Pressure-sensitive adhesive composition for polarizing plate, pressure-sensitive adhesive for polarizing plate, and image display device
The adhesive composition for polarizing plates, with a specific acrylic resin and ionic compound formulation, addresses durability and antistatic challenges in high-temperature environments, ensuring effective bonding and performance in liquid crystal display devices.
Patent Information
- Application Number
- JP2020128227
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing adhesives for polarizing plates in liquid crystal display devices fail to provide sufficient durability and antistatic performance in harsh high-temperature environments, particularly exceeding 100°C, and often require high amounts of ionic compounds that compromise durability due to plasticization.
An adhesive composition for polarizing plates containing an acrylic resin with a structural moiety derived from methyl methacrylate, limited to 5-30% by weight, and an ionic compound with specific anion and cation components, along with a controlled average carbon number in the side chain structure, ensuring excellent antistatic properties and high durability.
The adhesive composition achieves both high durability and antistatic performance in environments exceeding 100°C, effectively bonding polarizing plates to liquid crystal cells, preventing peeling and static-induced issues.
Smart Images

Figure 0007552121000002 
Figure 0007552121000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition for polarizing plates, a pressure-sensitive adhesive for polarizing plates obtained by using the pressure-sensitive adhesive composition for polarizing plates, and an image display device using the pressure-sensitive adhesive for polarizing plates, and more specifically to a pressure-sensitive adhesive composition for polarizing plates for forming a pressure-sensitive adhesive for polarizing plates having excellent antistatic performance and high durability in harsh high-temperature environments, a pressure-sensitive adhesive for polarizing plates obtained by using the same, and an image display device using the pressure-sensitive adhesive for polarizing plates. [Background technology]
[0002] Conventionally, liquid crystal display devices are manufactured by preparing a polarizing plate by covering both sides of a polarizer made of a polyvinyl alcohol-based film or the like to which polarizing properties have been imparted with protective films, and laminating the polarizing plate on the surface of a liquid crystal cell in which an oriented liquid crystal component is sandwiched between two glass plates. The lamination of the polarizing plate on the surface of the liquid crystal cell is usually performed by abutting and pressing an adhesive layer provided on the surface of the polarizing plate against the surface of the liquid crystal cell.
[0003] The adhesive used to bond the protective film of such a polarizing plate to the glass plate of the liquid crystal cell is required to have durability such that the polarizing plate does not lift or peel off from the glass plate of the liquid crystal cell, for example, in a harsh high-temperature environment of over 85°C. Furthermore, in recent years, liquid crystal display devices have been deployed in various applications, and for example, their use has been increasing outdoors, in vehicles, etc. Outdoors and in vehicles can become very hot depending on the season and environment, and therefore liquid crystal display devices are required to have higher durability at high temperatures than liquid crystal display devices used indoors.
[0004] On the other hand, because liquid crystal cells are driven by controlling the voltage, problems such as display unevenness and breakdowns can occur due to static electricity. Static electricity is easily generated when bonding or peeling off adhesive films, so as a countermeasure against static electricity, it is necessary to give the adhesive antistatic properties.
[0005] In order to achieve both durability and antistatic performance, for example, Patent Document 1 proposes a pressure-sensitive adhesive obtained from a pressure-sensitive adhesive composition containing a crosslinker and a (meth)acrylic acid ester copolymer containing, as monomer units constituting a polymer, an alicyclic structure-containing monomer, an aromatic ring-containing monomer, and an oxyalkylene group-containing monomer.
[0006] Furthermore, Patent Document 2 proposes an adhesive that combines an acrylic resin using a macromonomer with an antistatic agent such as an ionic compound as an adhesive that combines durability in the high-temperature environment of a liquid crystal cell and antistatic performance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2017-134134 A [Patent Document 2] International Publication No. 2015 / 141382 Summary of the Invention [Problem to be solved by the invention]
[0008] However, although the adhesive described in Patent Document 1 has been evaluated for antistatic performance and durability, the heat resistance evaluation has been carried out in a dry atmosphere at 85°C. In recent years, where durability is required even in harsh high-temperature environments of, for example, over 100°C, a satisfactory adhesive has not yet been developed. Furthermore, in order to impart the high antistatic performance required in recent years to the adhesive described in Patent Document 2, it is necessary to use a large amount of an ionic compound. In that case, the constraint on the molecular chains by the macromonomer is canceled out by the plasticization of the adhesive by the ionic compound, resulting in a problem of reduced durability, and further improvement is required.
[0009] Under such a background, the present invention has an object to provide a pressure-sensitive adhesive composition for polarizing plates which forms a pressure-sensitive adhesive having excellent antistatic performance and high durability in a severe high-temperature environment exceeding 100°C when a member used in an image display member such as a liquid crystal cell, for example, a metal layer such as a glass plate or a conductive layer, is used as an adherend, and further has an object to provide a pressure-sensitive adhesive for polarizing plates obtained by using the pressure-sensitive adhesive composition, and an image display device using the pressure-sensitive adhesive. [Means for solving the problem]
[0010] However, in view of these circumstances, the present inventors have conducted extensive research and found that, in an adhesive composition for polarizing plates containing an acrylic resin and an ionic compound, the acrylic resin contains a structural portion derived from methyl methacrylate, and the average number of carbon atoms (α) in the side chain structural portion of the acrylic resin is adjusted to be small, thereby obtaining an adhesive having excellent antistatic performance and also high durability even in harsh high-temperature environments, for example, at temperatures exceeding 100°C, and thus completed the present invention.
[0011] That is, the gist of the present invention is a pressure-sensitive adhesive composition for polarizing plates, which contains an acrylic resin (A) and an ionic compound (B), wherein the acrylic resin (A) contains a structural portion derived from methyl methacrylate and a structural portion derived from a polar group-containing monomer, the content of the methyl methacrylate is 5 to 30% by weight based on all polymerization components constituting the acrylic resin (A), the acrylic resin (A) contains a hydroxyl group-containing monomer as the polar group-containing monomer, the content of the hydroxyl group-containing monomer is 3 to 10% by weight based on all polymerization components constituting the acrylic resin (A), and the average carbon number (α) of side chain structural portions possessed by the acrylic resin (A) is 3.3 or less. The ionic compound (B) is a compound consisting of a cationic component and an anionic component, and the anionic component is Cl. - 、Br - 、I - , AlCl 4 - 、Al 2 Cl 7 - , B.F. 4 - , P.F. 6 - , ClO 4 - , NO 3 - , C.H. 3 COO - , C.F. 3 COO - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , (CF 3 SO 2 ) 3 C - , AsF 6 - , SbF 6 - , NbF 6 - , TaF 6 - 、(C 2 O 4 ) 2 B - , SCN - , (CN) 2 N - 、C 4 F 9 SO 3 - 、C 3 F 7 COO - , (CF 3 SO 2 )(CF 3 CO)N - 、 - O 3 S(CF 2 ) 3 SO 3 - and an anion selected from the anions represented by the following general formulas (1) to (4): (1):(C n F 2n+1 SO 2 ) 2 N - (wherein n is an integer from 1 to 10), (2):CF 2 (C m F 2m SO 2 ) 2 N - (where m is an integer from 1 to 10), (3):O 3 S(CF 2 ) l SO 3 - (wherein l is an integer from 1 to 10), (4):(C p F 2p+1 SO 2 )N - (C q F 2q+1 SO 2 ) (wherein p and q are integers from 1 to 10) The content of acrylic resin components other than the acrylic resin (A) is 5 parts by weight or less based on 100 parts by weight (solid content) of the acrylic resin (A). The present invention relates to a pressure-sensitive adhesive composition for polarizing plates.
