Optical film manufacturing method
A method for manufacturing optical films using crystalline alicyclic polymers addresses crack issues by controlling surface energy and applying a second resin layer, ensuring strong adhesion and reduced haze.
Patent Information
- Application Number
- JP2020143642
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-27
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-08-27
AI Technical Summary
Cracks occur in resin layers during the crystallization process when forming films with crystalline alicyclic structure-containing polymers due to the heat applied, compromising the adhesion strength between resin layers.
A manufacturing method involving a crystallization treatment followed by applying a second resin layer, with specific surface energy and hydrogen bond component differences, and optionally a hydrophilic treatment, to form an optical film that suppresses cracks in the resin layer.
The method effectively prevents cracks in the resin layer while maintaining high adhesion strength, resulting in an optical film with improved mechanical properties and reduced haze.
Smart Images

Figure 0007552147000002 
Figure 0007552147000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an optical film. [Background technology]
[0002] Although the alicyclic structure-containing polymer generally does not have crystallinity, some of the alicyclic structure-containing polymers may have crystallinity. The applicant has previously proposed a technique for producing a film using a crystalline alicyclic structure-containing polymer (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 079627 [Patent Document 2] International Publication No. 2019 / 003980 Summary of the Invention [Problem to be solved by the invention]
[0004] Resins containing crystalline alicyclic structure-containing polymers can usually improve the physical properties of the resins by promoting the crystallization of the alicyclic structure-containing polymers. Therefore, when a film is produced using a resin containing crystalline alicyclic structure-containing polymers, the production method may include a crystallization treatment to increase the crystallinity of the alicyclic structure-containing polymers contained in the film. Such crystallization treatment is generally carried out by heating.
[0005] By the way, when a film is manufactured using a resin containing a crystalline alicyclic structure-containing polymer, it may be desired to form a resin layer using another resin on the layer of the resin containing a crystalline alicyclic structure-containing polymer.In this case, in order to increase the adhesive strength between the layer of the resin containing a crystalline alicyclic structure-containing polymer and the resin layer formed on the layer, it is common to perform a crystallization process after forming a resin layer on the layer of the resin containing a crystalline alicyclic structure-containing polymer.However, in this case, the heat applied during the crystallization process may cause cracks in the resin layer.
[0006] The present invention has been devised in view of the above-mentioned problems, and an object of the present invention is to provide a method for producing an optical film comprising a resin layer (A) formed of a resin containing a crystalline alicyclic structure-containing polymer and a resin layer (B) formed on the resin layer (A), while suppressing cracks in the resin layer (B). [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by a production method including, in this order, a step of preparing a resin layer (A) formed of a first resin containing a crystalline alicyclic structure-containing polymer, a step of subjecting the resin layer (A) to a crystallization treatment, and a step of forming a resin layer (B) on the surface of the resin layer (A) of a second resin, thereby completing the present invention. That is, the present invention includes the following.
[0008] [1] A step (I) of preparing a resin layer (A) formed of a first resin containing a crystalline alicyclic structure-containing polymer; A step (II) of subjecting the resin layer (A) to a crystallization treatment; and (III) forming a resin layer (B) from a second resin on the surface of the resin layer (A). [2] the surface free energy γ(A) of the surface of the resin layer (A) in the step (III); The hydrogen bond component γ of the surface free energy γ(A) h (A), The surface free energy γ(B) of the resin layer (B) formed in the step (III), and The hydrogen bond component γ of the surface free energy γ(B) h The method for producing an optical film according to [1], wherein (B) satisfies the following formulas (1) and (2): 10mJ / m 2 ≦ γ(A)-γ(B) ≦ 40mJ / m 2 (1) 5mJ / m 2 ≦ γ h (A)-γ h (B) ≦ 20mJ / m 2 (2) [3] The method for producing an optical film according to [1] or [2], further comprising a step (IV) between the step (II) and the step (III) of subjecting the surface of the resin layer (A) to a hydrophilization treatment. [4] The method for producing an optical film according to any one of [1] to [3], wherein the step (III) includes a step (III-1) of applying a coating liquid containing the second resin to the surface of the resin layer (A). [5] The method for producing an optical film according to any one of [1] to [4], wherein the alicyclic structure-containing polymer is a hydrogenated product of a ring-opening polymer of dicyclopentadiene. [6] The method for producing an optical film according to any one of [1] to [5], wherein the alicyclic structure-containing polymer contained in the optical film has a crystallinity of 30% or more. Effect of the Invention
[0009] According to the present invention, there can be provided a production method for producing an optical film comprising a resin layer (A) formed of a resin containing a crystalline alicyclic structure-containing polymer and a resin layer (B) formed on the resin layer (A), while suppressing cracks in the resin layer (B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0011] In the following description, a "long" film refers to a film having a length of 5 times or more its width, preferably 10 times or more its width, specifically a film having a length long enough to be wound into a roll for storage or transportation. The upper limit of the ratio of the length to the width of the film is not particularly limited, but may be, for example, 100,000 times or less.
[0012] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effect of the present invention, for example, within a range of ±5°.
[0013] [1. Overview of optical film manufacturing method] A method for producing an optical film according to one embodiment of the present invention includes the steps of: A step (I) of preparing a resin layer (A) formed of a first resin containing a crystalline alicyclic structure-containing polymer; A step (II) of subjecting the resin layer (A) to a crystallization treatment; (III) forming a resin layer (B) on a surface of the resin layer (A) using a second resin; In the following description, the alicyclic structure-containing polymer having crystallinity may be referred to as a "crystalline alicyclic polymer".
[0014] According to the above-mentioned manufacturing method, an optical film including a resin layer (A) and a resin layer (B) can be manufactured while suppressing cracks in the resin layer (B). In the manufactured optical film, the resin layer (A) and the resin layer (B) are usually in direct contact with each other. Unless otherwise specified, the fact that the two layers are in "direct" contact means that there is no other layer between the two layers.
[0015] [2. Step (I) of preparing a resin layer (A)] In step (I), a resin layer (A) formed of a first resin is prepared. The first resin is usually a thermoplastic resin, and contains a crystalline alicyclic polymer.
[0016] As described above, the crystalline alicyclic polymer refers to a polymer containing an alicyclic structure having crystallinity. The alicyclic structure-containing polymer refers to a polymer containing an alicyclic structure in the molecule. The polymer containing an alicyclic structure may be, for example, a polymer obtained by a polymerization reaction using a cyclic olefin as a monomer, or a hydrogenated product thereof. In addition, the "polymer having crystallinity" refers to a polymer having a melting point Tm [i.e., the melting point can be observed by a differential scanning calorimeter (DSC)]. Therefore, the crystalline alicyclic polymer may be a polymer containing an alicyclic structure in the molecule and having a melting point Tm. By using such a crystalline alicyclic polymer, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability and light weight of the optical film can be improved.
[0017] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure. Among these, the cycloalkane structure is preferred because it is easy to obtain an optical film having excellent properties such as thermal stability. The number of carbon atoms contained in one alicyclic structure is preferably 4 or more, more preferably 5 or more, and preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less. When the number of carbon atoms contained in one alicyclic structure is within the above range, mechanical strength, heat resistance, and moldability are highly balanced.
[0018] In the crystalline alicyclic polymer, the ratio of the structural unit containing an alicyclic structure to all structural units is preferably 30% by weight or more, more preferably 50% by weight or more, and particularly preferably 70% by weight or more. When the ratio of the structural unit containing an alicyclic structure is high as described above, the heat resistance can be improved. The ratio of the structural unit containing an alicyclic structure to all structural units can be 100% by weight or less. In addition, in the crystalline alicyclic polymer, the remainder other than the structural unit containing an alicyclic structure is not particularly limited and can be appropriately selected according to the purpose of use.
