Photosensitive coloring composition, color filter, and image display device

The photosensitive coloring composition addresses the challenges of high colorant concentration in conventional compositions by using specific pigments and additives, resulting in thin color filters with improved developability, pattern shape, and chemical resistance for liquid crystal display devices.

JP7552240B2Active Publication Date: 2024-09-18TOYO INK MFG CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020173787
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-15
Publication Date
2024-09-18
Estimated Expiration
2040-10-15

AI Technical Summary

Technical Problem

Conventional photosensitive coloring compositions for color filters require high colorant concentrations to achieve thin films, leading to long development times and reduced pattern adhesion and shape integrity.

Method used

A photosensitive coloring composition comprising a green pigment, yellow pigment, and blue pigment, with specific metal azo pigments and halogenated zinc phthalocyanine pigments, along with a binder resin, polymerizable compound, and photopolymerization initiator, optimized for high pigment concentration and improved developability, pattern shape, and chemical resistance.

Benefits of technology

The composition enables the formation of thin color filters with good color tone, developability, pattern shape, and adhesion, while maintaining chemical resistance, suitable for applications in liquid crystal display devices and other image display technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552240000013
    Figure 0007552240000013
  • Figure 0007552240000012
    Figure 0007552240000012
  • Figure 0007552240000006
    Figure 0007552240000006
Patent Text Reader

Abstract

To provide a photosensitive coloring composition which enables formation of a color filter that has a good color tone while being thin, and has good developability, as well as, a good pattern shape and adhesion.SOLUTION: A photosensitive coloring composition contains a coloring agent (A), a binder resin (B), a polymerizable compound (C), and a photopolymerization initiator (D). The coloring agent (A) contains a green pigment, a yellow pigment and a blue pigment. The green pigment contains a zinc halide phthalocyanine pigment (A1) having, in one molecule: 10 to 16 halogen atoms on the average; 8 to 12 bromine atoms on the average; and 2 to 5 chlorine atoms on the average. The yellow pigment contains a metal azo pigment (A2) containing a compound represented by the following (a) and (b).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive coloring composition used for producing a color filter used in a liquid crystal display device, a solid-state imaging device, an organic EL display device, a quantum dot display device, electronic paper, etc. [Background technology]

[0002] As smartphones and tablet devices become thinner and lighter, there is a demand for thinner color filters to be incorporated into the liquid crystal display devices. In addition, as liquid crystal display devices become brighter and have a wider color gamut, the color filters themselves have high brightness, and thinner filters are required to increase the aperture ratio of the filter segments and thus increase brightness.

[0003] As a photosensitive coloring composition for forming a filter segment, Patent Documents 1 and 2 disclose a photosensitive coloring composition containing a zinc phthalocyanine pigment, a copper phthalocyanine pigment, and a specific dispersant. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-004009 A [Patent Document 2] JP 2018-010210 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in order to form a thin film while maintaining the color tone of the color filter, conventional photosensitive coloring compositions needed to contain a high concentration of colorant. On the other hand, this required a long development time, and there were problems such as the formation of a reverse tapered pattern and reduced adhesion of the pattern.

[0006] The present invention aims to provide a photosensitive coloring composition capable of forming a color filter having a good color tone even in a thin film, good developability, pattern shape and adhesion, and good chemical resistance. [Means for solving the problem]

[0007] The present invention relates to a photosensitive coloring composition comprising a colorant (A), a binder resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), the colorant (A) comprises a green pigment, a yellow pigment, and a blue pigment; the green pigment contains a halogenated zinc phthalocyanine pigment (A1) having an average of 10 to 16 halogen atoms in one molecule, of which the average is 8 to 12 bromine atoms and the average is 2 to 5 chlorine atoms; The present invention relates to a photosensitive coloring composition, wherein the yellow pigment comprises a metal azo pigment (A2) containing compounds represented by the following (a) and (b):

[0008] (a) a compound of formula (I) or a tautomeric form thereof [ka]

