Coating agent for modifying heat-sealable substrate, laminate and method for producing same

A block copolymer-based coating agent forms a lamellar structure on heat-sealing surfaces, addressing non-adsorption and heat-sealability issues in packaging materials, ensuring effective non-adsorption and strong heat-sealing for drugs and cosmetics.

JP7552162B2Active Publication Date: 2024-09-18TOPPAN HOLDINGS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020148719
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-04
Publication Date
2024-09-18
Estimated Expiration
2040-09-04

AI Technical Summary

Technical Problem

Existing heat-sealing compositions for packaging materials used in drugs and cosmetics suffer from reduced non-adsorption properties and heat-sealability, leading to increased costs and alignment issues due to complex processes.

Method used

A coating agent containing a block copolymer with a lamellar microphase-separated structure, comprising blocks (A) for non-adsorption and (B) for adhesion/fusion, is applied to the heat-sealing surface, forming a lamellar structure through self-assembly during heat treatment, ensuring excellent non-adsorption and heat-sealability.

Benefits of technology

The coating agent provides a heat-sealing surface with superior non-adsorption properties and heat-sealability, maintaining high heat-sealing strength while preventing adsorption of active ingredients, and reduces process complexity and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552162000003
    Figure 0007552162000003
  • Figure 0007552162000002
    Figure 0007552162000002
  • Figure 0007552162000001
    Figure 0007552162000001
Patent Text Reader

Abstract

To provide a coating agent for modifying heat-sealing base material which can impart excellent non-adsorptivity and heat sealability.SOLUTION: A coating agent for modifying heat-sealing base material contains a block copolymer capable of forming a lamellar micro phase separation structure and liquid medium, in which the block copolymer has a block (A) constituting a non-adsorption layer and a block (B) constituting a layer capable of adhering or fusing with heat-sealing base material, the block (A) consists of a copolymer including a nitrile group-containing (meth)acrylic monomer unit and a (meth)acrylic monomer unit having a partial structure expressed by general formula (1): -X-(R1-Y)m-R2, a ratio of the (meth)acrylic monomer unit having the partial structure expressed by the general formula (1) with respect to 1 mol of the nitrile group-containing (meth)acrylic monomer unit is 0.2 to 0.8 mol, a weight-average molecular weight of the block copolymer is 1000 or more, and a volume fraction of the block (A) is 0.35 to 0.65.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating agent for modifying a heat-sealable substrate, a laminate, and a method for producing the same. [Background technology]

[0002] In packaging materials for packaging medicines, cosmetics, etc., in order to prevent functional ingredients contained in the medicines, cosmetics, etc. from being adsorbed to the packaging material and losing their functions, a non-adsorptive material that is difficult for functional ingredients to adsorb is used as the outermost layer that comes into contact with the medicines, cosmetics, etc. Examples of non-adsorptive materials include ethylene-vinyl alcohol copolymer (EVOH), polyacrylonitrile (PAN), and cyclic olefin copolymer (COC) (e.g., ethylene-norbornene copolymer). Among them, PAN is known to exhibit excellent non-adsorptive properties. Therefore, a film in which PAN is used as a sealant layer and laminated with other plastic films by extrusion molding is used as a packaging material for medicines such as transdermal drugs, and as a packaging material for cosmetics containing medicinal ingredients and fragrance ingredients (Patent Document 1).

[0003] PAN films formed by extrusion molding have a thickness of about 20 to 30 μm, but since PAN resin is an expensive material, cost reduction is required. However, there is a limit to how thin a film can be made by extrusion molding, and it is difficult to meet the demand for cost reduction by extrusion molding. Therefore, a method has been proposed in which a non-adsorbing heat-sealable composition containing PAN resin particles, polyester resin, and a solvent is coated on a substrate to reduce the volume of the sealant layer and reduce costs (Patent Document 2).

[0004] In addition, a method has been proposed in which a non-adsorption layer is formed by coating a substrate with a coating agent for forming a non-adsorption layer, the coating agent containing a base material made of a polymer copolymerized with a nitrile group-containing acrylic monomer and a reactive functional group-containing acrylic monomer, an isocyanate-based curing agent, and a dispersion medium (Patent Documents 3 and 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-143452 [Patent Document 2] Patent No. 5656694 [Patent Document 3] Patent No. 6241590 [Patent Document 4] Patent No. 6402973 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the sealant layer formed from the non-adhesive heat sealable composition described in Patent Document 2 is a film of a mixture of PAN and polyester resin, and therefore has inferior non-adhesiveness compared to a film of PAN alone. The non-adhesive layer formed from the coating agent in Patent Documents 3 and 4 does not have heat sealability. Therefore, in order to heat seal the obtained laminate, it is necessary to apply the coating agent in a pattern so that a non-adhesive layer is not formed in the part to be heat sealed. Therefore, there are problems such as increased costs due to complicated processes and reduced non-adhesiveness due to poor alignment.

[0007] The present invention aims to provide a coating agent for modifying a heat-sealable substrate that can impart excellent non-adsorption to the heat-sealable surface of a heat-sealable substrate and that also has good heat-sealability after imparting the non-adsorption property; a laminate having a heat-sealable surface that is excellent in non-adsorption and also has good heat-sealability; and a method for producing the same. [Means for solving the problem]

[0008] The present invention has the following aspects. [1] A coating agent for modifying a heat seal substrate, which is to be coated on the heat seal surface of a heat seal substrate, comprising a block copolymer capable of forming a lamellar microphase separation structure and a liquid medium, wherein the block copolymer has a block (A) constituting a non-adsorbing layer and a block (B) constituting a layer capable of adhering or fusing to the heat seal substrate, and the block (A) is a copolymer characterized in that the block (A) contains a nitrile group-containing (meth)acrylic monomer unit and at least one of the blocks constituting the block copolymer contains a (meth)acrylic monomer unit having a partial structure represented by the following general formula (1): A random copolymer of acrylonitrile and azobenzyl methyl acrylate or stilbenzyl methyl acrylate. The ratio of the (meth)acrylic monomer unit having a partial structure to 1 mole of the nitrile group-containing (meth)acrylic monomer unit is 0.2 to 0.8 moles, The block (B) is made of polyvinyl acetate, a cyclic olefin polymer, or an octyl acrylate polymer, 1. A coating agent for modifying a heat-sealable substrate, wherein the block copolymer has a weight average molecular weight of 1000 or more and is a diblock copolymer in which the volume fraction of block (A) is 0.35 to 0.65. General formula (1): -X-(R 1 -Y) m -R 2 ( 1 ) (In the formula, X and Y, at each occurrence, are selected from the group consisting of an optionally substituted divalent hydrocarbon cyclic group and an optionally substituted divalent heterocyclic group; R 1 is selected for each occurrence from the group consisting of a single bond, -CHCH-, -CHO-, -OCH-, -C(=O)O-, -OC(=O)-, -C≡C-, -CH=CH-, -CF=CF-, -(CH)-, -CHCHCHO-, -OCHCHCH-, -CH=CH-CHCH-, -CHCH-CH=CH-, -N=N-, -CH=CH-COO-, -OCO-CH=CH-, -CH=CH-CO-, and -CO-CH=CH-; R 2 is selected from the group consisting of a hydrogen atom, a halogen, an alkyl group, an alkoxy group, a cyano group, a mercapto group, a nitro group, and an amino group, and m is an integer of 1 to 4. [2 ] a heat seal substrate and a coating layer formed on the heat seal surface of the heat seal substrate, the coating layer having a lamellar microphase separation structure formed by a block copolymer, the block copolymer has a block (A) constituting a non-adsorptive layer and a block (B) constituting a layer adhesive or fusible to the heat seal base material, The block (A) is a copolymer having a nitrile group-containing (meth)acrylic monomer unit and a (meth)acrylic monomer unit having a partial structure represented by the above general formula (1). A random copolymer of acrylonitrile and azobenzyl methyl acrylate or stilbenzyl methyl acrylate. the ratio of the (meth)acrylic monomer unit having the partial structure represented by the general formula (1) to 1 mole of the nitrile group-containing (meth)acrylic monomer unit is 0.2 to 0.8 moles, The block (B) is made of polyvinyl acetate, a cyclic olefin polymer, or an octyl acrylate polymer, A laminate, wherein the block copolymer has a weight average molecular weight of 1000 or more and is a diblock copolymer in which the volume fraction of block (A) is 0.35 to 0.65. [ 3 ] on the heat seal surface of the heat seal base material, 〕of A method for producing a laminate, comprising applying a coating agent for modifying a heat-sealable substrate and then heat-treating the coated substrate. Effect of the Invention