[0019] Examples of the crystalline alicyclic polymer include the following polymers (α) to (δ): Among these, polymer (β) is preferred because it is easy to obtain an optical film having excellent heat resistance and flexibility. Polymer (α): A ring-opening polymer of a cyclic olefin monomer, which has crystallinity. Polymer (β): A hydrogenated product of polymer (α) and has crystallinity. Polymer (γ): An addition polymer of a cyclic olefin monomer, which has crystallinity. Polymer (δ): A hydrogenated polymer (γ) having crystallinity.
[0020] Specifically, the crystalline alicyclic polymer is preferably a dicyclopentadiene ring-opening polymer having crystallinity, and a dicyclopentadiene ring-opening polymer hydrogenated product having crystallinity. Among them, a dicyclopentadiene ring-opening polymer hydrogenated product having crystallinity is particularly preferred. Here, the dicyclopentadiene ring-opening polymer refers to a polymer in which the ratio of dicyclopentadiene-derived structural units to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.
[0021] The hydrogenated ring-opening polymer of dicyclopentadiene preferably has a high ratio of racemo dyads. Specifically, the ratio of racemo dyads in the repeating units of the hydrogenated ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high ratio of racemo dyads indicates high syndiotactic stereoregularity. Therefore, the higher the ratio of racemo dyads, the higher the melting point of the hydrogenated ring-opening polymer of dicyclopentadiene tends to be. The ratio of racemo-dyads is described in the Examples below. 13 It can be determined based on C-NMR spectrum analysis.
[0022] As the polymer (α) to polymer (δ), polymers obtained by the production methods disclosed in WO 2018 / 062067 and WO 2018 / 079627 can be used.
[0023] The melting point Tm of the crystalline alicyclic polymer is preferably 200° C. or higher, more preferably 230° C. or higher, and preferably 290° C. or lower. When a crystalline alicyclic polymer having such a melting point Tm is used, an optical film having an even better balance between moldability and heat resistance can be obtained.
[0024] Generally, the crystalline alicyclic polymer has a glass transition temperature Tg. The specific glass transition temperature Tg of the crystalline alicyclic polymer is not particularly limited, but is generally 85°C or higher and generally 170°C or lower.
[0025] Since the crystalline alicyclic polymer has crystallinity, crystallization proceeds at a specific temperature. In this case, the temperature at which the crystallization rate is the fastest is sometimes called the "crystallization temperature". The crystallization temperature Tpc of the crystalline alicyclic polymer is preferably 100°C or higher, more preferably 130°C or higher, particularly preferably 160°C or higher, and preferably 230°C or lower, more preferably 210°C or lower, particularly preferably 190°C or lower.
[0026] The melting point Tm, glass transition temperature Tg, and crystallization temperature Tpc of a polymer can be measured by the following method. First, the polymer is melted by heating, and the melted polymer is quenched with liquid nitrogen. Then, using this polymer as a test specimen, the melting point Tm, glass transition temperature Tg, and crystallization temperature Tpc of the polymer can be measured at a heating rate of 10° C. / min (heating mode) using a differential scanning calorimeter (DSC).
[0027] The weight average molecular weight (Mw) of the crystalline alicyclic polymer is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. A crystalline alicyclic polymer having such a weight average molecular weight has an excellent balance between moldability and heat resistance.
[0028] The molecular weight distribution (Mw / Mn) of the crystalline alicyclic polymer is preferably 1.0 or more, more preferably 1.5 or more, and is preferably 4.0 or less, more preferably 3.5 or less. Here, Mn represents the number average molecular weight. The crystalline alicyclic polymer having such a molecular weight distribution has excellent moldability.
[0029] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer can be measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a developing solvent.
[0030] The crystallinity of the crystalline alicyclic polymer contained in the resin layer (A) prepared in step (I) is not particularly limited. Since the crystallinity of the crystalline alicyclic polymer can be increased by the crystallization treatment performed in step (II), even if the crystallinity of the crystalline alicyclic polymer contained in the resin layer (A) prepared in step (I) is low, an optical film containing a crystalline alicyclic polymer having a preferred crystallinity can be obtained according to the manufacturing method of this embodiment. The specific range of the crystallinity of the crystalline alicyclic polymer contained in the resin layer (A) prepared in step (I) is preferably 10% or less, more preferably 5% or less, and particularly preferably 3% or less, from the viewpoint of simplifying the manufacturing method of the optical film by omitting the steps for increasing the crystallinity other than step (II).
[0031] The degree of crystallinity is an index showing the proportion of crystallized crystalline alicyclic polymers contained in the first resin. The degree of crystallinity can be measured by X-ray diffraction. Specifically, in accordance with JIS K0131, the diffracted X-ray intensity from the crystalline portion is measured using a wide-angle X-ray diffractometer (e.g., Rigaku's "RINT 2000"), and the crystallinity can be calculated from the ratio to the total diffracted X-ray intensity according to the following formula (I). Xc=K·Ic / It (I) In the above formula (I), Xc represents the crystallinity of the test sample, Ic represents the diffracted X-ray intensity from the crystalline portion, It represents the total diffracted X-ray intensity, and K represents a correction term.
[0032] The crystalline alicyclic polymer may be used alone or in combination of two or more kinds in any ratio.
[0033] The proportion of the crystalline alicyclic polymer in the first resin is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the proportion of the crystalline alicyclic polymer is equal to or more than the lower limit of the above range, the birefringence expression and heat resistance of the optical film can be improved. The upper limit of the proportion of the crystalline alicyclic polymer can be 100% by weight or less.
[0034] The first resin may contain optional components in addition to the crystalline alicyclic polymer. Examples of the optional components include antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; light stabilizers such as hindered amine-based light stabilizers; waxes such as petroleum wax, Fischer-Tropsch wax, and polyalkylene wax; nucleating agents such as sorbitol-based compounds, metal salts of organic phosphoric acids, metal salts of organic carboxylic acids, kaolin, and talc; diaminostilbene derivatives, coumarin derivatives, and azole-based derivatives (e.g., benzoxazole derivatives, benzotriazole derivatives, and benzimidazoline derivatives); Examples of the optional components include fluorescent brighteners such as benzothiazole derivatives, carbazole derivatives, pyridine derivatives, naphthalic acid derivatives, and imidazolone derivatives; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, and benzotriazole-based ultraviolet absorbers; inorganic fillers such as talc, silica, calcium carbonate, and glass fibers; colorants; flame retardants; flame retardant assistants; antistatic agents; plasticizers; near-infrared absorbers; lubricants; fillers; and any polymer other than a crystalline alicyclic polymer, such as a soft polymer. One type of optional component may be used alone, or two or more types may be used in combination at any ratio.
[0035] The resin layer (A) is usually prepared as a film formed from the first resin. The resin layer (A) may be prepared by purchasing from the market, or may be prepared by manufacturing from the first resin. For example, a resin molding method for molding the first resin into a film shape may be mentioned as a method for manufacturing the resin layer (A) from the first resin. For example, the resin molding method may be injection molding, extrusion molding, press molding, inflation molding, blow molding, calendar molding, cast molding, compression molding, etc., and among them, the extrusion molding method is preferred because it is easy to control the thickness.
