Color filter, display device, electronic paper, white display method, and composition for forming color-adjusting member
The color filter with optimized subpixel arrangement and tint adjustment member enhances electronic paper displays by achieving bright and vivid colors, including a brighter white with low saturation, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2020164819
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing electronic paper technologies struggle to display vivid colors and bright white with low saturation due to limited external light and the absence of a black matrix, leading to dark and unsatisfactory displays.
A color filter with red, green, and blue subpixels, and optionally yellow subpixels, is designed to achieve Y values between 70 and 98 in the CIE1931 color system, accompanied by a tint adjustment member between subpixels to enhance brightness and saturation, particularly in white displays.
The solution enables bright and vivid color display with low saturation, particularly in white, by optimizing the color filter arrangement and using a tint adjustment member to maximize light transmission and improve display quality.
Smart Images

Figure 0007552207000004 
Figure 0007552207000005 
Figure 0007552207000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a color filter, a display device, electronic paper, a white display method, and a composition for forming a color adjusting member. [Background technology]
[0002] Taking advantage of their characteristics such as light weight, thinness, and low power consumption, liquid crystal display devices are used in various applications such as televisions, notebook computers, personal digital assistants, smartphones, digital cameras, etc. Liquid crystal display devices are required to have optimal colors out of three to six primary colors depending on the application, and color filter substrates that provide various color performance are used.
[0003] In recent years, electronic paper has been increasingly used as a display device other than liquid crystal display devices. Electronic paper has features such as low power consumption and being easy on the eyes, and efforts are being made to make it colorized. To achieve colorization, color ink methods and color filter methods are being considered, but the color filter method is attracting attention from the perspective of display switching speed.
[0004] Unlike general liquid crystal display devices, electronic paper does not adjust brightness using backlight light, but instead uses external light as a display principle, which means that the display is dark. To improve the vividness of the display, electronic paper that does not have a black matrix between pixels and electronic paper that has a white light-shielding material between pixels have been proposed (for example, Patent Document 1 and Patent Document 2). However, these technologies have not been able to achieve both vivid display of each color and low saturation and bright white display. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-107234 A [Patent Document 2] JP 2013-88750 A Summary of the Invention [Problem to be solved by the invention]
[0006] When displaying each color using electronic paper with color filters, the amount of external light required for display is small, and it is necessary to design each pixel color to display the desired color. Therefore, when displaying white, it is difficult to display the desired white, and improvement was required.
[0007] In view of this situation, the present invention aims to provide a color filter, and in particular a reflective display device, that is capable of displaying each color brightly and vividly, even in a reflective display device, and that is capable of displaying a bright white color with low saturation when displaying white. [Means for solving the problem]
[0008] The present invention is a color filter having at least any one of red, green and blue sub-pixels on a substrate, characterized in that a color-adjusting member having a Y value of 70 or more and 98 or less in the CIE 1931 color system is disposed between the sub-pixels.
[0009] The present invention also relates to a display device comprising the color filter of the present invention.
[0010] The present invention also relates to electronic paper having the color filter of the present invention.
[0011] The present invention also relates to a composition for forming a color adjusting member, which is characterized in that when formed into a film having a thickness of 2 μm, the Y value in the CIE 1931 color system is 70 or more and 98 or less. Effect of the Invention
[0012] According to the color filter of the present invention, even in a reflective display device, each color can be displayed brightly and vividly, and when white is displayed, bright white with low saturation can be displayed. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a diagram showing an example of the arrangement of red, green and blue sub-pixels and color adjusting members. [Diagram 2] FIG. 2 is a diagram showing an example of the arrangement of red, green, blue and fourth sub-pixels, as well as color adjusting members. [Diagram 3] FIG. 3 is a diagram showing an example of the arrangement of red, green, blue and yellow sub-pixels and color adjusting members. [Figure 4] FIG. 4 is a diagram showing another example of the arrangement of the red, green, blue and fourth sub-pixels, and the color adjusting members. [Diagram 5] FIG. 5 is a diagram showing another example of the arrangement of red, green, blue and yellow sub-pixels and color adjusting members. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below. In the present invention, the term "not less than" means that the value is equal to or greater than the indicated value. The term "not more than" means that the value is equal to or smaller than the indicated value.
[0015] The color filter of the present invention has a substrate. Examples of the substrate include inorganic glass plates such as soda glass, non-alkali glass, borosilicate glass, quartz glass, aluminoborosilicate glass, aluminosilicate glass, alkali aluminosilicate glass, and soda lime glass with a silica-coated surface, and organic plastic films and sheets. Two or more of these may be laminated. In addition, when the display device equipped with the color filter of the present invention is a reflective display device or a display device having a light-emitting element such as a silicon OLED, the substrate may be opaque.
[0016] The organic plastic film or sheet may be a self-supporting film, or may be a film formed by coating on a substrate such as a glass substrate. In the case of such a coating film, the adhesion between the substrate and the film can be appropriately adjusted by a laser or the like to peel it off. Examples of organic plastic materials include polyesters such as polypropylene, polyethylene, polystyrene, and polyethylene terephthalate (PET), fluorine-containing polymers such as polyphenylene sulfide (PPS), polyimide, polyamide, polyamideimide, polyethersulfone, and polytetrafluoroethylene (PTFE), polyetheretherketone, polyphenylene ether, polyarylate, and polysulfone.
[0017] When the substrate is an organic plastic film, the substrate is preferably a film having a thickness of 5 μm or more, more preferably 10 μm or more, from the viewpoint of substrate strength, whereas the substrate is preferably a film having a thickness of 100 μm or less, from the viewpoint of flexibility.
[0018] The color filter of the present invention has at least any one of red (R), green (G) and blue (B) subpixels on the substrate. In the present invention, a subpixel refers to each single-color point that constitutes one pixel on a display. By having any one of red, green and blue subpixels, it is possible to display a color corresponding to each pixel or an additive color mixture of these colors. In addition, it is preferable to have red, green and blue subpixels on the substrate, since this makes it possible to express colors inside the RGB color triangle, whose vertices are the three primary colors of RGB.
[0019] It is more preferable to have a yellow (Y) subpixel in addition to red, green, and blue. This allows the color inside the quadrilateral consisting of the four vertices of RYGB to be expressed, making the golden color of brass instruments more vivid.
[0020] Examples of materials constituting the coloring composition that forms the sub-pixels include coloring compositions that contain a coloring material, a binder resin such as an acrylic resin or a polyimide resin, and a radical polymerizable compound.
[0021] Examples of coloring materials contained in the coloring composition include organic pigments, inorganic pigments, dyes, etc., and the coloring composition may contain two or more of these. Among these, organic pigments and dyes are preferred from the viewpoint of further improving the transmittance.
[0022] Examples of red colorants include CI Pigment Red (hereinafter, "PR") 9, PR48, PR97, PR122, PR123, PR144, PR149, PR166, PR168, PR177, PR179, PR180, PR192, PR209, PR215, PR216, PR217, PR220, PR223, PR224, PR226, PR227, PR228, PR240, PR254, and diketopyrrolopyrrole colorants having a bromine group. From the viewpoint of the luminance characteristics of the subpixel, PR254, PR177, and diketopyrrolopyrrole colorants having a bromine group are preferred, and from the viewpoint of the brightness and vividness of the red display of the electronic paper, it is preferred to use a diketopyrrolopyrrole colorant having a bromine group. From the viewpoint of brightness, vividness and display color of red display of electronic paper, it is preferable that the ratio of the diketopyrrolopyrrole color material having a bromine group to the color materials contained in the red subpixel is 70% by mass or more.
[0023] Examples of green colorants include CI pigment green (hereinafter referred to as "PG") PG1, PG2, PG4, PG7, PG8, PG10, PG13, PG14, PG15, PG17, PG18, PG19, PG26, PG36, PG38, PG39, PG45, PG48, PG50, PG51, PG54, PG55, PG58, PG59, etc. From the viewpoint of the luminance characteristics of the subpixel, PG58 and PG59 are preferable.
[0024] Examples of yellow colorants include CI Pigment Yellow (hereinafter, "PY") 12, PY13, PY17, PY20, PY24, PY83, PY86, PY93, PY95, PY109, PY110, PY117, PY125, PY129, PY137, PY138, PY139, PY147, PY148, PY150, PY153, PY154, PY166, PY168, and PY185. From the viewpoints of color purity, transmittance, and contrast ratio, PY129, PY138, PY139, and PY150 are preferred, PY138 and PY150 are more preferred, and PY150 is even more preferred.
[0025] Examples of orange colorants include CI Pigment Orange (hereinafter, "PO") 13, PO31, PO36, PO38, PO40, PO42, PO43, PO51, PO55, PO59, PO61, PO64, PO65, and PO71.
[0026] Examples of blue colorants include CI Pigment Blue (hereinafter, "PB") 15, PB15:3, PB15:4, PB15:6, PB21, PB22, PB60, and PB64.
[0027] Examples of purple colorants include CI Pigment Violet (hereinafter referred to as "PV") 19, PV23, PV29, PV30, PV32, PV37, PV40, and PV50 (all numbers are Color Index Nos.).
[0028] The coloring material may be a dye, and examples of the dye include oil-soluble dyes, acid dyes, direct dyes, basic dyes, acid mordant dyes, etc. In addition, the dye may be made into a lake, or may be made into a salt-forming compound of the dye and a nitrogen-containing compound.
