Near-infrared absorbing composition, near-infrared absorbing film, near-infrared cut filter, image sensor for solid-state imaging device, and camera module

A near-infrared absorbing composition with optimized molar ratios of phosphonate copper complexes and ester compounds addresses the challenge of thin film absorption and moist heat resistance, achieving efficient spectral transmission and visibility correction.

JP7552193B2Active Publication Date: 2024-09-18KONICA MINOLTA INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020160339
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-25
Publication Date
2024-09-18
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing near-infrared absorbing films face challenges in achieving high near-infrared absorption while maintaining thin film thickness and resistance to moist heat, with phosphoric ester compounds exhibiting poor dispersibility and hydrolyzing in high temperature and humidity environments.

Method used

A near-infrared absorbing composition is formulated with specific molar ratios of phosphonate copper complexes and phosphoric or sulfuric acid ester compounds, optimized to achieve high absorption and resistance to moist heat, using compounds with specific structures and molar ratios to enhance dispersibility and stability.

Benefits of technology

The composition provides a thin film with high near-infrared absorption and improved resistance to moist heat, ensuring effective spectral transmission characteristics and visibility correction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552193000027
    Figure 0007552193000027
  • Figure 0007552193000028
    Figure 0007552193000028
  • Figure 0007552193000029
    Figure 0007552193000029
Patent Text Reader

Abstract

To provide a near-infrared absorptive composition, etc., which, of thin-film type, yet has high near-infrared absorptance and high wet heat resistance.SOLUTION: The near-infrared absorptive composition is such that a near-infrared absorbent contains a component (A) and a component (B), and a mole ratio CA / CE where CA represents the mole content of a compound of general formula (I) and CE represents the mole content of a compound of specific formula is in the range from 2.5 to 50, and a mole ratio CH / CC where CC represents the mole content of copper ions and CH represents the total amount of mole content of a reactive hydroxy group that the compound of general formula (I) and the compound of specific formula possess is in the range from 1.5 to 2.5. Component (A): Chemical compound of general formula (I), chemical compound of specific formula, and copper ion. Component (B): Copper complex to which the compound of general formula (I) is coordinated, and copper complex to which the compound of specific formula is coordinated.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a near-infrared absorbing composition, a near-infrared cut filter, an image sensor for a solid-state imaging device, and a camera module. More specifically, the present invention relates to a near-infrared absorbing composition which, although being a thin film, has high near-infrared absorbing properties and high resistance to moist heat. [Background technology]

[0002] In recent years, CCD and CMOS image sensors, which are solid-state image sensors for capturing color images, have come to be used in video cameras, digital still cameras, and mobile phones with camera functions. However, these solid-state image sensors use silicon photodiodes in their light receiving sections (light receiving elements) that are sensitive to light in the near-infrared wavelength range, making it necessary to perform visual sensitivity correction, and a near-infrared cut filter is often used.

[0003] As a near-infrared absorbent for forming a near-infrared absorbing layer in such a near-infrared cut filter, various near-infrared absorbents have been disclosed, which are made from raw materials such as a phosphate compound, a phosphonic acid compound, and a compound that serves as a copper ion source.

[0004] For example, Patent Document 1 discloses an optical material comprising at least one of a phosphonic acid monoester compound, a phosphinic acid compound, a phosphoric acid diester compound, and a phosphoric acid monoester compound, a phosphonic acid compound, and a metal ion, and claims that the optical material has improved spectral characteristic expression and compatibility with resins.

[0005] Patent Document 2 discloses a composition for an infrared absorbing layer, which is composed of copper ions, phosphonic acid, and at least one of a phosphoric acid diester and a phosphoric acid monoester, and the content of the phosphonic acid is specified to be less than 2.5 times the content of the phosphoric acid ester compound on a molar basis. According to this document, it is said that the composition can obtain optical properties in the infrared and visible regions that are desirable for a cut filter.

[0006] Furthermore, Patent Document 3 discloses a near-infrared absorbent composed of a phosphonic acid compound, a phosphoric ester compound, and a copper salt, and is said to provide a near-infrared cut filter that can suitably absorb near-infrared rays and has excellent transparency.

[0007] Furthermore, Patent Document 4 discloses a near-infrared absorbent comprising a phosphonic acid compound, a monopolyoxyethylene alkyl phosphate ester compound, and a copper ion, which is said to provide excellent transparency and heat resistance as an optical material.

[0008] However, with the methods disclosed in the above Patent Documents 1 to 4, it was difficult to produce a near-infrared absorbing film that is thin yet has high near-infrared absorptivity. In the methods disclosed in the above Patent Documents 1 to 4, the effect of the phosphate ester compound as a dispersant is insufficient, so that if the content of the phosphate ester compound is increased in consideration of dispersibility for near-infrared absorption, the film thickness becomes thick, and conversely, if the content of the phosphate ester compound is reduced in consideration of film thickness, the dispersibility becomes insufficient, resulting in a trade-off.

[0009] Therefore, from the viewpoint of ease of handling and miniaturization of solid-state imaging devices, there is a demand for a near-infrared absorbing composition capable of forming a near-infrared absorbing film that is thin yet has high near-infrared absorptivity.

[0010] Further, near infrared absorbing compositions containing a phosphate compound also have a problem in terms of resistance to moist heat, because a part of the phosphate compound that does not interact with other components such as copper ions is hydrolyzed in a high-temperature and high-humidity environment, causing visible precipitates and causing the composition to become cloudy. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 4500417 [Patent Document 2] International Publication No. 2017 / 051512 [Patent Document 3] Patent No. 5611631 [Patent Document 4] Patent No. 5554048 Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a near-infrared absorbing composition and the like which has high near-infrared absorptivity and high moist heat resistance even in the form of a thin film. [Means for solving the problem]

[0013] Means for Solving the Problems The present inventors have investigated the causes of the problems in order to solve the problems, and have found that it is possible to provide a near-infrared absorbing composition and the like which has high near-infrared absorbency and high moist heat resistance despite being a thin film by adjusting the content ratio of each component contained and further limiting the structure of a phosphate ester compound or a sulfate ester compound acting as a dispersant to a specific structure, and have arrived at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.

[0014] 1. A near infrared absorbing composition containing a near infrared absorbing agent, The near-infrared absorbent contains at least one of the following component (A) and the following component (B), The molar ratio CA / CE is expressed by the following general formula (I) as the molar content of the compound having the structure represented by the following general formula (II), where CA is the molar content of the compound having the structure represented by the following general formula (II) and CE is the molar ratio CA / CE. 3.8~10 and A near-infrared absorbing composition, characterized in that a molar ratio CH / CC, where CC is the molar content of copper ions and CH is the molar content of reactive hydroxy groups possessed by a compound having a structure represented by the following general formula (I) and a compound having a structure represented by the following general formula (II), is within a range of 1.5 to 2.5. <Ingredients>: Component (A): A component consisting of a compound having a structure represented by the following general formula (I), a compound having a structure represented by the following general formula (II), and copper ions. Component (B): A component consisting of a copper complex coordinated with a compound having a structure represented by the following general formula (I) and a copper complex coordinated with a compound having a structure represented by the following general formula (II). [ka] [In the above general formula (I), R 1 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent. [ka] [In the above general formula (II), R 2 R represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may further have a substituent. 21 ~R 24 Each of R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structures in which all are hydrogen atoms, and is within the range of 1 to 19. 21 ~R 24 represents the average number of partial structures added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 1 to 19. l+m is the total number of l and m, and is within the range of 2 to 20. Z represents a structural unit selected from the following general formulae (Z-1) to (Z-3). [ka] In the above general formulae (Z-1) to (Z-3), * represents a bonding site and bonds to O in the above general formula (II). 〕

[0015] 2 R in the general formula (I) 1 is an alkyl group having 1 to 20 carbon atoms. Section 1 The near infrared absorbing composition according to claim 1.

[0016] 3 .Characterized by containing organic dye Paragraph 1 or 2 The near infrared absorbing composition according to claim 1.

[0017] 4 The organic dye is a quaterrylene derivative, a phthalocyanine derivative, a cyanine derivative, or a squarylium derivative. Section 3 The near infrared absorbing composition according to claim 1.

[0018] 5. A near infrared absorbing composition according to any one of items 1 to 4, and a curable resin, A near-infrared absorbing film, characterized in that it is in a cured film state.

[0019] 6. The average spectral transmittance is 80% or more in the wavelength range of 450 to 600 nm; The average spectral transmittance is 10% or less in the wavelength range of 850 to 1,000 nm, and 6. The film thickness of the film according to claim 5, which is within the range of 10 to 150 μm. Near infrared absorbing film .

[0020] 7. The average spectral transmittance is 1% or less in the wavelength range of 750 to 1,080 nm; The spectral transmittance decreases with increasing wavelength within the wavelength range of 600 to 700 nm. When a wavelength at which the spectral transmittance is 50% within a wavelength range of 600 to 700 nm is defined as a cutoff wavelength, the cutoff wavelength for light incident on the surface at an incident angle of 0° is within a range of 600 to 680 nm, and Item 5 or 6, characterized in that the film thickness is within the range of 10 to 100 μm. Near infrared absorbing film .

[0021] 8. A near-infrared cut filter having a near-infrared absorbing layer on at least one surface of a transparent dielectric substrate, The near infrared absorbing layer is 5 Any one of the items to 7 Near infrared absorbing film A near-infrared cut filter.

[0022] 9 The present invention is characterized in that a dielectric multilayer film is further provided on at least one surface of the near infrared absorbing layer. Section 8 2. The near-infrared cut filter according to claim 1 .