[0036] The manufacturing conditions in the extrusion molding method are preferably as follows. The cylinder temperature (molten resin temperature) is preferably Tm or higher, more preferably "Tm+20°C" or higher, and preferably "Tm+100°C" or lower, more preferably "Tm+50°C" or lower. The cooling body that the molten resin extruded into a film first comes into contact with is not particularly limited, but a cast roll is usually used. The cast roll temperature is preferably "Tg-50°C" or higher, more preferably "Tg-30°C" or higher, preferably "Tg+70°C" or lower, more preferably "Tg+40°C" or lower, even more preferably Tg or lower, and particularly preferably "Tg-15°C" or lower. Furthermore, the cooling roll temperature is preferably "Tg-70°C" or higher, more preferably "Tg-50°C" or higher, and preferably "Tg+60°C" or lower, more preferably "Tg+30°C" or lower. When the resin layer (A) is manufactured under such conditions, the resin layer (A) having a thickness of 1 μm to 1 mm can be easily manufactured. Here, "Tm" represents the melting point of the crystalline alicyclic polymer, and "Tg" represents the glass transition temperature of the crystalline alicyclic polymer.
[0037] Step (I) may include a step of performing a preheating treatment to heat the resin layer (A) to a stretching temperature after preparing the resin layer (A) and before stretching the resin layer (A). Usually, the preheating temperature and the stretching temperature are the same, but they may be different. The preheating temperature is preferably T1-10°C or higher, more preferably T1-5°C or higher, and is preferably T1+5°C or lower, more preferably T1+2°C or lower, relative to the stretching temperature T1. The preheating time is optional, and is preferably 1 second or higher, more preferably 5 seconds or higher, and is preferably 60 seconds or lower, more preferably 30 seconds or lower.
[0038] Step (I) may include a step of preparing a resin layer (A), optionally preheating the resin layer (A), and then stretching the resin layer (A). Usually, the molecules of the crystalline alicyclic polymer contained in the resin layer (A) can be oriented in a direction corresponding to the stretching direction by stretching. In the following description, the film-like resin layer (A) before stretching may be called a "film before stretching" and the film after stretching may be called a "stretched film".
[0039] There is no limitation on the stretching direction, and examples thereof include the longitudinal direction, the width direction, and the oblique direction. Here, the oblique direction refers to a direction perpendicular to the thickness direction, and is neither parallel nor perpendicular to the width direction. The stretching direction may be one direction or two or more directions. Thus, examples of the stretching method include uniaxial stretching methods such as a method of uniaxially stretching a pre-stretched film in the longitudinal direction (longitudinal uniaxial stretching method) and a method of uniaxially stretching a pre-stretched film in the width direction (transverse uniaxial stretching method); biaxial stretching methods such as a simultaneous biaxial stretching method in which a pre-stretched film is stretched in the longitudinal direction and simultaneously stretched in the width direction, and a sequential biaxial stretching method in which a pre-stretched film is stretched in one of the longitudinal direction and the width direction and then stretched in the other direction; and a method of stretching a pre-stretched film in an oblique direction (oblique stretching method).
[0040] The stretching ratio is preferably 1.1 times or more, more preferably 1.2 times or more, and preferably 20.0 times or less, more preferably 10.0 times or less, even more preferably 5.0 times or less, and particularly preferably 2.0 times or less. For example, when stretching is performed in a plurality of different directions such as a biaxial stretching method, the stretching ratio refers to a total stretching ratio represented by the product of the stretching ratios in each stretching direction. It is desirable to appropriately set a specific stretching ratio according to factors such as the optical properties, thickness, and strength of the optical film to be produced. When the stretching ratio is equal to or greater than the lower limit of the above range, the birefringence can be significantly changed by stretching. Also, when the stretching ratio is equal to or less than the upper limit of the above range, the direction of the slow axis can be easily controlled and the breakage of the film can be effectively suppressed.
[0041] The stretching temperature is preferably "Tg-30°C" or higher, more preferably "Tg-10°C" or higher, even more preferably "Tg+5°C" or higher, particularly preferably "Tg+10°C" or higher, and is preferably "Tg+100°C" or lower, more preferably "Tg+90°C" or lower, even more preferably "Tg+60°C" or lower, and particularly preferably "Tg+50°C" or lower. Here, "Tg" represents the glass transition temperature of the crystalline alicyclic polymer. When the stretching temperature is equal to or higher than the lower limit of the above range, the first resin can be sufficiently softened to perform uniform stretching. When the stretching temperature is equal to or lower than the upper limit of the above range, the hardening of the first resin due to the progress of crystallization of the crystalline alicyclic polymer can be suppressed, so that the stretching can be performed smoothly, and large birefringence can be expressed by stretching.
[0042] [3. Step (II) of subjecting the resin layer (A) to a crystallization treatment] After preparing the resin layer (A) in step (I), step (II) is performed. In step (II), the resin layer (A) is subjected to a crystallization treatment. The crystallization treatment can increase the crystallinity of the crystalline alicyclic polymer contained in the resin layer (A).
[0043] As the crystallization treatment, any method capable of increasing the crystallinity of the crystalline alicyclic polymer contained in the resin layer (A) can be adopted. Among them, as the crystallization treatment, a heat treatment in which the temperature of the resin layer (A) is adjusted to a predetermined heating temperature is preferred.
[0044] The heating temperature in the heat treatment can be set in a temperature range of the glass transition temperature Tg or more and the melting point Tm or less of the crystalline alicyclic polymer. The specific heating temperature range is preferably Tg+20°C or more, more preferably Tg+30°C or more, and preferably Tm or less, more preferably Tm-20°C or less, and even more preferably Tm-40°C or less. The heating temperature is preferably close to the crystallization temperature Tpc of the crystalline alicyclic polymer, and is particularly preferably in the range of Tpc-10°C to Tpc+10°C. In step (II), the heating temperature may vary within the above range, but is preferably constant. When the heating temperature is equal to or more than the lower limit of the above range, the crystallization of the crystalline alicyclic polymer can be effectively promoted to enhance the heat resistance of the film. When the heating temperature is equal to or less than the upper limit of the above range, the haze of the resin layer (A) can be reduced, and an optical film with low haze can be obtained.
[0045] The heating device used in the heat treatment is preferably a heating device capable of increasing the atmospheric temperature of the resin layer (A) since no contact between the heating device and the resin layer (A) is required. Specific examples of suitable heating devices include an oven and a heating furnace.
[0046] In step (II), the crystallization time for maintaining the resin layer (A) in the above heating temperature range is preferably 1 second or more, more preferably 5 seconds or more, even more preferably 10 seconds or more, particularly preferably 20 seconds or more, and preferably 30 minutes or less, more preferably 10 minutes or less, even more preferably 50 seconds or less, particularly preferably 30 seconds or less. When the crystallization time is equal to or more than the lower limit of the above range, the crystallization of the crystalline alicyclic polymer can be sufficiently advanced, and the heat resistance of the optical film can be improved. When the crystallization time is equal to or less than the upper limit of the above range, the haze of the resin layer (A) can be reduced, and an optical film with low haze can be obtained.
[0047] The crystallization treatment is preferably performed in a state where at least two sides of the resin layer (A) are held. "A state where at least two sides of the resin layer (A) are held" refers to a state where the resin layer (A) is held by a holder to an extent that no bending is observed in the resin layer (A). However, this state does not include a holding state where the resin layer (A) is substantially stretched. In addition, "substantially stretched" refers to a stretching ratio of the resin layer (A) in any direction usually being 1.1 times or more. When the crystallization treatment is performed in a state where at least two sides of the resin layer (A) are held, the resin layer (A) is in a tensed state where tension is applied, so that shrinkage and bending are suppressed. Therefore, the resin layer (A) is maintained flat, so that deformation such as waving and wrinkles can be suppressed, and a resin layer (A) having a flat shape can be obtained. The mode of the crystallization treatment in a state in which at least two sides of the resin layer (A) are held may be the same as the modes described in, for example, WO 2018 / 061841 and WO 2018 / 079627.