[0009] According to the coating agent for modifying a heat-sealable substrate of the present invention, it is possible to impart excellent non-adsorption to the heat-sealable surface of the heat-sealable substrate, and the heat-sealability after imparting the non-adsorption is also good. The laminate of the present invention has a heat-sealable surface that is excellent in non-adsorption and has good heat-sealability. According to the method for producing a laminate of the present invention, it is possible to produce a laminate having a heat-sealable surface that is excellent in non-adsorption and has good heat-sealability. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram showing an example of a block copolymer. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a laminate; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described with reference to the following embodiments. Note that the embodiments are specifically described to better understand the gist of the invention, and do not limit the present invention unless otherwise specified.

[0012] In the present invention, the "non-adsorptive layer" refers to a layer having non-adsorptive properties. "Non-adsorbent" refers to the property of being less likely to adsorb certain substances, such as active ingredients contained in medicines, cosmetics, foods, etc. A "heat sealable substrate" is a substrate that has heat sealability. "Heat sealability" refers to the property of substrates fusing together by heat. The "weight average molecular weight" (hereinafter also referred to as "Mw") is a value calculated as a standard polyethylene glycol, measured by gel permeation chromatography (GPC). A "(meth)acrylic monomer" is a compound having a (meth)acryloyl group. The term "(meth)acryloyl group" is a general term for acryloyl groups and methacryloyl groups. "(Meth)acrylate" is a general term for acrylate and methacrylate. The dimensional ratios in FIGS. 1 and 2 are different from the actual ones for the sake of convenience of explanation.

[0013] [Coating agent for modifying heat sealable substrate] A coating agent for modifying a heat-sealable substrate according to one embodiment of the present invention (hereinafter also referred to as "the coating agent") is applied to the heat-sealable surface of a heat-sealable substrate, and contains a block copolymer and a liquid medium. The present coating agent may further contain a curing agent, if necessary. The present coating agent may further contain other components in addition to the block copolymer, the liquid medium and the curing agent, if necessary.

[0014] (Block Copolymer) The block copolymer in this embodiment is capable of forming a lamellar microphase-separated structure (hereinafter also referred to as a "lamellar structure") and has a block (A) and a block (B). The block copolymer may further have a block other than the block (A) and the block (B) within a range that does not impair the effects of the present invention.

[0015] Block (A) constitutes a non-adhesive layer. Block (B) constitutes a layer that can be adhered or fused to a heat seal substrate (hereinafter also referred to as an "adhesive / fusion layer"). Therefore, the lamellar structure formed from the block copolymer has a non-adhesive layer and an adhesive / fusion layer. Each block will be explained in detail later.

[0016] In general, when a block copolymer in which two or more types of blocks with low compatibility with each other are bonded at their ends is heated to a temperature above the phase transition temperature, it forms a periodic microphase-separated structure by self-organization. In the microphase-separated structure, each block of the block copolymer does not mix with each other and forms a micro domain.

[0017] Microphase-separated structures formed by the self-organization of block copolymers are known to be spherical, cylindrical, gyroid, lamellar, etc. The type of microphase-separated structure formed is determined by a phase diagram represented by the Flory-Huggins interaction parameter χ determined between each block constituting the block copolymer, the degree of polymerization N of the block copolymer, and the volume fraction of each block. The size of each microdomain also depends on the polymer chain length (molecular weight) of each block.

[0018] "Low compatibility" means that the formula χ×N>10.5 is satisfied (see Leibler, L., "Theory of Microphase Separation in Block Copolymers", Macromolecules, 1980, Vol. 13, pp. 1602-1617). Here, χ represents the Flory-Huggins interaction parameter between different blocks, and N represents the degree of polymerization of the block copolymer.

[0019] Blocks (A) and (B) are mutually incompatible blocks, and when heated to a temperature above the phase transition temperature, the blocks separate without mixing with each other due to the self-organization phenomenon, forming a microphase-separated structure. In addition, block (A) has a lower affinity with the heat-sealing substrate than block (B), so when the microphase-separated structure is formed, block (A) is densely oriented on the air interface side (the side that comes into contact with the contents when used as a packaging material) to form a non-adhesive layer. Inevitably, block (B) is oriented on the heat-sealing substrate side to form an adhesive / fusion layer. Therefore, by applying this coating agent to the heat-sealing surface and subjecting it to heat treatment (annealing treatment), a coating layer containing a lamellar structure in which two different functional layers (a non-adhesive layer and an adhesive / fusion layer) are laminated can be formed.

[0020] The block copolymer may have one or more blocks (A). The block copolymer may have one or more blocks (B). The bonding form of each block constituting the block copolymer may be any form capable of forming a lamellar structure, and examples thereof include a form in which two or more blocks are bonded in series (linear block copolymer) and a form in which three or more blocks are bonded at one point (star block copolymer).

[0021] An example of a block copolymer is shown in Figure 1. In this example, block copolymer 100 is a diblock copolymer in which one block (A) 101 and one polymer (B) 102 are bonded at their ends.

[0022] During heat sealing, the block (B) constituting the adhesive / fusion layer and the thermoplastic resin constituting the heat seal base material are entangled, thereby maintaining high heat seal strength. The fewer the number of layers constituting the lamellar structure, the easier it is for the block (B) and the thermoplastic resin to be entangled. Therefore, the fewer the number of blocks in the block copolymer, the more preferable, and two is particularly preferable. In other words, a diblock copolymer is particularly preferable as the block copolymer.

[0023] When the block copolymer is a diblock copolymer, the volume fraction of block (A) is preferably 0.35 to 0.65, more preferably 0.40 to 0.60. The microphase-separated structure formed from the diblock copolymer depends on the volume fractions of the two blocks of the diblock copolymer, and the microphase-separated structure formed differs depending on the difference in the volume fractions. When the volume fraction of block (A) is 0.35 to 0.65, a lamellar structure is likely to be formed. When the volume fraction of block (A) is less than 0.35 or more than 0.65, a spherical or cylindrical microphase-separated structure is likely to be formed.

[0024] The volume fraction of block (A) is the ratio of the volume of block (A) to the total volume of all blocks constituting the block copolymer. The volume fraction of block (A) is calculated from the Mw and density of each block constituting the block copolymer. The density of the block is calculated from the molar fraction of the monomers forming the block and the density of the homopolymer. The density of the homopolymer can be calculated from literature values ​​(for example, values ​​listed in the polymer database PolyInfo).

[0025] The Mw of the block copolymer is preferably 1000 or more, more preferably 1000 or more and less than 1 million, further preferably 5000 to 500000, and particularly preferably 10000 to 100000. If the Mw of the block copolymer is 1000 or more, a continuous lamellar structure is easily formed, and the non-adsorption property is more excellent. In addition, the coating suitability of the present coating agent is good. On the other hand, in the self-organization of block copolymers, the fluidity of the block copolymer increases when the block copolymer is heat-treated at a temperature equal to or higher than the phase transition temperature, and a microphase-separated structure is induced, but as the molecular weight of the block copolymer increases, the fluidity decreases. If the Mw of the block copolymer is less than 1 million, the self-organization speed is fast and the productivity is excellent.