[0029] Examples of red, green, blue, purple or yellow dyes include direct dyes, acid dyes, and basic dyes. Specific examples of these dyes include azo dyes, benzoquinone dyes, naphthoquinone dyes, anthraquinone dyes, xanthene dyes, cyanine dyes, squarylium dyes, croconium dyes, merocyanine dyes, stilbene dyes, diarylmethane dyes, triarylmethane dyes, fluoran dyes, spiropyran dyes, phthalocyanine dyes, indigo dyes, fulgide dyes, nickel complex dyes, and azulene dyes. The dye may be dissolved in the coloring composition or dispersed as particles.
[0030] The coloring composition may contain a radical polymerizable compound. Examples of the radical polymerizable compound contained in the coloring composition include ethylene oxide modified products or propylene oxide modified products such as dipentaerythritol penta(meth)acrylate, tetratrimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, penta(meth)acryloyloxy dipentaerythritol monosuccinic acid ester, dipentaerythritol hexa(meth)acrylate, styrene derivatives, polyfunctional maleimide compounds, poly(meth)acrylate carbamates, adipic acid 1,6-hexanediol (meth)acrylic acid esters, fluoroanhydrides, and the like. Examples of the methacrylic acid ester include oligomers such as propylene oxide methacrylate, diethylene glycol trimellitic acid ester, rosin-modified epoxy di(meth)acrylate, and alkyd-modified (meth)acrylate, bifunctional (meth)acrylates such as tripropylene glycol di(meth)acrylate and 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, triacrylformal, bisphenoxyethanol fluorene diacrylate, dicyclopentanedienyl diacrylate, and alkyl-modified, alkyl ether-modified, and alkyl ester-modified products thereof. Two or more of these may be contained.
[0031] From the viewpoint of patterning property, the content of the radical polymerizable compound is preferably 40% by mass or more in the solid content of the coloring composition. On the other hand, from the viewpoint of suppressing unevenness in film thickness during film formation and suppressing deformation of the pattern due to flow during baking, the content of the radical polymerizable compound is preferably 90% by mass or less in the solid content, more preferably 70% by mass or less, and even more preferably 60% by mass or less. Also, from the viewpoint of patterning property, the content of the radical polymerizable compound having three or more (meth)acryloyl groups and carboxyl groups is preferably 50% by mass or more in the radical polymerizable compound, and even more preferably 60% by mass or more.
[0032] The coloring composition may further contain a binder resin, a dispersant, a photopolymerization initiator, a chain transfer agent, a sensitizer, an organic solvent, a polymerization inhibitor, an adhesion improver, a surfactant, an organic acid, an organic amino compound, a curing agent, and the like.
[0033] Examples of the binder resin contained in the coloring composition include acrylic resin, epoxy resin, polyimide resin, urethane resin, urea resin, polyvinyl alcohol resin, melamine resin, polyamide resin, polyamideimide resin, polyester resin, polyolefin resin, etc. Two or more of these may be contained. From the viewpoint of stability, acrylic resin is preferably used.
[0034] The acrylic resin is preferably a copolymer of an unsaturated carboxylic acid and an ethylenically unsaturated compound.
[0035] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinylacetic acid, and acid anhydrides thereof. Two or more of these may be used.
[0036] Examples of the ethylenically unsaturated compounds include unsaturated carboxylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and benzyl (meth)acrylate; aromatic vinyl compounds such as styrene, p-methylstyrene, o-methylstyrene, m-methylstyrene, and α-methylstyrene; and aminoethyl Examples of the monomer include unsaturated carboxylic acid amino alkyl esters such as acrylate, unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate, carboxylic acid vinyl esters such as vinyl acetate and vinyl propionate, cyanide vinyl compounds such as acrylonitrile, methacrylonitrile and α-chloroacrylonitrile, aliphatic conjugated dienes such as 1,3-butadiene and isoprene, and macromonomers such as polystyrene having a (meth)acryloyl group at the end, polymethyl acrylate, polymethyl methacrylate, polybutyl acrylate, polybutyl methacrylate, and polysilicone. Two or more of these may be used.
[0037] The acrylic resin preferably has an ethylenically unsaturated group in the side chain, which can improve sensitivity. Examples of the ethylenically unsaturated group include vinyl groups, allyl groups, acrylic groups, and methacrylic groups. Examples of the acrylic resin having an ethylenically unsaturated group in the side chain include "Cyclomer" (registered trademark) P (Daicel Chemical Industries, Ltd.) and alkali-soluble cardo resins.
[0038] The weight average molecular weight of the binder resin is preferably 3,000 or more, more preferably 9,000 or more, from the viewpoint of the strength of the cured film. On the other hand, from the viewpoint of the stability of the coloring composition, the weight average molecular weight of the binder resin is preferably 200,000 or less, more preferably 100,000 or less. Here, the weight average molecular weight of the binder resin refers to a standard polystyrene equivalent value measured by gel permeation chromatography.
[0039] The content of the binder resin is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the solid content of the coloring composition from the viewpoint of suppressing unevenness in the film thickness during film formation. On the other hand, from the viewpoint of patterning properties, the content of the binder resin is preferably 60% by mass or less, more preferably 50% by mass or less, based on the solid content of the coloring composition.
[0040] The coloring material contained in the color filter of the present invention can be identified by laser Raman spectroscopy (Ar+ laser (457.9 nm)) or mass spectrometry using a MALDI mass spectrometer or a time-of-flight secondary ion mass spectrometer.
[0041] Examples of dispersants contained in the coloring composition include polyester, polyalkylamine, polyallylamine, polyimine, polyamide, polyurethane, polyacrylate, polyimide, polyamideimide, and copolymers thereof. Two or more of these may be contained. Among these polymer dispersants, those having an amine value of 5 mgKOH / g or more and 200 mgKOH / g or less and an acid value of 1 mgKOH / g or more and 100 mgKOH / g or less in terms of solid content are preferred. Among them, polymer dispersants having a basic group are preferred, and can improve the storage stability of the pigment dispersion liquid and the coloring composition. Examples of commercially available polymer dispersants having a basic group include "Solsperse" (registered trademark) (manufactured by Avecia), "EFKA" (registered trademark) (manufactured by EFKA), "Ajisper" (registered trademark) (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and "BYK" (registered trademark) (manufactured by BYK-Chemie). Two or more of these may be contained. Among these, "Solsperse" (registered trademark) 24000 (manufactured by Avecia), "EFKA" (registered trademark) 4300, 4330 (manufactured by EFKA), 4340 (manufactured by EFKA), "Ajisper" (registered trademark) PB821, PB822 (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and "BYK" (registered trademark) 161-163, 2000, 2001, 6919, 21116 (manufactured by BYK-Chemie) are preferred.
[0042] Examples of the photopolymerization initiator contained in the coloring composition include oxime ester compounds, benzophenone compounds, acetophenone compounds, oxanthone compounds, anthraquinone compounds, imidazole compounds, benzothiazole compounds, benzoxazole compounds, carbazole compounds, triazine compounds, phosphorus compounds, and titanocene compounds.
[0043] More specifically, examples of the oxime ester compounds include 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), ethanone, 1-[9-ethyl-6-(2-methyl-4-tetrahydrofuranylmethoxybenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), ethano Examples of the benzophenone compounds include benzophenone, N,N'-tetraethyl-4,4'-diaminobenzophenone, and 4-methoxy-4'-dimethylaminobenzophenone. ... Examples of acetophenone compounds include 2,2-diethoxyacetophenone, benzoin, benzoin methyl ether, benzoin isobutyl ether, benzyl dimethyl ketal, α-hydroxyisobutylphenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propane, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and "IRGACURE" (registered trademark) 369, 379, and 907 (manufactured by BASF Ltd.).Examples of anthraquinone compounds include t-butylanthraquinone, 1-chloroanthraquinone, 2,3-dichloroanthraquinone, 3-chloro-2-methylanthraquinone, 2-ethylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 1,2-benzoanthraquinone, 1,4-dimethylanthraquinone, and 2-phenylanthraquinone. Examples of imidazole compounds include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer. Examples of benzothiazole compounds include 2-mercaptobenzothiazole. Examples of benzoxazole compounds include 2-mercaptobenzoxazole. Examples of triazine compounds include 4-(p-methoxyphenyl)-2,6-di-(trichloromethyl)-s-triazine. Two or more of these may be included.
[0044] The content of the photopolymerization initiator is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, based on the solid content of the coloring composition excluding the coloring material, from the viewpoints of sensitivity, patterning ability, processability, and heat resistance. On the other hand, the content of the photopolymerization initiator is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on the solid content of the coloring composition excluding the coloring material, from the viewpoints of sensitivity, patterning ability, processability, and heat resistance.
[0045] Examples of the chain transfer agent contained in the coloring composition include thioglycolic acid, thiomalic acid, thiosalicylic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutyric acid, N-(2-mercaptopropionyl)glycine, 2-mercaptonicotinic acid, 3-[N-(2-mercaptoethyl)carbamoyl]propionic acid, 3-[N-(2-mercaptoethyl)amino]propionic acid, N-(3-mercaptopropionyl)alanine, 2-mercaptoethanesulfonic acid, 3-mercaptopropanesulfonic acid, 4-mercaptobutanesulfonic acid, dodecyl(4-methylthio)phenyl ether, 2-mercaptoethanol, 3-mercapto mercapto-1,2-propanediol, 1-mercapto-2-propanol, 3-mercapto-2-butanol, mercaptophenol, 2-mercaptoethylamine, 2-mercaptoimidazole, 2-mercapto-3-pyridinol, 2-mercaptobenzothiazole, mercaptoacetic acid, trimethylolpropane tris(3-mercaptopropionate), 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione), pentaerythritol tetrakis(3-mercaptopropionate), 1,4-bis(3-mercaptobutyryloxy)butane, "Kalends" (registered trademark) MT Examples of the mercapto compounds include PE-1 (manufactured by Showa Denko K.K.), Karenz (registered trademark) MT NR-1 (manufactured by Showa Denko K.K.), Karenz (registered trademark) MT BD-1 (manufactured by Showa Denko K.K.), etc., disulfide compounds obtained by oxidizing the mercapto compounds, and iodized alkyl compounds such as iodoacetic acid, iodopropionic acid, 2-iodoethanol, 2-iodoethanesulfonic acid, and 3-iodopropanesulfonic acid. Two or more of these may be contained.