[0048] [4. Step (IV) of subjecting the resin layer (A) to hydrophilic treatment] The method for producing an optical film according to an embodiment of the present invention preferably includes a step (IV) of subjecting the surface of the resin layer (A) to a hydrophilic treatment between the steps (II) and (III). The hydrophilic treatment usually enhances the adhesive strength between the resin layer (A) and the resin layer (B).
[0049] Examples of hydrophilic treatments include corona treatment, plasma treatment, electron beam irradiation treatment, ultraviolet irradiation treatment, and chemical treatment. By subjecting the surface of the resin layer (A) to these hydrophilic treatments, hydrophilic groups such as hydroxyl groups, carboxyl groups, and carbonyl groups are usually generated on the surface. Thus, the hydrophilicity of the surface of the resin layer (A) can be improved. Furthermore, the hydrophilic treatments usually allow the surface free energy of the surface of the resin layer (A) to be adjusted. Among the hydrophilic treatments, corona treatment and plasma treatment are preferred from the viewpoint of treatment efficiency, and corona treatment is particularly preferred.
[0050] In corona treatment, a corona is usually generated by applying a high voltage at a high frequency between a dielectric and an insulated electrode, and the surface of the resin layer (A) is treated by passing the resin layer (A) between the dielectric and the electrode. In general, the surface free energy of the surface that has been subjected to corona treatment is adjusted according to the type of electrode, electrode spacing, voltage, humidity, and the type of resin layer (A) to be treated.
[0051] The treatment conditions of the corona treatment are preferably set so as to increase the adhesive strength between the resin layer (A) and the resin layer (B). In one embodiment, the distance between the electrode and the resin layer (A) is preferably 0.5 mm to 10 mm, more preferably 1 mm to 5 mm, and particularly preferably 1 mm to 3 mm. The conveying speed of the resin layer (A) to be subjected to the corona treatment is preferably 0.01 m / min to 20 m / min, and more preferably 0.05 m / min to 10 m / min. The electrode length is preferably 0.1 m to 2 m. The corona output is preferably 20 W or more, more preferably 40 W or more, and particularly preferably 100 W or more, and from the viewpoint of suppressing damage to the resin layer (A), it is preferably 5 kW or less, more preferably 3 kW or less, and particularly preferably 1.5 kW or less. In the corona treatment performed while conveying the resin layer (A), the treatment intensity is calculated by "treatment intensity = (output) / (conveying speed x electrode length)". This treatment intensity is preferably 1 W·min / m 2 More than 10W·min / m 2 More than 100 W·min / m 2 More than 2000W·min / m 2 Less than or equal to 1000W·min / m 2 Less than 800W·min / m is especially preferable. 2 The following is the result.
[0052] In particular, from the viewpoint of effectively increasing the adhesive strength between the resin layer (A) and the resin layer (B), the treatment conditions for the hydrophilization treatment described above are preferably set so that the surface of the resin layer (A) has a surface free energy that satisfies the formulas (1) and (2) described below. Therefore, the specific treatment conditions for the hydrophilization treatment are preferably set depending on the composition of the second resin forming the resin layer (B).
[0053] [5. Step (III) of forming resin layer (B) on the surface of resin layer (A)] In the method for producing an optical film according to one embodiment of the present invention, step (III) is carried out after step (II). In step (III), a resin layer (B) is formed on the surface of the resin layer (A) using a second resin. In addition, when the method for producing an optical film includes step (IV), step (III) is carried out after step (IV). In this case, the resin layer (B) is usually formed on the hydrophilized surface of the resin layer (A).
[0054] The second resin may be a resin having a different composition from the first resin. Among them, the second resin is preferably a resin that satisfies specific requirements regarding surface free energy. Specifically, the second resin is preferably one that satisfies the requirements represented by the following formulas (1) and (2). 10mJ / m 2 ≦ γ(A)-γ(B) ≦ 40mJ / m 2 (1) 5mJ / m 2 ≦ γ h (A)-γ h (B) ≦ 20mJ / m 2 (2) (γ(A) represents the surface free energy of the surface of the resin layer (A) on which the resin layer (B) is formed in the step (III), Gamma h (A) represents the hydrogen bond component of the surface free energy γ(A), γ(B) represents the surface free energy of the resin layer (B) formed in step (III); Gamma h (B) represents the hydrogen bond component of the surface free energy γ(B).
[0055] The significance of the requirements expressed by formulas (1) and (2) will be explained below. According to the theory of Kitazaki and Hata, the surface free energy of a solid, γ SV is expressed by the following formula (3), and the surface free energy of the liquid γ LV is expressed by the following formula (4), and the adhesion work between the solid and the liquid WSL is expressed by equation (5). By applying the relationship in equation (5) to the Young-Dupre equation expressed by equation (6), equation (7) is derived. Here, γ SV d , γ SV p and γ SV h is the surface free energy of the solid, γ SV represents the dispersion component, polar component, and hydrogen bond component of γ LV d , γ LV p and γ LV h is the surface free energy of the liquid, γ LV represents the dispersion component, polar component, and hydrogen bonding component of the solid. θ represents the contact angle of the liquid with the solid.
[0056]
number
[0057] According to the Kitazaki-Hata theory, the surface free energy γ(A) of the surface of the resin layer (A) on which the resin layer (B) is formed in the step (III) is calculated by dividing the surface free energy γ(A) by its dispersion component γ d (A), polar component γ p (A) and hydrogen bond component γ h The surface free energy γ(B) of the resin layer (B) formed in step (III) is expressed by the following formula (8) based on (A). d (B), polar component γ p (B) and hydrogen bond component γ h (B) is expressed by the following formula (9). γ(A)=γ d (A)+γ p (A)+γ h (A) (8) γ(B)=γ d (B)+γ p (B)+γ h (B) (9)
[0058] Therefore, "γ(A)-γ(B)" in the above formula (1) represents the difference between the surface free energy of the surface of the resin layer (A) and the surface free energy of the resin layer (B) in contact with that surface. h (A)-γ h (B)" represents the difference between the hydrogen bond component of the surface free energy of the surface of resin layer (A) and the hydrogen bond component of the surface free energy of resin layer (B) in contact with that surface.
[0059] Therefore, formula (1) indicates that the difference in surface free energy Δγ (=γ(A)-γ(B)) between the surfaces in contact at the interface between resin layer (A) and resin layer (B) is within a specific range. Also, formula (2) indicates that the difference in surface free energy hydrogen bond components Δγ h (=γ h (A)-γ h (B)) is within a specific range. According to what the present inventors have found through repeated experiments, when the requirements represented by the above formulas (1) and (2) are satisfied, the adhesive strength between the resin layer (A) and the resin layer (B) can be significantly increased. According to the inventors' experiments, no correlation was found between the dispersion component and the polar component of the surface free energy and the adhesive strength, so it is presumed that the surface free energy and its hydrogen bond component have a specific action that affects the adhesive strength.