[0012] The gist of the present invention also relates to a pressure-sensitive adhesive for polarizing plates, which is obtained by using the pressure-sensitive adhesive composition for polarizing plates, and an image display device in which a polarizing plate and a liquid crystal cell are bonded together with the pressure-sensitive adhesive.
[0013] Generally, as a method for improving the durability of a pressure-sensitive adhesive composition using an acrylic resin at high temperatures, a method of copolymerizing a specific polar functional group-containing monomer when preparing an acrylic resin, or a method of copolymerizing a copolymerizable monomer having a high glass transition temperature of a homopolymer, etc., are known, and these methods can ensure the cohesive force in a high temperature environment and improve the durability at high temperatures. Therefore, when attempting to impart higher durability, a method such as copolymerizing a copolymerizable monomer having a higher glass transition temperature of a homopolymer or increasing the amount of introduction of such a copolymerizable monomer can be considered. However, on the other hand, there is a problem that the adhesion is reduced by the resin being too hard as a whole, and the durability at high temperatures is reduced instead. The present inventors have found that, although a copolymerizable monomer with a high glass transition temperature is copolymerized, which would normally harden the resin and reduce adhesion and durability at high temperatures, by using a specific copolymerizable monomer having a high glass transition temperature and by setting the average number of carbon atoms in the side chain structural portion of the acrylic resin to a predetermined value or less, excellent durability at high temperatures is achieved, and have completed the present invention. Effect of the Invention
[0014] The pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition for polarizing plates of the present invention has excellent antistatic performance and also has high durability even in a severe high-temperature environment, for example, above 100° C. The pressure-sensitive adhesive composition for polarizing plates of the present invention can be effectively used as a pressure-sensitive adhesive for polarizing plates for forming a pressure-sensitive adhesive layer on a polarizing plate, and as a pressure-sensitive adhesive for forming an image display device by laminating a polarizing plate and a liquid crystal cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate. Also, "acrylic resin" means a resin obtained by polymerizing a polymerization component containing at least one (meth)acrylate monomer. The side chain structural portion of the acrylic resin refers to a structural portion derived from an alcohol in an ethylenically unsaturated group-containing ester contained in a polymerization component of the acrylic resin.
[0016] The "weight average molecular weight" and "number average molecular weight" are weight average molecular weights calculated based on the molecular weight of standard polystyrene. The samples were analyzed using a high performance liquid chromatograph (Waters Japan, "Waters 2695 (main body)" and "Waters 2414 (detector)") with a Shodex GPC KF-806L column (exclusion limit molecular weight: 2 × 10 7 , Separation range: 100~2×10 7 The measurement is performed using three columns in series (theoretical plate number: 10,000 plates / column, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm). The "dispersity" is determined by the weight average molecular weight / number average molecular weight.
[0017] The "glass transition temperature" is calculated from the types and mass fractions of monomer units constituting the copolymer using the following Fox equation. In this specification, the glass transition temperature calculated using the Fox equation is also referred to as the "calculated glass transition temperature." 1 / (273+Tg)=Σ{Wi / (273+Tgi)} In the formula, Tg is the glass transition temperature (°C) of the copolymer, Wi is the weight fraction of monomer units derived from monomer i that constitutes the copolymer, and Tgi is the glass transition temperature (°C) of the homopolymer of monomer i. The value of Tgi can usually be determined by using the value described in Polymer Handbook, J. Brandrup, Interscience, 1989. The value of Tgi can also be measured by a differential scanning calorimeter (DSC) according to a method in accordance with JIS K7121-1987 or JIS K 6240.
[0018] [Adhesive composition for polarizing plate] The pressure-sensitive adhesive composition for polarizing plates of the present invention contains an acrylic resin (A) and an ionic compound (B). First, the acrylic resin (A) will be described.
[0019] <Acrylic resin (A)> The acrylic resin (A) used in the present invention contains a structural portion derived from methyl methacrylate and is a resin obtained by polymerizing a polymerization component containing at least methyl methacrylate. In addition to methyl methacrylate, the polymerization component preferably further contains a (meth)acrylic acid alkyl ester (a1) (excluding methyl methacrylate) and a polar group-containing monomer (a2), and if necessary, contains other polymerizable monomers (a3). Each of these monomers will be described below. The acrylic resin (A) used in the present invention is a resin obtained by copolymerizing polymerization components containing at least methyl methacrylate and an alkyl (meth)acrylate ester (a1), and therefore necessarily has a side chain structure portion.
[0020] [Methyl methacrylate] The content of methyl methacrylate is preferably 5 to 30% by weight, more preferably 7 to 25% by weight, and even more preferably 10 to 20% by weight, based on the total polymer components constituting the acrylic resin (A) (hereinafter simply referred to as "total polymer components"). If the content is too low, durability at high temperatures tends to decrease, and if the content is too high, adhesion tends to decrease.
[0021] [(Meth)acrylic acid alkyl ester (a1)] Examples of the (meth)acrylic acid alkyl ester (a1) include those having an alkyl group with a carbon number of usually 1 to 20, preferably 1 to 18, more preferably 1 to 12, and further preferably 1 to 8, and aliphatic (meth)acrylic acid alkyl esters are preferred. However, as described above, methyl methacrylate is excluded from the (meth)acrylic acid alkyl ester (a1). Specific examples of the (meth)acrylic acid alkyl ester (a1) include methyl acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, n-propyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, etc. These can be used alone or in combination of two or more.
[0022] Among these (meth)acrylic acid alkyl esters (a1), methyl acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred, and n-butyl (meth)acrylate is particularly preferred, because of their excellent adhesive properties and stability during polymerization.
[0023] The content of the (meth)acrylic acid alkyl ester (a1) is preferably 10% by weight or more, more preferably 30% by weight or more, still more preferably 50 to 97% by weight, and particularly preferably 60 to 95% by weight, based on the total polymerized components. If the content is too low, the adhesive properties tend to decrease.
[0024] In terms of excellent compatibility with the ionic compound (B), the polymerization components constituting the acrylic resin (A) preferably contain alkyl (meth)acrylates having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, such as methyl acrylate, ethyl (meth)acrylate, and n-butyl (meth)acrylate. The content of these monomers is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 40 to 97% by weight, and particularly preferably 50 to 95% by weight, based on the total polymerization components constituting the acrylic resin (A).
[0025] [Polar group-containing monomer (a2)] By including the polar group-containing monomer (a2) in the polymerization components constituting the acrylic resin (A), a structural moiety derived from the polar group-containing monomer is introduced into the acrylic resin (A). The polar group-containing monomer (a2) in the present invention refers to a polymerizable ethylenically unsaturated monomer containing a polar group such as a hydroxyl group, a carboxyl group, a nitrogen atom-containing group, etc. The polar group-containing monomer (a2) may be used alone or in combination of two or more kinds. In the present invention, the polymerization components preferably contain, as the polar group-containing monomer (a2), at least one selected from a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and a nitrogen atom-containing monomer. Among these, the hydroxyl group-containing monomer and the carboxyl group-containing monomer are more preferred, and the hydroxyl group-containing monomer is even more preferred, in terms of excellent reactivity with the crosslinking agent (C).
[0026] Examples of the hydroxyl group-containing monomer include acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, N-methylol (meth)acrylamide, and hydroxyethyl acrylamide; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro 2-hydroxypropyl (meth)acrylate; and hydroxyl group-containing monomers such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate.