[0023] 10 . Paragraph 8 or 9 2. An image sensor for a solid-state imaging device, comprising the near-infrared cut filter according to claim 1.

[0024] 11 . Section 10 2. A camera module comprising the image sensor for a solid-state imaging device according to claim 1. Effect of the Invention

[0025] According to the above-mentioned means of the present invention, it is possible to provide a near-infrared absorbing composition which, although being a thin film, has high near-infrared absorbing properties and high resistance to moist heat.

[0026] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.

[0027] The near-infrared absorbent according to the present invention is characterized in that the molar ratio CA / CE, where CA is the molar content of the compound having a structure represented by general formula (I) (phosphonic acid copper complex) and CE is the molar content of the compound having a structure represented by general formula (II) (phosphate ester compound or sulfate ester compound), is within a range of 2.5 to 50.

[0028] By setting the molar ratio CA / CE to 2.5 or more, the proportion of phosphonic acid copper complexes effective for absorbing near-infrared rays is increased, resulting in good near-infrared absorption properties. In addition, the proportion of ester compounds that cause clouding in high-temperature, high-humidity environments is low, resulting in good humidity and heat resistance.

[0029] When the molar ratio CA / CE is 50 or less, a certain amount or more of the phosphate ester compound or sulfate ester compound is present, and the dispersibility of the complex fine particles can be improved.

[0030] The near-infrared absorbent according to the present invention is characterized in that the molar ratio CH / CC, where CC is the molar content of copper constituting the copper ion or copper compound, and CH is the molar content of reactive hydroxy groups contained in the compound having a structure represented by general formula (I) and the compound having a structure represented by general formula (II), is within a range of 1.5 to 2.5.

[0031] When the molar ratio CH / CC is within this range, the transmittance of light in the visible wavelength range of 400 to 700 nm is increased, there is no leakage of transmitted light in the vicinity of 1,100 nm in the near-infrared region, and absorption performance is efficiently maintained. In addition, spectral transmittance characteristics can be achieved that have a certain degree of absorption characteristics even at 700 nm, which is at the long wavelength end of visible light, making it suitable for luminosity correction.

[0032] In addition, the compound (phosphate compound or sulfate compound) having a structure represented by general formula (II) according to the present invention is characterized in that the average number l of added ethylene oxide structures and the average number m of added alkyl-substituted ethylene oxide structures are both 1 or more.

[0033] The phosphoric acid and sulfuric acid structures have a high ability to form complexes with metals, which contributes to enhancing the effect as a dispersant. In addition, the combination of an ethylene oxide structure and an alkyl-substituted ethylene oxide structure increases the number of isomers, which increases the entropy and contributes to enhancing the effect as a dispersant. The increased dispersibility improves the storage stability of the dispersion. In addition, the improved effect as a dispersant allows the content of the compound to be reduced, which enables the thinning and improved resistance to moist heat when the compound is made into a film.

[0034] It is believed that these mechanisms of expression or action make it possible to provide a near-infrared absorbing composition that is a thin film but has high near-infrared absorptivity and high resistance to moist heat. [Brief description of the drawings]

[0035] [Figure 1] Schematic cross-sectional view showing an example of the configuration of a near-infrared cut filter. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of an image sensor for a solid-state imaging device. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a configuration of a camera module. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] The near infrared absorbing composition of the present invention is a near infrared absorbing composition containing a near infrared absorbing agent, the near infrared absorbing agent containing at least one of the following component (A) and the following component (B), The molar ratio CA / CE, in which CA is the molar content of the compound having the structure represented by the general formula (I) and CE is the molar content of the compound having the structure represented by the general formula (II), is within a range of 2.5 to 50; and The compound having the structure represented by general formula (I) and the compound having the structure represented by general formula (II) have a molar ratio CH / CC of 1.5 to 2.5, where CC is the molar content of copper ions and CH is the total molar content of reactive hydroxy groups contained in the compound having the structure represented by general formula (I) and the compound having the structure represented by general formula (II). <Ingredients>: Component (A): A component consisting of a compound having a structure represented by general formula (I), a compound having a structure represented by general formula (II), and copper ions. Component (B): A component consisting of a copper complex coordinated with a compound having a structure represented by general formula (I) above, and a copper complex coordinated with a compound having a structure represented by general formula (II) above. This feature is a technical feature common to or corresponding to the following embodiments.

[0037] The molar ratio CA / CE is preferably within the range of 3.8 to 10 in terms of near-infrared absorptivity and resistance to moist heat.

[0038] R in the general formula (I) 1 However, an alkyl group having 1 to 20 carbon atoms is preferred in terms of near infrared absorbing properties and resistance to moist heat.

[0039] It is preferable that the organic dye is contained, since the absorption wavelength can be adjusted.

[0040] The organic dye is preferably a quaterrylene derivative, a phthalocyanine derivative, a cyanine derivative or a squarylium derivative, in that it sufficiently absorbs near infrared rays, has high visible light transmittance and is highly heat resistant.

[0041] The near infrared absorbing composition of the present invention may further contain a curable resin and may be in the state of a cured film.

[0042] The average spectral transmittance is 80% or more in the wavelength range of 450 to 600 nm, The average spectral transmittance is 10% or less in the wavelength range of 850 to 1,000 nm, and The film thickness is preferably within the range of 10 to 150 μm in order to achieve both a thin film and good near-infrared absorptivity.

[0043] The average spectral transmittance is 1% or less in the wavelength range of 750 to 1,080 nm, The spectral transmittance decreases with increasing wavelength within the wavelength range of 600 to 700 nm. When a wavelength at which the spectral transmittance is 50% within a wavelength range of 600 to 700 nm is defined as a cutoff wavelength, the cutoff wavelength for light incident on the surface at an incident angle of 0° is within a range of 600 to 680 nm, and The film thickness is preferably within the range of 10 to 100 μm in terms of achieving both a thin film and near-infrared absorptivity suitable for luminosity correction.

[0044] The near-infrared cut filter of the present invention is a near-infrared cut filter comprising a near-infrared absorbing layer on at least one surface of a transparent dielectric substrate, and is characterized in that the near-infrared absorbing layer contains the near-infrared absorbing composition of the present invention.

[0045] The near-infrared cut filter of the present invention preferably further comprises a dielectric multilayer film on at least one surface of the transparent dielectric substrate, in that the spectral characteristics of the near-infrared cut filter can be more freely adjusted.

[0046] The image sensor for a solid-state imaging device of the present invention is characterized by comprising the near-infrared cut filter of the present invention.

[0047] The camera module of the present invention is characterized by comprising the near infrared absorbing composition of the present invention.

[0048] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0049] (1) Overview of near infrared absorbing composition The near infrared absorbing composition of the present invention is characterized by containing a near infrared absorbing agent, and may further contain an organic dye, an ultraviolet absorbing agent, and other additives.

[0050] In addition, the near infrared absorbing composition of the present invention may be in the state of a dispersion in which a component such as a near infrared absorbing agent is dispersed in a solvent, or may be in the state of a film cured together with a curable resin.

[0051] (1.1) Near infrared absorbing agent The near-infrared absorbent according to the present invention is characterized by containing at least one of the following component (A) and the following component (B): <Ingredients>: (A) Ingredients: The following three ingredients A compound having a structure represented by the following general formula (I): A compound having a structure represented by the following general formula (II): Copper ions (B) Ingredients: The following two ingredients A copper complex coordinated with a compound having a structure represented by the following general formula (I): A copper complex coordinated with a compound having a structure represented by the following general formula (II):

[0052] Each component will be described below.

[0053] <Compound having a structure represented by general formula (I)> The compound having the structure represented by the general formula (I) is a phosphonic acid compound, and is capable of absorbing near-infrared radiation by forming a copper phosphonate complex, which will be described later.

[0054] <Structure represented by general formula (I)> [ka]

[0055] In the general formula (I), R 1 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent. 1 It is preferable that R is an alkyl group having 1 to 20 carbon atoms in terms of good resistance to moisture and heat and near infrared absorption. 1However, an alkyl group having 1 to 4 carbon atoms is more preferable in terms of achieving both near infrared ray absorptivity and visible light transmittance.

[0056] R 1 Examples of the compound having a structure represented by general formula (I) in which is an alkyl group having 1 to 20 carbon atoms include methylphosphonic acid, ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, nonylphosphonic acid, and decylphosphonic acid.

[0057] R 1 Examples of compounds having a structure represented by general formula (I) in which is an aryl group having 6 to 20 carbon atoms include phenylphosphonic acid, 4-methoxyphenylphosphonic acid, (4-aminophenyl)phosphonic acid, (4-bromophenyl)phosphonic acid, 3-phosphonobenzoic acid, 4-phosphonobenzoic acid, and (4-hydroxyphenyl)phosphonic acid.

[0058] R 1 Examples of the substituent that may be included in the formula (I) include an alkyl group (e.g., a methyl group, an ethyl group, a trifluoromethyl group, an isopropyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, etc.), a halogen atom (e.g., a fluorine atom, etc.), a cyano group, a nitro group, a dialkylamino group (e.g., a dimethylamino group, etc.), a trialkylsilyl group (e.g., a trimethylsilyl group, etc.), a triarylsilyl group (e.g., a triphenylsilyl group, etc.), a triheteroarylsilyl group (e.g., a tripyridylsilyl group, etc.), a benzyl group, and a heteroaryl group (e.g., a pyridyl group, a carbazolyl group, etc.). Examples of the condensed ring include 9,9′-dimethylfluorene, carbazole, and dibenzofuran.

