method of holding a cold-formed body at a relatively low temperature for a relatively long period of time to simultaneously remove strain introduced during cold working and form a short-range ordered phase.
[0044] If the annealing temperature is too low, the short-range ordered phase cannot be sufficiently formed within a practical annealing time, so the annealing temperature is preferably 400° C. or higher. On the other hand, if the annealing temperature is too high, ordering may proceed excessively, or the ordered phase may disappear due to a part or all of the metal structure becoming a solid solution state, and the volume resistivity may decrease or the rate of resistance change may increase. Therefore, the annealing temperature is preferably 700°C or less. The annealing temperature is preferably 650°C or less.
[0045] If the annealing time is too short, the formation of the short-range ordered phase becomes insufficient. Therefore, the annealing time is preferably 3 minutes or more. The annealing time is preferably 30 minutes or more, and more preferably 60 minutes or more. On the other hand, if the annealing time is too long, the ordering may proceed excessively, and the volume resistivity may decrease or the resistance change rate may increase. Therefore, the annealing time is preferably less than 48 hours. The annealing time is preferably 24 hours or less, and more preferably 16 hours or less.
[0046] Either the solution treatment or the annealing treatment may be performed, or both may be performed. When both the solution treatment and the annealing treatment are performed, it is preferable to perform the annealing treatment after the solution treatment. This is because the formation of the short-range ordered phase can be completed in a shorter time than when the annealing treatment is performed alone.
[0047] [4. Effect] In a Ni-based alloy containing Cr and Mo, by optimizing the amount of Cr and Mo and performing heat treatment under appropriate conditions, a resistor with high volume resistivity, small temperature coefficient of resistance, and excellent characteristic stability at high temperatures can be obtained. This is because (a) The volume resistivity increases due to the solid solution effect of Cr and Mo, and (b) By applying appropriate heat treatment, a short-range ordered phase consisting of the three elements Ni-Cr-Mo is formed. It is thought that. EXAMPLES
[0048] (Examples 1 to 25, Comparative Examples 1 to 6) [1. Sample preparation] The raw materials mixed to obtain the composition shown in Table 1 were melted in a vacuum induction furnace to obtain a 30 kg ingot. The ingot was then subjected to a homogenization treatment in which it was heated at 1200°C for 24 hours. Thereafter, it was forged at 1150°C and formed into a plate shape with a thickness of 10 mm. In addition, the plate-shaped hot-formed body was subjected to a solution treatment in which it was held at 1050°C for 2 hours and then air-cooled. Furthermore, the hot-formed body was cold-rolled at room temperature to obtain a cold-formed body with a thickness of 2 mm.
[0049] Next, the obtained cold-formed body was subjected to solution treatment by holding at 1050°C for 1 hour and then air-cooling (AC). In addition, for Examples 3 and 10, in addition to the samples solution-treated under the above conditions, (a) A solution treatment for a cold-formed body at 1050°C for 1 hour followed by water quenching (WC), or (b) annealing the cold-formed material at 500°C for 3 hours; Samples were also prepared in which the above procedure was performed.
[0050] [Table 1]
[0051] 2. Test Method 2.1. Cutting out test pieces A test piece for measuring electrical resistance, measuring 2 mm x 2 mm x 80 mm, was cut out from the cold-formed body after heat treatment. The test piece was cut by discharge cutting to avoid the introduction of distortion due to cutting. The cutting direction was the same as the rolling direction and the longitudinal direction of the test piece.
[0052] [2.2. Measurement of volume resistivity and calculation of temperature coefficient of resistance] The volume resistivity (ρ) was measured by the four-terminal method. The measurement temperature was 20°C or 200°C. The volume resistivity was measured three times at each temperature, and the average value was calculated. The measurement at 200°C was performed after increasing the temperature from 20°C to 200°C at a rate of 1°C / s and holding the temperature at 200°C for 5 minutes. Furthermore, the temperature coefficient of resistance was calculated using the above-mentioned formula (5).
[0053] [3. Results] Table 2 shows the volume resistivity (ρ) and temperature coefficient of resistance (TCR) of the test pieces heat-treated under the conditions of 1050°C / 1h / AC. With regard to the hot workability in Table 2, "○" indicates that no cracks appear on the material surface during hot working, and that consistent processing is possible. "△" indicates that cracks appear on the material surface during hot working, and if processing is continued to the end, the cracks will progress to the inside, so surface scratches must be removed halfway through processing. "×" indicates that cracks instantly appear from the surface to the inside at the early stage of hot working, making hot working extremely difficult.