[0027] Among the above hydroxyl group-containing monomers, primary hydroxyl group-containing monomers are preferred because of their excellent reactivity with the crosslinking agent (C), 2-hydroxyethyl(meth)acrylate is preferred because of its stability during polymerization, and 4-hydroxybutyl(meth)acrylate is preferred because of its rapid reactivity with the crosslinking agent (C) and its short aging time. Furthermore, 2-hydroxyethyl(meth)acrylate and 4-hydroxybutyl(meth)acrylate are preferred because they contain less impurities such as di(meth)acrylate during monomer preparation, and are easy to produce because they have high purity.
[0028] In addition, when the above-mentioned hydroxyl group-containing monomer is prepared and used, or when a commercially available product is used, it is preferable to use one having a di(meth)acrylate content as an impurity of 0.5% by weight or less, more preferably 0.2% by weight or less, and even more preferably 0.1% by weight or less. Specifically, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, and 2-hydroxypropyl acrylate having such impurity amounts are particularly preferred.
[0029] Examples of the carboxy group-containing monomer include (meth)acrylic acid and dimer acids of acrylic acid such as β-carboxyethyl acrylate, and among these, (meth)acrylic acid is preferred from the standpoint of heat resistance and stability during polymerization.
[0030] Examples of the nitrogen atom-containing monomer include amino group-containing monomers, amide group-containing monomers, and other nitrogen atom-containing monomers.
[0031] Examples of the amino group-containing monomer include primary amino group-containing monomers such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; secondary amino group-containing monomers such as t-butylaminoethyl (meth)acrylate; and tertiary amino group-containing monomers such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate. Among the above amino group-containing monomers, tertiary amino group-containing monomers are preferred in terms of their high crosslinking promoting effect and high storage stability of the resin.
[0032] Examples of the amide group-containing monomer include (meth)acrylamide; alkoxyalkyl (meth)acrylamide monomers such as methoxymethyl (meth)acrylamide, ethoxymethyl (meth)acrylamide, propoxymethyl (meth)acrylamide, isopropoxymethyl (meth)acrylamide, n-butoxymethyl (meth)acrylamide, and isobutoxymethyl (meth)acrylamide; dialkyl (meth)acrylamide monomers such as dimethyl (meth)acrylamide and diethyl (meth)acrylamide; hydroxyl group-containing amide monomers such as N-(hydroxymethyl)acrylamide; and heterocyclic amide monomers such as (meth)acryloylmorpholine.
[0033] Among the above-mentioned amide group-containing monomers, (meth)acryloylmorpholine, alkoxyalkyl (meth)acrylamide monomers, and dialkyl (meth)acrylamide monomers are preferred from the viewpoint of the stability of the resin solution and the inhibition of migration of the ionic compound (B).
[0034] From the viewpoint of ease of the crosslinking reaction, the molecular weight of the polar group-containing monomer (a2) is preferably not more than 500. The lower limit of the molecular weight is usually 50.
[0035] The content of the polar group-containing monomer (a2) is preferably from 0.1 to 30% by weight, more preferably from 0.5 to 20% by weight, and further preferably from 1 to 10% by weight, based on the total polymerizable components. Among these, in particular when a hydroxyl group-containing monomer is used, the content is preferably 0.1 to 30% by weight, more preferably 0.1 to 20% by weight, particularly preferably 1 to 15% by weight, and even more preferably 3 to 10% by weight, in terms of reactivity with the crosslinking agent and durability. When a carboxyl group-containing monomer is used among the polar group-containing monomers (a2), the content is preferably 0.1 to 10% by weight, more preferably 0.1 to 5% by weight, based on the total polymer components in terms of durability, and is preferably 1% by weight or less, more preferably 0.5% by weight or less, particularly preferably 0.1% by weight or less, based on the total polymer components in terms of corrosion resistance and suppression of hydrolysis of the substrate or adherend. When using a nitrogen atom-containing monomer among the polar group-containing monomers (a2), the content thereof is preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, based on the polymerization components, from the viewpoints of imparting durability and suppressing hydrolysis of the base material.
[0036] [Other polymerizable monomers (a3)] The other polymerizable monomers (a3) are polymerizable ethylenically unsaturated monomers other than methyl methacrylate, the (meth)acrylic acid alkyl esters (a1) and the polar group-containing monomers (a2). For example, aromatic ring-containing monomers such as benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and orthophenylphenoxyethyl (meth)acrylate; alicyclic ring-containing monomers such as cyclohexyl (meth)acrylate, cyclohexyloxyalkyl (meth)acrylate, t-butylcyclohexyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, and the like. acrylate, 2-butoxyethyl (meth)acrylate, 2-butoxydiethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, octoxypolyethylene glycol-polypropylene glycol-mono(meth)acrylate, lauroxypolyethylene glycol mono(meth)acrylate, stearoxypolyethylene glycol mono(meth)acrylate, etc. These can be used alone or in combination of two or more.
[0037] Among these, aromatic ring-containing monomers are preferred in terms of ease of adjusting the refractive index and birefringence and excellent light leakage resistance, and benzyl (meth)acrylate, phenoxy (meth)ethyl acrylate, and phenoxy diethylene glycol (meth)acrylate are particularly preferred. Alicyclic ring-containing monomers are preferred in terms of ease of adjusting the refractive index and birefringence and excellent adhesion to low polarity adherends (e.g., cycloolefins, etc.). The light leakage resistance refers to the performance of an adhesive to prevent backlight light from leaking after high temperature or moist heat tests when the adhesive is used to bond a polarizing plate and a liquid crystal cell, etc.
[0038] The content of the other polymerizable monomers (a3) is preferably 25% by weight or less based on the total polymerizable components in order not to impair the effects of the present invention.
[0039] [Production of acrylic resin (A)] The acrylic resin (A) used in the present invention contains at least methyl methacrylate, and preferably further contains a (meth)acrylic acid alkyl ester (a1), a polar group-containing monomer (a2), and other polymerizable monomers (a3) suitably selected and combined as polymerization components. For example, the polymerization components and a polymerization initiator are mixed or dropped into an organic solvent, followed by polymerization.
[0040] The polymerization reaction can be carried out by a conventionally known polymerization method such as solution radical polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc., among which solution radical polymerization and bulk polymerization are preferred, and solution radical polymerization is particularly preferred.
[0041] Examples of the organic solvent used in the polymerization reaction include aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as hexane; esters such as ethyl acetate and butyl acetate; aliphatic alcohols such as n-propyl alcohol and isopropyl alcohol; and ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.
[0042] Among these organic solvents, ethyl acetate, acetone, methyl ethyl ketone, butyl acetate, toluene, and methyl isobutyl ketone are preferably used from the viewpoints of ease of polymerization reaction, chain transfer effect, ease of drying during adhesive coating, and high safety, and particularly preferably ethyl acetate, acetone, and methyl ethyl ketone. These organic solvents can be used alone or in combination of two or more kinds. The amount of these organic solvents used is usually 10 to 900 parts by weight per 100 parts by weight of all the polymer components.
[0043] In addition, as the polymerization initiator used in such solution radical polymerization, a normal radical polymerization initiator can be used. For example, azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(methylpropionic acid), etc.; organic peroxides such as benzoyl peroxide, lauroyl peroxide, di-t-butyl peroxide, cumene hydroperoxide, etc.; etc. can be appropriately selected and used according to the monomer to be used. These polymerization initiators can be used alone or in combination of two or more. The amount of these polymerization initiators used is usually 0.01 to 5% by weight based on the total polymerization components.
[0044] [Physical properties of acrylic resin (A)] The average carbon number (α) of the side chain structural portion possessed by the acrylic resin (A) of the present invention is 3.3 or less, preferably 1 to 3.3, more preferably 1.5 to 3.2, and further preferably 2 to 3.1. If the average carbon number (α) is too large, the durability at high temperatures will be poor.