[0009] [In formula (I), R 1 and R 2 are each independently OH, NH2, or NHR 5 and R 3 and R 4 are each independently =O or =NR 5 and R 5 is a hydrogen atom or an alkyl group, and Me is Ni 2+ , Zn 2+ , Cu 2+ , Al 3+ 2 / 3 , Fe 2+ , Fe 3+ 2 / 3 , Co 2+ , and Co 3+2 / 3 are two or more divalent or trivalent metal ions selected from the following series: Cu based on 1 mole of the total of compounds (a) 2+ , Zn 2+ and Ni 2+ The total amount of ions is 95 to 100 mol %, and Al 3+ 2 / 3 , Fe 2+ , Fe 3+ 2 / 3 , Co 2+ , and Co 3+ The total amount of ions is 0 to 5 mol %, And the Cu 2+ , Zn 2+ and Ni 2+ Based on the total amount of ions, Ni 2+ The amount of ions is 10 to 95 mol %.

[0010] (b) A compound represented by formula (II) [ka]

[0011] [In formula (II), R 6 are each independently a hydrogen atom or an optionally substituted alkyl group.

[0012] The present invention also relates to the above photosensitive coloring composition, wherein the blue pigment comprises one or more pigments selected from the group consisting of CI Pigment Blue 15:3, CI Pigment Blue 15:4, and CI Pigment Blue 15:6.

[0013] Further, the present invention is directed to a photosensitive coloring composition, wherein the total amount of the colorant (A) is 10 to 50% by weight based on 100% by weight of the nonvolatile content of the photosensitive coloring composition, The present invention relates to the photosensitive coloring composition, wherein a mass ratio of the green pigment, the yellow pigment, and the blue pigment is 1:0.05 to 1:0.001 to 0.10.

[0014] The present invention also relates to a photopolymerization initiator (D) that contains an oxime ester compound. The present invention relates to the photosensitive coloring composition.

[0015] The present invention also relates to the above photosensitive coloring composition, which further contains a thermosetting compound.

[0016] The present invention also relates to a color filter comprising a substrate and a filter segment formed from the above-mentioned photosensitive coloring composition.

[0017] The present invention also relates to an image display device comprising the above color filter. Effect of the Invention

[0018] According to the present invention described above, the present invention can provide a photosensitive coloring composition, a color filter, and an image display device that can form a color filter that has a good color tone even though it is a film, has good developability, pattern shape and adhesion, and further has good chemical resistance. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a schematic cross-sectional view of an image display device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The terms used in this specification are defined below. When "(meth)acryloyl", "(meth)acrylic", "(meth)acrylic acid", "(meth)acrylate", or "(meth)acrylamide" is written, it means "acryloyl and / or methacryloyl", "acrylic and / or methacrylic", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", or "acrylamide and / or methacrylamide", respectively, unless otherwise specified. "CI" means Color Index (CI). Pixel and filter segment are synonymous. Colorants include pigments and dyes.

[0021] The photosensitive coloring composition of the present invention is preferably used by forming a coating film by coating. The coating film can be patterned by, for example, exposing to ultraviolet light and developing using a photolithography method. The pattern is preferably used as a filter segment constituting a color filter.

[0022] <Colorant (A)> The photosensitive coloring composition of the present invention contains a green pigment, a yellow pigment, and a blue pigment as colorants, and may contain dyes and other pigments as necessary. The photosensitive coloring composition of the present invention has high brightness and can achieve both developability and solvent resistance, even when the pigment concentration is high. Here, a high pigment concentration means that the pigment concentration is 40% by mass or more, preferably 45 to 60% by mass, based on 100% by mass of the nonvolatile content of the photosensitive coloring composition. As the pigment, organic or inorganic pigments can be used alone or in combination of two or more kinds. The pigment is preferably a pigment having high color development and high heat resistance, particularly a pigment having high thermal decomposition resistance, and usually an organic pigment is used. Specific examples of organic pigments that can be used in the photosensitive coloring composition are shown below by color index number.

[0023] <Green pigment> The green pigment of the present invention contains a halogenated zinc phthalocyanine pigment (A1) having an average of 10 to 16 halogen atoms in one molecule, of which the average number of bromine atoms is 8 to 12 and the average number of chlorine atoms is 2 to 5. The content of the green pigment is preferably 40 to 95% by mass in 100% by mass of the colorant (A).