[0026] <Block (A)> The block (A) is a block that constitutes the non-adsorption layer. By including the block (A) in the block copolymer, non-adsorption can be imparted to the heat seal surface when the coating agent is applied thereto.

[0027] The block (A) is composed of a copolymer having a nitrile group-containing (meth)acrylic monomer unit and a (meth)acrylic monomer unit having a partial structure represented by the general formula (1). Examples of the nitrile group-containing (meth)acrylic monomer include acrylonitrile and methacrylonitrile. These monomers may be used alone or in combination of two or more.

[0028] The (meth)acrylic monomer unit having a partial structure represented by formula (1) has a function of a liquid crystal mesogen chain. -X-(R 1 -Y) m -R 2 (1)

[0029] In the general formula (1), X and Y are each selected from the group consisting of a divalent hydrocarbon cyclic group which may have a substituent and a divalent heterocyclic group which may have a substituent. The hydrocarbon cyclic group may be an aliphatic hydrocarbon cyclic group or an aromatic hydrocarbon cyclic group. The aliphatic hydrocarbon cyclic group may be saturated or unsaturated. Non-limiting examples of the aliphatic hydrocarbon group include a 1,4-cyclohexylene group, a 1,4-cyclohexenylene group, a decahydronaphthalene-2,6-diyl group, and a 1,4-bicyclo[2.2.2]octylene group. Non-limiting examples of the aromatic hydrocarbon cyclic group include a 1,4-phenylene group and a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group.

[0030] Heterocyclic groups preferably have oxygen or nitrogen atoms in the ring structure. Heterocyclic groups may have aromaticity. Non-limiting examples of heterocyclic groups include 1,3-dioxane-2,5-diyl group, pyridine-2,5-diyl group, pyrazine-2,5-diyl group, pyridazine-3,6-diyl group, and pyrimidine-2,5-diyl group.

[0031] Non-limiting examples of substituents for the hydrocarbon cyclic and heterocyclic groups include alkyl groups and halogen atoms. The halogens that can be used include fluorine, chlorine, bromine and iodine.

[0032] R in general formula (1) 1 is selected from the group consisting of a single bond, -CH2CH2-, -C2O-, -OCH2-, -C(=O)O-, -OC(=O)-, -C≡C-, -CH=CH-, -CF=CF-, -(CH2)4-, -CH2CH2CH2O-, -OCH2CH2CH2-, -CH=CH-CH2CH2-, -CH2CH2-CH=CH-, -N=N-, -CH=CH-COO-, -OCO-CH=CH-, -CH=CH-CO-, and -CO-CH=CH-, for each occurrence. In order to impart reactivity to the partial structure of general formula (1), R 1 Preferably, R contains a carbon-carbon double bond or a nitrogen-nitrogen double bond. More preferred R 1Non-limiting examples of include -CH=CH-, -N=N-, -CH=CH-CO- and -COCH=CH-. When these groups are used, crosslinking of the block copolymer can be carried out by, for example, a dimerization reaction of a carbon-carbon double bond or a nitrogen-nitrogen double bond. Crosslinking of the block copolymer can be carried out by, for example, ultraviolet irradiation or electron beam irradiation.

[0033] R in general formula (1) 2 is selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a cyano group, a mercapto group, a nitro group, and an amino group. 2 is selected from the group consisting of a hydrogen atom, an alkyl group and an alkoxy group. More preferably, R 2 is selected from the group consisting of a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and an alkoxy group having 1 to 10 carbon atoms. The alkyl group and the alkoxy group may be linear (straight-chain) or branched.

[0034] In the general formula (1), m is an integer of 1 to 4. More preferably, m is 1.

[0035] The block copolymer of the present invention can be prepared by any means known in the art. Also, the block containing a repeating unit having a partial structure of general formula (1) can be prepared by any means known in the art. For example, a polymerization process using a monomer having a partial structure of general formula (1) may be used. Alternatively, the partial structure of general formula (1) may be introduced into at least one block of a preformed block copolymer.

[0036] The partial structure of general formula (1) is oriented in a direction perpendicular to the surface of the heat seal substrate 204 by subjecting the coating film of the block copolymer to heat treatment, forming a liquid crystal phase. This orienting force accelerates the self-organization phenomenon of the block copolymer, promoting the formation of the coating layer 201 having a lamellar structure. Therefore, by using a block copolymer containing a block having the partial structure of general formula (1), the time required for forming the coating layer 201 having a lamellar structure can be shortened.

[0037] In block (A), the ratio of the (meth)acrylic monomer units having the partial structure represented by general formula (1) to 1 mole of the nitrile group-containing (meth)acrylic monomer units is 0.2 to 0.8 moles, preferably 0.2 to 0.5 moles. When the ratio of the (meth)acrylic monomer units having the partial structure represented by general formula (1) is equal to or greater than the lower limit, the solubility of the block copolymer in a liquid medium, the coatability of the coating agent, the rapid formation of a microphase separation structure, the non-adsorption property and heat sealability of the heat seal surface coated with the coating agent are excellent. When the ratio of the (meth)acrylic monomer units having the partial structure represented by general formula (1) is equal to or less than the upper limit, the non-adsorption property of the heat seal surface coated with the coating agent is excellent.

[0038] The total ratio of the nitrile group-containing (meth)acrylic monomer units and the (meth)acrylic monomer units having a partial structure represented by general formula (1) to the total monomer units constituting block (A) (100 mol %) is preferably 50 mol % or more, more preferably 80 mol % or more, and may be 100 mol %.

[0039] <Block (B)> The block (B) is a block that constitutes the adhesive / fusion layer. By including the block (B) in the block copolymer, good heat sealability can be ensured even when the heat seal surface is coated with the coating agent.

[0040] The polymer constituting block (B) is selected so that block (A) and block (B) are in the above-mentioned combination of "low compatibility with each other" so as to enable the formation of a microphase-separated structure.

[0041] Examples of the polymer constituting block (B) include a polymer having a nitrile group-containing (meth)acrylic monomer unit, a copolymer having a reactive functional group-containing (meth)acrylic monomer unit and a nitrile group-containing (meth)acrylic monomer unit, a polymer having a (meth)acrylic monomer unit containing a side group capable of adhering or fusing to a heat seal substrate, a polymer having a reactive functional group-containing vinyl monomer unit, or a polymer having a cyclic olefin unit. Among these, from the viewpoint of compatibility with block (A), a polymer having a functional group-containing vinyl monomer unit or a polymer having a cyclic olefin unit is preferred.

[0042] Examples of the nitrile group-containing (meth)acrylic monomer include acrylonitrile and methacrylonitrile. These monomers may be used alone or in combination of two or more. The polymer having a nitrile group-containing (meth)acrylic monomer unit may further have other monomer units. Examples of the polymer having a nitrile group-containing (meth)acrylic monomer unit include polyacrylonitrile and polymethacrylonitrile.

[0043] The reactive functional group of the reactive functional group-containing (meth)acrylic monomer is a functional group that can react with the reactive functional group of the heat seal surface of the heat seal substrate or other reactive functional groups in the present coating agent (e.g., the reactive functional group of another reactive functional group-containing (meth)acrylic monomer, or the reactive functional group of the curing agent when the present coating agent contains a curing agent). Examples of the reactive functional group include at least one selected from the group consisting of a hydroxy group, a carboxy group, an epoxy group, and an amino group. Examples of reactive functional group-containing (meth)acrylic monomers include hydroxy group-containing (meth)acrylic monomers such as 2-hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate, carboxy group-containing (meth)acrylic monomers such as (meth)acrylic acid, maleic acid and itaconic acid, epoxy group-containing (meth)acrylic monomers such as glycidyl (meth)acrylate, and amino group-containing (meth)acrylic monomers such as 2-(dimethylamino)ethyl methacrylate. These monomers may be used alone or in combination of two or more. The copolymer having reactive functional group-containing (meth)acrylic monomer units and nitrile group-containing (meth)acrylic monomer units may further have other monomer units.