[0060] Formula (1) will be explained in more detail. From the viewpoint of significantly increasing the adhesive strength between the resin layer (A) and the resin layer (B), the difference in surface free energy Δγ (=γ(A)-γ(B)) represented by formula (1) is preferably 10 mJ / m 2 More preferably, 12 mJ / m 2 More preferably, 14 mJ / m 2 or more, preferably 40 mJ / m 2 Less than or equal to 38 mJ / m 2 Less than 35 mJ / m, particularly preferably 35 mJ / m 2 The following is the result.
[0061] Formula (2) will be described in more detail. From the viewpoint of significantly increasing the adhesive strength between the resin layer (A) and the resin layer (B), the difference Δγ in the hydrogen bond component of the surface free energy represented by formula (2) is h (=γ h (A)-γ h (B)) is preferably 5 mJ / m 2 More preferably, 6 mJ / m 2 More than 7 mJ / m, particularly preferably 7 mJ / m 2 or more, preferably 20 mJ / m 2 Less than or equal to 18 mJ / m 2 Less than 16 mJ / m 2 The following is the result.
[0062] The surface free energy γ(A) of the resin layer (A) and its hydrogen bond component γ h (A) is measured on the surface of the resin layer (A) on which the resin layer (B) is to be formed. In addition, the surface free energy γ(A) and its hydrogen bond component γ h It is preferable that (A) is measured immediately before forming the resin layer (B). Therefore, when the method for producing an optical film includes step (IV), the surface free energy γ(A) and its hydrogen bond component γ are measured after the step (IV). h (A) can be measured.
[0063] Usually, the surface free energy of both sides of the resin layer (B) is equal. Therefore, the surface free energy γ(B) of the resin layer (B) and its hydrogen bond component γ h (B) can be measured on the surface opposite to the resin layer (A). The surface free energy γ(B) of the resin layer (B) measured on the surface opposite to the resin layer (A) in this manner and its hydrogen bond component γ h (B) is usually determined by the surface free energy γ(B) of the surface of the resin layer (B) in contact with the resin layer (A) (i.e., the surface of the resin layer (B) on the resin layer (A) side) and its hydrogen bond component γ h (B). Formulas (1) and (2) utilize this to define the relationship between the surfaces in contact at the interface between resin layer (A) and resin layer (B).
[0064] The surface free energy and hydrogen bond components of a solid sample (such as resin layer (A) and resin layer (B)) can be measured by measuring the contact angle θ with respect to the solid sample using three types of liquids with known surface free energies, and then applying the measured value to equation (7) to solve a simultaneous equation with three unknowns. Specific measurement conditions may be those described in the examples below.
[0065] The surface free energy γ(A) of the surface of the resin layer (A) is preferably in a range that satisfies the above-mentioned formula (1). From the viewpoint of significantly obtaining the effects of the present invention, the specific range of the surface free energy γ(A) is preferably 40 mJ / m 2 More preferably, 50 mJ / m 2 More than 55 mJ / m 2 or more, preferably 90 mJ / m 2 Less than or equal to 85 mJ / m 2 Less than 80 mJ / m 2 The following is the result.
[0066] Hydrogen bond component γ of surface free energy γ(A) of the surface of resin layer (A) h (A) is preferably in a range that satisfies the above formula (2). From the viewpoint of obtaining the effects of the present invention remarkably, the hydrogen bond component γ h The specific range of (A) is preferably 5 mJ / m 2 More preferably, 8 mJ / m 2 More than 10 mJ / m 2 or more, preferably 30 mJ / m 2 Less than or equal to 25 mJ / m 2 Less than 20 mJ / m, particularly preferably 20 mJ / m 2 The following is the result.
[0067] The surface free energy γ(A) of the surface of the resin layer (A) and its hydrogen bond component γ h (A) can be adjusted, for example, by the type and amount of functional groups contained in the crystalline alicyclic polymer, the composition of the first resin, the conditions of the hydrophilization treatment carried out in step (IV), and the like.
[0068] The surface free energy γ(B) of the resin layer (B) is preferably in a range that satisfies the above-mentioned formula (1). From the viewpoint of significantly obtaining the effects of the present invention, the specific range of the surface free energy γ(B) is preferably 30 mJ / m 2 More preferably, 35 mJ / m 2 More than 40 mJ / m 2 or more, preferably 70 mJ / m 2 Less than or equal to 60 mJ / m 2 Less than 55 mJ / m, particularly preferably 55 mJ / m 2 The following is the result.
[0069] Hydrogen bond component γ of surface free energy γ(B) of resin layer (B) h (B) is preferably in a range that satisfies the above formula (2). From the viewpoint of obtaining the effects of the present invention remarkably, the hydrogen bond component γ h The specific range of (B) is preferably 1 mJ / m 2 More preferably, 2 mJ / m 2 or more, preferably 20 mJ / m 2 Less than or equal to 15 mJ / m 2 The following is the result.
[0070] The surface free energy γ(B) of the surface of the resin layer (B) and its hydrogen bond component γ h (B) can be adjusted, for example, by changing the structure and functional groups of the polymer contained in the second resin, the types and amounts of optional components that the second resin may contain, and the like.
[0071] Examples of the second resin include urethane resin, olefin resin, polyester resin, epoxy resin, carbonate resin, and acrylic resin. Among them, the type of the second resin is preferably selected so that the resin layer (B) formed by the second resin satisfies the above-mentioned requirements related to surface free energy. For example, when a commercially available resin is used as the second resin, it is preferable to select a resin that forms a resin layer and whose surface free energy and hydrogen bond component satisfy the above-mentioned requirements.
[0072] The second resin may contain a polymer. However, the polymer contained in the second resin is usually a polymer other than a crystalline alicyclic polymer. This polymer may be used alone or in combination of two or more types in any ratio. The proportion of the polymer in the second resin is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more.
[0073] The second resin may contain an optional component in addition to the polymer. Examples of the optional component include the same examples as the optional components that the first resin may contain. The optional components may be used alone or in combination of two or more types in any ratio.
[0074] The second resin may be a curable resin such as a thermosetting resin or a photocurable resin. When a curable resin is used as the second resin, usually, in the step (III), a layer of the second resin in an uncured state is formed on the surface of the resin layer (A), and then the second resin is cured to obtain a resin layer (B) containing the second resin in a cured state.
[0075] There is no limitation on the method for forming the resin layer (B) in the step (III). Usually, the step (III) includes a step (III-1) of applying a coating liquid containing a second resin onto the surface of the resin layer (A).
[0076] The coating liquid may contain a solvent in combination with the second resin, if necessary. The solvent that the coating liquid may contain may be either a liquid that dissolves the second resin or a liquid that disperses the second resin, or both may be used in combination. The type of solvent may be appropriately selected depending on the types of the first resin and the second resin. Examples of the solvent include water; alcohol solvents such as methanol, ethanol, and isopropyl alcohol; ketone solvents such as acetone, methyl ethyl ketone, and N-methylpyrrolidone; ether solvents such as tetrahydrofuran, ethylene glycol monomethyl ether, and ethylene glycol monobutyl ether; dimethyl sulfoxide; and triethylamine. The solvent may be used alone or in combination of two or more.
[0077] Examples of the method for applying the coating liquid include wire bar coating, dipping, spraying, spin coating, roll coating, gravure coating, air knife coating, curtain coating, slide coating, and extrusion coating.
[0078] When the coating liquid contains a solvent, step (III) usually includes step (III-2) of drying the coating liquid after step (III-1). Any drying method may be used, such as drying under reduced pressure or drying by heating. By drying, the solvent is removed from the layer of the coating liquid formed on the surface of the resin layer (A), and thus a resin layer (B) containing the second resin is obtained.