[0054] Regarding the volume resistivity in Table 2, "◯" indicates that the volume resistivity is 125 μΩcm or more, and "×" indicates that the volume resistivity is less than 125 μΩcm. Furthermore, with regard to the TCR in Table 2, "◎" indicates that the TCR is 50 ppm / °C or less, "○" indicates that the TCR is more than 50 ppm / °C and less than 100 ppm / °C, and "×" indicates that the TCR is more than 100 ppm / °C.
[0055] Moreover, the resistivity and temperature coefficient of resistance (TCR) of the test pieces (Examples 3 and 10) that were heat-treated under various conditions are shown in Table 3. From Tables 2 and 3, the following can be seen.
[0056] [Table 2]
[0057] [Table 3]
[0058] (1) Comparative Examples 1 and 2 have low volume resistivity and high TCR. This is believed to be due to the small amount of Cr+Mo. (2) Comparative Example 3 has slightly poor hot workability, low volume resistivity, and high TCR. This is believed to be due to the excessive amount of Cr+Mo. (3) Comparative Example 4 has slightly poor hot workability, low volume resistivity, and high TCR. This is believed to be due to the excessive Cr content.
[0059] (4) In Comparative Example 5, the hot workability was extremely poor, and a cold-formed product having a thickness of 2 mm could not be obtained. This is believed to be due to the small amount of Cr. (5) Comparative Example 6 has a significantly low volume resistivity and a high TCR. This is believed to be due to an insufficient amount of Mo. (6) All of Examples 1 to 25 have good hot workability, high volume resistivity, and small TCR.
[0060] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]
[0061] The resistor according to the present invention can be used as various resistors for use in power supply devices, electric vehicles, and the like.
Claims
1. A resistor having the following configuration: (1) The resistor is made of a Ni-based alloy, The Ni-based alloy is 2.5≦Cr≦25.0at%, 5.0≦Mo≦25.0at%, 0≦Ti≦1.2at%, 0≦Al≦1.8at%, 0≦Mn≦4.0 at%; and 0≦Si≦7.0at% The balance is Ni and unavoidable impurities. Furthermore, the following formulas (1) and (2) are satisfied. 20.0≦Cr+Mo≦35.0at%…(1) 0.2≦Mo / Cr≦10.0 ... (2) (2) The resistor is The volume resistivity at 20° C. is 125 μΩcm or more, The temperature coefficient of resistance in the range of 20 to 200° C. is 100 ppm / ° C. or less.
2. The resistor according to claim 1 , wherein the Ni-based alloy further satisfies the following formula (3): Ti+Al+Mn+Si≦7.0at%…(3)
3. The resistor according to claim 1 or 2, wherein the Ni-based alloy further satisfies the following formula (4): [Cr]+[Mo]≦0.55×(Cr)+28…(4) In the formula (4), [X] represents the atomic percentage of the element X, and (Y) represents the mass percentage of the element Y.
4. 4. The resistor according to claim 1, wherein the resistor has a thickness of 3 mm or less.
5. A melting and casting process for melting and casting a raw material blended to obtain the resistor according to any one of claims 1 to 4 to obtain an ingot; a homogenization heat treatment step of performing a homogenization heat treatment on the ingot to obtain a heat-treated body; a hot working step of hot working the heat-treated body to obtain a hot-formed body; a cold working step of performing cold working on the hot-formed body to obtain a cold-formed body; a heat treatment step of subjecting the cold-formed body to a heat treatment to generate a short-range ordered phase and obtain the resistor according to any one of claims 1 to 4; A method for manufacturing a resistor comprising the steps of:
6. The heat treatment step includes: (a) holding the cold-formed body at a solution treatment temperature of 600° C. or more and 1200° C. or less for 3 minutes to 1 hour; (b) Thereafter, cooling is performed at an average cooling rate of 0.01° C. / s or more and 20° C. / s or less in the section from the solution treatment temperature to 400° C. The method for producing a resistor according to claim 5, further comprising a solution treatment step.
7. The method for producing a resistor according to claim 5 or 6, wherein the heat treatment step includes an annealing step of holding the cold-formed body at an annealing temperature of 400° C. or more and 700° C. or less for 3 minutes or more and less than 48 hours.
Citation Information
Patent Citations
JP1971022331Y1
Ni-cr alloy material