[0024] <Yellow pigment> In the present invention, the yellow pigment is a photosensitive coloring composition comprising a metal azo pigment (A2) containing compounds represented by the following (a) and (b): (a) a compound of formula (I) or a tautomeric form thereof [ka] [In formula (I), R1 and R 2 are each independently OH, NH2, or NHR 5 and R 3 and R 4 are each independently =O or =NR 5 and R 5 is a hydrogen atom or an alkyl group, and Me is Ni 2+ , Zn 2+ , Cu 2+ , Al 3+ 2 / 3 , Fe 2+ , Fe 3+ 2 / 3 , Co 2+ , and Co 3+ 2 / 3 are two or more divalent or trivalent metal ions selected from the following series: Cu based on 1 mole of the total of compounds (a) 2+ , Zn 2+ and Ni 2+ The total amount of ions is 95 to 100 mol %, and Al 3+ 2 / 3 , Fe 2+ , Fe 3+ 2 / 3 , Co 2+ , and Co 3+ The total amount of ions is 0 to 5 mol %, And the Cu 2+ , Zn 2+ and Ni 2+ Based on the total amount of ions, Ni 2+ The amount of ions is 10 to 95 mol %. (b) A compound represented by formula (II) [ka] [In formula (II), R 6 are each independently a hydrogen atom or an optionally substituted alkyl group.

[0025] Other yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123, 126, 127, 128, 129, 138, 139, 147, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 192, 193, 194, 196, 198, 199, 213, 214, 231, 233, and the pigments described in JP-A-2012-226110. Preferred are CI Pigment Yellow 138, 139, 150, 185, 231, and 233, and the pigments described in JP-A-2012-226110.

[0026] <Blue pigment> The blue pigment of the present invention is not particularly limited as long as it does not impair the effects of the present invention, and known materials can be used.

[0027] Examples of blue pigments include CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, and 79. Among these, from the viewpoints of heat resistance, light resistance, and transmittance of the filter segment, preferred are CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, and 15:6, and more preferred are CI Pigment Blue 15:2, 15:3, and 15:6.

[0028] The blue pigments can be used alone or in combination of two or more kinds.

[0029] Examples of inorganic pigments include titanium oxide, barium sulfate, zinc oxide, lead sulfate, yellow lead, zinc yellow, red iron oxide (red iron (III) oxide), cadmium red, ultramarine, Prussian blue, chromium oxide green, cobalt green, amber, and synthetic iron black.

[0030] In the present specification, it has been discovered that the inclusion of a metal azo pigment (A2) can suppress the decrease in the UV curing properties of a coating film containing a halogenated zinc phthalocyanine pigment (A1), which tends to absorb UV light, and also has the unexpected effect of suppressing the formation of a reverse tapered pattern.

[0031] <Mixing pigments> It is preferable that the organic pigment is mixed with other raw materials after being subjected to a micronization treatment. Examples of the method of the micronization treatment include wet grinding, dry grinding, and dissolution precipitation. Among these, a salt milling treatment using a kneader method, which is a type of wet grinding, is preferable. The average primary particle size of the organic pigment after the micronization treatment is preferably 10 to 80 nm, more preferably 15 to 70 nm. A moderate particle size improves dispersibility and the contrast ratio of the coating. The average primary particle size is the average value of about 20 particles arbitrarily selected from an enlarged image of a TEM (transmission electron microscope). When the particle has a vertical axis length and a horizontal axis length, the vertical axis length is used.

[0032] The salt milling process is a process in which a mixture of a pigment, a water-soluble inorganic salt, and a water-soluble organic solvent is mechanically kneaded while being heated using a batch or continuous kneader such as a kneader, a two-roll mill, a three-roll mill, a ball mill, an attritor, a sand mill, or a planetary mixer, and then the water-soluble inorganic salt and the water-soluble organic solvent are removed by washing with water. The water-soluble inorganic salt acts as a crushing aid, and the pigment is crushed during salt milling by utilizing the high hardness of the inorganic salt. By optimizing the conditions for salt milling the pigment, it is possible to obtain a pigment having a very fine primary particle diameter, a narrow distribution width, and a sharp particle size distribution.