[0046] Examples of the sensitizer contained in the coloring composition include thioxanthone-based sensitizers, aromatic or aliphatic tertiary amines, etc. Examples of the thioxanthone-based sensitizers include thioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthen-9-one, "KAYACURE" (registered trademark) DETX-S (manufactured by Nippon Kayaku Co., Ltd.), etc. Two or more of these may be contained.
[0047] The coloring composition may further contain an organic solvent. Examples of the organic solvent include diethylene glycol monobutyl ether acetate, benzyl acetate, ethyl benzoate, methyl benzoate, diethyl malonate, 2-ethylhexyl acetate, 2-butoxyethyl acetate, ethylene glycol monobutyl ether acetate, diethyl oxalate, ethyl acetoacetate, cyclohexyl acetate, 3-methoxy-butyl acetate, methyl acetoacetate, ethyl-3-ethoxypropionate, 2-ethylbutyl acetate, isopentyl propionate, propylene glycol monomethyl ether propionate, pentyl acetate, propylene glycol monomethyl ether acetate, ethylene Examples of the monomer unit include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, monoethyl ether, methyl carbitol, ethyl carbitol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol tertiary butyl ether, dipropylene glycol monomethyl ether, ethyl acetate, butyl acetate, isopentyl butanol acetate, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol, cyclopentanone, cyclohexanone, xylene, ethylbenzene, and solvent naphtha. Two or more of these may be contained.
[0048] When the color filter of the present invention has a red subpixel, the hue of the red subpixel is determined by the L * a * b * Color system chromaticity coordinates (a * , b* ) in a * is between 70 and 80, b * It is preferable that the L value of the red subpixel is 30 or more and 40 or less. By satisfying these requirements, it is possible to display red on the electronic paper with excellent saturation and brightness. From the viewpoint of brightness of the display, the L value of the red subpixel measured with a D65 light source is preferably 30 or more and 40 or less. * a * b * L in the color space chromaticity diagram * is preferably 55 or more, and more preferably 60 or more.
[0049] When the color filter of the present invention has a green subpixel, the hue of the green subpixel is determined by the L * a * b * Color system chromaticity coordinates (a * , b * ) in a * is between -80 and -70, b * It is preferable that the L value of the green subpixel is 40 or more and 60 or less. By satisfying these requirements, the green display of the electronic paper can be excellent in saturation and brightness. From the viewpoint of display brightness, the L value of the green subpixel measured with a D65 light source is preferably 40 or more and 60 or less. * a * b * L in the color space chromaticity diagram * is preferably 80 or more, and more preferably 85 or more.
[0050] When the color filter of the present invention has a blue subpixel, the hue of the blue subpixel is determined by the L * a * b * Color system chromaticity coordinates (a * , b * ) in a * is between 20 and 30, b * It is preferable that the L value of the blue subpixel is -80 or more and -70 or less. By satisfying these conditions, it is possible to display blue color on the electronic paper with excellent saturation and brightness. From the viewpoint of display brightness, the L value of the blue subpixel measured with a D65 light source is preferably -80 or more and -70 or less. * a * b *L in the color space chromaticity diagram * is preferably 40 or more, and more preferably 45 or more.
[0051] The hue of the fourth subpixel is measured with a D65 light source. * a * b * Color system chromaticity coordinates (a * , b * ) in a * is between -5 and 7, b * is preferably in the range of −7 to 5. By satisfying these conditions, the white display of the electronic paper can be brightened.
[0052] When the color filter of the present invention has a yellow subpixel, the hue of the yellow subpixel is determined by the L * a * b * Color system chromaticity coordinates (a * , b * ) in a * is between -50 and -20, b * It is preferable that the L value of the yellow subpixel is 80 or more and 100 or less. By satisfying these requirements, it is possible to display a yellow color on the electronic paper with excellent saturation and brightness. From the viewpoint of brightness of the display, the L value of the yellow subpixel measured with a D65 light source is preferably 80 or more and 100 or less. * a * b * L in the color space chromaticity diagram * is preferably 85 or more, and more preferably 90 or more.
[0053] Regarding the arrangement of subpixels in the color filter of the present invention, when the color filter has red, green, and blue subpixels, examples of the arrangement include, but are not limited to, the arrangement shown in Figure 1. When the color filter has red, green, blue, and a fourth subpixel, examples of the arrangement include, but are not limited to, the arrangement shown in Figures 2 and 4. When the color filter has red, green, blue, and yellow subpixels, examples of the arrangement include, but are not limited to, the arrangement shown in Figures 3 and 5.
[0054] The thickness of the subpixel is preferably 0.5 μm or more and 3.0 μm or less. By making it 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.4 μm or more, the color purity can be improved. On the other hand, by making it 3.0 μm or less, more preferably 2.8 μm or less, the flatness, pattern processability, and reliability of the color filter can be improved.
[0055] When the color filter of the present invention has a red subpixel, from the viewpoint of making the red display vivid, R / M is preferably 0.16 or more, and more preferably 0.17 or more, where M is the area of one pixel and R is the colored area of the red subpixel. The area M of one pixel includes the smallest repeating unit of a group of red, green, blue, yellow, etc. subpixels and the area between adjacent subpixels where these subpixels are the closest subpixels. The area M of one pixel can be measured as the average area of 50 pixels near the center of the color filter. The colored area of the subpixel can be measured as the average area of 50 subpixels of that color near the center of the color filter substrate.
[0056] When the color filter of the present invention has a green subpixel, when the colored area of the green subpixel is G, from the viewpoint of making the green display vivid, G / M is preferably 0.16 or more, and more preferably G0.17 or more.
[0057] When the color filter of the present invention has a blue subpixel, where M is the area of the minimum repeating unit and B is the colored area of the blue pixel, from the viewpoint of making the blue display vivid, B / M is preferably 0.16 or more, and more preferably 0.17 or more.
[0058] When the color filter of the present invention has a yellow subpixel, when the area of the minimum repeating unit is M and the colored area of the yellow pixel is Y, from the viewpoint of making the yellow display vivid, Y / M is preferably 0.16 or more, and more preferably 0.17 or more.
[0059] The shape of the sub-pixel may be a rectangle such as a rectangle or a square, or may be a circle, an ellipse, etc. From the viewpoint of improving the accuracy of bonding the array substrate and the color filter, the shape of the sub-pixel is preferably a square.
[0060] The color filter of the present invention has a color-adjusting member between subpixels. The color-adjusting member in the present invention refers to a member formed between subpixels, and having a Y value of 70 or more and 98 or less in the CIE1931 color system. By having a color-adjusting member between subpixels, it is possible to display a bright white color with low saturation in white display. The white display referred to here refers to a display method when the color filter is adjusted so that the light passing through the entire color filter is maximized.
[0061] In particular, having red, green, and blue, as well as yellow, sub-pixels tends to result in high saturation when white is displayed, making it necessary to adjust the size of the sub-pixels. However, by using a color-adjusting component with a Y value of 70 or more and 98 or less in the CIE 1931 color system, the saturation when white is displayed can be improved, making it possible to effectively display a brighter white color with lower saturation.
[0062] The color-adjusting member-forming composition of the present invention, when formed into a film having a thickness of 2 μm, preferably has a Y value in the CIE 1931 color system of 70 or more and 98 or less. In this way, the color-adjusting member in the color filter of the present invention can be efficiently formed using the color-adjusting member-forming composition.
[0063] Examples of materials constituting the color adjusting member forming composition for forming the color adjusting member include compositions containing color materials, binder resins such as acrylic resins and polyimide resins, and the like.
[0064] Examples of coloring materials contained in the color adjusting member or the composition for forming the color adjusting member include organic pigments, inorganic pigments, dyes, etc., and two or more of these may be contained. Among these, organic pigments are preferred from the viewpoint of light resistance.
[0065] Examples of red colorants for the composition for forming a color adjusting member include CI Pigment Red (hereinafter referred to as "PR") 9, PR48, PR97, PR122, PR123, PR144, PR149, PR166, PR168, PR177, PR179, PR180, PR192, PR209, PR215, PR216, PR217, PR220, PR223, PR224, PR226, PR227, PR228, PR240, PR254, and diketopyrrolopyrrole colorants having a bromine group.
[0066] Examples of green colorants for the composition for forming a color adjusting member include CI Pigment Green (hereinafter referred to as "PG") PG1, PG2, PG4, PG7, PG8, PG10, PG13, PG14, PG15, PG17, PG18, PG19, PG26, PG36, PG38, PG39, PG45, PG48, PG50, PG51, PG54, PG55, PG58, PG59, etc.
[0067] Examples of the yellow colorant for the composition for forming a color adjusting member include CI Pigment Yellow (hereinafter referred to as "PY") 12, PY13, PY17, PY20, PY24, PY83, PY86, PY93, PY95, PY109, PY110, PY117, PY125, PY129, PY137, PY138, PY139, PY147, PY148, PY150, PY153, PY154, PY166, PY168, and PY185.