[0044] An example of the adhesive / fusible side group of the (meth)acrylic monomer containing a side group capable of adhering or fusing to a heat seal base material (hereinafter also referred to as "adhesive / fusible side group") is a long-chain alkyl group. The long-chain alkyl group has 4 or more carbon atoms, preferably 4 to 18. The long-chain alkyl group may be linear or branched. Examples of (meth)acrylic monomers containing adhesive / fusible side groups include long-chain alkyl (meth)acrylates such as hexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, docosyl (meth)acrylate, etc. These monomers may be used alone or in combination of two or more. The polymer having a (meth)acrylic monomer containing an adhesive / fusible side group may further have other monomer units.

[0045] Examples of the functional group of the functional group-containing vinyl monomer include a hydroxy group, an acyl group (such as an acetyl group), and an isocyanate group. Examples of the functional group-containing vinyl monomer include vinyl alcohol and vinyl acetate. The polymer having the functional group-containing vinyl monomer unit may further have other monomer units, such as olefins such as ethylene and propylene. Examples of polymers having a functional group-containing vinyl monomer unit include polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinyl acetate, and ethylene-vinyl acetate copolymer.

[0046] The cyclic olefin may be monocyclic or polycyclic. The number of carbon atoms in the ring skeleton of the cyclic olefin is, for example, 4 to 8. The cyclic olefin may have a substituent such as an alkyl group. Examples of the cyclic olefin include norbornene, tetracyclododecene, methyltetracyclododecene, dimethylcyclotetradodecene, dimethanooctahydronaphthalene, cyclobutene, cyclopentene, and cyclooctene. These cyclic olefins may be used alone or in combination of two or more. The polymer having a cyclic olefin unit may further have other monomer units. Examples of the other monomers include olefins such as ethylene and propylene, and cyclic unsaturated hydrocarbons other than cyclic olefins such as dicyclopentadiene, dihydrodicyclopentadiene, methyldicyclopentadiene, dimethyldicyclopentadiene, tricyclopentadiene, tetracyclopentadiene, and cyclooctadiene.

[0047] The block (B) may be composed of a polymer other than those mentioned above. Examples of the other polymers include (co)polymers of (meth)acrylates containing a short-chain alkyl group having 1 to 3 carbon atoms, (co)polymers of aromatic vinyl monomers such as styrene and vinyl toluene, (co)polymers of acrylamide monomers such as acrylamide, N-methylolacrylamide and diacetoneacrylamide, and polymers having adhesive functional groups such as catechol groups at the ends or side chains.

[0048] The polymer constituting block (B) is preferably the same type of polymer as the thermoplastic resin constituting the heat seal base material, in view of ease of adhesion or fusion with the heat seal base material. "The same type" means having a similar main chain structure or a similar side chain structure. Examples of "the same type" include the following. When the thermoplastic resin of the heat seal base material is an ethylene-vinyl acetate copolymer and block (B) is a polymer containing vinyl acetate units (polyvinyl acetate, etc.). When the thermoplastic resin of the heat seal base material is a cyclic olefin copolymer and block (B) is a polymer having cyclic olefin units.

[0049] <Method of producing block copolymer> The block copolymer can be produced by a known method such as living radical polymerization, living anionic polymerization, living cationic polymerization, etc. For example, the block copolymer can be produced according to the synthesis example in Example 2 of JP-A-2006-299278.

[0050] (Liquid medium) The liquid medium may be any liquid medium capable of dissolving the block copolymer. When the present coating agent contains a curing agent, the liquid medium is preferably capable of dissolving the block copolymer and the curing agent. Examples of the liquid medium include ketone-based solvents, ester-based solvents, glycol-based solvents, and hydrocarbon-based solvents. Examples of the ketone-based solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, and anone. Examples of the ester-based solvents include ethyl acetate, n-propyl acetate, n-butyl acetate, and isobutyl acetate. Examples of the glycol-based solvents include butyl cellosolve, propylene glycol monomethyl ether, and propylene glycol-1-monomethyl ether-2-acetate. Examples of the hydrocarbon-based solvents include toluene, xylene, n-hexane, and methylcyclohexane. These liquid media may be used alone or in combination of two or more, and can be appropriately selected according to the solubility of the block copolymer. As the liquid medium, a ketone-based solvent, an ester-based solvent, or a hydrocarbon-based solvent is preferable.

[0051] The boiling point of the liquid medium is preferably 120° C. or lower, and more preferably 100° C. or lower, in order to reduce the process load during coating. The lower limit of the boiling point of the liquid medium is not particularly limited, but is, for example, 40° C. Examples of liquid media having a boiling point of 120° C. or less include methyl ethyl ketone and methyl isobutyl ketone.

[0052] (hardening agent) The curing agent is used to crosslink and harden the block copolymer when the block copolymer has a reactive functional group (for example, when block (A) or (B) has a reactive functional group-containing (meth)acrylic monomer unit). Crosslinking the block copolymer that has formed a microphase separation structure can increase the density of the coating layer and improve the non-adsorption properties.

[0053] As the curing agent, when the reactive functional group of the block copolymer is a hydroxyl group, a polyisocyanate compound having two or more isocyanate groups is preferable. Examples of the polyisocyanate compound include aromatic diisocyanates such as tolylene diisocyanate and 4,4'-diphenylmethane diisocyanate, aliphatic diisocyanates such as xylylene diisocyanate and hexamethylene diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, and diisocyanate compounds, as well as polymers, derivatives, and mixtures of these diisocyanate compounds. These curing agents may be used alone or in combination of two or more.

[0054] The content of the curing agent can be appropriately selected depending on the content of the reactive functional group in the block copolymer. The molar ratio represented by "reactive functional group of the curing agent / reactive functional group of the block copolymer" is preferably 0.5 to 5.0, more preferably 0.8 to 3.5. If this molar ratio is 0.5 or more, the block copolymer can be sufficiently cured, and if it is 5.0 or less, blocking of the coating layer surface can be prevented.

[0055] (Other ingredients) Examples of other components include antiblocking agents, ultraviolet absorbers, antistatic agents, antioxidants, antibacterial agents, pigments, dyes, defoamers, leveling agents, etc. These components may be used alone or in combination of two or more.

[0056] (solid content concentration) The solid content of the coating agent is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass. If the solid content is 0.1% by mass or more, the block copolymer, which is the main component of the coating agent, can be uniformly coated without unevenness, and a continuous film can be easily obtained. If the solid content is 20% by mass or less, the block copolymer and the like can be sufficiently dissolved. In addition, it becomes easy to form a thin film, the microphase separation structure formed by self-organization is less likely to be disturbed, the non-adsorption property is excellent, and sufficient heat seal strength is easily obtained.

[0057] The present coating agent can be produced by mixing the block copolymer, the liquid medium, and, if necessary, the curing agent and other components.

[0058] The coating agent of the present invention described above contains a specific block copolymer, and therefore when the coating agent is applied to the heat seal surface of a heat seal base material, it can impart excellent non-adsorption properties, and the heat sealability after imparting the non-adsorption properties is also good. As mentioned above, by applying this coating agent to a heat seal surface and subjecting it to heat treatment (annealing treatment), a coating layer containing a lamellar structure in which two different functional layers (a non-adhesive layer and an adhesive / fusion layer) are stacked together is formed through a self-organization phenomenon. In the lamellar structure, the non-adhesive layer is formed without any defects on the entire surface of the air interface side, so that excellent non-adhesive properties are exhibited. In addition, the adhesive / fusion layer is formed on the entire surface of the heat seal substrate side, so that the adhesion between the coating layer and the heat seal substrate is excellent, and defects such as peeling are unlikely to occur. When a laminate having a coating layer on the heat seal surface of the heat seal substrate is heat sealed, the block (B) flows and is mixed so as to be entangled with the thermoplastic resin constituting the heat seal substrate. Accordingly, the block (A) chemically bonded to the block (B) is also mixed with the thermoplastic resin. Therefore, the heat seal inhibition by the block (A) is suppressed, and high heat seal strength is maintained even in the area where the coating layer is formed.