[0033] Examples of water-soluble inorganic salts include sodium chloride, potassium chloride, and sodium sulfate. Among these, sodium chloride (table salt) is preferred from the viewpoint of cost. The amount of the water-soluble inorganic salt used is preferably 50 to 2000 parts by mass, and more preferably 300 to 1000 parts by mass, per 100 parts by mass of the pigment, from the viewpoints of both treatment efficiency and production efficiency.

[0034] The water-soluble organic solvent moistens the pigment and the water-soluble inorganic salt. The water-soluble organic solvent is a compound that dissolves (is mixed) in water and does not substantially dissolve the water-soluble inorganic salt. The water-soluble organic solvent is preferably a high-boiling solvent having a boiling point of 120°C or more, in that it is less likely to volatilize due to the temperature rise during salt milling. Examples of the water-soluble organic solvent include 2-methoxyethanol, 2-butoxyethanol, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, liquid polyethylene glycol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and liquid polypropylene glycol. The amount of the water-soluble organic solvent used is preferably 5 to 1000 parts by mass, more preferably 50 to 500 parts by mass, relative to 100 parts by mass of the pigment.

[0035] During the salt milling treatment, a resin can be added as necessary. Examples of the resin include natural resins, modified natural resins, synthetic resins, and synthetic resins modified with natural resins. The resin is preferably solid at room temperature and insoluble in water, and more preferably partially soluble in a water-soluble organic solvent. The amount of the resin used is preferably 5 to 200 parts by mass relative to 100 parts by mass of the pigment. <dye> Examples of the dye include acid dyes, direct dyes, basic dyes, salt-forming dyes, oil-soluble dyes, disperse dyes, reactive dyes, mordant dyes, vat dyes, sulfur dyes, etc. Also included are dye derivatives and lake pigments obtained by converting dyes into lakes.

[0036] The acid dye preferably has an acid group such as sulfonic acid or carboxylic acid. The direct dye preferably forms an inorganic salt of the acid dye, or a salt-forming compound between the acid dye and a nitrogen-containing compound such as a quaternary ammonium salt compound, a tertiary amine compound, a secondary amine compound, or a primary amine compound. Also preferred are salt-forming compounds that are salts between a resin component having these functional groups and an acid dye. The salt-forming compound is also sulfonamidated to modify it into a sulfonic acid amide compound, which makes it easy to obtain a photosensitive coloring composition with excellent resistance (light resistance, solvent resistance). In addition, a salt-forming compound of an acid dye and a compound having an onium salt group is also preferable because it has excellent resistance (light resistance, solvent resistance). The compound having an onium salt group is preferably a resin having a cationic group.

[0037] Examples of the basic dye include salt-forming compounds with organic acids, perchloric acid, or metal salts thereof. Among the salt-forming compounds, salt-forming compounds of basic dyes are preferred because they have excellent resistance to various types of substances and are compatible with pigments.

[0038] The chemical structure of the dye may be, for example, an azo dye, a disazo dye, an azomethine dye (such as an indoaniline dye or an indophenol dye), a dipyrromethene dye, a quinone dye (such as a benzoquinone dye, a naphthoquinone dye, anthraquinone dye, or anthrapyridone dye), a carbonium dye (such as a diphenylmethane dye, a triphenylmethane dye, a xanthene dye, or an acridine dye), a quinoneimine dye (such as an oxazine dye), or a quinoneimine dye (such as an oxazine dye). dyes, thiazine dyes, etc.), azine dyes, polymethine dyes (oxonol dyes, merocyanine dyes, arylidene dyes, styryl dyes, cyanine dyes, squarylium dyes, croconium dyes, etc.), quinophthalone dyes, phthalocyanine dyes, subphthalocyanine dyes, perinone dyes, indigo dyes, thioindigo dyes, quinoline dyes, nitro dyes, nitroso dyes, rhodamine dyes, etc. Among these, from the viewpoint of color characteristics such as hue, color separation, and color unevenness, azo dyes, xanthene dyes, cyanine dyes, triphenylmethane dyes, anthraquinone dyes, dipyrromethene dyes, squarylium dyes, quinophthalone dyes, phthalocyanine dyes, and subphthalocyanine dyes are preferred, and xanthene dyes, cyanine dyes, triphenylmethane dyes, anthraquinone dyes, dipyrromethene dyes, and phthalocyanine dyes are more preferred. Specific structures of dyes are described in "New Edition Dye Handbook" (edited by Organic Synthesis Chemistry Association; Maruzen, 1970), "Color Index" (The Society of Dyers and colourists), "Dye Handbook" (edited by Okawara et al.; Kodansha, 1986), and the like.