[0068] Examples of the orange colorant for the color adjusting member forming composition include CI Pigment Orange (hereinafter, "PO") 13, PO31, PO36, PO38, PO40, PO42, PO43, PO51, PO55, PO59, PO61, PO64, PO65, and PO71.
[0069] Examples of the blue colorant for the composition for forming a color adjusting member include CI Pigment Blue (hereinafter, "PB") 15, PB15:3, PB15:4, PB15:6, PB21, PB22, PB60, and PB64.
[0070] Examples of the purple colorant for the composition for forming a color adjusting member include CI Pigment Violet (hereinafter referred to as "PV") 19, PV23, PV29, PV30, PV32, PV37, PV40, and PV50 (all numbers are Color Index Nos.).
[0071] The coloring material of the composition for forming a color adjusting member may be a dye, and examples of the dye include oil-soluble dyes, acid dyes, direct dyes, basic dyes, acid mordant dyes, etc. In addition, the dye may be made into a lake or may be made into a salt-forming compound of the dye and a nitrogen-containing compound.
[0072] Examples of red, green, blue, purple or yellow dyes include direct dyes, acid dyes, and basic dyes. Specific examples of these dyes include azo dyes, benzoquinone dyes, naphthoquinone dyes, anthraquinone dyes, xanthene dyes, cyanine dyes, squarylium dyes, croconium dyes, merocyanine dyes, stilbene dyes, diarylmethane dyes, triarylmethane dyes, fluoran dyes, spiropyran dyes, phthalocyanine dyes, indigo dyes, fulgide dyes, nickel complex dyes, and azulene dyes. The dye may be dissolved in the coloring composition or dispersed as particles.
[0073] The colorant contained in the color-adjusting member or the composition for forming the color-adjusting member may be any colorant, such as a red colorant, a yellow colorant, a blue colorant, or a purple colorant. From the viewpoint of displaying a bright white color with low saturation in white display, however, a blue colorant or a purple colorant is preferred, and a purple colorant is more preferred.
[0074] In addition, as the coloring material contained in the color adjusting member, PR254, a diketopyrrolopyrrole coloring material having a bromine group, PR177, PY150, PY185, PG58, PG59, PB15:3, PB15:4, PB15:6, PV23, etc. can be used. Among them, from the viewpoint of displaying a low saturation and bright white color in white display, PG58, PG59, PB15:6, and PV23 are preferred, PB15:6 and PV23 are more preferred, and PV23 is even more preferred.
[0075] The content of the coloring material contained in the color adjusting member or the composition for forming the color adjusting member is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on the solid content, from the viewpoint of displaying a low saturation and bright white color in the white display. Also, from the viewpoint of displaying a low saturation and bright white color in the white display, the content is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, based on the solid content. The solid content referred to here refers to all components, excluding the organic solvent, contained in the color adjusting member or the composition for forming the color adjusting member.
[0076] The color-adjusting member forming composition may contain a radically polymerizable compound. Examples of the radically polymerizable compound contained in the color-adjusting member forming composition include ethylene oxide modified products or propylene oxide modified products such as dipentaerythritol penta(meth)acrylate, tetratrimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, penta(meth)acryloyloxydipentaerythritol monosuccinic acid ester, dipentaerythritol hexa(meth)acrylate, styrene derivatives, polyfunctional maleimide compounds, poly(meth)acrylate carbamates, and adipic acid 1,6-hexanediol(meth)acrylic acid esters. Examples of the monomer include oligomers such as phthalic anhydride propylene oxide (meth)acrylic acid ester, trimellitic acid diethylene glycol (meth)acrylic acid ester, rosin-modified epoxy di(meth)acrylate, and alkyd-modified (meth)acrylate, bifunctional (meth)acrylates such as tripropylene glycol di(meth)acrylate and 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, triacrylformal, bisphenoxyethanol fluorene diacrylate, dicyclopentanedienyl diacrylate, and alkyl-modified, alkyl ether-modified, and alkyl ester-modified monomers thereof. Two or more of these may be contained.
[0077] The radical polymerizable compound contained in the composition for forming a color adjusting member contains dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate, and the ratio A / B of the mass (A) of dipentaerythritol hexa(meth)acrylate to the mass (B) of pentaerythritol tri(meth)acrylate is preferably 0.16 or more and 3 or less. By making it 0.16 or more, more preferably 0.17 or more, and even more preferably 0.3 or more, it is possible to provide excellent patterning properties and to make it difficult for the pattern to peel off even when fired at a low temperature. In addition, by making A / B 2.4 or less, more preferably 1.6 or less, it is possible to suppress color mixing of the pattern. In particular, when the base material of the color filter is an organic plastic film or sheet made of polyethylene terephthalate (PET), firing at a low temperature is required, so it is preferable that the radical polymerizable compound satisfies the above A / B.
[0078] From the viewpoint of patterning, the content of the radical polymerizable compound is preferably 40% by mass or more in the solid content of the composition for forming a color-adjusting member. On the other hand, from the viewpoint of suppressing unevenness in the film thickness during film formation and suppressing deformation of the pattern due to flow during firing, the content of the radical polymerizable compound is preferably 90% by mass or less in the solid content of the composition for forming a color-adjusting member, more preferably 70% by mass or less, and even more preferably 60% by mass or less. Also, from the viewpoint of patterning, the content of the radical polymerizable compound having three or more (meth)acryloyl groups and carboxyl groups is preferably 50% by mass or more in the radical polymerizable compound, and even more preferably 60% by mass or more.
[0079] The composition for forming a color adjusting member may further contain a binder resin, a dispersant, a photopolymerization initiator, a chain transfer agent, a sensitizer, an organic solvent, a polymerization inhibitor, an adhesion improver, a surfactant, an organic acid, an organic amino compound, a curing agent, a crosslinking agent, etc.
[0080] Examples of the binder resin contained in the composition for forming a color-adjusting member include acrylic resin, epoxy resin, polyimide resin, urethane resin, urea resin, polyvinyl alcohol resin, melamine resin, polyamide resin, polyamideimide resin, polyester resin, polyolefin resin, etc. Two or more of these may be contained. From the viewpoint of stability, acrylic resin is preferable. In addition, it is preferable that these resins have a functional group that reacts by heating. By having a functional group that reacts by heating, it can be suitably used for a color-adjusting member formed by photolithography processing or a color-adjusting member formed by applying by inkjet or the like, drying and baking.
[0081] The acrylic resin is preferably a copolymer of an unsaturated carboxylic acid and an ethylenically unsaturated compound.
[0082] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinylacetic acid, and acid anhydrides thereof. Two or more of these may be used.
[0083] Examples of the ethylenically unsaturated compounds include unsaturated carboxylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and benzyl (meth)acrylate; aromatic vinyl compounds such as styrene, p-methylstyrene, o-methylstyrene, m-methylstyrene, and α-methylstyrene; and aminoethyl Examples of the monomer include unsaturated carboxylic acid amino alkyl esters such as acrylate, unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate, carboxylic acid vinyl esters such as vinyl acetate and vinyl propionate, cyanide vinyl compounds such as acrylonitrile, methacrylonitrile and α-chloroacrylonitrile, aliphatic conjugated dienes such as 1,3-butadiene and isoprene, and macromonomers such as polystyrene having a (meth)acryloyl group at the end, polymethyl acrylate, polymethyl methacrylate, polybutyl acrylate, polybutyl methacrylate, and polysilicone. Two or more of these may be used.
[0084] The acrylic resin preferably has an ethylenically unsaturated group in the side chain, which can improve sensitivity. Examples of the ethylenically unsaturated group include vinyl groups, allyl groups, acrylic groups, and methacrylic groups. Examples of the acrylic resin having an ethylenically unsaturated group in the side chain include "Cyclomer" (registered trademark) P (Daicel Chemical Industries, Ltd.) and alkali-soluble cardo resins.
[0085] The weight average molecular weight of the binder resin is preferably 3,000 or more, more preferably 9,000 or more, from the viewpoint of the strength of the cured film. On the other hand, from the viewpoint of the stability of the coloring composition, the weight average molecular weight of the binder resin is preferably 200,000 or less, more preferably 100,000 or less. Here, the weight average molecular weight of the binder resin refers to a standard polystyrene equivalent value measured by gel permeation chromatography.
[0086] From the viewpoint of suppressing unevenness in the thickness during film formation, the content of the binder resin is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the solid content. On the other hand, from the viewpoint of patterning properties, the content of the binder resin is preferably 60% by mass or less, and more preferably 50% by mass or less, based on the solid content.
[0087] The coloring material contained in the color adjusting member or the composition for forming a color adjusting member of the present invention can be identified by laser Raman spectroscopy (Ar+ laser (457.9 nm)) or mass analysis using a MALDI mass spectrometer or a time-of-flight secondary ion mass spectrometer.
[0088] Examples of the dispersant contained in the composition for forming a color adjusting member include polyester, polyalkylamine, polyallylamine, polyimine, polyamide, polyurethane, polyacrylate, polyimide, polyamideimide, and copolymers thereof. Two or more of these may be contained. Among these polymer dispersants, those having an amine value of 5 mgKOH / g or more and 200 mgKOH / g or less and an acid value of 1 mgKOH / g or more and 100 mgKOH / g or less in terms of solid content are preferable. Among them, polymer dispersants having a basic group are preferable, and can improve the storage stability of the pigment dispersion liquid and the coloring composition. Examples of commercially available polymer dispersants having a basic group include "Solsperse" (registered trademark) (manufactured by Avecia), "EFKA" (registered trademark) (manufactured by EFKA), "Ajisper" (registered trademark) (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and "BYK" (registered trademark) (manufactured by BYK-Chemie). Two or more of these may be contained. Among these, "Solsperse" (registered trademark) 24000 (manufactured by Avecia), "EFKA" (registered trademark) 4300, 4330 (manufactured by EFKA), 4340 (manufactured by EFKA), "Ajisper" (registered trademark) PB821, PB822 (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and "BYK" (registered trademark) 161-163, 2000, 2001, 6919, 21116 (manufactured by BYK-Chemie) are preferred.