[0059] This will be explained in more detail with reference to FIG. The laminate 200 has a heat seal substrate 204 and a coating layer 201 formed on the heat seal surface of the heat seal substrate 204. The coating layer 201 is formed using a coating agent containing a block copolymer similar to the block copolymer 100 shown in Fig. 1, and has a lamellar structure in which a non-adsorption layer 202 composed of block (A) of the block copolymer and an adhesive / fusion layer 203 composed of block (B) are laminated in this order from the heat seal substrate 204 side.

[0060] When the laminate 200 is heat-sealed, the block (B) of the adhesive / fusion layer 203 flows and mixes with a part of the thermoplastic resin of the heat-sealing substrate 204 so as to be entangled, and further the block (A) of the non-adhesive layer 202 is mixed with the thermoplastic resin of the heat-sealing substrate 204, and they are fused together. As a result, a layer made of a fusion of the block copolymer and the thermoplastic resin in which the non-adhesive layer 202, the adhesive / fusion layer 203, and a part of the heat-sealing substrate are integrated is formed. As a result, in the heat-sealed portion, the density of the block (A) on the outermost surface of the laminate 200 is low, and the non-adhesive property is not expressed, so it is considered that a high heat-sealing strength is obtained. On the other hand, when the block copolymer does not have the block (B), it is considered that the block (A) is difficult to mix with the thermoplastic resin of the heat-sealing substrate 204 during heat-sealing, and therefore the heat-sealing strength is low.

[0061] A laminated film in which two different functional layers are sequentially laminated can also be formed by a multilayer coextrusion method in which different resins are simultaneously extruded onto a substrate. However, in the multilayer coextrusion method, it is difficult to form a multilayer thin film of a few micrometers or less, and it is also difficult to form two different functional layers in a chemically bonded state. With this coating agent that utilizes the self-organization phenomenon, a laminated film in which two different functional layers are chemically bonded can be formed by only one application and heat treatment.

[0062] In addition, in this coating agent, since block (A) has 0.1 mole or more of (meth)acrylic monomer units having a partial structure represented by general formula (1) per mole of nitrile group-containing (meth)acrylic monomer units, the block copolymer dissolves well in low boiling point solvents such as methyl ethyl ketone and methyl isobutyl ketone. Therefore, such low boiling point solvents can be used as liquid media, and the process load during coating can be reduced.

[0063] [Laminate] A laminate according to one embodiment of the present invention (hereinafter, also referred to as "the laminate") has a heat seal substrate and a coating layer formed on the heat seal surface of the heat seal substrate. The laminate may further have other substrates or layers other than the heat seal substrate and the coating layer, as necessary.

[0064] (Heat seal base material) A heat sealable substrate is a substrate that has heat sealability. The heat seal base material usually contains a thermoplastic resin. The thermoplastic resin is preferably one that can be molded by heat compression bonding or the like, such as a polyethylene resin, a polypropylene resin, a cyclic polyolefin resin, a polyester resin, or a vinyl acetate resin. These thermoplastic resins may be used alone or in combination of two or more. The thickness of the heat seal base material is not particularly limited, but is, for example, 1 to 100 μm.

[0065] (Coating layer) The coating layer has a lamellar structure formed by a block copolymer, which is the same as the block copolymer in the coating agent. As described above, the lamellar structure has a non-adhesive layer constituted by block (A) and an adhesive / fusion layer constituted by block (B). The layer closest to the air interface of the lamellar structure is the non-adhesive layer, and the layer closest to the heat seal substrate is the adhesive / fusion layer.

[0066] The lamellar structure may have one or more non-adsorbent layers, and the lamellar structure may have one or more adhesive / fusible layers. As described above, the fewer the number of layers constituting the lamellar structure, the more easily the block (B) and the thermoplastic resin of the heat seal base material become entangled. Therefore, the lamellar structure is preferably a two-layer structure in which one adhesive / fusible layer and one non-adhesive layer are laminated from the heat seal base material side.

[0067] When the coating layer is formed by a roll-to-roll method, for example, the thickness of the coating layer is preferably about 0.01 μm or more and 10 μm or less, and more preferably about 0.1 μm or more and 1 μm or less. However, the thickness of the coating layer is not limited to the above range. For example, the thickness of the coating layer can be selected according to the Mw of the block copolymer. As described above, the fewer the number of layers of the lamellar structure, the better in order to maintain high heat seal strength by entangling the block (B) with the thermoplastic resin of the heat seal base material. Therefore, it is preferable to select the thickness of the coating layer so that orientation can be achieved with a small number of layers according to the Mw of the block copolymer.

[0068] (Other substrates or layers) The present laminate may further have a supporting substrate on the side opposite to the coating layer side of the heat seal substrate in order to facilitate forming the present laminate into a packaging bag or the like. The supporting substrate may have a single layer structure or a multilayer structure.

[0069] As the single-layer support substrate, various plastic films can be used, for example, polyolefin films such as polyethylene film and polypropylene film; polyester films such as polyethylene terephthalate film, polybutylene terephthalate film, and polyethylene naphthalate film; polyamide films such as nylon-6 film and nylon-66 film; polyimide films, etc. Among these, polypropylene film or polyethylene terephthalate film is preferable from the viewpoints of film strength and price, and polyamide film is preferable from the viewpoints of improving mechanical strength and imparting resistance to breakage of the bag due to piercing or other external forces.

[0070] When the supporting substrate has a multi-layer structure, it is preferable that one layer of the multi-layer structure is made of the above-mentioned plastic film. In this case, the other layers can be made of any material. For example, a plastic film, a coating film, paper, a metal foil, a vapor deposition layer, etc. When a metal foil, a metal vapor deposition film, an inorganic vapor deposition film, etc. is used, excellent gas barrier properties can be imparted. The metal foil may be aluminum or copper foil, which may be laminated to the plastic film with an adhesive.

[0071] The present laminate may have a printed layer. The printed layer can be provided at a position visible from the outside (the side opposite to the coating layer) when used as a packaging bag, etc. For example, when a transparent supporting substrate is used, the printed layer can be provided between the supporting substrate and the heat seal substrate.

[0072] The printing method and printing ink for the printed layer are appropriately selected from known printing methods, taking into consideration the printability on the film, design such as color tone, adhesion, safety as a pharmaceutical or cosmetic container, etc. Examples of printing methods that can be used include gravure printing, offset printing, gravure offset printing, flexographic printing, and inkjet printing.

[0073] [Method for producing laminate] The method for producing a laminate according to one embodiment of the present invention (hereinafter also referred to as "the present production method") is a method in which the present coating agent is applied to the heat-sealed surface of a heat-sealed substrate, followed by heat treatment. As a result, a coating layer is formed on the heat-sealed surface of the heat-sealed substrate.

[0074] As the coating method, for example, a solution casting method can be used. Specifically, a bar coating method, a dip coating method, a spin coating method, a flow coating method, a spray coating method, a roll coating method, a gravure roll coating method, an air doctor coating method, a blade coating method, a wire doctor coating method, a knife coating method, a reverse coating method, a transfer roll coating method, a microgravure coating method, a kiss coating method, a cast coating method, a slot orifice coating method, a calendar coating method, a die coating method, or the like can be used.

[0075] The heat treatment is carried out for the purposes of drying the coating agent applied to the heat seal surface (removing the liquid medium) and promoting the self-organization of the block copolymer to form a lamellar structure. As the heat treatment method, a known drying method can be appropriately adopted, for example, heating, blowing air, hot air, etc. can be used.