[0059] Examples of the compound having the structure represented by general formula (I) are shown below as compounds (H-1) to (H-8).

[0060] [ka]

[0061] In the present invention, the compound having a structure represented by general formula (I) (phosphonic acid compound) is preferably at least one alkylphosphonic acid selected from the following group of phosphonic acid compounds.

[0062] 1: Methylphosphonic acid 2: Ethylphosphonic acid 3: Propylphosphonic acid 4: Butylphosphonic acid 5: Pentylphosphonic acid 6: Hexylphosphonic acid 7: Octylphosphonic acid 8: 2-Ethylhexylphosphonic acid 9: 2-Chloroethylphosphonic acid 10: 3-Bromopropylphosphonic acid 11: 3-Methoxybutylphosphonic acid 12: 1,1-Dimethylpropylphosphonic acid 13: 1,1-Dimethylethylphosphonic acid 14: 1-Methylpropylphosphonic acid

[0063] <Compound having a structure represented by general formula (II)> The compound having a structure represented by general formula (II) is a phosphate compound or a sulfate compound, which disperses the phosphonic copper complex and contributes to preventing the particle size of the particles formed by the phosphonic copper complex from increasing.

[0064] <Structure represented by general formula (II)> [ka]

[0065] In the general formula (II), R 2 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent.

[0066] In the general formula (II), R 2 The alkyl group having 1 to 20 carbon atoms represented by the formula (I) may be linear or branched, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, n-octyl, 2-butyloctyl, 2-hexyloctyl, n-decyl, 2-hexyldecyl, n-dodecyl, and n-stearyl. Each alkyl group may further have a substituent. From the viewpoint of dispersibility of the copper complex and resistance to heat and humidity, the alkyl group is preferably an alkyl group having 6 to 16 carbon atoms.

[0067] Also, R 2 Examples of the aryl group having 6 to 20 carbon atoms and represented by the formula (1) include a phenyl group, a mesityl group, a tolyl group, a xylyl group, a naphthyl group, an anthryl group, an azulenyl group, an acenaphthenyl group, a fluorenyl group, a phenanthryl group, an indenyl group, a pyrenyl group, a biphenylyl group, and the like, and preferably a phenyl group, a naphthyl group, a fluorenyl group, a phenanthryl group, a biphenylyl group, or a fluorenonyl group. Each of the aryl groups may further have a substituent.

[0068] R 2 Examples of the substituent that may be included include an alkyl group (e.g., a methyl group, an ethyl group, a trifluoromethyl group, an isopropyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, etc.), a halogen atom (e.g., a fluorine atom, etc.), a cyano group, a nitro group, a dialkylamino group (e.g., a dimethylamino group, etc.), a trialkylsilyl group (e.g., a trimethylsilyl group, etc.), a triarylsilyl group (e.g., a triphenylsilyl group, etc.), a triheteroarylsilyl group (e.g., a tripyridylsilyl group, etc.), a benzyl group, an aryl group (e.g., a phenyl group, etc.), and a heteroaryl group (e.g., a pyridyl group, a carbazolyl group, etc.). Examples of the condensed ring include, but are not limited to, 9,9′-dimethylfluorene, carbazole, and dibenzofuran.

[0069] In the general formula (II), R 21 ~R 24Each of R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 When all are hydrogen atoms, the partial structure in the parentheses in the formula is also called the "ethylene oxide structure." 21 ~R 24 A partial structure in the parentheses in the formula, in which at least one of the above is an alkyl group having 1 to 4 carbon atoms and the others are hydrogen atoms, is also referred to as an "alkyl-substituted ethylene oxide structure."

[0070] R 21 ~R 24 Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, and an n-butyl group. From the viewpoint of dispersibility of the copper complex, the methyl group is particularly preferred.

[0071] In the general formula (II), l is R 21 ~R 24 represents the average number of partial structures (ethylene oxide structures) in which all are hydrogen atoms, and is within the range of 1 to 19.

[0072] In the general formula (II), m is R 21 ~R 24 represents the average number of partial structures (alkyl-substituted ethylene oxide structures) in which at least one of the groups is an alkyl group having 1 to 4 carbon atoms and the others are hydrogen atoms, and is within the range of 1 to 19.

[0073] In the general formula (II), l+m is the total of the average number of additions l and the average number of additions m, and is within the range of 2-20.

[0074] The compound having the structure represented by the general formula (II) according to the present invention is characterized in that the average number of added ethylene oxide structures, l, and the average number of added alkyl-substituted ethylene oxide structures, m, are both 1 or more. The phosphoric acid and sulfuric acid structures have high complex forming ability with metals, which contributes to improving the effect as a dispersant. In addition, the combination of an ethylene oxide structure and an alkyl-substituted ethylene oxide structure increases the number of isomers, which increases the entropy and contributes to improving the effect as a dispersant. The increased dispersibility improves the storage stability of the dispersion. In addition, the improved effect as a dispersant allows the content of the compound to be reduced, which enables the thinning and improved resistance to moist heat when the compound is made into a film.

[0075] As described above, the compound having a structure represented by general formula (II) according to the present invention is characterized in that the average number of additions l and the average number of additions m are both within the range of 1 to 19. However, it is preferable that the average number of additions l and the average number of additions m are both within the range of 1 to 5, in terms of achieving a well-balanced effect of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure and enabling the film to be thin-filmed.

[0076] In general formula (II), Z represents a structural unit selected from the following general formulae (Z-1) to (Z-3).

[0077] [ka]

[0078] In the general formulae (Z-1) to (Z-3), * represents a bonding site and bonds to O in the above general formula (II).

[0079] When Z is (Z-1), the compound is a diester, and when Z is (Z-2) or (Z-3), the compound is a monoester.

[0080] The mixing ratio of the diester and monoester is preferably such that the molar ratio of the monoester to the total amount of the diester and monoester is within the range of 20 to 95%.

[0081] <Examples of compounds having a structure represented by general formula (II)> Specific examples of the compound having the structure represented by formula (II) will be described below.

[0082] First, specific examples of the compound having the structure represented by general formula (II) are listed in the following Tables I to IV. Note that the compound having the structure represented by general formula (II) according to the present invention is not limited to these compounds.

[0083] In Tables I to IV, "ethylene oxide structure" means R 21 ~R 24 In addition, an "alkyl-substituted ethylene oxide structure" refers to a partial structure in which R 21 ~R 24 It refers to a partial structure in which at least one of the above is an alkyl group having 1 to 4 carbon atoms, and the rests are hydrogen atoms.

[0084] In Tables I to IV, the column "Z: Structure" indicates whether Z in the formula is (Z-1), (Z-2), or (Z-3). An example compound having both (Z-1) and (Z-2) is a mixture of a compound in which Z is (Z-1) and a compound in which Z is (Z-2). In the table, the column "Z: molar ratio of monoester [%]" indicates the molar ratio [%] of monoester.

[0085] [Table 1]

[0086] [Table 2]

[0087] [Table 3]

[0088] [Table 4]

[0089] Some of the exemplary compounds shown in the table will be specifically described below.

[0090] (Example Compound 1) Exemplary compound 1 is a mixture of a compound (diester) in which Z is (Z-1) and a compound (monoester) in which Z is (Z-2). The compound (monoester) in which Z is (Z-2) is represented, for example, by the structure of Exemplary compound 1-1 below, and the compound (diester) in which Z is (Z-1) is represented, for example, by the structure of Exemplary compound 1-2 below.

[0091] [ka]

[0092] In the case of Exemplary Compound 1, the molar ratio of the compound (monoester) in which Z is (Z-2) is 50%, and Exemplary Compound 1-1 and Exemplary Compound 1-2 are contained in the same molar amount.

[0093] Since l and m are the average addition numbers, even in the case of Exemplified Compound 1 in which l is 5 and m is 5, the number of ethylene oxide structures and the number of alkyl-substituted ethylene oxide structures in one molecule are not necessarily 5.

[0094] (Example Compound 6) Exemplary compound 6 is a compound in which Z is (Z-3), and is represented, for example, by the following exemplary compound 6-1.

[0095] [ka]

[0096] Since l and m are the average addition numbers, even in the case of Exemplary Compound 6 in which l is 10 and m is 5, the number of ethylene oxide structures in one molecule is not necessarily 10 and the number of alkyl-substituted ethylene oxide structures is not necessarily 5.

[0097] In the present invention, the order of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure is not particularly limited, and the compound in which each structure is randomly arranged is also included in the compound defined in the present invention. The order of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure can be arbitrarily changed depending on the synthesis method. For example, the following exemplary compound 6-2 is also included in exemplary compound 6.

[0098] [ka]

[0099] <Method for synthesizing a compound having a structure represented by general formula (II)> The compound having a structure represented by general formula (II) according to the present invention can be synthesized by referring to known methods described in, for example, JP-A-2005-255608, JP-A-2015-000396, JP-A-2015-000970, JP-A-2015-178072, JP-A-2015-178073, and Japanese Patent No. 4,422,866.

[0100] Hereinafter, some of the synthesis methods of the exemplary compounds shown in the table will be specifically explained. Note that the synthesis method of the compound having the structure represented by the general formula (II) according to the present invention is not limited to the synthesis methods described below.

[0101] (Method of synthesizing exemplary compound 53) 130g (1.0 mol) of n-octanol is placed in an autoclave, and potassium hydroxide is used as a catalyst. Under conditions of a pressure of 147 kPa and a temperature of 130°C, 116g (2.0 mol) of propylene oxide is added, and then 88g (2.0 mol) of ethylene oxide is added.