[0089] The color-adjusting member forming composition may contain a photopolymerization initiator. Examples of the photopolymerization initiator contained in the color-adjusting member forming composition include oxime ester compounds, benzophenone compounds, acetophenone compounds, oxanthone compounds, anthraquinone compounds, imidazole compounds, benzothiazole compounds, benzoxazole compounds, carbazole compounds, triazine compounds, phosphorus compounds, and titanocene compounds.
[0090] More specifically, examples of the oxime ester compounds include 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), ethanone, 1-[9-ethyl-6-(2-methyl-4-tetrahydrofuranylmethoxybenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), ethano Examples of the benzophenone compounds include benzophenone, N,N'-tetraethyl-4,4'-diaminobenzophenone, and 4-methoxy-4'-dimethylaminobenzophenone. ... Examples of acetophenone compounds include 2,2-diethoxyacetophenone, benzoin, benzoin methyl ether, benzoin isobutyl ether, benzyl dimethyl ketal, α-hydroxyisobutylphenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propane, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and "IRGACURE" (registered trademark) 369, 379, and 907 (manufactured by BASF Ltd.).Examples of anthraquinone compounds include t-butylanthraquinone, 1-chloroanthraquinone, 2,3-dichloroanthraquinone, 3-chloro-2-methylanthraquinone, 2-ethylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 1,2-benzoanthraquinone, 1,4-dimethylanthraquinone, and 2-phenylanthraquinone. Examples of imidazole compounds include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer. Examples of benzothiazole compounds include 2-mercaptobenzothiazole. Examples of benzoxazole compounds include 2-mercaptobenzoxazole. Examples of triazine compounds include 4-(p-methoxyphenyl)-2,6-di-(trichloromethyl)-s-triazine. Two or more of these may be included. Among these, from the viewpoint of processability, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one is preferred, and it is even more preferred to use a sensitizer described later in addition to 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one.
[0091] The content of the photopolymerization initiator is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, based on the solid content of the composition for forming a color adjusting member, from the viewpoints of sensitivity, patterning ability, and processability. On the other hand, the content of the photopolymerization initiator is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on the solid content of the composition for forming a color adjusting member, from the viewpoints of sensitivity, patterning ability, processability, and heat resistance.
[0092] The color-adjusting member forming composition may contain a chain transfer agent. Examples of the chain transfer agent contained in the color-adjusting member forming composition include thioglycolic acid, thiomalic acid, thiosalicylic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutyric acid, N-(2-mercaptopropionyl)glycine, 2-mercaptonicotinic acid, 3-[N-(2-mercaptoethyl)carbamoyl]propionic acid, 3-[N-(2-mercaptoethyl)amino]propionic acid, N-(3-mercaptopropionyl)alanine, 2-mercaptoethanesulfonic acid, 3-mercaptopropanesulfonic acid, 4-mercaptobutanesulfonic acid, dodecyl(4-methylthio)phenyl ether, 2-mercaptoethanol, 3-mercaptobutyric acid, 3-mercaptopropanesulfonic ... Mercapto-1,2-propanediol, 1-mercapto-2-propanol, 3-mercapto-2-butanol, mercaptophenol, 2-mercaptoethylamine, 2-mercaptoimidazole, 2-mercapto-3-pyridinol, 2-mercaptobenzothiazole, mercaptoacetic acid, trimethylolpropane tris(3-mercaptopropionate), 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione), pentaerythritol tetrakis(3-mercaptopropionate), 1,4-bis(3-mercaptobutyryloxy)butane, Karenz (registered trademark) MT Examples of the mercapto compounds include PE-1 (manufactured by Showa Denko K.K.), Karenz (registered trademark) MT NR-1 (manufactured by Showa Denko K.K.), Karenz (registered trademark) MT BD-1 (manufactured by Showa Denko K.K.), etc., disulfide compounds obtained by oxidizing the mercapto compounds, and iodized alkyl compounds such as iodoacetic acid, iodopropionic acid, 2-iodoethanol, 2-iodoethanesulfonic acid, and 3-iodopropanesulfonic acid. Two or more of these may be contained.
[0093] The color-adjusting member forming composition may contain a sensitizer. Examples of the sensitizer contained in the color-adjusting member forming composition include thioxanthone-based sensitizers and aromatic or aliphatic tertiary amines. Examples of the thioxanthone-based sensitizers include thioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthen-9-one, "KAYACURE" (registered trademark) DETX-S (manufactured by Nippon Kayaku Co., Ltd.). Two or more of these may be contained.
[0094] The color-adjusting member forming composition may contain a crosslinking agent. The crosslinking agent contained in the color-adjusting member forming composition refers to a compound having a functional group that reacts by heat, such as an epoxy group, a methylol group, an alkoxymethyl group, an isocyanate group, a blocked isocyanate group, etc. In addition, the epoxy group referred to here refers to a glycidyl group, an oxetanyl group, and an alicyclic epoxy group.Examples of the crosslinking agent contained in the composition for forming a color adjusting member include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerin diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, and the like. N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N,-diglycidyl-benzylamine, N,N-diglycidyl-aminomethylcyclohexane, and commercially available products with an average of 3.7 methoxymethyl groups per triazine ring. MX-750, MW-30, MX-100LM (all manufactured by Sanwa Chemical Co., Ltd.), which have an average of 5.8 methoxymethyl groups per triazine ring, Cymel 300, 301, 303, 350, 370, 771, 325, 327, 703, 712, etc., methoxymethylated butoxymethylated melamines such as Cymel 235, 236, 238, 212, 253, 254, etc., butoxymethylated melamines such as Cymel 506, 508, etc., and carbocyclic melamines such as Cymel 1141, etc. Examples of carboxyl group-containing methoxymethylated isobutoxymethylated melamine include methoxymethylated ethoxymethylated benzoguanamine such as Cymel 1123, methoxymethylated butoxymethylated benzoguanamine such as Cymel 1123-10, butoxymethylated benzoguanamine such as Cymel 1128, and carboxyl group-containing methoxymethylated ethoxymethylated benzoguanamine such as Cymel 1125-80 (all manufactured by Mitsui Cyanamid Co., Ltd.), but are not limited to these.
[0095] The color-adjusting member forming composition may further contain an organic solvent. Examples of the organic solvent include diethylene glycol monobutyl ether acetate, benzyl acetate, ethyl benzoate, methyl benzoate, diethyl malonate, 2-ethylhexyl acetate, 2-butoxyethyl acetate, ethylene glycol monobutyl ether acetate, diethyl oxalate, ethyl acetoacetate, cyclohexyl acetate, 3-methoxy-butyl acetate, methyl acetoacetate, ethyl-3-ethoxypropionate, 2-ethylbutyl acetate, isopentyl propionate, propylene glycol monomethyl ether propionate, pentyl acetate, propylene glycol monomethyl ether acetate, ethylene Examples of the monomer unit include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, monoethyl ether, methyl carbitol, ethyl carbitol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol tertiary butyl ether, dipropylene glycol monomethyl ether, ethyl acetate, butyl acetate, isopentyl butanol acetate, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol, cyclopentanone, cyclohexanone, xylene, ethylbenzene, and solvent naphtha. Two or more of these may be contained.
[0096] The color adjusting member may be formed by applying a color adjusting member forming composition by inkjet or the like, drying and baking, or by applying a photosensitive color adjusting member forming composition by slit coating or the like, drying, and then exposing with a mask, developing and baking (photolithography). From the viewpoint of processing dimensional accuracy, it is preferable to form the color adjusting member by photolithography using a photosensitive color adjusting member forming composition.
[0097] From the viewpoint of processability, the thickness of the color-adjusting member is preferably 0.5 μm or more, and more preferably 1.0 μm or more, and from the viewpoint of flatness and processability, the thickness of the color-adjusting member is preferably 3.0 μm or less, and more preferably 2.8 μm or less.
[0098] From the viewpoint of achieving low saturation in white display and displaying a bright and good white color, it is preferable that the transmittance of the color-adjusting member is such that the transmittance T450 at a wavelength of 450 nm is 90% or more, the transmittance T550 at a wavelength of 550 nm is 65% to 98%, and the transmittance T700 at a wavelength of 700 nm is 80% or more.
[0099] The ratio H / M of the area H of the color-adjusting member to the area M of one pixel is preferably 0.05 or more, more preferably 0.10 or more, from the viewpoint of displaying a bright and good white color with low saturation in white display. Also, from the viewpoint of displaying each color vividly, the ratio is preferably 0.36 or less, more preferably 0.30 or less, and even more preferably 0.20 or less.
[0100] From the viewpoint of displaying each color brightly and vividly, it is preferable to form the color adjusting member at the center between the pixels, but the color adjusting member may be arranged so that the distance between the color adjusting member and the sub-pixel of a certain color is narrow, while the distance between the color adjusting member and the sub-pixel of another color is wide. The distance between the color adjusting member and each pixel may be 0 μm, or may be several μm to several tens of μm, or may be several hundred μm. From the viewpoint of displaying vivid colors, the distance between the color adjusting member and each pixel is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less.