[0076] The self-organization of the block copolymer proceeds by heat treatment at a temperature equal to or higher than the phase transition temperature of the block copolymer to give it fluidity. Therefore, the heat treatment temperature is selected within a range equal to or higher than the phase transition temperature of the block copolymer used and equal to or lower than the melting temperature of the heat seal base material. In addition, the heat treatment time is selected according to the time required for the formation of a microphase separation structure. The phase transition temperature of the block copolymer can be confirmed by differential scanning calorimetry (DSC).

[0077] In order to promote the self-organization phenomenon, the heat treatment may be performed in the presence of a solvent vapor having an affinity for the block copolymer. When the heat treatment is performed in the presence of a solvent vapor having an affinity for the block copolymer, the fluidity of the block copolymer is improved due to the presence of the solvent vapor, and the self-organization is promoted, so that the heat treatment time and the heat treatment temperature can be reduced. The solvent used in this case is not particularly limited as long as it has an affinity for the block copolymer. Examples of the solvent that can be used include chloroform, toluene, tetrahydrofuran, and propylene glycol-1-monomethyl ether-2-acetate (PGMEA). In addition, when the heat treatment is performed under solvent vapor, the heat treatment temperature is preferably lower than the boiling point of the solvent used. If the treatment is performed at a temperature equal to or higher than the boiling point of the solvent, the solvent may volatilize around the coating film, and the solvent vapor may not sufficiently penetrate into the coating film, which may result in failure to obtain the effect of improving the fluidity of the block copolymer.

[0078] [Uses of the laminate] The laminate can be used, for example, as a packaging material. When the present laminate is used as a packaging material, it may be used in the form of a film, or may be molded into a bag or the like by heat sealing. For example, a packaging bag can be produced by stacking two sheets of the present laminate with their coating layer sides facing each other and heat sealing the periphery. Packaging bags made with the coating layer formed from this coating agent on the inside have a non-adsorbent inner surface (the surface that comes into contact with the contents) and excellent heat seal strength, making them suitable as packaging materials for liquid contents containing fragrances or active ingredients.

[0079] Examples of liquid contents include liquid medicines containing medicinal ingredients (infusions used for drip infusions, pharmaceutical drugs, etc.), insecticides, liquid cosmetics containing active ingredients (lotions, milky lotions, etc.), alcoholic drinks containing flavoring ingredients, aroma oils, etc. Examples of medicinal ingredients include terpenes such as methyl salicylate, limonene, citral, 1-menthol, d1-camphor, etc., aromatic compounds such as salicylic acid and naphthalene, vitamins, etc. EXAMPLES

[0080] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the examples shown here. The abbreviations used in each example are as follows: PET: Polyethylene terephthalate. PE: Polyethylene COC: Cyclic olefin copolymer. MEK: methyl ethyl ketone. PGMEA: propylene glycol-1-monomethyl ether-2-acetate. EVA: Ethylene-vinyl acetate copolymer. AN: Acrylonitrile. OA: octyl acrylate. POA: Polymeric octyl acrylate. PVAc: polyvinyl acetate. COP: Cyclic olefin polymer. MA(Az): Azobenzene group attached to the methyl group of methyl acrylate (in the general formula (1), X and Y are 1,4-phenylene groups, and R 1 is -N=N-, and R 2 is a hydrogen atom and m is 1). MA(Stb): A stilbene group attached to the methyl group of methyl acrylate (in the general formula (1), X and Y are 1,4-phenylene groups, and R 1 is -C=C- and R 2 is a hydrogen atom and m is 1). P(AN-rand-MA(Az)): Poly(acrylonitrile-rand-azobenzylmethylacrylate). P(AN-rand-MA(Stb)): Poly(acrylonitrile-rand-stilbenzyl methyl acrylate). "P1-b-P2" (P1 and P2 are any polymers) refers to a block copolymer in which a block of P1 and a block of P2 are bonded together. For example, PVAc-bP(AN-rand-MA(Az)) is a block copolymer in which a block of PVAc and a block of P(AN-rand-MA(Az)) are bonded together. "P(m1-rand-m2)" (m1 and m2 are arbitrary monomers) indicates a random copolymer of m1 and m2. For example, P(AN-rand-MA(Az)) is a random copolymer of AN and MA(Az).

[0081] Example 1 A laminated film (EVA thickness 30 μm) was obtained by extrusion molding EVA (Novatec™ EVA, manufactured by Mitsubishi Chemical Corporation) onto a PET film (E5100, manufactured by Toyobo Co., Ltd., thickness 12 μm). The EVA surface of the obtained laminated film was subjected to a corona treatment. Separately, a 5% by mass solution (coating agent) of a block copolymer, PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 13,300, AN / MA(Az) molar ratio = 1 / 0.21, P(AN-rand-MA(Az)) volume fraction 0.47) was dissolved in MEK. The above 5% by mass solution was applied once using a wire bar #6 to the corona-treated EVA surface of the laminated film, and then heat-treated at 105°C for 30 seconds to form a coating layer with a thickness of 0.5 μm. This resulted in a laminate in which PET / EVA / coating layer were laminated in this order.

[0082] Example 2 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 16,910, AN / MA(Az) molar ratio = 1 / 0.51, P(AN-rand-MA(Az)) volume fraction 0.53) was used as the block copolymer.

[0083] Example 3 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 16,250, AN / MA(Az) molar ratio = 1 / 0.78, P(AN-rand-MA(Az)) volume fraction 0.52) was used as the block copolymer.

[0084] Example 4 A PET film (E5100, manufactured by Toyobo Co., Ltd., thickness 12 μm) and a COC film (Coxec TCS-2, manufactured by Kurabo Industries, Ltd., thickness 20 μm) were laminated together to obtain a laminated film. The COC surface of the laminated film was subjected to a corona treatment. Separately, a block copolymer, COP-bP(AN-rand-MA(Az)) (COP Mw 12000, P(AN-rand-MA(Az)) Mw 9810, AN / MA(Az) molar ratio = 1 / 0.34, P(AN-rand-MA(Az)) volume fraction 0.45) was dissolved in PGMEA to obtain a 1 mass% solution (coating agent). The above 1% by mass solution was applied once using a wire bar #6 to the corona-treated COC surface of the laminated film, and then heat-treated at 110°C for 30 seconds to form a coating layer with a thickness of 0.6 μm. This resulted in a laminate in which PET / COC / coating layer were laminated in this order.

[0085] Example 5 A PET film (E5100, manufactured by Toyobo Co., Ltd., thickness 12 μm) and a PE film (MC-S, manufactured by Mitsui Chemicals Tocello Co., Ltd., thickness 40 μm) were laminated together to obtain a laminated film. The PE surface of the laminated film was subjected to a corona treatment. Separately, a block copolymer, POA-bP(AN-rand-MA(Az)) (POA Mw 12000, P(AN-rand-MA(Az)) Mw 11500, AN / MA(Az) molar ratio = 1 / 0.23, P(AN-rand-MA(Az)) volume fraction 0.49) was dissolved in MEK to obtain a 1 mass% solution (coating agent). The above 5% by mass solution was applied once using a wire bar #6 to the corona-treated PE surface of the laminated film, and then heat-treated at 110°C for 30 seconds to form a coating layer with a thickness of 0.6 μm. This resulted in a laminate in which PET / PE / coating layer were laminated in this order.

[0086] Example 6 A coating layer was formed on the corona-treated PE surface of the laminated film in the same manner as in Example 5, except that POA-bP(AN-rand-MA(Az)) (POA Mw 12000, P(AN-rand-MA(Az)) Mw 13500, AN / MA(Az) molar ratio = 1 / 0.49, P(AN-rand-MA(Az)) volume fraction 0.53) was used as the block copolymer.