[0102] Next, after confirming that no n-octanol remains, the above adduct is placed in a reactor and reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80° C. for 5 hours. The mixture is then washed with distilled water and the solvent is removed under reduced pressure to obtain the following exemplary compound 53.

[0103] [ka]

[0104] (Method of synthesizing exemplary compound 54) 130g (1.0 mol) of n-octanol is placed in an autoclave, and potassium hydroxide is used as a catalyst. Under conditions of a pressure of 147 kPa and a temperature of 130°C, 116g (2.0 mol) of propylene oxide is added, and then 44g (1.0 mol) of ethylene oxide is added.

[0105] Next, after confirming that no n-octanol remains, the above adduct is placed in a reactor and reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80° C. for 5 hours. The mixture is then washed with distilled water and the solvent is removed under reduced pressure to obtain the following exemplary compound 54.

[0106] [ka]

[0107] (Method of synthesizing exemplary compound 60) 130g (1.0 mol) of 2-ethylhexanol is placed in an autoclave, and potassium hydroxide is used as a catalyst. Under conditions of a pressure of 147 kPa and a temperature of 130°C, 145g (2.5 mol) of propylene oxide is added, and then 110g (2.5 mol) of ethylene oxide is added.

[0108] Next, after confirming that no 2-ethylhexanol remains, the above adduct is placed in a reactor and reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80° C. for 5 hours. The mixture is then washed with distilled water and the solvent is removed under reduced pressure to obtain the exemplary compound 60 shown below.

[0109] [ka]

[0110] (Method of synthesizing exemplary compound 61) 130g (1.0 mol) of 2-ethylhexanol is placed in an autoclave, and potassium hydroxide is used as a catalyst. Under conditions of a pressure of 147 kPa and a temperature of 130°C, 87g (1.5 mol) of propylene oxide is added, and then 66g (1.5 mol) of ethylene oxide is added.

[0111] Next, after confirming that no 2-ethylhexanol remains, the above adduct is placed in a reactor and reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80° C. for 5 hours. The mixture is then washed with distilled water and the solvent is removed under reduced pressure to obtain the following exemplary compound 61.

[0112] [ka]

[0113] <Copper content> The near infrared absorbing agent according to the present invention contains at least one of the component (A) containing a copper ion and the component (B) containing a copper complex, and therefore contains at least either a copper ion or a copper complex.

[0114] <Copper ions> The copper ion contained in the near infrared absorbing agent according to the present invention is a divalent copper ion, which may be solvated.

[0115] <Copper complex> The component (B) contained in the near infrared absorbent according to the present invention is a copper complex coordinated with a compound having a structure represented by general formula (I) and a copper complex coordinated with a compound having a structure represented by general formula (II). The near infrared absorbent according to the present invention may also contain a copper complex coordinated with another compound (e.g., copper acetate, etc.).

[0116] (Copper complex coordinated with a compound having a structure represented by general formula (I)) A copper complex (phosphonate copper complex) coordinated with a compound having a structure represented by general formula (I) is sufficient as long as at least one compound having a structure represented by general formula (I) is coordinated, and also includes a complex coordinated with other compounds.

[0117] The structure of a copper complex (phosphonic acid copper complex) coordinated with a compound having a structure represented by general formula (I) can be represented, for example, by the following general formula (IC).

[0118] [ka]

[0119] In the near infrared absorbing composition of the present invention, the copper complex (phosphonic acid copper complex) in which the compound having the structure represented by general formula (I) is coordinated is mainly in the form of fine particles.

[0120] In the present application, among the hydroxy groups contained in the compound having the structure represented by general formula (I), a hydroxy group that is directly bonded to a phosphorus atom is also referred to as a "reactive hydroxy group".

[0121] The copper complex having the structure represented by general formula (IC) is formed by reacting two reactive hydroxyl groups of the compound having the structure represented by general formula (I) with the same copper ion, but the form of the copper complex coordinated with the compound having the structure represented by general formula (I) according to the present invention is not limited to this form.

[0122] (Copper complex coordinated with a compound having a structure represented by general formula (II)) The copper complex (phosphate ester copper complex or sulfate ester copper complex) coordinated with a compound having a structure represented by general formula (II) may include a complex coordinated with at least one compound having a structure represented by general formula (II), and may also include a complex coordinated with other compounds.

[0123] In the near infrared absorbing composition of the present invention, the copper complex (phosphate ester copper complex or sulfate ester copper complex) coordinated with the compound having the structure represented by general formula (II) is mainly in the form of fine particles or in a dissolved state.

[0124] In the present application, among the hydroxy groups contained in the compound having the structure represented by general formula (II), a hydroxy group that is directly bonded to a phosphorus atom or a sulfur atom is also referred to as a "reactive hydroxy group".

[0125] The form of the copper complex coordinated with the compound having the structure represented by general formula (II) according to the present invention is not necessarily a form formed by reacting two reactive hydroxy groups of the compound having the structure represented by general formula (II) with the same copper ion.

[0126] (Average particle size of copper complex particles) In the near-infrared absorbing composition of the present invention, the copper complex fine particles are preferably uniformly dispersed when a near-infrared absorbing film described later is formed from the viewpoint of spectroscopic characteristics, and for this purpose, it is preferable that the particle size of the copper complex fine particles in the near-infrared absorbing dispersion liquid is small.

[0127] The average particle size of the copper complex fine particles in the near infrared absorbing dispersion is preferably 200 nm or less, more preferably 100 nm or less, and even more preferably 80 nm or less.

[0128] The average particle size of the copper complex fine particles in the near-infrared absorbing dispersion can be measured by a dynamic light scattering method using a zeta potential / particle size measuring system ELSZ-1000ZS manufactured by Otsuka Electronics Co., Ltd.

[0129] <Content of each ingredient> The near-infrared absorbent according to the present invention is characterized in that, when the molar content of the compound having a structure represented by general formula (I) is CA and the molar content of the compound having a structure represented by general formula (II) is CE, the molar ratio CA / CE is within a range of 2.5 to 50. In addition, the molar ratio CA / CE is preferably 3.8 to 10 in terms of near-infrared absorbency and moist heat resistance.

[0130] The high ratio of the phosphonic acid copper complex, which is effective for near-infrared absorbing properties, improves near-infrared absorbing properties. In addition, the low ratio of the ester compound, which causes clouding in a high-temperature, high-humidity environment, improves humidity and heat resistance. For these reasons, the molar ratio CA / CE is preferably 2.5 or more, and more preferably 3.8 or more.

[0131] A certain amount of the phosphate ester compound or sulfate ester compound is necessary to maintain the dispersibility of the complex fine particles, and therefore the molar ratio CA / CE is preferably 50 or less, and more preferably 10 or less.

[0132] The near-infrared absorbent according to the present invention is characterized in that the molar ratio CH / CC, where CC is the molar content of copper constituting the copper ion or copper compound, and CH is the molar content of reactive hydroxy groups contained in the compound having a structure represented by general formula (I) and the compound having a structure represented by general formula (II), is within a range of 1.5 to 2.5.

[0133] By setting the molar ratio CH / CC within this range, the transmittance of light in the visible wavelength range of 400 to 700 nm is increased, and there is no leakage of transmitted light in the vicinity of 1100 nm in the near infrared region, so that efficient absorption performance is maintained and spectral transmittance characteristics with a certain degree of absorption characteristics even at 700 nm, which is at the long wavelength end of visible light, can be realized.

[0134] In the CA regulations, "a compound having a structure represented by general formula (I)" is not limited to the compound having the structure represented by general formula (I) itself used as a raw material, but also includes those that have reacted with other components. For example, it also includes those that have reacted with copper ions to form copper complexes. In this case, the content is counted not by compound unit, but by the unit of "the portion that had the structure represented by general formula (I)" in the copper complex.

[0135] In the CE regulations, the term "compound having a structure represented by general formula (II)" refers not only to the compound having the structure represented by general formula (II) itself used as a raw material, but also to those that have reacted with other components. For example, it also includes those that have reacted with copper ions to form copper complexes. In this case, the content is counted not by compound unit, but by the unit of "the portion that had the structure represented by general formula (II)" in the copper complex.

[0136] In the CC regulations, "copper constituting copper ions or copper compounds" refers to copper in atomic units constituting copper ions or copper compounds.

[0137] In the definition of CH, "a reactive hydroxy group possessed by a compound having a structure represented by general formula (I) and a compound having a structure represented by general formula (II)" refers to a hydroxy group directly bonded to a phosphorus atom or a sulfur atom among the hydroxy groups possessed by a compound having a structure represented by general formula (I) and a compound having a structure represented by general formula (II), and further includes a hydroxy group in which the hydroxy group has reacted with another component, for example, a hydroxy group in which hydrogen has been liberated and oxygen is coordinated to a copper ion.

[0138] (1.2)Organic dyes The near infrared absorbing composition of the present invention preferably contains an organic dye, in that it can adjust the absorption wavelength.The organic dye that can be used can be, for example, a cyanine dye, a squarylium dye, a croconium dye, an azo dye, an anthraquinone dye, a naphthoquinone dye, a phthalocyanine dye, a naphthalocyanine dye, a quaterrylene dye, a dithiol metal complex dye, etc., and is preferably a quaterrylene derivative, a phthalocyanine derivative, a cyanine derivative, or a squarylium derivative, in that it can sufficiently absorb near infrared rays, has high visible light transmittance, and has high heat resistance.

[0139] Specific examples of the quaterrylene derivative include the compounds described in JP-A-2008-009206 and JP-A-2011-225608, and the compounds can be synthesized according to the methods described in these publications.