[0045] The average carbon number (α) is represented by the sum of the products of the carbon numbers of the side chain structural portions of each polymer component constituting the acrylic resin (A) and the weight ratios of the polymer components to the total polymer components. To explain this more specifically using the acrylic resin A-1 shown in Table 1 as an example, the polymerization components constituting the acrylic resin A-1 are BA (n-butyl acrylate), MA (methyl acrylate), 4HBA (4-hydroxybutyl acrylate) and MMA (methyl methacrylate), the numbers of carbon atoms in the side chain structure portions of each polymerization component are 4, 1, 4 and 1, respectively, and the weight ratios of each polymerization component to the total polymerization components are 0.66, 0.2, 0.04 and 0.1, so the average number of carbon atoms (α) in the side chain structure portions is 4×0.66+1×0.2+4×0.04+1×0.1=3.1. The average carbon number (α) can be adjusted by selecting the polymerization components constituting the acrylic resin (A) and adjusting the composition ratio of the polymerization components.
[0046] The acid value of the acrylic resin (A) is preferably 30 mgKOH / g or less, more preferably 10 mgKOH / g or less, even more preferably 5 mgKOH / g or less, and particularly preferably 1 mgKOH / g or less, from the viewpoints of thermal stability, low metal corrosivity, and excellent antistatic performance. The acid value in the present invention is determined by neutralization titration using potassium hydroxide or potentiometric measurement.
[0047] The weight average molecular weight of the acrylic resin (A) is preferably 200,000 to 3,000,000, more preferably 400,000 to 2,000,000, even more preferably 600,000 to 1,800,000, and particularly preferably 800,000 to 1,600,000. If the weight average molecular weight is too small, durability tends to decrease, whereas if it is too large, a large amount of dilution solvent is required during production, drying properties decrease, and the amount of residual solvent in the pressure-sensitive adhesive layer increases, tending to decrease durability.
[0048] The dispersity (weight average molecular weight / number average molecular weight) of the acrylic resin (A) is preferably 20 or less, more preferably 15 or less, and further preferably 10 or less. If the degree of dispersion is too high, reworkability and durability tend to decrease. The lower limit of the degree of dispersion is usually 1.
[0049] The glass transition temperature (Tg) of the acrylic resin (A) is preferably −100 to 10° C., more preferably −70 to 0° C., and even more preferably −65 to −15° C. If the glass transition temperature is too high, the adhesion decreases and the antistatic performance tends to decrease, whereas if the glass transition temperature is too low, the ionic compound (B) serving as the antistatic agent tends to move easily and bleed, resulting in decreased durability.
[0050] In the pressure-sensitive adhesive composition for polarizing plates of the present invention, the acrylic resin (A) is usually dissolved in a solvent or the like, and the viscosity is adjusted. As the solvent used to dissolve the acrylic resin (A), an organic solvent used in preparing the acrylic resin (A) is preferably used. The solid content (wt%) of the acrylic resin (A) solution is usually 5 to 40, preferably 10 to 30.
[0051] From the viewpoint of ease of handling, the viscosity of the acrylic resin (A) solution is preferably 100 to 30,000 mPa·s / 25°C, more preferably 500 to 15,000 mPa·s / 25°C, still more preferably 1,000 to 8,000 mPa·s / 25°C, and particularly preferably 2,000 to 4,000 mPa·s / 25°C. If the viscosity is too high, the fluidity decreases and handling tends to become difficult, whereas if the viscosity is too low, application of the resulting adhesive tends to become difficult.
[0052] The viscosity of the acrylic resin (A) solution is measured by adjusting the temperature of the acrylic resin (A) solution to 25° C. and by a rotational viscosimetry using a B-type viscometer.
[0053] <Ionic Compound (B)> The pressure-sensitive adhesive composition for polarizing plates of the present invention further contains an ionic compound (B) from the viewpoint of countermeasures against static electricity. The ionic compound (B) is a compound consisting of a cationic component and an anionic component, and is a compound consisting of a combination of an organic cation or an inorganic cation as the cationic component and an organic anion or an inorganic anion as the anionic component. The ionic compound (B) can be used alone or in combination of two or more kinds.
[0054] As the inorganic cation, an alkali metal cation is preferred from the viewpoint of antistatic performance, and a lithium cation is particularly preferred. Examples of organic cations include pyridinium cations, piperidinium cations, pyrrolidinium cations, cations having a pyrroline skeleton, cations having a pyrrole skeleton, imidazolium cations, tetrahydropyrimidinium cations, dihydropyrimidinium cations, pyrazolium cations, pyrazolinium cations, tetraalkylammonium cations, trialkylsulfonium cations, and tetraalkylphosphonium cations. Among the cationic components, organic cations are preferred, and nitrogen-containing organic cations are particularly preferred in terms of compatibility with the resin. In terms of compatibility with the acrylic resin (A), tetraalkylammonium cations, pyridinium cations, and imidazolium cations are preferred, and tetraalkylammonium cations are particularly preferred in terms of low crystallinity of the ionic compound and thus less prone to precipitation.
[0055] Examples of the anion component include Cl. - , Br - , I - , AlCl 4 - , Al 2 Cl 7 - , B.F. 4 - , P.F. 6 - , ClO 4 - , NO 3 - , C.H. 3 COO - , C.F. 3 COO - , C.H. 3 SO 3 - , C.F. 3 SO 3 - , (CF 3 SO 2 ) 3 C - , AsF 6 - , SbF 6 - , NbF 6 - , TaF 6- , (C 2 O 4 ) 2 B - , SCN - , (CN) 2 N - , C 4 F 9 SO 3 - , C 3 F 7 COO - , (CF 3 SO 2 )(CF 3 CO)N - , - O 3 S(CF 2 ) 3 SO 3 - or those represented by the following general formulas (1) to (4) are used. (1): (C n F 2n+1 SO 2 ) 2 N - (wherein n is an integer from 1 to 10), (2):CF 2 (C m F 2m SO 2 ) 2 N - (where m is an integer from 1 to 10), (3): O 3 S(CF 2 ) l SO 3 - (wherein l is an integer from 1 to 10), (4): (C p F 2p+1 SO 2 )N - (C q F 2q+1 SO 2 ), (where p and q are integers from 1 to 10)
[0056] Among the above, anions containing a fluorine atom are particularly preferred, and fluorine-containing sulfonium anions, fluorine-containing imide anions and fluorine-containing sulfonylimide anions are more preferred in terms of antistatic performance, durability and compatibility with the acrylic resin (A).
[0057] As the ionic compound (B), a quaternary ammonium salt is particularly preferred. Specific examples of quaternary ammonium salts include tributylmethylammonium N,N-bis(trifluoromethanesulfonyl)imide, tetrabutylammonium bis(trifluoromethylsulfonyl)imide, tetrabutylammonium bromide, tetrapentylammonium bromide, tetraoctylammonium bromide, ethyldimethylpropylammonium bis(trifluoromethylsulfonyl)imide, n-butyltrimethylammonium bis(trifluoromethanesulfonyl)imide, methyltrioctylammonium bis(trifluoromethylsulfonyl)imide, tributylmethylammonium methylsulfate, tributylmethylammonium methylsulfate, tetrabutylammonium bis(trifluoromethylsulfonyl)imide, tetraethylammonium trifluoromethanesulfonate, tetrabutylammonium benzoate, tetrabutylammonium methanesulfate, tetrabutylammonium nonafluorobutanesulfonate, tetra-n-butylammonium hexafluorophosphate, tetrabutylammonium trifluoroacetate, tetrahexylammonium tetrafluoroborate, and tetrahexylammonium bromide.