[0079] For example, when the second resin is a curable resin, the above-mentioned step (III) may include a step (III-3) of curing the second resin applied to the surface of the resin layer (A). By carrying out the step (III-3), the second resin can be cured, so that a resin layer (B) having excellent mechanical strength can be obtained. The curing method may be a method according to the type of the second resin. For example, when the second resin is a thermosetting resin, the second resin can be cured by heating. Also, for example, when the second resin is a photocurable resin, the second resin can be cured by irradiating it with light such as ultraviolet light. However, when the second resin is a thermosetting resin, if heat drying is performed in the step (III-2), the effect of the second resin can progress simultaneously with drying, so the step (III-3) may be omitted.
[0080] [6. Optional process] The above-mentioned method for producing an optical film may further include any step as necessary. For example, the method for producing an optical film may include a step of thermally shrinking the resin layer (A) after the step (II) and before the step (III) to remove residual stress contained in the resin layer (A).
[0081] According to the above-described method for producing an optical film, a long optical film can be produced. Therefore, the method for producing an optical film may include a step of winding up the obtained optical film to obtain a roll. The method for producing the optical film may also include a step of trimming the optical film into a desired shape.
[0082] Furthermore, the method for producing an optical film may further include a step of providing an optional layer, such as a conductive layer, an antireflection layer, a hard coat layer, an antistatic layer, an antiglare layer, an antifouling layer, a separator film, etc.
[0083] [7. Optical films manufactured] According to the above-mentioned method for producing an optical film, an optical film can be obtained that includes a resin layer (A) formed of a first resin and a resin layer (B) formed on the resin layer (A) of a second resin. The above-mentioned production method does not include a step of applying a large amount of heat to the resin layer (B), so that the occurrence of cracks in the resin layer (B) can be suppressed. Therefore, the resin layer (B) of the obtained optical film can have a small number of cracks or no cracks. In one embodiment, the number of cracks having a length of 100 μm or more per 2 mm×2 mm area of the resin layer (B) can be less than 3.
[0084] The adhesive strength between the resin layer (A) and the resin layer (B) of the optical film is preferably high. Such high adhesive strength can be achieved when the requirements regarding the surface free energy expressed by the formulas (1) and (2) are satisfied. In one embodiment, as described in the examples below, the optical film is subjected to a cellophane tape checkerboard peeling test in accordance with JIS K5600-5-6. In this case, the number of the sections that remain on the optical film without peeling off even when the cellophane tape is peeled off per 100 sections formed on the resin layer (B) can be 90 or more.
[0085] The resin layer (A) of the optical film contains a first resin. Since the first resin contains a crystalline alicyclic polymer, the optical film can exhibit the excellent properties exhibited by the crystalline alicyclic polymer. Therefore, the optical film usually has excellent properties such as mechanical strength, transparency, dimensional stability, light weight, flexibility, heat resistance, folding resistance, and low water absorption.
[0086] The degree of crystallinity of the crystalline alicyclic polymer contained in the resin layer (A) of the optical film can be higher than that of step (I). The range of the degree of crystallinity of the crystalline alicyclic polymer contained in the resin layer (A) of the optical film is preferably 30% or more, more preferably 35% or more, and particularly preferably 40% or more. The upper limit of the degree of crystallinity is usually 100%, and may be 90% or less, 80% or less, 70% or less, 60% or less, etc. When the crystalline alicyclic polymer has such a high degree of crystallinity, the optical film can have particularly good properties such as flexibility, heat resistance, folding resistance, and low water absorption.
[0087] The thickness of the resin layer (A) is not particularly limited. The specific thickness of the resin layer (A) included in the optical film is preferably 5 μm or more, more preferably 10 μm or more, particularly preferably 15 μm or more, and is preferably 100 μm or less, more preferably 75 μm or less, particularly preferably 50 μm or less.
[0088] As described above, the optical film has a resin layer (B) on the surface of the resin layer (A). The resin layer (B) may be formed on only one surface of the resin layer (A) or on both surfaces. In the optical film having the resin layer (B) on both surfaces of the resin layer (A), both resin layers (B) may be formed simultaneously.
[0089] By providing the resin layer (B), the optical film can exhibit excellent properties based on the resin layer (B). For example, when the resin layer (B) contains a resin having excellent adhesiveness such as a urethane resin or an acrylic resin as the second resin, the optical film can exhibit excellent adhesiveness on the surface of the resin layer (B).
[0090] The thickness of the resin layer (B) is not particularly limited. The specific thickness of the resin layer (B) included in the optical film is preferably 10 nm or more, more preferably 50 nm or more, and even more preferably 100 nm or more, and is preferably 5 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.
[0091] The optical film preferably has a high total light transmittance. Specifically, the total light transmittance of the optical film is preferably 80% or more, more preferably 85% or more, and particularly preferably 88% or more. The total light transmittance can be measured in the wavelength range of 400 nm to 700 nm using an ultraviolet-visible spectrometer.
[0092] The optical film preferably has a small haze. Specifically, the haze of the optical film is preferably less than 3.0%, more preferably less than 2%, particularly preferably less than 1%, and ideally 0%. The haze can be measured using a haze meter (for example, "NDH5000" manufactured by Nippon Denshoku Industries Co., Ltd.).
[0093] The optical film can be arbitrarily applied to optical applications, and can be used as a component of a display device such as a liquid crystal display device or an organic electroluminescence display device. In particular, the optical film is preferably used as a component of a touch sensor of a display device, taking advantage of its excellent heat resistance and mechanical strength (particularly, flexibility). In particular, an optical film having a resin layer (A) containing a crystalline alicyclic polymer is preferable because it has excellent folding resistance and can be applied to a flexible display device. EXAMPLES
[0094] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.
[0095] In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature (25°C), at normal pressure (1 atm) and in the atmosphere unless otherwise specified.
[0096] [Evaluation method] (Method of measuring weight average molecular weight Mw and number average molecular weight Mn of polymer) The weight average molecular weight Mw and number average molecular weight Mn of the polymer were measured as polystyrene equivalent values using a gel permeation chromatography (GPC) system (Tosoh Corporation, "HLC-8320"). In the measurement, an H-type column (Tosoh Corporation) was used as the column, and tetrahydrofuran was used as the solvent. The temperature during the measurement was 40°C.
[0097] (Method of measuring hydrogenation rate of polymer) The hydrogenation rate of the polymer is 4 as a solvent at 145°C, 1 Measured by H-NMR measurement.
[0098] (Methods for measuring glass transition temperature Tg, crystallization temperature Tpc, and melting point Tm) The sample was heated to 320°C in a nitrogen atmosphere and melted, and then quenched with liquid nitrogen. The sample was heated at 10°C / min using a differential scanning calorimeter (DSC) to measure the glass transition temperature Tg, crystallization temperature Tpc, and melting point Tm of the sample. The glass transition temperature Tg is the minimum value of the endothermic peak, the crystallization temperature Tpc is the maximum value of the exothermic peak, and the melting point Tm is the minimum value of the endothermic peak.
[0099] (Method for measuring the ratio of racemo-dyads in polymers) The ratio of racemo-dyads in the polymer was determined as follows. 4 The inverse-gated decoupling method was applied to the polymer at 200°C using 13 C-NMR measurements were performed. 13 The results of C-NMR measurement showed that o-dichlorobenzene-d 4Using the peak at 127.5 ppm as the reference shift, the signal at 43.35 ppm from the meso-dyad and the signal at 43.43 ppm from the racemo-dyad were identified. The ratio of the racemo-dyads in the polymer was calculated based on the intensity ratio of these signals.