[0087] Example 7 A coating layer was formed on the corona-treated PE surface of the laminated film in the same manner as in Example 5, except that POA-bP(AN-rand-MA(Stb)) (POA Mw 12000, P(AN-rand-MA(Stb)) Mw 11000, AN / MA(Stb) molar ratio = 1 / 0.33, P(AN-rand-MA(Az)) volume fraction 0.48) was used as the block copolymer.

[0088] Example 8 A coating layer was formed on the corona-treated PE surface of the laminated film in the same manner as in Example 5, except that POA-bP(AN-rand-MA(Stb)) (POA Mw 12000, P(AN-rand-MA(Stb)) Mw 15270, AN / MA(Stb) molar ratio = 1 / 0.43, P(AN-rand-MA(Az)) volume fraction 0.56) was used as the block copolymer.

[0089] Comparative Example 1 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 13,800, AN / MA(Az) molar ratio = 1 / 0.15, volume fraction of P(AN-rand-MA(Az)) 0.48) was used as the block copolymer.

[0090] Comparative Example 2 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 15,600, AN / MA(Az) molar ratio = 1 / 0.91, P(AN-rand-MA(Az)) volume fraction 0.51) was used as the block copolymer.

[0091] Comparative Example 3 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 500, P(AN-rand-MA(Az)) Mw 460, AN / MA(Az) molar ratio = 1 / 0.33, P(AN-rand-MA(Az)) volume fraction 0.48) was used as the block copolymer.

[0092] Comparative Example 4 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 6,740, AN / MA(Az) molar ratio = 1 / 0.43, P(AN-rand-MA(Az)) volume fraction 0.31) was used as the block copolymer.

[0093] Comparative Example 5 A coating layer was formed on the corona-treated EVA surface of the laminated film in the same manner as in Example 1, except that PVAc-bP(AN-rand-MA(Az)) (PVAc Mw 15,000, P(AN-rand-MA(Az)) Mw 36,730, AN / MA(Az) molar ratio = 1 / 0.42, P(AN-rand-MA(Az)) volume fraction 0.71) was used as the block copolymer.

[0094] Comparative Example 6 A coating layer was formed on the corona-treated PE surface of the laminated film in the same manner as in Example 5, except that POA-bP(AN-rand-MA(Az)) (POA Mw 12000, P(AN-rand-MA(Az)) Mw 9400, AN / MA(Az) molar ratio = 1 / 0.17, P(AN-rand-MA(Az)) volume fraction 0.44) was used as the block copolymer.

[0095] Comparative Example 7 A coating layer was formed on the corona-treated PE surface of the laminated film in the same manner as in Example 5, except that POA-bP(AN-rand-MA(Stb)) (POA Mw 12000, P(AN-rand-MA(Stb)) Mw 32400, AN / MA(Stb) molar ratio = 1 / 0.52, volume fraction of P(AN-rand-MA(Stb)) 0.73) was used as the block copolymer.

[0096] Table 1 shows the laminated film (support substrate / heat seal substrate), block copolymer used in the coating agent, and liquid medium in each of the above examples. For the block copolymer, the polymers constituting each block (A) and (B) and their Mw, the nitrile / liquid crystal mesogen chain molar ratio (AN / MA(Az) molar ratio or AN / MA(Stb) molar ratio) and volume fraction of block (A), and the Mw of the entire block copolymer are shown. The "nitrile / liquid crystal mesogen chain molar ratio" is the molar ratio of "nitrile group-containing (meth)acrylic monomer unit / (meth)acrylic monomer unit having a partial structure represented by general formula (1)".

[0097] The block copolymer used in each example was produced according to the procedure described in Example 2 of JP-A-2006-299278.

[0098] (Confirmation of microphase separation structure) The laminate of each example was embedded in UV-curable resin, and the UV-curable resin was cured by UV irradiation to prepare a sample. The obtained sample was cut with a microtome to expose the cross section of the laminate. The cross section was stained with iodine or ruthenium oxide, and the coating layer was observed with a scanning electron microscope (SEM). Cases in which a lamellar structure (lamellar microphase separation structure) was uniformly formed were marked with an ◯, and cases in which a lamellar structure was not formed were marked with an ×. The results are shown in Table 1.

[0099] (evaluation) <Coating suitability> The coating layer formed in each example was visually observed for the applicability of the coating agent, and was evaluated according to the following criteria. The results are shown in Table 1. ◯: The coating is uniform and without any unevenness. ×: Unevenness or foreign matter was observed, and the coating was not uniform.

[0100] <Structure formation time> Regarding the time for forming the microphase-separated structure in each example, the heating time of the coating layer formed in each example was changed according to the following criteria, and the formation of the microphase-separated structure was evaluated. The results are shown in Table 1. ◯: A microphase-separated structure was formed after heating for 30 seconds. ×: No microphase-separated structure was formed within a heating time of 30 seconds.

[0101] <Non-adsorption> The laminate of each example was cut to prepare two rectangular samples (100 mm x 100 mm), and each sample was stacked so that the coating layers faced each other. Three of the four sides were heat-sealed under conditions of 0.15 MPa, 190°C, and 1 second to form a packaging bag. 0.1 g of 1-menthol was enclosed in the obtained packaging bag, and the remaining side was heat-sealed under the same conditions as above to seal it, and the bag was left to stand for three days in an environment of 40°C and 75% RH. Thereafter, the packaging bag was opened to remove the 1-menthol, and the bag was exposed to air for 10 minutes, after which the residual scent of 1-menthol was sensorily evaluated according to the following criteria. The less the residual scent, the better the non-adsorption. The results are shown in Table 1. 〇: Almost no residual fragrance is detectable. △: A slight lingering scent is detectable. ×: A noticeable lingering scent is detectable.

[0102] <Heat seal strength> The laminate of each example was cut to prepare two rectangular samples (50 mm x 50 mm), and the samples were stacked so that the coating layers faced each other, and one edge was heat-sealed at a width of 15 mm under conditions of 0.15 MPa, 190°C, and 1 second. The heat-sealed sample was cut into a strip of 15 mm width, and a T-peel test was performed using a tensile tester at a tension speed of 300 mm / min in an atmosphere of 23°C and 65% RH to measure the peel strength. The measurement was performed on 10 samples, and the average value was taken as the heat seal strength of the laminate. Separately, the laminated film of each example (before the coating layer was formed) was cut to prepare two rectangular samples (50 mm x 50 mm), and each sample was stacked with the heat seal surfaces (EVA surface, COC surface, or PE surface) facing each other, and one edge was heat sealed at a width of 15 mm under conditions of 0.15 MPa, 190°C, and 1 second. The heat-sealed sample was cut into a 15 mm-wide strip, and the peel strength was measured in the same manner as above, and the average value was taken as the heat seal strength of the laminated film. From the measurement results, the rate of decrease in heat seal strength was calculated using the following formula. The results are shown in Table 1. Reduction rate of heat seal strength (%) = (heat seal strength of laminated film (N / mm) - heat seal strength of laminate (N / mm)) / heat seal strength of laminated film (N / mm) x 100 From the obtained rate of decrease, the heat seal strength of the laminate was evaluated according to the following criteria. The results are shown in Table 1. Good: Reduction in heat seal strength is less than 10%. ×: The reduction in heat seal strength is 10% or more.

[0103] [Table 1]

[0104] From the results shown in Table 1, it was confirmed that a microphase-separated structure was formed within 30 seconds when block (A) had 0.2 mol or more of (meth)acrylic monomer units having a partial structure represented by general formula (1) per 1 mol of nitrile group-containing (meth)acrylic monomer units.

[0105] As shown in Table 1, Examples 1 to 8 were excellent in coatability, microphase separation structure formation, formation time, non-adsorption property, and heat seal strength.