[0039] <Dye derivatives> The photosensitive coloring composition may use a dye derivative as necessary. The dye derivative is a compound having an acidic group, a basic group, a neutral group, etc. in an organic dye residue. Examples of the dye derivative include compounds having an acidic substituent such as a sulfo group, a carboxy group, or a phosphoric acid group, as well as amine salts thereof, compounds having a basic substituent such as a sulfonamide group or a tertiary amino group at the terminal, and compounds having a neutral substituent such as a phenyl group or a phthalimidoalkyl group. Examples of organic pigments include diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thiazine indigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzoisoindole, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, naphthol pigments, threne pigments, metal complex pigments, and azo pigments such as azo, disazo, and polyazo.

[0040] Specifically, diketopyrrolopyrrole dye derivatives are described in JP 2001-220520 A, WO 2009 / 081930 B, WO 2011 / 052617 B, WO 2012 / 102399 B, and JP 2017-156397 A; phthalocyanine dye derivatives are described in JP 2007-226161 A, WO 2016 / 163351 B, JP 2017-165820 B, and Japanese Patent No. 5753266 A; and anthraquinone dye derivatives are described in JP-A-63-264674, JP-A-09-272812, JP-A-10-245501, JP-A-10-265697, JP-A-2007-079094, WO2009 / 025325 pamphlet; quinacridone dye derivatives are disclosed in JP-A-48-54128, JP-A-03-9961, JP-A-2000-273383; dioxazine dye derivatives are disclosed in JP-A-2011-162662; thiazine indigo dye derivatives are disclosed in JP-A-2007-3147 85, triazine-based dye derivatives are disclosed in JP-A-61-246261, JP-A-11-199796, JP-A-2003-165922, JP-A-2003-168208, JP-A-2004-217842, and JP-A-2007-314681, benzoisoindole-based dye derivatives are disclosed in JP-A-2009-57478, quinophthalone-based dye derivatives are disclosed in JP-A-2003-167112, JP-A-2006-291194, JP-A-2008-31281, and JP-A-2007-314681. Examples of naphthol-based dye derivatives include those described in JP-A-2012-208329 and JP-A-2014-5439, examples of azo-based dye derivatives include those described in JP-A-2001-172520 and JP-A-2012-172092, examples of acidic substituents include those described in JP-A-2004-307854, and examples of basic substituents include those described in JP-A-2002-201377, JP-A-2003-171594, JP-A-2005-181383, and JP-A-2005-213404. In these documents, the dye derivative may be referred to as a derivative, a pigment derivative, a dispersant, a pigment dispersant, or simply as a compound, but the compound having a substituent such as an acidic group, a basic group, or a neutral group in the organic dye residue is synonymous with the dye derivative.

[0041] The dye derivatives can be used alone or in combination of two or more kinds.

[0042] The content of the dye derivative is preferably from 1 to 100 parts by mass, more preferably from 3 to 70 parts by mass, and even more preferably from 5 to 50 parts by mass, relative to 100 parts by mass of the organic pigment.

[0043] When a dye derivative is added to a pigment and a micronization treatment such as acid pasting, acid slurry, dry milling, salt milling, or solvent salt milling is performed, the dye derivative is adsorbed onto the pigment surface, and the primary particles of the pigment can be made finer than when the dye derivative is not added.

[0044] In addition, by adding a dye derivative to a pigment and carrying out a dispersion treatment such as wet dispersion using a two-roll roll, a three-roll roll, or beads, the dye derivative is adsorbed onto the pigment surface, the pigment surface has polarity, and adsorption of the resin-type dispersant is promoted, and compatibility with the pigment, the dye derivative, the resin-type dispersant, the solvent, and other additives is improved, and the dispersion stability and viscosity stability over time when the pigment is made into a colored composition or a colored curable composition are improved.