[0140] Specific examples of phthalocyanine derivatives include compounds described in, for example, JP-A-2000-26748, JP-A-2000-63691, JP-A-2001-106689, JP-A-2004-149752, JP-A-2004-18561, JP-A-2005-220060, JP-A-2007-169343, JP-A-2016-204536, and JP-A-2016-218167, and can be synthesized according to the methods described in these publications.

[0141] The organic dyes that can be used in the present invention are also commercially available, and examples of such dyes include FDR002, FDR003, FDR004, FDR005, and FDN001 (all manufactured by Yamada Chemical Co., Ltd.), Excolor TX-EX720, and Excolor TX-EX708K (all manufactured by Nippon Shokubai Co., Ltd.), Lumogen IR765, Lumogen IR788 (all manufactured by BASF), ABS694, IRA735, IRA742, IRA751, IRA764, IRA788, IRA800 (all manufactured by Exciton), epolight5548, epolight5768 (all manufactured by aako), VIS680E, VIS695A, NIR700B, NIR735B, NIR757A, NIR762A, NIR775B, NIR778A, NIR783C, NIR783I, NIR790B, NIR795A (all manufactured by QCR Examples of such products include trade names such as DLS740A, DLS740B, DLS740C, DLS744A, DLS745B, DLS771A, DLS774A, DLS774B, DLS775A, DLS775B, DLS780A, DLS780C, DLS782F (all manufactured by Crystalin), B4360, B4361, D4773, and D5013 (all manufactured by Tokyo Chemical Industry Co., Ltd.).

[0142] From the viewpoint of spectral characteristics, it is preferable that the organic dye contained in the near infrared absorbing composition of the present invention has a maximum absorption wavelength in the wavelength region of 650 to 800 nm.

[0143] The content of the organic dye is preferably within a range of 0.01 to 1.0% by mass relative to 100% by mass of the near-infrared absorbing agent constituting the near-infrared absorbing composition.

[0144] When the content of the organic dye is 0.01% by mass or more relative to 100% by mass of the near-infrared absorbent, the near-infrared absorption can be sufficiently increased, and when the content is 1.0% by mass or less, the visible light transmittance of the obtained near-infrared absorbing composition is not impaired.

[0145] (1.3) Ultraviolet absorbers From the viewpoints of spectral characteristics and light resistance, it is preferable that the near infrared absorbing composition of the present invention further contains an ultraviolet absorbing agent.

[0146] The ultraviolet absorbing agent is not particularly limited, but examples thereof include benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, salicylic acid ester-based ultraviolet absorbing agents, cyanoacrylate-based ultraviolet absorbing agents, and triazine-based ultraviolet absorbing agents.

[0147] Benzotriazole-based ultraviolet absorbents include, for example, 5-chloro-2-(3,5-di-sec-butyl-2-hydroxylphenyl)-2H-benzotriazole, (2-2H-benzotriazol-2-yl)-6-(straight-chain and side-chain dodecyl)-4-methylphenol, etc. Benzotriazole-based ultraviolet absorbents are also available as commercial products, such as the TINUVIN series, including TINUVIN109, TINUVIN171, TINUVIN234, TINUVIN326, TINUVIN327, TINUVIN328, and TINUVIN928, all of which are commercial products manufactured by BASF.

[0148] Examples of benzophenone-based ultraviolet absorbers include 2-hydroxy-4-benzyloxybenzophenone, 2,4-benzyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfobenzophenone, and bis(2-methoxy-4-hydroxy-5-benzoylphenylmethane).

[0149] Examples of the salicylic acid ester-based ultraviolet absorbers include phenyl salicylate and p-tert-butyl salicylate.

[0150] Examples of cyanoacrylate ultraviolet absorbers include 2'-ethylhexyl-2-cyano-3,3-diphenylacrylate, and ethyl-2-cyano-3-(3',4'-methylenedioxyphenyl)-acrylate.

[0151] Examples of triazine-based ultraviolet absorbents include 2-(2'-hydroxy-4'-hexyloxyphenyl)-4,6-diphenyltriazine, etc. Examples of commercially available triazine-based ultraviolet absorbents include TINUVIN477 (manufactured by BASF).

[0152] The content of the ultraviolet absorbing agent is preferably within the range of 0.1 to 5.0% by mass relative to 100% by mass of the near infrared absorbing agent constituting the near infrared absorbing composition.

[0153] When the content of the ultraviolet absorber is 0.1% by mass or more relative to 100% by mass of the near-infrared absorber, the light resistance can be sufficiently increased, and when the content is 5.0% by mass or less, the visible light transmittance of the obtained near-infrared absorbing composition is not impaired.

[0154] (1.4) Form and production method of near infrared absorbing composition The near-infrared absorbing composition of the present invention may be in the form of a dispersion in which a component such as a near-infrared absorbent is dispersed in a solvent (hereinafter, this state is also referred to as a near-infrared absorbing dispersion), or may be in the form of a film cured together with a curable resin (hereinafter, this state is also referred to as a near-infrared absorbing film).

[0155] <Method for producing near infrared absorbing dispersion> The near-infrared absorbing dispersion can be produced by adding at least a compound having a structure represented by general formula (I), a compound having a structure represented by general formula (II), and a compound serving as a copper ion source to a solvent and mixing them. Depending on the purpose, additives such as organic dyes and ultraviolet absorbers may be added.

[0156] Each component may be added in an amount within the above-mentioned range of content.

[0157] <Solvent> The solvent that can be used in the present invention is not particularly limited, but examples thereof include hydrocarbon solvents, and more preferably, aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, and halogenated solvents.

[0158] Examples of the aliphatic hydrocarbon solvent include non-cyclic aliphatic hydrocarbon solvents such as hexane and heptane, cyclic aliphatic hydrocarbon solvents such as cyclohexane, alcohol solvents such as methanol, ethanol, n-propanol, and ethylene glycol, ketone solvents such as acetone and methyl ethyl ketone, and ether solvents such as diethyl ether, diisopropyl ether, tetrahydrofuran, 1,4-dioxane, and ethylene glycol monomethyl ether. Examples of the aromatic hydrocarbon solvent include toluene, xylene, mesitylene, cyclohexylbenzene, and isopropyl biphenyl. Examples of the halogen-based solvent include methylene chloride, 1,1,2-trichloroethane, and chloroform. In addition, examples of the halogen-based solvent include anisole, 2-ethylhexane, sec-butyl ether, 2-pentanol, 2-methyltetrahydrofuran, 2-propylene glycol monomethyl ether, 2,3-dimethyl-1,4-dioxane, sec-butylbenzene, and 2-methylcyclohexylbenzene. Among these, toluene and tetrahydrofuran are preferred in terms of boiling point and solubility.

[0159] In addition, the ratio of solids (components other than the solvent) to the entire near-infrared absorbing dispersion is preferably within a range of 5 to 30% by mass, since the concentration of solids (e.g., copper complex fine particles) is appropriate, particle aggregation during storage is suppressed, and better stability over time (dispersion stability and near-infrared absorbing properties of copper complex fine particles) can be obtained. A ratio within a range of 10 to 20% by mass is more preferable.

[0160] <Compound having a structure represented by general formula (I)> The compound having a structure represented by general formula (I) (phosphonic acid compound) to be added may be a commercially available product.

[0161] <Compound having a structure represented by general formula (II)> The compound having the structure represented by general formula (II) (phosphate ester compound or sulfate ester compound) to be added may be one obtained by the above-mentioned synthesis method.

[0162] <Copper ion source compound> The compound to be added as the copper ion source is a copper salt capable of supplying divalent copper ions. For example, a copper salt of an organic acid or a copper salt of an inorganic acid can be used. For example, anhydrous copper acetate, anhydrous copper formate, anhydrous copper stearate, anhydrous copper benzoate, anhydrous copper acetoacetate, anhydrous copper ethylacetoacetate, anhydrous copper methacrylate, anhydrous copper pyrophosphate, anhydrous copper naphthenate, anhydrous copper citrate, and other organic acid copper salts, hydrates or hydrates of the copper salts of the organic acids; copper oxide, copper chloride, copper sulfate, copper nitrate, copper phosphate, basic copper sulfate, basic copper carbonate, and other inorganic acid copper salts, hydrates or hydrates of the copper salts of the inorganic acids; and copper hydroxide. <Other additives> The organic dye and the ultraviolet absorbing agent can be those described above.

[0163] <Method for producing near-infrared absorbing film> The near-infrared absorbing film can be produced by dissolving a matrix resin in the above-mentioned near-infrared absorbing dispersion liquid to prepare a coating liquid for forming a near-infrared absorbing film, coating the near-infrared absorbing film-forming liquid on a substrate by spin coating or a wet coating method using a dispenser, and then curing the coating film by performing a predetermined heat treatment. In addition, when coating, the near-infrared absorbing film can be coated on a transparent dielectric substrate, and the near-infrared absorbing film can be directly formed as a near-infrared absorbing layer on the transparent dielectric substrate, so that a near-infrared cut filter described later can be easily produced.

[0164] The thickness of the near infrared absorbing film of the present invention is preferably within the range of 10 to 150 μm, and more preferably within the range of 10 to 100 μm.

[0165] The thickness of the near infrared absorbing film can be measured, for example, using a thickness meter in the following combination. Terminal: DIGIMICRO MH-15M (NIKON) Stand: DIGIMICRO STAND MS-5C (NIKON) Reader: DIGITAL READ OUT TC-101A (NIKON)

[0166] <Matrix resin>

[0167] The matrix resin (also called binder resin) used for forming the near-infrared absorbing film is preferably a curable resin, has optical transparency to visible light and near-infrared light, and is capable of dispersing fine particles of the near-infrared absorbing composition. The copper phosphonate complex is a substance with relatively low polarity, and disperses well in hydrophobic materials. For this reason, it is preferable to use a resin having a polysiloxane structure (silicone), or a resin having an acrylic group, an epoxy group, or a phenyl group as the matrix resin for forming the near-infrared absorbing film.