[0058] From the viewpoint of the balance between antistatic performance and durability, ionic compounds in which the anion component of the ionic compound (B) is a fluorine-containing anion are preferred, and among these, tributylmethylammonium N,N-bis(trifluoromethanesulfonyl)imide (manufactured by 3M) is particularly preferably used.
[0059] The melting point of the ionic compound (B) is preferably −100° C. to 150° C., more preferably 0° C. to 80° C., and even more preferably 25° C. to 50° C. If the melting point is too low, durability tends to decrease when bleeding out occurs, while if the melting point is too high, the compound tends to become cloudy when precipitated or to have a decreased compatibility with resins.
[0060] The content of the ionic compound (B) is preferably 0.5 to 30 parts by weight, more preferably 1 to 15 parts by weight, and further preferably 2 to 10 parts by weight, based on 100 parts by weight (solid content) of the acrylic resin (A). If the content of such ionic compound (B) is too low, the antistatic performance will be reduced, and static electricity will tend to cause touch panel malfunctions and uneven display on liquid crystal cells. If the content of ionic compound (B) is too high, the adhesive layer will plasticize, reducing durability and making the plastic substrate or adherend more susceptible to hydrolysis.
[0061] <Crosslinking agent (C)> The pressure-sensitive adhesive composition for polarizing plates of the present invention preferably contains a crosslinking agent (C) in addition to the acrylic resin (A) and the ionic compound (B). The crosslinking agent (C) is preferred in that it improves the elastic modulus of the pressure-sensitive adhesive when formed, prevents migration of components contained in the substrate or adherend, and improves durability.
[0062] The crosslinking agent (C) is a compound that reacts with functional groups in the acrylic resin (A) to form a crosslinked structure, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, aldehyde-based crosslinking agents, amine-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among these, it is preferable to use an isocyanate-based crosslinking agent or an epoxy-based crosslinking agent, and in particular, an isocyanate-based crosslinking agent is preferable, in terms of improving adhesion to the adherend and excellent reactivity with the acrylic resin (A). The crosslinking agent (C) may be used alone or in combination of two or more kinds.
[0063] Examples of the isocyanate crosslinking agent include aromatic isocyanate compounds, alicyclic isocyanate compounds, and aliphatic isocyanate compounds. Examples of the aromatic isocyanate compounds include tolylene diisocyanate compounds such as 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate; xylylene diisocyanate compounds such as 1,3-xylylene diisocyanate; diphenylmethane compounds such as diphenylmethane-4,4-diisocyanate; and naphthalene diisocyanate compounds such as 1,5-naphthalene diisocyanate. Examples of the alicyclic isocyanate compounds include isophorone diisocyanate, 1,4-cyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, methylcyclohexane diisocyanate, isopropylidenedicyclohexyl-4,4'-diisocyanate, 1,3-diisocyanatomethylcyclohexane, and norbornane diisocyanate. Examples of the aliphatic isocyanate compounds include hexamethylene diisocyanate and trimethylhexamethylene diisocyanate. Further, examples of the isocyanate compounds include adducts, biuret compounds, and isocyanurates.
[0064] Among these isocyanate crosslinking agents, tolylene diisocyanate compounds are preferred in terms of pot life and durability, xylylene diisocyanate compounds and isocyanurate skeleton-containing isocyanate compounds are preferred in terms of shortening aging time, and aromatic ring-free isocyanate compounds are preferred in terms of yellowing resistance.Specific examples of these include an adduct of an isocyanate compound selected from tolylene diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate with trimethylolpropane, and an isocyanurate of an isocyanate compound selected from tolylene diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate with trimethylolpropane, and these adducts and isocyanurates are preferred in terms of excellent balance between durability, pot life, and crosslinking speed.
[0065] Examples of the epoxy crosslinking agent include bisphenol A-epichlorohydrin type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, and diglycerol polyglycidyl ether.
[0066] Examples of the aziridine crosslinking agent include tetramethylolmethane-tri-β-aziridinylpropionate, trimethylolpropane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide).
[0067] Examples of the melamine-based crosslinking agent include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexaptoxymethylmelamine, hexapentyloxymethylmelamine, hexahexyloxymethylmelamine, melamine resins, and the like.
[0068] Examples of the aldehyde crosslinking agent include glyoxal, malondialdehyde, succindialdehyde, maleic dialdehyde, glutaric dialdehyde, formaldehyde, acetaldehyde, and benzaldehyde.
[0069] Examples of the amine-based crosslinking agent include hexamethylenediamine, triethyldiamine, polyethyleneimine, hexamethylenetetraamine, diethylenetriamine, triethyltetraamine, isophoronediamine, amino resins, and polyamides.
[0070] Examples of the metal chelate crosslinking agent include coordination compounds of polyvalent metals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, and zirconium with ligands such as acetylacetone and acetoacetyl ester.
[0071] When the crosslinking agent (C) is used, its content is preferably 0.005 to 30 parts by weight, more preferably 0.01 to 10 parts by weight, even more preferably 0.03 to 5 parts by weight, and particularly preferably 0.05 to 3 parts by weight, relative to 100 parts by weight (solid content) of the acrylic resin (A). If the content is too small, it tends to be difficult to obtain the effect of improving durability, while if the content is too large, the stress relaxation property decreases, making the adherend substrate more likely to warp, or requiring long-term aging.
[0072] <Silane coupling agent (D)> From the viewpoint of improving durability, the pressure-sensitive adhesive composition for polarizing plates of the present invention preferably further contains a silane coupling agent (D).
[0073] The silane coupling agent (D) is an organosilicon compound containing, in its structure, at least one reactive functional group and at least one alkoxy group bonded to a silicon atom, and examples of the silane coupling agent include monomeric and oligomeric types. Examples of the reactive functional group in the silane coupling agent (D) include an epoxy group, a (meth)acryloyl group, a mercapto group, a hydroxyl group, a carboxy group, an amino group, an amide group, an isocyanate group, and the like. Among these, an epoxy group and a mercapto group are preferred from the viewpoints of excellent durability and reworkability.
[0074] The content ratio of reactive functional group in silane coupling agent (D) is preferably 3,000g / mol or less, more preferably 1,500g / mol or less, and even more preferably 1000g / mol or less.If the reactive functional group is in the above range, the balance between durability and reworkability tends to be excellent.The lower limit of the content ratio of reactive functional group in silane coupling agent (D) is 200g / mol.
[0075] As the alkoxy group bonded to a silicon atom in the silane coupling agent (D), from the viewpoints of durability and storage stability, an alkoxy group having 1 to 8 carbon atoms is preferred, and among these, a methoxy group and an ethoxy group are more preferred.
[0076] The silane coupling agent (D) may have an organic functional group other than the reactive functional group and the alkoxy group bonded to the silicon atom, such as an alkyl group or a phenyl group.
[0077] From the viewpoint of reworkability and durability, the silane coupling agent (D) preferably has a weight average molecular weight of 1,000 or more, more preferably 2,300 to 30,000, and even more preferably 3,000 to 20,000. When the weight average molecular weight is within the above range, there is a tendency for the balance between reworkability and durability to be excellent.