[0101] In addition, the shape of the color adjusting member may be a shape that surrounds each pixel as in Figures 1, 2, 3, and 5, or it may be rectangular as in Figure 4, or it may be circular, elliptical, star-shaped, wavy, or other shape.
[0102] In order to display a bright white color with low saturation in white display, it is preferable to arrange the color adjustment member between two or more combinations of subpixels, for example, between the red subpixel and the green subpixel and between the red subpixel and the blue subpixel, and it is more preferable to arrange the color adjustment member between three or more combinations of subpixels, for example, between the red subpixel and the green subpixel, between the red subpixel and the blue subpixel, and between the green subpixel and the blue subpixel, and the more the number of combinations of subpixels between which the color adjustment member is arranged, the more preferable it is. Note that the combinations of subpixels between which the color adjustment member is arranged are not limited to the above examples.
[0103] As an example of the arrangement of the color adjusting members and the sub-pixels, a mode can be shown in which square red, green and blue sub-pixels are repeatedly arranged and the color adjusting members are formed between these sub-pixels, as shown in Fig. 1. Note that the positional relationship between the red, green and blue sub-pixels is not particularly limited to the mode shown in Fig. 1.
[0104] Also, for example, as shown in Fig. 2, a mode can be shown in which square red, green, and blue subpixels and a fourth subpixel are repeatedly arranged and a color adjusting member is formed between these subpixels. Note that the positional relationship between the red, green, blue, and fourth subpixels is not particularly limited to the mode shown in Fig. 2.
[0105] Also, for example, as shown in Fig. 3, a mode can be shown in which square red, green, blue and yellow sub-pixels are repeatedly arranged and color-adjusting members are formed between these sub-pixels. Note that the positional relationship between the red, green, blue and yellow sub-pixels is not particularly limited to the mode shown in Fig. 3.
[0106] Also, for example, as shown in Fig. 4, a mode can be shown in which square red, green, and blue subpixels and a fourth subpixel are repeatedly arranged, and color-adjusting members are formed between these subpixels so as to surround a part of each color pixel. Note that the positional relationship between the red, green, blue, and fourth subpixels is not particularly limited to the mode shown in Fig. 4.
[0107] Also, for example, as shown in Fig. 5, a mode can be shown in which square red, green, blue and yellow sub-pixels are repeatedly arranged and color-adjusting members are formed adjacent to these sub-pixels. Note that the positional relationship of the red, green, blue and yellow sub-pixels is not particularly limited to the mode shown in Fig. 5.
[0108] The width of the color adjusting member is preferably 5 μm or more, more preferably 8 μm or more, from the viewpoint of the workability of the color adjusting member and displaying a bright white color with low saturation in white display. Also, from the viewpoint of displaying a bright white color with low saturation in white display, the width of the color adjusting member is preferably 40 μm or less, more preferably 30 μm or less. The width of the color adjusting member here refers to the length of the color adjusting member in the spacing direction between adjacent subpixels.
[0109] The color filter of the present invention may further have a black matrix. The black matrix prevents a decrease in contrast and color purity due to light leakage between pixels, and may be disposed between sub-pixels, a part between sub-pixels, or in the frame. Examples of materials constituting the black matrix include a photosensitive composition containing a binder resin such as an acrylic resin or a polyimide resin and a radical polymerizable compound, and a non-photosensitive resin composition colored black. From the viewpoint of light shielding, the film thickness of the black matrix is preferably 0.5 μm or more, and more preferably 1.0 μm or more. On the other hand, from the viewpoint of processability, it is preferably 2.0 μm or less, and more preferably 1.5 μm or less.
[0110] The color filter of the present invention may further have an overcoat layer. The overcoat layer suppresses the transmission of impurities from the subpixels of the color filter and flattens the steps caused by the subpixels of the color filter. Examples of materials constituting the overcoat layer include epoxy resins, acrylic epoxy resins, acrylic resins, siloxane resins, polyimide resins, and photosensitive or non-photosensitive materials that are commercially available as flattening materials. From the viewpoint of processability, the film thickness of the overcoat layer is preferably 0.5 μm or more, and more preferably 1.0 μm or more. On the other hand, from the viewpoint of flatness of the color filter, it is preferably 5.0 μm or less, and more preferably 3.0 μm or less.
[0111] The color filter of the present invention may further include a transparent electrode. Examples of materials constituting the transparent electrode include metals such as aluminum, chromium, tantalum, titanium, neodymium, and molybdenum, indium-tin-oxide (ITO), and indium-zinc-oxide (InZnO).
[0112] The color filter of the present invention may further include a diffusion plate or the like.
[0113] The manufacturing method will be described below by taking as examples a color adjusting member made of a photosensitive color adjusting member forming composition and a color filter having sub-pixels made of a photosensitive coloring composition.
[0114] A color filter can be obtained by applying a composition for forming a color adjusting member or a coloring composition onto a substrate, patterning the composition by selective exposure using a photomask and development, and then baking the composition to form color adjusting members and sub-pixels.
[0115] Examples of methods for applying the color adjusting member forming composition or coloring composition for forming a color adjusting member or a subpixel onto a substrate include a method using a spin coater, a bar coater, a blade coater, a roll coater, a die coater, an inkjet printing method, a screen printing method, a method of immersing a substrate in the color adjusting member forming composition or coloring composition, and a method of spraying the color adjusting member forming composition or coloring composition onto a substrate.
[0116] Subsequently, the substrate coated with the composition for forming a color adjusting member or the coloring composition is dried to form a coating film of the composition for forming a color adjusting member or the coloring composition on the substrate. Examples of the drying method include air drying, heat drying, and vacuum drying. Two or more of these may be combined, and for example, it is preferable to perform heat drying after performing reduced pressure drying. The heat drying temperature is preferably 80 to 130°C, and the heat drying device is preferably a hot air oven or a hot plate. In the case of a color filter having a black matrix, it is preferable to form a coating film of the coloring composition on a substrate on which a black matrix has been formed in advance.
[0117] Next, a photomask is placed on the coating film of the color-adjusting member forming composition or the coloring composition, and selective exposure is performed. Examples of the exposure machine include a proximity exposure machine, a mirror projection exposure machine, a lens scan exposure machine, a stepper, etc. From the viewpoint of accuracy, a lens scan exposure machine is preferred. Examples of the light source used for exposure include an ultra-high pressure mercury lamp, a chemical lamp, a high pressure mercury lamp, etc.
[0118] Thereafter, the unexposed portion is removed by development with an alkaline developer to form a coating film pattern. Examples of the alkaline substance used in the alkaline developer include inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium silicate, sodium metasilicate, and aqueous ammonia, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-propylamine, tertiary amines such as triethylamine and methyldiethylamine, and organic alkalis such as tetramethylammonium hydroxide. Examples of the alkaline developer include 0.02 to 1 mass % potassium hydroxide or tetramethylammonium hydroxide. Examples of the development method include a method in which the coating film after exposure is immersed in an alkaline developer for 20 to 300 seconds.
[0119] The resulting coating film pattern is then heat-treated to obtain a color filter having a pattern of color-adjusting members and sub-pixels. The heat treatment may be performed in air, in a nitrogen atmosphere, or in a vacuum. The heating temperature is preferably 150 to 350°C, and more preferably 180 to 250°C. The heating time is preferably 5 minutes to 5 hours. As the heat treatment device, a hot air oven or a hot plate is preferable. The heat treatment may be performed continuously or stepwise.
[0120] The order of forming the color adjusting member and the sub-pixels may be such that the sub-pixels are formed first and then the color adjusting member, or the sub-pixels are formed first and then the color adjusting member. When the color filter has sub-pixels of multiple colors, the pixel formation is performed for each sub-pixel in sequence by the above method. The order of forming each color is not particularly limited.
[0121] The color filter of the present invention can be used as a component of display devices such as liquid crystal displays, organic EL displays, and electronic paper.
[0122] That is, the display device of the present invention is characterized by having the color filter of the present invention. The display device refers to a device that displays an image by visually viewing a part of a screen using a display element. Examples of the display element include a liquid crystal element, an organic EL element, an inorganic EL element, a display element using MEMS, a display element using quantum dots, electronic ink, electronic liquid powder, and an electrophoretic element. Examples of the display device include a transmissive liquid crystal display, a semi-transmissive liquid crystal display, a reflective liquid crystal display, an organic EL display, an inorganic EL display, a quantum dot display, and electronic paper. Examples of the reflective display device include devices that display images using outdoor light or indoor light, such as a wearable terminal, an electronic signboard, a digital signage, and an electronic shelf label. In addition to the color filter and the display element of the present invention, the display device may also include a light source such as an external light source, and various films such as a brightness enhancing film and a diffusion plate.
[0123] The electronic paper of the present invention is characterized by having the color filter of the present invention. The display method of the electronic paper can be an electrophoretic method using an electrophoretic display layer. The electrophoretic display layer refers to a member having a display medium that switches between black and white display by moving white and black particles by an electric field. The electrophoretic display layer can be, for example, a microcapsule containing a dispersion liquid made of a transparent dispersion medium and fixed with a binder resin. As the transparent dispersion medium, for example, various organic compounds such as alcohol-based solvents and aliphatic hydrocarbons can be used. As the white particles, for example, a white pigment such as titanium dioxide can be used, and as the black particles, for example, a black pigment such as carbon black and titanium black can be used. As the material for forming the wall film of the microcapsule, for example, a composite film of urethane resin, urea resin, gum arabic and gelatin can be used. As the binder resin, a material that has good affinity with the wall film of the microcapsule and has insulating properties can be used. Such an electrophoretic display layer can be formed, for example, by dispersing the microcapsules in a binder resin and applying the ink made by forming the ink.