[0100] (Method of measuring the degree of crystallinity of a polymer) The crystallinity was confirmed by X-ray diffraction in accordance with JIS K 0131. Specifically, the diffracted X-ray intensity from the crystallized portion was determined using a wide-angle X-ray diffractometer (Rigaku Corporation, "RINT 2000"), and the crystallinity was calculated from the ratio to the total diffracted X-ray intensity according to the following formula (I). Xc=K·Ic / It (I) In the above formula (I), Xc represents the crystallinity of the test sample, Ic represents the diffracted X-ray intensity from the crystallized portion, It represents the total diffracted X-ray intensity, and K represents a correction term.
[0101] (Method of measuring surface free energy) The contact angles of water, diiodomethane and diethylene glycol were measured at 10 points on the surface of the sample using an automatic contact angle meter (Kyowa Interface Science Co., Ltd. "AutoDispenser AD-31"). The measurement was performed using the sessile drop method, and the contact angle was measured from the shape of the drop 3000 ms after it landed. The surface free energy was calculated from the average value of the contact angles obtained according to the Kitazaki-Hata method (Japan Adhesion Association Journal, Vol. 8, No. 3, 1972, pp. 131-141).
[0102] (Method for evaluating crack suppression ability (method for evaluating film appearance)) Nine samples measuring 2 mm x 2 mm were cut out from the optical film. The surface of the resin layer (B) of each sample was observed using an optical microscope (Olympus BX51) to determine the average number of cracks with a length of 100 μm or more. An average number of cracks less than 3 was judged as "good", and 3 or more was judged as "poor".
[0103] (Method for evaluating adhesion strength (peel test)) Nine samples were cut out from the optical film. Each sample was subjected to a cellophane tape checkerboard peeling test in accordance with JIS K5600-5-6. Specifically, the resin layer (B) was scored to form 100 sections of 2 mm x 2 mm in a checkerboard pattern. Cellophane tape (manufactured by Nichiban Co., Ltd., width 24 mm) was attached onto the 100 sections and peeled off within 1 second. The number of sections that remained on the optical film without peeling off even after the cellophane tape was peeled off was counted. Of the 100 sections, those with an average of 90 or more remaining were judged to be "good," and those with less than 90 remaining were judged to be "poor."
[0104] [Production Example 1. Production of Crystalline Alicyclic Structure-Containing Polymer] A metal pressure reactor was thoroughly dried and then purged with nitrogen. 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (endo isomer content of 99% or more) (30 parts as dicyclopentadiene), and 1.9 parts of 1-hexene were added to the metal pressure reactor and heated to 53°C.
[0105] A catalyst solution was prepared by adding 0.061 parts of a 19% diethylaluminum ethoxide / n-hexane solution to a solution of 0.014 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex dissolved in 0.70 parts of toluene and stirring for 10 minutes. This catalyst solution was added to a pressure-resistant reactor to initiate a ring-opening polymerization reaction. The reaction was then continued for 4 hours while maintaining the temperature at 53°C, to obtain a solution of a ring-opening polymer of dicyclopentadiene. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8750 and 28,100, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.21.
[0106] To 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, 0.037 parts of 1,2-ethanediol was added as a terminator, heated to 60°C, and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the adsorbent and the solution were filtered using a PP pleated cartridge filter (ADVANTEC Toyo Co., Ltd.'s "TCP-HX").
[0107] 100 parts of cyclohexane was added to 200 parts of the solution of the ring-opened polymer of dicyclopentadiene after filtration (polymer amount: 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and the hydrogenation reaction was carried out at a hydrogen pressure of 6 MPa and 180°C for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opened polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product had precipitated.
[0108] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated product of a crystalline ring-opening polymer of dicyclopentadiene. The hydrogenation rate of this hydrogenated product was 99% or more, the glass transition temperature (Tg) was 94°C, the melting point (Tm) was 262°C, the crystallization temperature (Tpc) was 170°C, and the ratio of racemo-dyads was 89%.
[0109] 100 parts of the hydrogenated product of the ring-opening polymer of dicyclopentadiene was mixed with 0.5 parts of an antioxidant (tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.) to obtain crystalline resin A as the first resin.
[0110] [Example 1] (1-1. Production of pre-stretched film) Crystalline resin A was charged into a twin-screw extruder (Toshiba Machine Co., Ltd., "TEM-37B") equipped with four die holes with an inner diameter of 3 mm. The twin-screw extruder molded the crystalline resin A into a strand-shaped molded body by hot melt extrusion molding. The molded body was chopped with a strand cutter to obtain pellets of crystalline resin A.
[0111] The pellets obtained were then fed to a hot melt extrusion film molding machine equipped with a T-die. Using this film molding machine, a long pre-stretched film (width 120 mm, thickness 20 μm) formed from the crystalline resin A was produced and wound around a roll at a speed of 27 m / min. The operating conditions of the film molding machine are shown below. Barrel temperature setting: 280℃~290℃ Die temperature: 270℃ Screw speed: 30 rpm Cast roll temperature: 70℃
[0112] (1-2. Stretching of pre-stretched film) A small-sized stretching machine equipped with an oven was prepared, and the oven temperature was set to 130° C. Using this small-sized stretching machine, a long unstretched film was stretched in the longitudinal direction at a stretching temperature of 130° C., a stretching speed of 4.0 mm / min, and a stretching ratio of 1.2 times to obtain a long stretched film.
[0113] (1-3. Crystallization treatment) A 350 mm x 350 mm square stretched film was cut out from the long stretched film. This cutting was performed so that each edge of the square of the obtained stretched film was parallel to the longitudinal direction or width direction of the long stretched film. The square stretched film was then placed in a small stretching machine ("EX10-B type" manufactured by Toyo Seiki Seisakusho Co., Ltd.). This small stretching machine had a structure equipped with multiple clips capable of gripping the four edges of the film and capable of stretching the film by moving the clips.
[0114] The stretched film placed in the small stretching machine was subjected to a heat treatment as a crystallization treatment. This heat treatment was performed by holding the four edges of the film and bringing the secondary heating plates attached to the small stretching machine close to the upper and lower surfaces of the stretched film and holding them for 30 seconds. The temperature of the secondary heating plates was 170°C, and the distance from the film was 8 mm both above and below. The crystallinity of the hydrogenated product of the ring-opening polymer of dicyclopentadiene contained in the stretched film after the treatment was 45%.
[0115] (1-4. Surface treatment) Using a corona treatment device (manufactured by Kasuga Denki Co., Ltd.), the surface of the stretched film was subjected to a discharge treatment as a hydrophilic treatment under the conditions of an output of 300 W, an electrode length of 340 mm, and a conveying speed of 6 m / min. The surface free energy γ(A) of the surface of the stretched film after the discharge treatment and its hydrogen bond component γ h (A) was measured.
[0116] (1-5. Formation of resin layer (B)) A coating liquid containing a chlorinated polypropylene modified acrylic resin (DIC Corporation's "WML-350") and methyl ethyl ketone was prepared. This coating liquid was applied to the discharge-treated surface of the stretched film using a bar coater. The coating thickness of the coating liquid was adjusted so that the thickness of the resulting resin layer (B) was 0.5 μm. The applied coating liquid was then dried under drying conditions of a drying temperature of 90° C. and a drying time of 120 seconds to form a resin layer (B) on the surface of the stretched film. By the above method, an optical film including a stretched film as the resin layer (A) and a resin layer (B) was obtained.