[0045] <Resin-type dispersant> The photosensitive coloring composition of the present invention can use a known resin type dispersant. The resin type dispersant has a colorant affinity site that has the property of adsorbing to the colorant and a site that is compatible with components other than the colorant, and functions to stabilize the dispersion in the photosensitive coloring composition by adsorbing to the colorant. Examples of resin-type dispersants include urethane-based dispersants such as polyurethane; polycarboxylate esters such as polyacrylate, unsaturated polyamides, polycarboxylates, polycarboxylate (partial) amine salts, polycarboxylate ammonium salts, and polycarboxylate alkylamine salts; polysiloxanes; long-chain polyaminoamide phosphates, hydroxyl group-containing polycarboxylate esters; oil-based dispersants such as amides formed by the reaction of poly(lower alkylene imines) with polyesters having free carboxyl groups, and their salts; water-soluble resins and water-soluble polymer compounds such as (meth)acrylic acid-styrene copolymers, (meth)acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, polyvinyl alcohol, and polyvinylpyrrolidone; polyesters, modified polyacrylates, ethylene oxide / propylene oxide adducts, and phosphate esters.

[0046] In terms of the type of functional group, examples of the resin-type dispersant include an acidic functional group-containing resin-type dispersant and a basic functional group-containing resin-type dispersant.

[0047] Examples of the acidic functional group-containing resin-type dispersant include a resin-type dispersant having an aromatic carboxylic acid structure. These are described in, for example, WO2008 / 007776, JP2008-029901A, JP2009-155406A, JP2010-185934A, JP2011-157416A, JP2009-251481A, JP2007-23195A, and JP1996-143651A.

[0048] Examples of basic functional group-containing resin-type dispersants include nitrogen atom-containing graft copolymers, and nitrogen atom-containing acrylic block copolymers and urethane polymer dispersants having functional groups including tertiary amino groups, quaternary ammonium bases, nitrogen-containing heterocycles, etc., in the side chains.

[0049] In addition, as disclosed in JP 2009-185277 A, a resin-type dispersant having an aromatic carboxyl group and a vinyl-based resin having a tertiary amino group (having the function of a resin-type dispersant) can be used in combination.

[0050] The resin-type dispersants can be used alone or in combination of two or more kinds.

[0051] The content of the resin-type dispersant is preferably about 3 to 200 mass %, and more preferably about 5 to 100 mass %, relative to 100 parts by mass of the colorant (A). When an appropriate amount is contained, film formability is improved.

[0052] <Binder resin (B)> The binder resin (B) is preferably a resin having a transmittance of 80% or more in the entire wavelength range of 400 to 700 nm when a coating having a thickness of 2 μm is formed. The transmittance is preferably 95% or more. The binder resin (B) is preferably a thermoplastic resin or a photosensitive resin. The binder resin (B) is preferably alkali-soluble. This allows the coating formed from the photosensitive coloring composition to be patterned by a photolithography method. The photosensitive resin not having alkali solubility and the alkali-soluble resin can have a thermosetting group. Examples of the thermosetting group include an epoxy group and an oxetanyl group.

[0053] Thermoplastic resins are not alkali-soluble. Examples of thermoplastic resins include acrylic resins, butyral resins, styrene-maleic acid copolymers, chlorinated polyethylene, chlorinated polypropylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, polyvinyl acetate, polyurethane resins, polyester resins, vinyl resins, alkyd resins, polystyrene resins, polyamide resins, rubber resins, cyclized rubber resins, celluloses, polyethylenes (HDPE, LDPE), polybutadiene, and polyimide resins. Examples of the alkali-soluble resin having no photosensitivity include resins having an acidic group such as a carboxyl group or a sulfone group. Examples of the alkali-soluble resin having no photosensitivity include acrylic resins having an acidic group, α-olefin / maleic acid (anhydride) copolymers, styrene / styrene sulfonic acid copolymers, ethylene / (meth)acrylic acid copolymers, and isobutylene / maleic acid (anhydride) copolymers. Among these, acrylic resins having an acidic group and styrene / styrene sulfonic acid copolymers are preferred in terms of improving developability, heat resistance, and transparency.