[0078] The weight average molecular weight mentioned above is a weight average molecular weight calculated based on the molecular weight of standard polystyrene, and can be measured by the following method. Equipment: Gel permeation chromatograph Detector: Differential refractive index detector RI (Tosoh Corporation, RI-8020 type, sensitivity 32) Column: TSKgel guardcolumn HHR-H (1 column) (Tosoh Corporation, diameter 6 mm x 4 cm), TSKgel GMHHR-N (2 columns) (Tosoh Corporation, diameter 7.8 mm x 30 cm) Solvent: Tetrahydrofuran (THF) Column temperature: 23℃ ·Flow rate: 1.0mL / min
[0079] As the silane coupling agent (D), an oligomeric organosilicon compound (organosiloxane compound) such as a dimer or trimer formed by partial hydrolysis and polycondensation of an organosilicon compound is preferred from the viewpoint of reworkability and durability. Examples of such oligomeric organosilicon compounds include mercapto-group-containing oligomeric silane coupling agents obtained by partial hydrolysis and polycondensation of mercapto-group-containing silane compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; mercapto-group-containing oligomeric silane coupling agents which are co-condensates of the above-mentioned mercapto-group-containing silane compounds with alkyl-group-containing silane compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane; γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyltrieth ... Epoxy group-containing oligomer-type silane coupling agents obtained by hydrolysis and polycondensation of a portion of an epoxy group-containing silane compound such as silaneoxypropylmethyldimethoxysilane, methyltri(glycidyl)silane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc.; epoxy group-containing oligomer-type silane coupling agents which are co-condensates of the above-mentioned epoxy group-containing silane compounds with alkyl group-containing silane compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, etc.; epoxy group-containing oligomer-type silane coupling agents obtained by ether-modifying a portion of these epoxy group-containing oligomer-type silane coupling agents; and the like. These can be used alone or in combination of two or more.
[0080] In terms of achieving an excellent balance between durability and reworkability, the oligomer type silane coupling agent preferably has an alkoxy group content of 1 to 70% by weight, more preferably 5 to 60% by weight, and even more preferably 10 to 55% by weight.
[0081] Specific examples of the monomeric or oligomeric silane coupling agent (D) include commercially available silane coupling agents "KBM-403", "X-41-1053", "X-41-1059A", "X-24-9590", "KBM-803", "X-41-1805", "X-41-1810", "X-41-1818", and the like manufactured by Shin-Etsu Chemical Co., Ltd.
[0082] When the silane coupling agent (D) is used, the content thereof is preferably 0.001 to 3 parts by weight, more preferably 0.005 to 1 part by weight, still more preferably 0.01 to 0.5 part by weight, and particularly preferably 0.015 to 0.3 part by weight, relative to 100 parts by weight (solid content) of the acrylic resin (A). If the content is too low, it will be difficult to obtain the effect of improving reworkability, whereas if the content is too high, the silane coupling agent (D) will tend to bleed, resulting in a decrease in durability.
[0083] <Other ingredients> The pressure-sensitive adhesive composition for polarizing plates of the present invention may contain, as other components, various additives such as a resin component, an acrylic monomer, a polymerization inhibitor, an antioxidant, a corrosion inhibitor, a crosslinking accelerator, a radical generator, a peroxide, a radical scavenger, an ultraviolet absorber, a plasticizer, a pigment, a stabilizer, a filler, metal particles, resin particles, etc. In addition to the above, the pressure-sensitive adhesive composition may contain small amounts of impurities contained in the production raw materials of the components of the pressure-sensitive adhesive composition.
[0084] The content of the other components is preferably 5 parts by weight or less, particularly preferably 1 part by weight or less, and further preferably 0.5 parts by weight or less, based on 100 parts by weight (solid content) of the acrylic resin (A). If the content is too high, the compatibility with the acrylic resin (A) decreases, and the durability tends to decrease.
[0085] Thus, by mixing the acrylic resin (A) and the ionic compound (B), preferably further comprising a crosslinking agent (C), a silane coupling agent (D), and other components, the pressure-sensitive adhesive composition for polarizing plates of the present invention can be obtained.
[0086] The mixing method is not particularly limited, and various methods can be used, such as a method of mixing the components all at once, or a method of mixing any components and then mixing the remaining components all at once or sequentially.
[0087] [Adhesive for polarizing plates, image display devices] The pressure-sensitive adhesive composition for polarizing plates of the present invention can be made into a pressure-sensitive adhesive for polarizing plates by crosslinking (curing), and further, a polarizing plate with a pressure-sensitive adhesive layer can be obtained by laminating a pressure-sensitive adhesive layer made of such a pressure-sensitive adhesive on a polarizing plate. The above-mentioned pressure-sensitive adhesive layer-attached polarizing plate preferably further has a release sheet provided on the surface of the pressure-sensitive adhesive layer opposite to the surface on the optical member side.
[0088] Examples of the manufacturing method of the polarizing plate with the pressure-sensitive adhesive layer include [1] a method of applying a pressure-sensitive adhesive composition for polarizing plates onto a polarizing plate, drying the composition, attaching a release sheet, and performing an aging treatment at least at room temperature (23° C.) or at a heated state, and [2] a method of applying a pressure-sensitive adhesive composition for polarizing plates onto a release sheet, drying the composition, attaching a polarizing plate, and performing an aging treatment at least at room temperature (23° C.) or at a heated state, etc. Among these, the method [2] in which aging is performed at room temperature is preferred in that it does not damage the polarizing plate and has excellent adhesion to the polarizing plate.
[0089] Such aging treatment is carried out to balance the adhesive properties as the reaction time of the chemical crosslinking of the adhesive. The aging conditions are a temperature of 20 to 70°C and a time of usually 1 to 30 days, and specific conditions include, for example, 1 to 20 days at 23°C, 3 to 10 days at 23°C, and 1 to 7 days at 40°C.
[0090] When applying the pressure-sensitive adhesive composition for polarizing plates, it is preferable to dilute the pressure-sensitive adhesive composition in a solvent and apply it. The dilution concentration is preferably 5 to 60% by weight, more preferably 10 to 30% by weight in terms of solid content.
[0091] The solvent is not particularly limited as long as it dissolves the pressure-sensitive adhesive composition for polarizing plates, and examples of the solvent that can be used include ester-based solvents such as methyl acetate, ethyl acetate, methyl acetoacetate, and ethyl acetoacetate; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic solvents such as toluene and xylene; and alcohol-based solvents such as methanol, ethanol, and propyl alcohol. Among these, ethyl acetate and methyl ethyl ketone are preferably used in terms of solubility, drying property, cost, and the like. These solvents can be used alone or in combination of two or more.
[0092] The pressure-sensitive adhesive composition can be applied by a conventional method such as roll coating, die coating, gravure coating, comma coating, screen printing, or the like.
[0093] The gel fraction of the pressure-sensitive adhesive layer produced by the above method is preferably 30 to 98% by weight, more preferably 35 to 95% by weight, and even more preferably 50 to 90% by weight, from the viewpoints of durability and suppression of a decrease in the degree of polarization. If the gel fraction is too low, foaming tends to occur in a harsh high-temperature environment, and if it is too high, lifting or peeling tends to occur easily.
[0094] The gel fraction is an indication of the degree of crosslinking (degree of hardening) and is calculated, for example, by the following method. First, the adhesive is picked from the adhesive film on which the adhesive layer is formed. Next, the collected adhesive is wrapped in a 200-mesh SUS wire netting and immersed in ethyl acetate adjusted to 23°C for 24 hours. The weight of the adhesive before immersion in ethyl acetate and the insoluble adhesive components remaining in the wire netting after immersion are weighed, and the weight of the insoluble adhesive components divided by the weight of the adhesive before immersion is taken as the gel fraction (%).
[0095] If the pressure-sensitive adhesive layer produced by the above method has a suitable tackiness when touched with the fingers, it has good wettability when actually applied to an adherend, which tends to improve workability, and is therefore preferable.