[0117] The surface free energy γ(B) and its hydrogen bond component γ of the surface opposite to the stretched film of the resin layer (B) of the obtained optical film h The adhesive strength between the stretched film and the resin layer (B) was measured. Furthermore, the appearance of the optical film was observed by the above-mentioned method to evaluate the crack suppression ability. Furthermore, a peel test was performed by the above-mentioned method to evaluate the adhesive strength between the stretched film and the resin layer (B).
[0118] [Example 2] The coating liquid was changed to one containing a urethane acrylate resin ("FA-3291" manufactured by Nippon Kako Toryo Co., Ltd.) and methyl ethyl ketone. After drying the coating liquid applied to the discharge-treated surface of the stretched film, ultraviolet light was irradiated to harden the urethane acrylate resin on the discharge-treated surface. This ultraviolet light irradiation was performed using a high-pressure mercury lamp with an illuminance of 350 mW / cm. 2 , cumulative light intensity 1000mJ / cm 2 Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0119] [Example 3] An optical film was produced and evaluated in the same manner as in Example 1, except that the conveying speed during the discharge treatment of the stretched film was changed to 1.2 m / min.
[0120] [Example 4] During the discharge treatment of the stretched film, the conveying speed was changed to 1.2 m / min. The coating liquid was also changed to a coating liquid containing a urethane acrylate resin ("FA-3291" manufactured by Nippon Kako Toryo Co., Ltd.) and methyl ethyl ketone. After the coating liquid applied to the discharge-treated surface of the crystallized film was dried, ultraviolet light was irradiated to harden the urethane acrylate resin on the discharge-treated surface. This ultraviolet light irradiation was performed using a high-pressure mercury lamp with an illuminance of 350 mW / cm. 2 , cumulative light intensity 1000mJ / cm 2 Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0121] [Example 5] An optical film was produced and evaluated in the same manner as in Example 1, except that the coating liquid was changed to a coating liquid containing an isocyanate carbonate resin ("Superflex 420" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and water.
[0122] [Example 6] During the discharge treatment of the stretched film, the conveying speed was changed to 1.2 m / min. The coating liquid was also changed to a coating liquid containing an acrylic resin (Hitachi Chemical's "Hitaloid 7975D") and methyl ethyl ketone. After the coating liquid applied to the discharge-treated surface of the stretched film was dried, ultraviolet light was irradiated to harden the urethane acrylate resin on the discharge-treated surface. This ultraviolet light irradiation was performed using a high-pressure mercury lamp with an illuminance of 350 mW / cm. 2 , cumulative light intensity 1000mJ / cm 2 Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0123] [Example 7] An optical film was produced and evaluated in the same manner as in Example 1, except that the coating liquid was changed to a coating liquid containing an aromatic isocyanate ether resin ("Superflex 870" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and water.
[0124] [Comparative Example 1] (C1-1. Surface treatment) A long unstretched film was produced in the same manner as in Example 1, and stretched to obtain a long stretched film. The surface of this stretched film was subjected to a discharge treatment as a hydrophilization treatment using a corona treatment device (manufactured by Kasuga Electric Co., Ltd.) under conditions of output of 300 W, electrode length of 340 mm, and conveying speed of 6 m / min. The surface free energy γ(A) and its hydrogen bond component γ of the surface of the stretched film after the discharge treatment were h The crystallinity of the hydrogenated ring-opening polymer of dicyclopentadiene contained in this stretched film was 3%.
[0125] (C1-2. Formation of resin layer (B)) A coating liquid containing a chlorinated polypropylene modified acrylic resin (DIC Corporation's "WML-350") and methyl ethyl ketone was prepared. This coating liquid was applied to the discharge-treated surface of the stretched film using a bar coater. The coating thickness of the coating liquid was adjusted so that the thickness of the resulting resin layer (B) was 0.5 μm. The applied coating liquid was then dried under drying conditions of a drying temperature of 90° C. and a drying time of 120 seconds to form a resin layer (B) on the surface of the stretched film, thereby obtaining an intermediate film.
[0126] (C1-3. Crystallization treatment) A square intermediate film measuring 350 mm x 350 mm was cut out from the long intermediate film and subjected to heat treatment as a crystallization treatment. The cutting out and crystallization treatment of the intermediate film were performed under the same conditions as those of the cutting out and crystallization treatment of the stretched film in Example 1. The crystallization treatment promoted crystallization of the hydrogenated product of the ring-opening polymer of dicyclopentadiene in the stretched film, and an optical film was obtained. This optical film was evaluated in the same manner as in Example 1.
[0127] [result] The results of the Examples and Comparative Examples are shown in the following table. In the table, the abbreviations have the following meanings. Crystallized DCPD: A hydrogenated product (crystallized) of a crystalline ring-opening polymer of dicyclopentadiene. DCPD: A crystalline hydrogenated ring-opening polymer of dicyclopentadiene. WML-350: Chlorinated polypropylene modified acrylic resin "WML-350" manufactured by DIC. FA-3291: "FA-3291" is a urethane acrylate resin manufactured by Nippon Kako Paint Co., Ltd. SF420: "Superflex 420", an isocyanate carbonate resin manufactured by Daiichi Kogyo Seiyaku Co., Ltd. 7975D: Hitachi Chemical's acrylic resin "Hitaroid 7975D". SF870: Superflex 870, an aromatic isocyanate ether resin manufactured by Daiichi Kogyo Seiyaku Co., Ltd. MEK: methyl ethyl ketone. In the process order column, "Sequential" means that the resin layer (B) was formed after the crystallization treatment. "Reverse" in the process order column: The crystallization treatment was carried out after the resin layer (B) was formed.
[0128] [Table 1]
Claims
1. A step (I) of preparing a resin layer (A) formed of a first resin containing an alicyclic structure-containing polymer having crystallinity; A step (II) of subjecting the resin layer (A) to a crystallization treatment; and (III) forming a resin layer (B) on the surface of the resin layer (A) using a second resin, the surface free energy γ(A) of the surface of the resin layer (A) in the step (III); the hydrogen bond component γ h (A) of the surface free energy γ(A); The surface free energy γ(B) of the resin layer (B) formed in the step (III), and The method for producing an optical film, wherein a hydrogen bond component γ h (B) of the surface free energy γ(B) satisfies the following formulas (1) and (2): 10mJ / m 2 ≦ γ(A) - γ(B) ≦ 40mJ / m 2 (1) 5mJ / m 2 ≦ γ h (A) - γ h (B) ≦ 20mJ / m 2 (2)
2. The method for producing an optical film according to claim 1 , further comprising a step (IV) between the step (II) and the step (III) of subjecting the surface of the resin layer (A) to a hydrophilic treatment.
3. The method for producing an optical film according to claim 1 or 2, wherein the step (III) comprises a step (III-1) of applying a coating liquid containing the second resin to the surface of the resin layer (A).
4. The method for producing an optical film according to any one of claims 1 to 3, wherein the alicyclic structure-containing polymer is a hydrogenated product of a ring-opening polymer of dicyclopentadiene.
5. The method for producing an optical film according to any one of claims 1 to 4, wherein the alicyclic structure-containing polymer contained in the optical film has a crystallinity of 30% or more.
Citation Information
Patent Citations
Battery and electronic apparatus
JP2018049839A
Conductive film and method for producing same
WO2018016442A1
Optical film, production method and multilayer film
WO2018079627A1
Optical film, production method, and multilayer film
WO2018142959A1
Method for manufacturing optical film
WO2019003980A1