[0124] In addition to the color filter and electrophoretic display layer of the present invention, the electronic paper may have an optical film for improving visibility and light reflection characteristics, a surface protective film, a barrier layer, a touch panel layer, and the like.
[0125] When the color filter of the present invention in the electronic paper of the present invention has a combination of red, green, and blue subpixels, or a combination of red, green, blue, and yellow subpixels, it is preferable to make the reflectance of the portion of the electrophoretic display layer of the electronic paper corresponding to the blue subpixel larger than the reflectance of the portion corresponding to any other subpixel in order to display a white color closer to white in the white display of the electronic paper. In particular, when the electronic paper has red, green, blue, and yellow subpixels, the white display tends to be yellowish, and this embodiment is useful. The white display referred to here refers to the display of white used as the background of characters when characters are displayed on the electronic paper. In this way, by controlling the reflectance corresponding to the color of the subpixel, it is possible to display a white color closer to white while making the color of each color displayed vivid. EXAMPLES
[0126] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. First, the evaluation methods used in the examples and comparative examples will be described.
[0127] [Measurement and evaluation method] (1) Chromaticity, Y value, and transmittance of color-adjusting materials For the color-adjusting members obtained in the examples, the chromaticity xy, CIE 1931 color system tristimulus value (Y), transmittance T450 at 450 nm, transmittance T550 at 550 nm, and transmittance T700 at 700 nm were measured using a microspectrophotometer (LCF-100MA manufactured by Otsuka Electronics Co., Ltd.).
[0128] (2) Evaluation of white display The L when the color filter and the array substrate of each Example and Comparative Example are bonded together and the reflection intensity of the sub-pixel of each color is maximized (hereinafter, white display). *The chroma was measured using a spectrophotometer (CM2600d manufactured by Konica Minolta, Inc.).
[0129] [Example 1] (Preparation of Dispersion A1) In a 500 mL three-neck flask under a nitrogen atmosphere, 176.3 g of anhydrous tert-amyl alcohol (2.0 mol) and 114.7 g of sodium tert-amyl alkoxide (1.1 mol) were placed, and the internal temperature was raised to 100° C. with stirring to react them, thereby preparing an alcoholate solution.
[0130] Into another 500 mL three-neck flask, 84.9 g of diisopropyl succinate (0.4 mol) and 145.6 g of 4-bromobenzonitrile (0.8 mol) were charged, and the internal temperature was raised to 85° C. with stirring to dissolve, thereby preparing a mixed solution.
[0131] The internal temperature of the three-neck flask containing the alcoholate solution was adjusted to 100° C., and the mixed solution was added dropwise over 3 hours while stirring. After the dropwise addition was completed, the mixture was heated and stirred at an internal temperature of 90° C. for 12 hours to obtain a suspension.
[0132] Further, 640 g of methanol (20.0 mol), 720 g of water (40.0 mol) and 300 g of acetic acid (10.0 mol) were charged into another 500 mL three-neck flask, and the mixture was stirred while cooling the internal temperature to -10°C to obtain a mixture.
[0133] The suspension was added dropwise over 3 hours while stirring at high speed and keeping the internal temperature of the three-neck flask containing the mixture below -5°C. After the dropwise addition, the mixture was stirred for an additional 7 hours, and then the reaction liquid was washed and filtered until the filtrate was no longer colored and no salt precipitated. The collected filtrate was dried at 80°C for 24 hours, and the resulting solid was pulverized to obtain 112 g of a diketopyrrolopyrrole pigment having a bromine group represented by general formula (1).
[0134] [ka]
[0135] A slurry was prepared by mixing 100 g of the obtained diketopyrrolopyrrole pigment having a bromine group, 50 g of a polymer dispersant (BYK-6919 manufactured by BYK Japan Co., Ltd.), 66.7 g of a binder polymer (Cyclomer (registered trademark) P manufactured by Daicel Corporation, ACA250, 45 mass% solution), and 450 g of PGME. The beaker containing the slurry was connected to a Dyno Mill via a tube, and a dispersion treatment was carried out for 8 hours at a peripheral speed of 14 m / s using zirconia beads with a diameter of 0.5 mm as a medium, to prepare a dispersion liquid A1 of a diketopyrrolopyrrole pigment having a bromine group.
[0136] (Preparation of Dispersion A2) A slurry was prepared by mixing 150 g of CI Pigment Green 58, 75 g of a polymer dispersant (BYK-6919 manufactured by BYK Japan Co., Ltd.), 100 g of a binder polymer (Cyclomer (registered trademark) P manufactured by Daicel Corporation, ACA250, 45 mass% solution), and 675 g of PGME. The beaker containing the slurry was connected to a Dyno Mill via a tube, and a dispersion treatment was carried out for 8 hours at a peripheral speed of 14 m / s using zirconia beads with a diameter of 0.5 mm as a medium, to prepare a dispersion liquid A2 of Pigment Green 58.
[0137] (Preparation of Dispersion A3) A slurry was prepared by mixing 150g of CI Pigment Yellow 150, 75g of a polymer dispersant (BYK-6919, manufactured by BYK Japan Co., Ltd.), 100g of a binder polymer (Cyclomer (registered trademark) P, ACA250, 45% by mass solution, manufactured by Daicel Corporation), and 675g of PGME. The beaker containing the slurry was connected to a Dyno Mill via a tube, and a dispersion treatment was carried out for 8 hours at a peripheral speed of 14 m / s using zirconia beads with a diameter of 0.5 mm as a medium, to prepare a dispersion liquid A3 of Pigment Yellow 150.
[0138] (Preparation of Dispersion A4) A slurry was prepared by mixing 150g of CI Pigment Blue 15:6, 75g of polymer dispersant (BYK-6919 manufactured by BYK Japan Co., Ltd.), 100g of binder polymer (Cyclomer (registered trademark) P manufactured by Daicel Corporation, ACA250, 45 mass% solution), and 675g of PGME. The beaker containing the slurry was connected to a Dyno Mill via a tube, and dispersion treatment was carried out for 8 hours at a peripheral speed of 14 m / s using zirconia beads with a diameter of 0.5 mm as a medium, to prepare Pigment Blue 15:6 Dispersion A4.
[0139] (Preparation of Dispersion A5) A slurry was prepared by mixing 150 g of CI Pigment Violet 23, 75 g of a polymer dispersant (BYK-6919 manufactured by BYK Japan Co., Ltd.), 100 g of a binder polymer (Cyclomer (registered trademark) P manufactured by Daicel Corporation, ACA250, 45 mass% solution), and 675 g of PGME. The beaker containing the slurry was connected to a Dyno Mill via a tube, and a dispersion treatment was carried out for 8 hours at a peripheral speed of 14 m / s using zirconia beads with a diameter of 0.5 mm as a medium, to prepare a dispersion liquid A5 of Pigment Violet 23.
[0140] (Synthesis of binder resin solution B1) In a 500mL three-neck flask, 33g (0.3mol) of methyl methacrylate, 33g (0.3mol) of styrene, 34g (0.4mol) of methacrylic acid, 3g (0.02mol) of 2,2'-azobis (2-methylbutyronitrile) and 150g of propylene glycol monomethyl ether acetate (PGMEA) were charged, and the mixture was stirred at 90°C for 2 hours, and then the internal temperature was raised to 100°C and stirred for another hour to obtain a reaction solution. To the resulting reaction solution, 33g (0.2mol) of glycidyl methacrylate, 1.2g (0.009mol) of dimethylbenzylamine and 0.2g (0.002mol) of p-methoxyphenol were added, and the mixture was stirred at 90°C for 4 hours, and then 50g of PGMEA was added to obtain a binder resin solution B1 having a solid content concentration of 40% by mass. The acid value of the binder resin was measured using an automatic potentiometer AT-610 manufactured by Kyoto Electronics Manufacturing Co., Ltd., and was found to be 80.0 (mgKOH / g) in a 0.1 mol / L potassium hydroxide-ethanol solution. The weight average molecular weight, calculated as polystyrene, was 22,000 as measured using a GPC device.
[0141] (Preparation of Coloring Composition R) Into a 50 mL plastic bottle, 5.42 g of Dispersion A1, 0.11 g of Dispersion A3, 3.11 g of Binder Resin Solution B1, 1.49 g of Penta(meth)acryloyloxydipentaerythritol monosuccinic acid ester (C1), 0.12 g of N-1919 (manufactured by ADEKA Corporation), and 19.75 g of dipropylene glycol methyl ether acetate (hereinafter, DPMA) were added and stirred for 3 hours to prepare a red coloring composition R.
[0142] (Preparation of Coloring Composition G) Into a 50 mL plastic bottle, 6.40 g of Dispersion A2, 1.03 g of Dispersion A3, 3.11 g of Binder Resin Solution B1, 1.05 g of Penta(meth)acryloyloxydipentaerythritol monosuccinic acid ester (C1), 0.04 g of N-1919 (manufactured by ADEKA CORPORATION), and 18.35 g of DPMA were added and stirred for 3 hours to prepare a green coloring composition G.
[0143] (Preparation of Coloring Composition B) Into a 50 mL plastic bottle, 2.09 g of Dispersion A4, 1.12 g of Dispersion A5, 3.24 g of Binder Resin Solution B1, 0.95 g of Penta(meth)acryloyloxydipentaerythritol monosuccinic acid ester (C1), 0.07 g of N-1919 (manufactured by ADEKA CORPORATION), and 21.36 g of DPMA were added and stirred for 3 hours to prepare a blue coloring composition B.