[0096] As for the electrical properties of the pressure-sensitive adhesive layer obtained using the pressure-sensitive adhesive composition for polarizing plates of the present invention, it is preferable that the surface resistivity is low as a countermeasure against static electricity, and more preferably 2.0×10 12 Ω / cm 2 More preferably, 2.0×10 11 Ω / cm 2 Less than 2.0×10 is particularly preferable. 10 Ω / cm 2 If the surface resistivity is too high, the adhesive will be easily charged, and therefore, when used for liquid crystal display applications, display unevenness due to static electricity will tend to occur.
[0097] In the present invention, the polarizing plate with the pressure-sensitive adhesive layer is bonded, directly or after peeling off a release sheet in the case where the polarizing plate has the pressure-sensitive adhesive layer, to, for example, a glass substrate of a liquid crystal cell to form a liquid crystal display panel.
[0098] The pressure-sensitive adhesive composition for polarizing plates of the present invention can provide a pressure-sensitive adhesive for polarizing plates that can achieve both high durability and high antistatic performance, for example, in a harsh high-temperature environment of over 100°C, and is therefore useful as a pressure-sensitive adhesive for polarizing plates for bonding a polarizing plate to a liquid crystal cell. In this specification, the term "liquid crystal cell" refers to a cell having a structure in which a liquid crystal material is sandwiched between a pair of substrates and does not have a polarizing plate.
[0099] In general, a polarizing plate has a polyvinyl alcohol (PVA) film in which iodine molecules are adsorbed and aligned, and a protective film for protecting the PVA film. Examples of such a protective film include a triacetyl cellulose film, an acrylic film, a polyethylene film, a polypropylene film, and a cycloolefin film.
[0100] Furthermore, by using the pressure-sensitive adhesive for polarizing plates of the present invention, it is possible to produce an image display device such as a liquid crystal display device by bonding a polarizing plate and a liquid crystal cell, and the obtained image display device can be produced with high precision and has excellent durability. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are by weight.
[0102] First, various acrylic resins (A) were prepared as follows, and other raw materials for the pressure-sensitive adhesive composition were also prepared. The weight average molecular weight, dispersity, and glass transition temperature of the acrylic resins (A) were measured according to the methods described above. The viscosity was measured at 25°C using a Brookfield viscometer.
[0103] <Acrylic resin (A)> The following materials were prepared as raw materials for the acrylic resin (A) (see Table 1).
[0104] [Production of Acrylic Resins (A-1 to A-2, A'-1 to A'-5)] A four-necked round-bottom flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet, and a thermometer was charged with the monomer composition shown in Table 1, and then 50 parts of ethyl acetate, 10 parts of acetone, and 0.01 parts of azobisisobutyronitrile (AIBN) as a polymerization initiator were charged, and the internal temperature was raised to the boiling point to start the reaction. Next, a mixture containing 30 parts of ethyl acetate and 0.01 parts of AIBN was added dropwise while reacting at the reflux temperature for 4 hours, and then the mixture was diluted with ethyl acetate to obtain an acrylic resin solution.
[0105] [Table 1]
[0106] The monomers used above were from the following manufacturers: BA (n-butyl acrylate) (manufactured by Mitsubishi Chemical Corporation, side chain structure has 4 carbon atoms, glass transition temperature -56°C) MA (methyl acrylate) (manufactured by Mitsubishi Chemical Corporation, carbon number in the side chain structure is 1, glass transition temperature is 8°C) 4HBA (4-hydroxybutyl acrylate) (Osaka Organic Chemical Industry Co., Ltd., carbon number of the side chain structure part is 4, glass transition temperature is -32℃) MMA (methyl methacrylate) (manufactured by Mitsubishi Chemical Corporation, carbon number in the side chain structure is 1, glass transition temperature is 105°C) tBMA (t-butyl methacrylate) (Kyoeisha Chemical Co., Ltd., carbon number in the side chain structure is 4, glass transition temperature is 107°C) IBXA (isobornyl acrylate) (Osaka Organic Chemical Industry, carbon number of the side chain structure part is 10, glass transition temperature is 97℃) EMA (Ethyl methacrylate) (Kyoeisha Chemical Co., Ltd., carbon number of the side chain structure part is 2, glass transition temperature 65°C) The above glass transition temperatures are those of homopolymers obtained from the respective monomers.
[0107] <Ionic Compound (B)> The following was prepared as the ionic compound (B). (B-1): Tributylmethylammonium N,N-bis(trifluoromethanesulfonyl)imide (3M, FC-4400) (melting point 27.5° C.)
[0108] <Crosslinking agent (C)> The following was prepared as the crosslinking agent (C). (C-1): Adduct of xylylene diisocyanate and trimethylolpropane (Mitsui Chemicals, Takenate D110N)
[0109] <Silane coupling agent (D)> The following silane coupling agent (D) was prepared. Incidentally, for the type of reactive functional group, reactive functional group equivalent, type of alkoxy group contained, and alkoxy group content of the silane coupling agent (D), catalog values were used unless otherwise specified. (D-1): X-41-1805: manufactured by Shin-Etsu Chemical Co., Ltd., Reactive functional group: mercapto group, Reactive functional group equivalent: 800 g / mol, Alkoxy group: methoxy group and ethoxy group, Alkoxy content: 50%
[0110] <Examples 1 to 4 and Comparative Examples 1 to 5> The above components were mixed as shown in Table 2 below, and the solid content was adjusted with ethyl acetate to obtain a pressure-sensitive adhesive composition for polarizing plates.
[0111] Using the pressure-sensitive adhesive composition for polarizing plates obtained above, evaluation samples were prepared as described below, and the following performances were evaluated. The evaluation results are also shown in Table 2 below.
[0112] [Preparation of polarizing plate with adhesive layer [I]] The obtained pressure-sensitive adhesive composition for polarizing plates was applied to a 38 μm-thick release sheet (Toray, Therapeel WZ) so that the thickness after drying would be 20 μm, and dried for 3 minutes at 100° C. The pressure-sensitive adhesive layer surface on the release sheet was attached to one of the TAC film surfaces of a polarizing plate having a TAC film laminated on both sides of a polarizer, and aged for 7 days in an environment of 23° C. and 50% RH to obtain a polarizing plate with a pressure-sensitive adhesive layer [I] (layer structure: release sheet / pressure-sensitive adhesive layer / TAC film 1 / polarizer / TAC film 2). The above TAC films are triacetyl cellulose films, and the thickness of TAC film 1 is 40 μm, and the thickness of TAC film 2 is 40 μm. The pressure-sensitive adhesive layer-attached polarizing plate [I] was subjected to the following evaluations.
[0113] <Gel fraction> The release sheet of the obtained polarizing plate with an adhesive layer [I] was peeled off, and the adhesive was picked from the adhesive layer surface, wrapped in a 200-mesh SUS wire netting, and then immersed for 24 hours in ethyl acetate adjusted to 23° C. The weight of the adhesive before immersion in ethyl acetate and the insoluble adhesive component remaining in the wire netting after immersion were each weighed, and the weight of the insoluble adhesive component divided by the weight of the adhesive before immersion was taken as the gel fraction (%).
[0114] <Durability: Heat resistance test> The obtained polarizing plate with adhesive layer [I] was cut to 165 mm x 95 mm, the release sheet was peeled off, and the adhesive layer surface was pressed against alkali-free glass (Corning Eagle XG, thickness 1.1 mm) and laminated by rolling twice back and forth with a 2 kg roller. After that, the plate was autoclaved (0.5 MPa x 50°C x 20 minutes) to prepare a sample for durability evaluation. The obtained samples were exposed to various conditions for heat resistance (95°C x 500 hours or 105°C x 500 hours) and then evaluated according to the following criteria. (Evaluation Criteria) ◎ No bubbles are observed on the entire surface of the polarizing plate or lifting at the edges. ◯: Only a very slight lift was observed at the corners of the polarizing plate. △: Slight lifting is observed at the edge of the polarizing plate. ×: Bubbles are observed over the entire surface of the polarizing plate, or floating of 1 mm or more is observed at the edges.