[0168] Resins having a polysiloxane structure are particularly preferred because they are difficult to thermally decompose, have high optical transparency to visible light and near infrared rays, and have high heat resistance.Specific examples of resins having a polysiloxane structure include KR-255, KR-300, KR-2621-1, KR-211, KR-311, KR-216, KR-212, and KR-251 manufactured by Shin-Etsu Chemical Co., Ltd., and SS-6203, SS-6309, VS-9301, and VS-9506 manufactured by Sanyu Rec Co., Ltd.

[0169] From the viewpoint of low gas permeability and moisture resistance, it is also a preferred embodiment to use a matrix resin having an epoxy group. Specific examples of resins having an epoxy group include KJC-X5 (manufactured by Shin-Etsu Chemical Co., Ltd.), NLD-L-672 (manufactured by Sanyu Rec Co., Ltd.), LE-1421 (manufactured by Sanyu Rec Co., Ltd.), and EpiFine series (manufactured by KISCO Co., Ltd.).

[0170] It is also preferable to use, as the matrix resin of the near-infrared absorbing film, the above-mentioned resin having both a polysiloxane structure and an epoxy group.

[0171] Matrix resins having both a polysiloxane structure and an epoxy group have high heat resistance and moisture resistance, and therefore have suitable properties as materials for image sensors for solid-state imaging devices. Specific examples of resins having both a polysiloxane structure and an epoxy group include the EpiFine series (manufactured by KISCO) and the ILLUMIKA series (manufactured by Kaneka).

[0172] <Other additives> Other additives can be applied to the near-infrared absorbing film of the present invention within a range that does not impair the intended effect of the present invention. Examples of such additives include sensitizers, crosslinking agents, curing accelerators, fillers, heat curing accelerators, thermal polymerization inhibitors, plasticizers, etc., and further, adhesion accelerators to the substrate surface and other auxiliary agents (e.g., conductive particles, fillers, defoamers, flame retardants, leveling agents, peeling accelerators, antioxidants, fragrances, surface tension adjusters, chain transfer agents, etc.) may be used in combination.

[0173] By appropriately incorporating these components, it is possible to adjust the properties such as the stability and film properties of the desired near infrared absorbing film.

[0174] For these components, reference can be made to the contents described in, for example, paragraphs 0183 to 0102 of JP 2012-003225 A, paragraphs 0101 to 0102 of JP 2008-250074 A, paragraphs 0103 to 0104 of JP 2008-250074 A, and paragraphs 0107 to 0109 of JP 2008-250074 A.

[0175] (1.5) Spectral characteristics <Spectral transmittance of near-infrared absorbing dispersion> The near-infrared absorbing composition of the present invention, in the state of a near-infrared absorbing dispersion, when diluted with a solvent and measured so that the maximum spectral transmittance in the wavelength range of 850 to 1,000 nm is 10%, preferably has an average spectral transmittance of 70% or more in the wavelength region of 450 to 600 nm, from the viewpoint of visible light transmittance, more preferably 80% or more, and even more preferably 90% or more.

[0176] As a measuring device for the spectral transmittance, for example, a spectrophotometer V-570 manufactured by JASCO Corporation can be used.

[0177] <Spectral characteristics of near-infrared absorbing film> <Average spectral transmittance> In terms of visible light transmittance, the near infrared absorbing composition of the present invention, in the state of a near infrared absorbing film, preferably has an average spectral transmittance of 80% or more in the wavelength range of 450 to 600 nm.

[0178] Moreover, it is preferable from the viewpoint of near infrared absorptivity that the absorption rate is 10% or less within a wavelength range of 850 to 1,000 nm.

[0179] Moreover, it is preferable from the viewpoint of near infrared absorption that the content is 1% or less within the wavelength range of 750 to 1,080 nm.

[0180] <Cutoff wavelength> The near-infrared absorbing composition of the present invention, in the form of a near-infrared absorbing film, has a spectral transmittance that decreases with increasing wavelength within a wavelength range of 600 to 700 nm, and when a wavelength at which the spectral transmittance is 50% within a wavelength range of 600 to 700 nm is defined as a cut-off wavelength, it is preferable from the viewpoint of near-infrared absorbency that the cut-off wavelength for light incident on the surface at an incident angle of 0° is within a range of 600 to 680 nm.

[0181] The spectral transmittance in the state of the near-infrared absorbing film can also be measured using a spectrophotometer V-570 manufactured by JASCO Corporation.

[0182] (1.6) Uses of near infrared absorbing composition The near-infrared absorbing film of the present invention (the near-infrared absorbing composition in the state of a film cured together with a curable resin) is suitable for constituting, for example, visibility correction members for CCDs, CMOSs ​​or other light receiving elements, photometric members, heat ray absorbing members, composite optical filters, lens members (eyeglasses, sunglasses, goggles, optical systems, optical waveguide systems), fiber members (optical fibers), noise cutting members, display covers or display filters such as plasma display front panels, projector front panels, light source heat ray cutting members, color tone correction members, illumination brightness adjustment members, optical elements (light amplification elements, wavelength conversion elements, etc.), Faraday elements, optical communication functional devices such as isolators, elements for optical disks, etc.

[0183] (2) Near-infrared cut filter The near-infrared cut filter of the present invention is a near-infrared cut filter comprising a near-infrared absorbing layer on at least one surface of a transparent dielectric substrate, and is characterized in that the near-infrared absorbing layer contains the near-infrared absorbing composition of the present invention.

[0184] It is also preferable to further provide a dielectric multilayer film on at least one surface of the transparent dielectric substrate, since this allows the spectral characteristics of the near-infrared cut filter to be more freely adjusted.

[0185] The near-infrared absorbing layer and the dielectric multilayer film may be provided in contact with the transparent dielectric substrate, or may be provided via another intermediate layer.

[0186] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of the near-infrared cut filter of the present invention.

[0187] The near-infrared cut filter 9 shown in FIG. 1 comprises a near-infrared absorbing layer 22 on one surface of a transparent dielectric substrate 21, and further comprises a dielectric multilayer film 23 on the other surface.

[0188] The transparent dielectric substrate is not particularly limited in terms of material as long as the object of the present invention is achieved. For example, it may be made of glass or an optical resin such as polycarbonate (PC), polymethyl methacrylate (PMMA), cycloolefin polymer (COP), or silicone.

[0189] The transparent dielectric substrate preferably has a thickness of 0.01 to 1 mm.

[0190] Since the transparent dielectric substrate needs to transmit visible light, it preferably has an average spectral transmittance of 80% or more in the wavelength range of 450 to 600 nm.

[0191] The near-infrared absorbing film of the present invention can be applied to the near-infrared absorbing layer. As described above, a near-infrared absorbing film can be directly formed as a near-infrared absorbing layer on a transparent dielectric substrate to produce a near-infrared cut filter.

[0192] A dielectric multilayer film is a film formed by laminating multiple layers made of materials with different refractive indices, and is used to control the transmittance of each wavelength of light. By providing it together with a near-infrared absorbing layer, the spectral characteristics of the near-infrared cut filter can be adjusted more freely.

[0193] The spectral characteristics of the dielectric multilayer film can be adjusted by the thickness and type of material of each layer. For example, the material of each layer can be a dielectric material such as titanium oxide, silicon oxide, aluminum oxide, zirconium oxide, tantalum pentoxide, niobium pentoxide, lanthanum oxide, yttrium oxide, zinc oxide, zinc sulfide, indium oxide, silica, alumina, lanthanum fluoride, magnesium fluoride, sodium aluminum hexafluoride, etc.

[0194] A near-infrared cut filter having a dielectric multilayer film can be manufactured by laminating each dielectric layer on a transparent dielectric substrate by a method such as a vacuum deposition method, a chemical vapor deposition (CVD) method, a sputtering method, etc. Alternatively, the near-infrared cut filter can be manufactured by bonding a separately prepared dielectric multilayer film to a transparent dielectric substrate with an adhesive.

[0195] (3) Image sensors for solid-state imaging devices The image sensor for a solid-state imaging device of the present invention is characterized by comprising the near-infrared cut filter of the present invention.

[0196] The image sensor for a solid-state imaging element refers to a component that mainly comprises a solid-state imaging element substrate having a light receiving element.

[0197] The image sensor for a solid-state imaging device of the present invention is not particularly limited in terms of other members, etc., as long as it includes the near-infrared cut filter of the present invention. For example, it may include a planarizing layer, a glass substrate, etc.

[0198] FIG. 2 is a schematic cross-sectional view showing an example of the configuration of an image sensor for a solid-state imaging device according to the present invention.

[0199] 2 is composed of a solid-state imaging element substrate 10 having a light receiving element on the light receiving side surface of a silicone substrate, a planarization layer 8 provided on the solid-state imaging element substrate 10, a near infrared cut filter 9 provided on the planarization layer 8, and a glass substrate 3 (light-transmitting substrate) arranged above the near infrared cut filter 9. Each member is bonded with an adhesive 2.

[0200] (4) Camera module The camera module of the present invention is characterized by including the image sensor for solid-state imaging device of the present invention.

[0201] The camera module of the present invention is not particularly limited in terms of other components, etc., so long as it includes the image sensor for solid-state imaging device of the present invention, and may include, for example, an imaging lens, a lens holder, a light-shielding and electromagnetic shield, etc.