[0144] (Preparation of Coloring Composition Y) Into a 50 mL plastic bottle, 2.60 g of Dispersion A2, 4.83 g of Dispersion A3, 3.11 g of Binder Resin Solution B1, 1.05 g of Penta(meth)acryloyloxydipentaerythritol monosuccinic acid ester (C1), 0.04 g of N-1919 (manufactured by ADEKA CORPORATION), and 18.35 g of DPMA were added and stirred for 3 hours to prepare a yellow coloring composition Y.
[0145] (Preparation of color-adjusting member forming composition H1) Into a 50 mL plastic bottle, 0.06 g of the dispersion A5, 5.82 g of the binder resin solution B1, 1.42 g of dipentaerythritol hexaacrylate (D1) and 1.42 g of pentaerythritol triacrylate (D2) as radical polymerizable compounds, 0.10 g of IRGACURE907 (manufactured by BASF Ltd.) (E1) as a photopolymerization initiator, 0.10 g of 2,4-diethylthioxanthone (F1) as a photosensitizer, and 21.06 g of propylene glycol monomethyl ether acetate (G1) as an organic solvent were added and stirred for 3 hours to prepare a color adjusting member forming composition (H1).
[0146] (Red sub-pixel formation) The coloring composition R was applied by spin coating onto a glass substrate having a thickness of 0.5 mm, and then dried by heating at 90° C. for 10 minutes. The obtained coloring composition coating film was irradiated with 200 mJ / cm of i-line through a negative photomask in the arrangement pattern shown in FIG. 2After exposure to light at 1000 K, the substrate was developed in a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. Then, heat treatment was performed at 230° C. for 30 minutes to form red subpixels. The red subpixels were squares with a side length of 129 μm, and the length of the minimum repeating unit, i.e., the distance between the centers of adjacent subpixels of the same color, was 318 μm. The L * a * b * The color of each color pixel in the color space chromaticity diagram (L * , a * , b * ) were (62.6, 70.2, 33.4).
[0147] (Green sub-pixel formation) Coloring composition G was applied by spin coating onto the substrate on which the red subpixels were formed, and then heated and dried for 10 minutes at 90° C. The obtained coloring composition coating film was irradiated with 200 mJ / cm i-line through a negative photomask in the positional relationship with the red subpixels as shown in FIG. 2 After exposure to light at 400 K, the substrate was developed in a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. Then, the substrate was heated at 230° C. for 30 minutes to form green subpixels. The green subpixels were squares with sides of 129 μm long, and the length of the minimum repeating unit, i.e., the distance between the centers of adjacent subpixels of the same color, was 318 μm. The L * a * b * The color of each color pixel in the color space chromaticity diagram (L * , a * , b * ) was (85.8, -77.3, 50.7).
[0148] (Formation of blue sub-pixel) Coloring composition B was applied by spin coating onto the substrate on which the red and green subpixels were formed, and then dried by heating at 90° C. for 10 minutes. The obtained coloring composition coating film was irradiated with 200 mJ / cm i-rays through a negative photomask in the positional relationship with the red and green subpixels as shown in FIG. 2After exposure to light at 1000 K, the resist was developed in a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. Then, heat treatment was performed at 230° C. for 30 minutes to form blue subpixels. The blue subpixels were squares with a side length of 129 μm, and the length of the minimum repeating unit, i.e., the distance between the centers of adjacent subpixels of the same color, was 318 μm. The L * a * b * The color of each color pixel in the color space chromaticity diagram (L * , a * , b * ) was (48.6, 27.5, -71.7).
[0149] (Formation of yellow sub-pixel) A coloring composition Y was applied by spin coating onto a substrate on which red, green, and blue subpixels had been formed, and then the substrate was dried by heating at 90° C. for 10 minutes. The obtained coloring composition coating film was irradiated with 200 mJ / cm of i-line through a negative photomask in the positional relationship with the red, green, and blue subpixels as shown in FIG. 2 After exposure to light at 400 K, the resist was developed in a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. Then, heat treatment was performed at 230° C. for 30 minutes to form yellow subpixels. The yellow subpixels were squares with a side length of 129 μm, and the length of the minimum repeating unit, i.e., the distance between the centers of adjacent subpixels of the same color, was 318 μm. The L * a * b * The color of each color pixel in the color space chromaticity diagram (L * , a * , b * ) was (94.8, -38.6, 83.3).
[0150] (Formation of color-adjusting material) Composition H1 for forming a color adjusting member was applied by spin coating onto a substrate on which red, green, blue and yellow subpixels were formed, and then dried by heating at 90° C. for 10 minutes. The obtained coating film of composition H1 for forming a color adjusting member was irradiated with 200 mJ / cm of i-line through a negative photomask in the positional relationship with the red, green, blue and yellow subpixels as shown in FIG. 2After exposure to light at 400° C., development was performed with a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. Then, heat treatment was performed at 230° C. for 30 minutes to form a color-adjusting member with a film thickness of 2.0 μm and a width of 30 μm, producing a color filter with the arrangement shown in FIG. 5. The ratio H / M of the area H of the color-adjusting member to the area M of one pixel was 0.342.
[0151] The chromaticity xy of the color-adjusting material was 0.308 and 0.306, respectively, the Y value in the CIE1931 color system was 92.7, and the T450, T550, and T700 were 99.1, 90.2, and 99.7, respectively.
[0152] (Display device manufacturing) The obtained color filter was attached to an array substrate for evaluation to prepare a display device. * The color was 60.5 and the saturation was 9.2.
[0153] [Examples 2 to 4] Instead of H1, H2 to H4 were prepared as compositions for forming color-adjusting members in the amounts shown in Table 1, and were used in Examples 2 to 4. Otherwise, color filters and display devices were manufactured in the same manner as in Example 1. The evaluation results are summarized in Table 2.
[0154] [Table 1]
[0155] [Table 2]
[0156] [Comparative Example 1] A color filter and a display device were manufactured in the same manner as in Example 1, except that no color-adjusting member was formed. The chromaticity xy of the portions corresponding to the portions where the color-adjusting members were formed in Examples 1 to 4 was 0.310 and 0.316, respectively, and the Y value in the CIE1931 color system was 100.0, and the T450, T550, and T700 were 100.0, 100.0, and 100.0, respectively. In addition, the L * The color was 62.7 and the saturation was 13.2. [Explanation of symbols]
[0157] 1 Red subpixel 2 Green subpixel 3 Blue subpixel 4. Color-adjusting materials 5 pixels 6 Red subpixel 7 Green subpixel 8 Blue subpixel 9. Color-adjusting materials 10 pixels 11 Red subpixel 12 Green subpixel 13 Blue subpixel 14 Yellow subpixel 15 Color-adjusting materials 16 pixels 17 Red subpixel 18 Green subpixel 19 Blue subpixel 20 Color Adjusting Materials 21 pixels 22 Red subpixel 23 Green subpixel 24 Blue subpixel 25 Yellow subpixel 26 Color Adjusting Materials 27 pixels [Industrial Applicability]
[0158] The color filter substrate of the present invention can be suitably used for electronic paper.
Claims
1. A color filter having at least any one of red, green and blue sub-pixels on a substrate, wherein a color adjusting member having a Y value of 70 or more and 98 or less in the CIE 1931 color system is disposed between the sub-pixels, the color adjusting member contains a color material, and a content of the color material in a solid content of the color adjusting member is 0.01% by mass or more and 1% by mass or less.
2. 2. The color filter of claim 1, having at least red, green and blue subpixels on said substrate.
3. 3. The color filter according to claim 1, wherein the color adjusting member has a transmittance T450 of 90% or more for light with a wavelength of 450 nm, a transmittance T550 of 65% to 98% or less for light with a wavelength of 550 nm, and a transmittance T700 of 80% or more for light with a wavelength of 700 nm.
4. The color filter according to claim 2 or 3, further comprising a yellow subpixel.
5. A color filter described in any one of claims 1 to 4, wherein the content of the color material in the solid content of the color adjusting member is 0.05 mass % or more and 1 mass % or less.
6. 6. The color filter according to claim 1, wherein the color material is a blue color material or a purple color material.
7. A display device comprising the color filter according to any one of claims 1 to 6.
8. 7. An electronic paper comprising the color filter according to claim 1.
9. A method for displaying white on electronic paper having the color filter and electrophoretic display layer according to any one of claims 2 to 6, comprising making the reflectance of a portion of the electrophoretic display layer corresponding to the blue sub-pixel higher than the reflectance of a portion of the electrophoretic display layer corresponding to any sub-pixel of any other color.
10. A composition for forming a color-adjusting member capable of forming a color-adjusting member between sub-pixels of a color filter having at least red, green, and blue sub-pixels on a substrate, the composition for forming a color-adjusting member being characterized in that, when formed into a film having a thickness of 2 μm, the Y value in the CIE 1931 color system is 70 or more and 98 or less, the composition contains a colorant, and the content of the colorant in the solid content is 0.01% by mass or more and 1% by mass or less.
Citation Information
Patent Citations
Color filter for reflection type color display and the reflection type color display equipped with the same
JP2003107234A
Electrophoretic display device, driving method thereof and electronic apparatus
JP2012181450A
Reflection type color display device and manufacturing method thereof
JP2013088750A
Reflection type color display
JP2014123049A
Color filter for reflective display device and reflective display device including the same
JP2018101050A