[0115] <Antistatic performance: Surface resistivity> The above-mentioned polarizing plate [I] with the adhesive layer was left to stand for 24 hours under an atmosphere of 23°C x 50% RH, after which the release sheet of the adhesive layer was removed, and the surface resistivity (Ω / cm 2 ) was measured.
[0116] [Table 2]
[0117] The pressure-sensitive adhesive compositions for polarizing plates of Examples 1 to 4, which use methyl methacrylate as a copolymerizable monomer having a high glass transition temperature of the homopolymer as a copolymerization component and further contain acrylic resins (A-1 to A-2) in which the average carbon number (α) of the side chain structure portion of the acrylic resin is adjusted within a predetermined range, all have excellent antistatic performance and are highly durable even in extremely harsh high-temperature environments such as not only 95°C but also 105°C.
[0118] On the other hand, the pressure-sensitive adhesive composition for polarizing plates of Comparative Example 1, which contains an acrylic resin (A'-1) that is not copolymerized with a copolymerizable monomer having a high glass transition temperature, and the pressure-sensitive adhesive compositions for polarizing plates of Comparative Examples 2 and 3, which contain acrylic resins (A'-2 to A'-3) copolymerized with a copolymerizable monomer having a high glass transition temperature other than methyl methacrylate, all showed poor durability at 105°C. In addition, the adhesive composition for polarizing plates of Comparative Example 4, which contains an acrylic resin (A'-4) copolymerized with a copolymerizable monomer other than methyl methacrylate as a copolymerizable monomer having a high glass transition temperature, although the average carbon number (α) of the side chain structure portion of the acrylic resin is 3.3 or less, also showed poor durability at 105°C. In addition, the adhesive composition for polarizing plates of Comparative Example 5, which contains an acrylic resin (A'-5) in which methyl methacrylate is copolymerized as a copolymerizable monomer with a high glass transition temperature but in which the average carbon number (α) of the side chain structure portion exceeds 3.3, also showed poor durability at 105°C. Therefore, it can be seen that a pressure-sensitive adhesive obtained using a pressure-sensitive adhesive composition for polarizing plates containing an acrylic resin (A) which contains a structural portion derived from methyl methacrylate and in which the average carbon number (α) of the side chain structural portion of the acrylic resin (A) is 3.3 or less can completely solve the problems of the present invention, has excellent antistatic performance, and has high durability in harsh high-temperature environments, for example, at temperatures exceeding 100°C.
[0119] In addition, since a polarizing plate with a pressure-sensitive adhesive layer obtained using the pressure-sensitive adhesive composition for polarizing plates of the present invention has both high durability and high antistatic performance, an image display device obtained by bonding a polarizing plate and an image display member such as a liquid crystal cell via the pressure-sensitive adhesive layer will be of excellent quality. [Industrial Applicability]
[0120] The adhesive composition for polarizing plates of the present invention is useful as an adhesive for polarizing plates for bonding a polarizing plate to a glass substrate of a liquid crystal cell, a substrate having a conductive layer, etc. For example, in the manufacturing process of a liquid crystal display device, by using the adhesive composition for polarizing plates of the present invention for bonding a protective film of a polarizing plate to a metal surface of a glass substrate of a liquid crystal cell, a conductive layer, etc., the adhesive composition for polarizing plates of the present invention exhibits excellent durability in a harsh high-temperature environment of, for example, more than 100°C, and also has excellent antistatic properties.
Claims
1. A pressure-sensitive adhesive composition for polarizing plates, comprising an acrylic resin (A) and an ionic compound (B), The acrylic resin (A) contains a structural portion derived from methyl methacrylate and a structural portion derived from a polar group-containing monomer, the content of the methyl methacrylate is 5 to 30% by weight based on the total weight of the polymer components constituting the acrylic resin (A); the polar group-containing monomer contains a hydroxyl group-containing monomer, and the content of the hydroxyl group-containing monomer is 3 to 10% by weight based on all polymerization components constituting the acrylic resin (A); the average number of carbon atoms (α) of the side chain structural moieties of the acrylic resin (A) is 3.3 or less, The ionic compound (B) is a compound comprising a cationic component and an anionic component, The anion components are Cl - , Br - , I - , AlCl 4 - , Al 2 Cl 7 - , BF 4 - , PF 6 -, ClO 4 -, NO 3 -, CH 3 COO -, CF 3 COO -, CH 3 SO 3 -, CF 3 SO 3 -. , (CF3SO2)3C-, AsF6-, SbF6-, NbF6-, TaF6-, (C2O4)2B-, SCN-, (CN)2N-, C4F9SO3-, C3F7COO- , (CF3SO2)(CF3CO)N-, -O3S(CF 2) 3SO3- and an anion selected from the group consisting of anions represented by the following general formulas (1) to (4): (1): (C n F 2n+1 SO 2 ) 2 N - (wherein n is an integer from 1 to 10); (2): CF2(CmF2mSO2)2N- (wherein m is an integer from 1 to 10); (3): O 3 S(CF 2 ) l SO 3 − (wherein l is an integer from 1 to 10); (4): (C p F 2p+1 SO 2 )N - (C q F 2q+1 SO 2 ) (wherein p and q are integers from 1 to 10) a pressure-sensitive adhesive composition for polarizing plates, characterized in that a content of an acrylic resin component other than the acrylic resin (A) is 5 parts by weight or less per 100 parts by weight (solid content) of the acrylic resin (A).
2. The adhesive composition for polarizing plates described in claim 1, characterized in that the cationic component is a cation selected from alkali metal cations, pyridinium cations, piperidinium cations, pyrrolidinium cations, cations having a pyrroline skeleton, cations having a pyrrole skeleton, imidazolium cations, tetrahydropyrimidinium cations, dihydropyrimidinium cations, pyrazolium cations, pyrazolinium cations, tetraalkylammonium cations, trialkylsulfonium cations, and tetraalkylphosphonium cations.
3. 3. The pressure-sensitive adhesive composition for polarizing plates according to claim 1, wherein the content of the polar group-containing monomer is 3 to 30% by weight based on the total polymer components constituting the acrylic resin (A).
4. The pressure-sensitive adhesive composition for polarizing plates according to any one of claims 1 to 3, characterized in that the content of the ionic compound (B) is 1 to 30 parts by weight based on 100 parts by weight of the acrylic resin (A).
5. The pressure-sensitive adhesive composition for polarizing plates according to any one of claims 1 to 4, further comprising a crosslinking agent (C).
6. The pressure-sensitive adhesive composition for polarizing plates according to any one of claims 1 to 5, further comprising a silane coupling agent (D).
7. 7. A pressure-sensitive adhesive for polarizing plates, comprising the pressure-sensitive adhesive composition for polarizing plates according to claim 1, which is crosslinked.
8. 8. An image display device comprising a polarizing plate and a liquid crystal cell bonded together with the pressure-sensitive adhesive for polarizing plates according to claim 7.
Citation Information
Patent Citations
Antistatic acrylic pressure-sensitive adhesive and antistatic pressure-sensitive adhesive film using the same
JP2009084541A
Antistatic acrylic pressure-sensitive adhesive and antistatic pressure-sensitive adhesive film using the same
JP2009173721A
Self-adhesive layer for optical film and method for producing the same, optical film with self-adhesive layer, and image display
JP2012087290A
Optical formed body
JP2014051601A
Adhesive composition for polarizing plate, adhesive layer, adhesive sheet and polarizing plate with adhesive layer
JP2015206858A