[0202] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of a camera module of the present invention.

[0203] 3 is configured to include a solid-state imaging element image sensor (solid-state imaging element substrate 10, planarization layer 8, near-infrared cut filter 9, glass substrate 3), a lens holder 5 arranged above the solid-state imaging element image sensor and having an imaging lens 4 in its internal space, and a light-shielding and electromagnetic shield 6 arranged to surround the solid-state imaging element image sensor. Each member is bonded with an adhesive 7.

[0204] Furthermore, the camera module 1 is connected to a circuit board 12, which is a mounting board, via solder balls 11 (connecting material), which are connecting members.

[0205] In the camera module 1, incident light L from the outside passes through the imaging lens 4, the glass substrate 3, the infrared cut filter 9, and the planarization layer 8 in this order, before reaching the light receiving element of the solid-state imaging element substrate . EXAMPLES

[0206] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.

[0207] Example 1 <Preparation of near infrared absorbing composition (dispersion)> [Preparation of near infrared absorbing composition (dispersion) 1] 2.00 g (CC=10 mmol) of copper(II) acetate monohydrate (Kanto Chemical Co., Ltd.; hereinafter, simply referred to as "copper acetate") and 82 g of tetrahydrofuran (THF) were mixed and stirred for 3 hours. The liquid was then filtered to remove insoluble matter, to prepare a copper acetate solution.

[0208] 1.73 g (CE=2.8 mmol) of the synthesized exemplary compound 76, which is a compound having a structure represented by general formula (II), was dissolved in 7 g of THF. The synthesized exemplary compound 76 was used.

[0209] The above THF solution was added to the above copper acetate solution, and the mixture was stirred at room temperature for 30 minutes to prepare liquid A.

[0210] Liquid B was prepared by dissolving 0.78 g (CA=7.1 mmol) of ethylphosphonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), which is a compound having a structure represented by general formula (I), in 7 g of THF.

[0211] While stirring the solution A, solution B was added to the solution A, and the mixture was stirred at room temperature for 16 hours to prepare solution C (CH=18.7 mmol).

[0212] Liquid C and 30 g of toluene were placed in a flask, and while heating at 50 to 100°C in an oil bath (Tokyo Rika Kikai Co., Ltd., model: OSB-2100), the solvent and acetic acid were removed for 30 minutes using a rotary evaporator (Tokyo Rika Kikai Co., Ltd., model: N-1000).

[0213] Thereafter, the amount of the solvent was adjusted so that the solid content concentration of the liquid C in the flask became 10 mass %.

[0214] CH was calculated as follows: The molar content of reactive hydroxy groups in the compound having the structure represented by general formula (I) is 7.1 mmol x 2, or 14.2 mmol. The molar content of reactive hydroxy groups in the compound having the structure represented by general formula (II) is (2.8 mmol×60%×2)+(2.8 mmol×40%×1), which is 4.5 mmol. Therefore, the total molar content of reactive hydroxy groups in the compound having the structure represented by general formula (I) and the compound having the structure represented by general formula (II), CH, is 14.2 mmol + 4.5 mmol, or 18.7 mmol.

[0215] [Preparation of near infrared absorbing compositions (dispersions) 2 to 43] Near infrared absorbing compositions (dispersions) 2 to 43 were prepared in the same manner as in the preparation of the near infrared absorbing composition (dispersion) 1, except that the type and addition amount [mmol] of the phosphonic acid compound represented by general formula (I) and the type and addition amount [mmol] of the phosphate ester compound or sulfate ester compound represented by general formula (II) were changed to the configurations shown in Table V.

[0216] The exemplary compounds used as the phosphate ester compound or sulfate ester compound represented by the general formula (II) are the exemplary compounds shown in Tables I to IV, and were synthesized.

[0217] As the comparative compound A, Plysurf A208F (manufactured by Daiichi Kogyo Co., Ltd.) was used. Comparative Example Compound A is a compound represented by the general formula (II): 2 is an alkyl group having 8 carbon atoms, the average number of added ethylene oxide structures, l, is 3, and the average number of added alkyl-substituted ethylene oxide structures, m, is 0.

[0218] Comparative Example Compound B was a synthesized compound. Comparative Example Compound B is a compound represented by the general formula (II): 2 is an n-octyl group, the average number of added ethylene oxide structures l is 0, the average number of added alkyl-substituted ethylene oxide structures m is 3, Z is (Z-1) and (Z-2), and the molar ratio of the monoester (Z-2) is 50%.

[0219] The compositions of the near infrared absorbing compositions (dispersions) 1 to 43 prepared as above are shown in Table V below.

[0220] [Table 5]

[0221] <Evaluation of near-infrared absorbing dispersion> The near infrared absorbing dispersions prepared as above were evaluated as follows.

[0222] [Average visible light transmittance of dispersion] The near infrared absorbing dispersions 1 to 43 prepared above were each diluted with toluene so that the maximum spectral transmittance in the wavelength range of 850 to 1,000 nm was 10%. The spectral transmittance of the diluted dispersion in the wavelength range of 450 to 600 nm was measured using a spectrophotometer V-570 manufactured by JASCO Corporation, and the average spectral transmittance in the range was calculated. The calculated average spectral transmittance in the wavelength range of 450 to 600 nm was evaluated according to the following criteria. The evaluation results are shown in Table VI as the average visible light transmittance.

[0223] ⊚: The average spectral transmittance in the range is 90% or more. ◯: The average spectral transmittance in the range is 80% or more and less than 90%. Δ: The average spectral transmittance in the range is 70% or more and less than 80%. ×: The average spectral transmittance in the range is less than 70%.

[0224] [Average particle size of fine particles in dispersion] The near infrared absorbing dispersions 1 to 43 prepared above were each diluted with toluene so that the solid content concentration was 0.5% by mass. The average particle size of the fine particles in the diluted dispersion was measured by dynamic light scattering using a zeta potential / particle size measurement system ELSZ-1000ZS manufactured by Otsuka Electronics Co., Ltd. The measured average particle size was evaluated according to the following criteria. The evaluation results are shown in Table VI.

[0225] ◎: The average particle size is 80 nm or less. ◯: The average particle size is greater than 80 nm and less than or equal to 100 nm. Δ: The average particle size is greater than 100 nm and less than 200 nm. ×: The average particle size is greater than 200 nm.

[0226] <Preparation of near-infrared absorbing composition (film)> Each of the near-infrared absorbing compositions (dispersions) 1 to 43 prepared above was mixed with a curable resin having a polysiloxane structure (KR-311 manufactured by Shin-Etsu Chemical Co., Ltd.) so that the solid content ratio of the resin was 70 mass %, to prepare each coating liquid for forming a near-infrared absorbing film.

[0227] Next, each near-infrared absorbing film-forming coating liquid was cast onto a glass substrate so as to have a film thickness that would result in a maximum spectral transmittance of 10% in the wavelength range of 850 to 1,000 nm after curing, and pre-baked on a hot plate at 50° C. for 60 minutes. Next, the coating liquid was cured by heating on a hot plate at 150° C. for 2 hours to form near-infrared absorbing compositions (films) 1 to 43.

[0228] <Evaluation of near-infrared absorbing film> The near infrared absorbing films prepared as above were evaluated as follows.

[0229] [Average visible light transmittance of film] The spectral transmittance of the near infrared absorbing films 1 to 43 prepared above in the wavelength range of 450 to 600 nm was measured using a spectrophotometer V-570 manufactured by JASCO Corporation, and the average spectral transmittance in the range was calculated. At this time, the influence of the reflection at the interface was eliminated by using the glass substrate as a base. The calculated average spectral transmittance in the wavelength range of 450 to 600 nm was evaluated according to the following criteria. The evaluation results are shown in Table VI as the average visible light transmittance.

[0230] ⊚: The average spectral transmittance in the range is 90% or more. ◯: The average spectral transmittance in the range is 80% or more and less than 90%. Δ: The average spectral transmittance in the range is 70% or more and less than 80%. ×: The average spectral transmittance in the range is less than 70%.

[0231] [Wet and heat resistance of film] The near infrared absorbing films 1 to 43 prepared above were stored at 85°C and 85% RH for 7 days. The average visible light transmittance after storage was measured in the same manner as before storage. The average visible light transmittance value after storage was subtracted from the average visible light transmittance value before storage to calculate a value (average visible light transmittance difference). The calculated average visible light transmittance difference was evaluated according to the following criteria. The evaluation results are shown in Table VI as humidity heat resistance.

[0232] ⊚: The average visible light transmittance difference is 3% or less. ◯: The average visible light transmittance difference is greater than 3% and equal to or less than 5%. △: The average visible light transmittance difference is greater than 5% and equal to or less than 10%. ×: The average visible light transmittance difference is greater than 10%.

[0233] [Film Thickness] The thicknesses of the near-infrared absorbing films 1 to 43 prepared above were measured using a thickness meter in the following combination. Terminal: DIGIMICRO MH-15M (NIKON) Stand: DIGIMICRO STAND MS-5C (NIKON) Reader: DIGITAL READ OUT TC-101A (NIKON)

[0234] The measured film thickness was evaluated according to the following criteria, and the evaluation results are shown in Table VI.

[0235] ⊚: The film thickness is 100 μm or less. ◯: The film thickness is greater than 100 μm and less than 150 μm. ×: The film thickness is greater than 150 μm.