[0106] In Comparative Example 1, the ratio of the (meth)acrylic monomer units having a partial structure represented by general formula (1) to 1 mole of the nitrile group-containing (meth)acrylic monomer units in block (A) was less than 0.2 moles, and therefore the time for the formation of the lamellar structure was insufficient, resulting in poor formation of the lamellar structure and poor non-adsorption properties. In Comparative Example 2, the ratio of the (meth)acrylic monomer units having a partial structure represented by general formula (1) to 1 mole of the nitrile group-containing (meth)acrylic monomer units in block (A) was more than 0.8 moles, and therefore the non-adsorption property was poor. In Comparative Example 3, the overall molecular weight was 1000 or less, resulting in poor film formation. This is believed to be because the block (A) was unable to form a continuous film, and adsorption of 1-menthol progressed from areas that were not non-adsorbed layers. In Comparative Example 4, the volume fraction of the block (A) was low and a lamellar structure was not formed, so that the non-adsorption property was poor. In Comparative Example 5, the volume fraction of block (A) was large and a lamellar structure was not formed, so the non-adsorption property was poor, and the volume fraction of block (B) was small, so the heat seal strength was also poor. In Comparative Example 6, the ratio of the (meth)acrylic monomer units having a partial structure represented by general formula (1) to 1 mole of the nitrile group-containing (meth)acrylic monomer units in block (A) was less than 0.2 moles, and therefore the time for the formation of the lamellar structure was insufficient, resulting in poor formation of the lamellar structure and poor non-adsorption properties. In Comparative Example 7, the volume fraction of block (A) was large and a lamellar structure was not formed, so the non-adsorption property was poor, and the volume fraction of block (B) was small, so the heat seal strength was also poor. [Industrial Applicability]

[0107] According to the coating agent for modifying a substrate of the present invention, excellent non-adsorption can be imparted to the heat-sealed surface of a heat-sealed substrate. In addition, the heat-sealing surface after imparting non-adsorption also has good heat-sealing properties, and for example, high heat-sealing strength can be obtained when heat-sealing surfaces are heat-sealed together. In addition, since the block copolymer dissolves well in low-boiling point solvents such as MEK, a low-boiling point solvent can be used as a liquid medium, and the process load during coating can be reduced. Furthermore, since the coating agent contains an acrylate having a liquid crystal mesogen chain, the orientation effect shortens the time required for lamellar structure formation, improving productivity.

[0108] The laminate of the present invention has a heat seal surface that is excellent in non-adsorption and has good heat sealability. Therefore, the laminate of the present invention can be used as a packaging material for medicines, cosmetics, etc., particularly as a packaging material for liquids. By using the laminate of the present invention as a packaging material for medicines, cosmetics, etc., it is possible to suppress the functional deterioration caused by the adsorption of medicinal ingredients, etc. to the packaging material. [Explanation of symbols]

[0109] 100...Block copolymer 101...Block (A) 102...Block (B) 200...Laminate 201...coating layer 202…Non-adsorption layer 203…adhesion / fusion layer 204...Heat seal base material

Claims

1. A coating agent for modifying a heat-sealable substrate, which is applied to a heat-sealable surface of a heat-sealable substrate, comprising: The present invention comprises a block copolymer capable of forming a lamellar microphase-separated structure and a liquid medium, the block copolymer has a block (A) constituting a non-adsorptive layer and a block (B) constituting a layer adhesive or fusible to the heat seal base material, The block (A) is a copolymer comprising a nitrile group-containing (meth)acrylic monomer unit and a (meth)acrylic monomer unit having a partial structure represented by the following general formula (1), and is composed of a random copolymer of acrylonitrile and azobenzyl methyl acrylate or stilbenzyl methyl acrylate: the ratio of the (meth)acrylic monomer unit having the partial structure represented by the general formula (1) to 1 mole of the nitrile group-containing (meth)acrylic monomer unit is 0.2 to 0.8 moles, The block (B) is made of polyvinyl acetate, a cyclic olefin polymer, or an octyl acrylate polymer, The weight average molecular weight of the block copolymer is 1000 or more, The coating agent for modifying a heat-sealable substrate, wherein the block copolymer is a diblock copolymer in which the volume fraction of the block (A) is 0.35 to 0.

65. General formula (1): -X-(R 1 -Y) m -R 2 ( 1 ) wherein X and Y, at each occurrence, are selected from the group consisting of an optionally substituted divalent hydrocarbon cyclic group and an optionally substituted divalent heterocyclic group; R 1 Each occurrence represents a single bond, -CH 2 CH 2 --, --CH 2 O-, -OCH 2 -, -C(=O)O-, -OC(=O)-, -C≡C-, -CH=CH-, -CF=CF-, -(CH 2 ) 4 --, --CH 2 CH 2 CH 2 O-, -OCH 2 CH 2 CH 2 -, -CH=CH-CH 2 CH 2 --, --CH 2 CH 2 selected from the group consisting of -CH=CH-, -N=N-, -CH=CH-COO-, -OCO-CH=CH-, -CH=CH-CO-, and -CO-CH=CH-; R 2 is selected from the group consisting of a hydrogen atom, a halogen, an alkyl group, an alkoxy group, a cyano group, a mercapto group, a nitro group, and an amino group, and m is an integer from 1 to 4.

2. A heat seal substrate and a coating layer formed on a heat seal surface of the heat seal substrate, the coating layer having a lamellar microphase separation structure formed by a block copolymer, the block copolymer has a block (A) constituting a non-adsorptive layer and a block (B) constituting a layer adhesive or fusible to the heat seal base material, The block (A) is a copolymer characterized in that it contains a nitrile group-containing (meth)acrylic monomer unit and at least one of the blocks constituting the block copolymer contains a (meth)acrylic monomer unit having a partial structure represented by the following general formula (1), and the block (A) is a random copolymer of acrylonitrile and azobenzyl methyl acrylate or stilbenzyl methyl acrylate, the ratio of the (meth)acrylic monomer unit having the partial structure to 1 mole of the nitrile group-containing (meth)acrylic monomer unit is 0.2 to 0.8 moles, The block (B) is made of polyvinyl acetate, a cyclic olefin polymer, or an octyl acrylate polymer, The weight average molecular weight of the block copolymer is 1000 or more, The block copolymer is a diblock copolymer in which the volume fraction of the block (A) is 0.35 to 0.

65. General formula (1): -X-(R 1 -Y) m -R 2 ( 1 ) wherein X and Y, at each occurrence, are selected from the group consisting of an optionally substituted divalent hydrocarbon cyclic group and an optionally substituted divalent heterocyclic group; R 1 Each occurrence represents a single bond, -CH 2 CH 2 --, --CH 2 O-, -OCH 2 -, -C(=O)O-, -OC(=O)-, -C≡C-, -CH=CH-, -CF=CF-, -(CH 2 ) 4 --, --CH 2 CH 2 CH 2 O-, -OCH 2 CH 2 CH 2 -, -CH=CH-CH 2 CH 2 --, --CH 2 CH 2 selected from the group consisting of -CH=CH-, -N=N-, -CH=CH-COO-, -OCO-CH=CH-, -CH=CH-CO-, and -CO-CH=CH-; R 2 is selected from the group consisting of a hydrogen atom, a halogen, an alkyl group, an alkoxy group, a cyano group, a mercapto group, a nitro group, and an amino group, and m is an integer from 1 to 4.

3. A method for producing a laminate, comprising applying the coating agent for modifying a heat-sealable substrate according to claim 1 to a heat-sealable surface of a heat-sealable substrate, and then heat-treating the substrate.

Citation Information

Patent Citations

  • Method of manufacturing printed circuit board

    JP1981056694A

  • Repairing device of plate type heat exchanger

    JP1987041590A

  • Printing paper loading machine

    JP1989002973A

  • Laminate for suppressing adhesion of 1-menthol

    JP1996143452A

  • Production method of microstructure, and composite

    JP2014141711A