[0236] [Table 6]

[0237] Example 2 <Preparation of near infrared absorbing composition (dispersion)> [Preparation of near infrared absorbing composition (dispersion) 44] The following organic dye was dissolved in 36 g of anisole and added to Liquid C, which had been prepared so as to have the same composition as the near-infrared absorbing composition (dispersion liquid) 3 prepared above. FDR004 (Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 716 nm) 1.98 mg FDR005 (Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 725 nm) 1.07 mg LumogenIR765 (BASF) 4.07mg

[0238] Liquid C, to which an organic dye dissolved in anisole had been added, was placed in a flask, and while heating at 55-90°C in an oil bath (Tokyo Rika Kikai Co., Ltd., model: OSB-2100), the solvent and acetic acid were removed for 3 hours using a rotary evaporator (Tokyo Rika Kikai Co., Ltd., model: N-1000).

[0239] Thereafter, the amount of the solvent was adjusted so that the solid content concentration of the liquid C in the flask became 10 mass %.

[0240] [Preparation of near infrared absorbing composition (dispersion) 45] Near infrared absorbing composition (dispersion liquid) 45 was prepared in the same manner, except that the organic dye added to the C liquid was changed to the following organic dye. 1,1'-Dibutyl-3,3,3',3'-tetramethyl-indotricarbocyanineHexafluorophosphate (maximum absorption wavelength: 766 nm, manufactured by Tokyo Chemical Industry Co., Ltd.) 8.03 mg FDR004 (Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 716 nm) 2.47 mg

[0241] [Preparation of near infrared absorbing composition (dispersion) 46] Near infrared absorbing composition (dispersion liquid) 46 was prepared in the same manner, except that the organic dye added to the solution C was changed to the following organic dye. Squarylium dye (maximum absorption wavelength: 710 nm) 1.23 mg FDR005 (Yamada Chemical Industry Co., Ltd., maximum absorption wavelength: 725 nm) 1.34 mg LumogenIR765 (BASF) 3.05mg

[0242] As the squarylium dye (maximum absorption wavelength: 710 nm), the dye (A11-1) described in Japanese Patent No. 624895 was used.

[0243] The compositions of near infrared absorbing compositions 44 to 46 are shown in Table VII below. [Table 7]

[0244] <Evaluation of near-infrared absorbing dispersion> For the near-infrared absorbing dispersions 44 to 46 prepared above, the "average visible light transmittance of the dispersion" and the "average particle size of the fine particles in the dispersion" were measured in the same manner as in Example 1, and evaluated according to the same criteria. The evaluation results are shown in Table VIII.

[0245] <Preparation of near-infrared absorbing composition (film)> Each of the near-infrared absorbing compositions (dispersions) 44 to 46 prepared above was mixed with a curable resin having a polysiloxane structure (KR-311 manufactured by Shin-Etsu Chemical Co., Ltd.) so that the solid content ratio of the resin was 50 mass %, to prepare each coating liquid for forming a near-infrared absorbing film.

[0246] Next, each near-infrared absorbing film-forming coating liquid was cast onto a glass substrate so as to have a film thickness that would result in a maximum spectral transmittance of 10% in the wavelength range of 850 to 1,000 nm after curing, and pre-baked on a hot plate at 50° C. for 60 minutes. Next, the coating liquid was cured by heating on a hot plate at 150° C. for 2 hours to form near-infrared absorbing compositions (films) 44 to 46.

[0247] <Evaluation of near-infrared absorbing film> For the near infrared absorbing films 44 to 46 prepared above, the "average visible light transmittance of the film," "humid heat resistance of the film," and "film thickness" were measured in the same manner as in Example 1, and evaluated according to the same criteria. The evaluation results are shown in Table VIII.

[0248] [Table 8]

[0249] Example 3 <Preparation of near-infrared absorbing composition (film)> The near-infrared absorbing composition (dispersion) 44 prepared above and a curable resin having a polysiloxane structure (KR-311 manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed so that the solid content ratio of the resin was 50 mass %, to prepare each coating liquid for forming a near-infrared absorbing film.

[0250] Next, each near-infrared absorbing film-forming coating liquid was cast onto a glass substrate so that the film thickness after curing would be 100 μm, and pre-baked on a hot plate at 50° C. for 60 minutes. Next, it was cured by heating on a hot plate at 150° C. for 2 hours to form a near-infrared absorbing composition (film) 47.

[0251] Near infrared absorbing compositions (dispersions) 45 and 46 prepared above were similarly used to form near infrared absorbing compositions (films) 48 and 49 so as to have a film thickness of 100 μm.

[0252] <Evaluation of near-infrared absorbing film> [Cutoff wavelength of film] For the near infrared absorbing composition films 47 to 49 prepared above, the spectral transmittance of light in the wavelength range of 600 to 700 nm incident on the surface at an incident angle of 0° was measured. As a result, it was confirmed that in all the near infrared absorbing composition films, the spectral transmittance decreased with increasing wavelength within the range. In addition, it was confirmed that in all the near infrared absorbing composition films, the cutoff wavelength within the range (the wavelength at which the spectral transmittance is 50%) was in the wavelength range of 600 to 680 nm.

[0253] [Spectral transmittance of film in the wavelength range of 750 to 1,080 nm] For the near-infrared absorbing composition films 47 to 49 prepared above, the spectral transmittance was measured in the wavelength range of 750 to 1,080 nm. As a result, it was confirmed that the spectral transmittance was 1% or less in that range for all of the near-infrared absorbing composition films, that is, the average spectral transmittance in that range was 1% or less. [Explanation of symbols]

[0254] 1 Camera module 2, 7 Adhesive 3. Glass substrate 4 Imaging lens 5 Lens holder 6 Light shielding and electromagnetic shielding 8 Planarization layer 9 Near infrared cut filter 10 Solid-state image sensor board 11 Solder ball 12 Circuit Board 14. Image sensors for solid-state imaging devices 21 Transparent dielectric substrate 22 Near infrared absorbing layer 23 Dielectric multilayer film

Claims

1. A near infrared absorbing composition containing a near infrared absorbing agent, The near-infrared absorbent contains at least one of the following components (A) and (B): The molar ratio CA / CE, where CA is the molar content of the compound having a structure represented by the following general formula (I) and CE is the molar content of the compound having a structure represented by the following general formula (II), is within a range of 3.8 to 10, and A near infrared absorbing composition, characterized in that a molar ratio CH / CC, where CC is the molar content of copper ions and CH is the molar content of reactive hydroxy groups possessed by a compound having a structure represented by the following general formula (I) and a compound having a structure represented by the following general formula (II), is within a range of 1.5 to 2.

5. Ingredients: Component (A): A component consisting of a compound having a structure represented by the following general formula (I), a compound having a structure represented by the following general formula (II), and copper ions. Component (B): A component consisting of a copper complex coordinated with a compound having a structure represented by the following general formula (I) and a copper complex coordinated with a compound having a structure represented by the following general formula (II): [Case 1] [In the above general formula (I), R 1 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent. [Case 2] [In the above general formula (II), R 2 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent. 21 ~R 24 Each of R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structures each of which is a hydrogen atom, and is within the range of 1 to 19. 21 ~R 24represents the average number of partial structures added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 1 to 19. l+m is the total number of l and m, and is within the range of 2 to 20. Z represents a structural unit selected from the following general formulae (Z-1) to (Z-3). [C3] (In the above general formulas (Z-1) to (Z-3), * represents a bonding site and bonds to O in the above general formula (II).)

2. R in the general formula (I) 1 The near infrared absorbing composition according to claim 1, wherein is an alkyl group having 1 to 20 carbon atoms.

3. 3. The near infrared absorbing composition according to claim 1, further comprising an organic dye.

4. 4. The near infrared absorbing composition according to claim 3, wherein the organic dye is a quaterrylene derivative, a phthalocyanine derivative, a cyanine derivative or a squarylium derivative.

5. A near infrared absorbing composition according to any one of claims 1 to 4, and a curable resin, A near-infrared absorbing film, characterized in that it is in a cured film state.

6. The average spectral transmittance is 80% or more in the wavelength range of 450 to 600 nm, The average spectral transmittance is 10% or less in the wavelength range of 850 to 1,000 nm, and 6. The near infrared absorbing film according to claim 5, wherein the film thickness is within a range of 10 to 150 μm.

7. The average spectral transmittance is 1% or less in the wavelength range of 750 to 1,080 nm; The spectral transmittance decreases with increasing wavelength within the wavelength range of 600 to 700 nm, When a wavelength at which the spectral transmittance is 50% within a wavelength range of 600 to 700 nm is defined as a cutoff wavelength, the cutoff wavelength for light incident on the surface at an incident angle of 0° is within a range of 600 to 680 nm, and 7. The near infrared absorbing film according to claim 5, wherein the film thickness is within a range of 10 to 100 μm.

8. A near-infrared cut filter having a near-infrared absorbing layer on at least one surface of a transparent dielectric substrate, A near-infrared cut filter, wherein the near-infrared absorbing layer is the near-infrared absorbing film according to any one of claims 5 to 7.

9. 9. The near infrared cut filter according to claim 8, further comprising a dielectric multilayer film on at least one surface of the transparent dielectric substrate.

10. 10. An image sensor for a solid-state imaging device, comprising the near-infrared cut filter according to claim 8.

11. A camera module comprising the image sensor for a solid-state imaging device according to claim 10.

Citation Information

Patent Citations

  • Holeless basket type centrifugal separator

    JP1980054048A

  • Optical recording and reproducing unit

    JP1981011631A

  • Near-infrared ray absorber, method for producing the same and optical material

    JP2011099038A

  • Infrared absorptive composition, infrared-cut filter, and imaging optical system

    JP2018090809A

  • Optical filter, camera module, and information terminal

    JP2019028163A