[0054] <Alkali-soluble photosensitive resin> The alkali-soluble photosensitive resin has photosensitivity because it has a polymerizable unsaturated group. Any known resin can be used as the alkali-soluble photosensitive resin as long as it is alkali-soluble and photosensitive, but resins synthesized by the following methods (i) and (ii) are preferred. When the alkali-soluble photosensitive resin is used, it undergoes three-dimensional crosslinking by light irradiation, increasing the crosslink density, improving the chemical resistance of the coating.

[0055] [Method (i)] Method (i) is, for example, a method in which a polymer of an epoxy group-containing monomer and other monomers is first synthesized. Next, a monocarboxyl group-containing monomer is added to the epoxy group of the polymer, and the resulting hydroxyl group is reacted with a polybasic acid anhydride to obtain an alkali-soluble photosensitive resin. The monocarboxyl group-containing monomer is a monomer having one carboxyl group.

[0056] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 2-glycidoxyethyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, and 3,4-epoxycyclohexyl (meth)acrylate. Among these, glycidyl (meth)acrylate is preferred from the viewpoint of reactivity.

[0057] Examples of the monocarboxyl group-containing monomer include monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, and p-vinylbenzoic acid, and (meth)acrylic acid substituted with haloalkyl, alkoxyl, halogen, nitro, or cyano at the α-position.

[0058] Examples of polybasic acid anhydrides include tetrahydrophthalic anhydride, phthalic anhydride, hexahydrophthalic anhydride, succinic anhydride, maleic anhydride, etc. The polybasic acid anhydride may have a carboxyl group that does not form an acid anhydride.

[0059] Examples of other monomers include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, and ethoxypolyethylene glycol (meth)acrylate; Alternatively, examples of the monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, and acryloylmorpholine; styrenes such as styrene and α-methylstyrene; vinyl ethers such as ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, and isobutyl vinyl ether; and fatty acid vinyls such as vinyl acetate and vinyl propionate.

[0060] Also, cyclohexylmaleimide, phenylmaleimide, methylmaleimide, ethylmaleimide, 1,2-bismaleimidoethane 1,6-bismaleimidohexane, 3-maleimidopropionic acid, 6,7-methylenedioxy-4-methyl-3-maleimidocoumarin, 4,4'-bismaleimidodiphenylmethane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, N,N'-1,3-phenylenedimaleimide, N,N'-1,4-phenylenedimaleimide, N-(1-pyrenyl)maleimide, N-(2,4,6-trichlorophenyl)maleimide, N-(4-aminophenyl)maleimide, N-(4-nitrophenyl)maleimide, N-benzylmaleimide, N-bromomethyl-2,3-dichloromaleimide, N-succinimidyl-3-maleimide N-substituted maleimides such as N-phenylenediamine benzoate, N-succinimidyl-3-maleimidopropionate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidohexanoate, N-[4-(2-benzimidazolyl)phenyl]maleimide and 9-maleimidoacridine, EO-modified cresol acrylate, n-nonylphenoxy polyethylene glycol acrylate, phenoxyethyl acrylate, ethoxylated phenyl acrylate, ethylene oxide (EO)-modified (meth)acrylate of phenol, EO- or propylene oxide (PO)-modified (meth)acrylate of paracumylphenol, EO-modified (meth)acrylate of nonylphenol, and PO-modified (meth)acrylate of nonylphenol.

[0061] In the method (ii), for example, a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and other monomers are synthesized to prepare a polymer, and then the hydroxyl group of the polymer is reacted with an isocyanate group of an isocyanate group-containing monomer to synthesize an alkali-soluble photosensitive resin.

[0062] Examples of the hydroxyl group-containing monomer include hydroxyalkyl methacrylates such as 2-hydroxyethyl (meth)acrylate, 2- or 3-hydroxypropyl (meth)acrylate, 2-, 3- or 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate. Other examples include polyether mono(meth)acrylates obtained by addition polymerization of ethylene oxide, propylene oxide, and / or butylene oxide to hydroxyalkyl (meth)acrylates, and polyester mono(meth)acrylates obtained by addition of polyγ-valerolactone, polyε-caprolactone, and / or poly12-hydroxystearic acid. Among these, 2-hydroxyethyl methacrylate and glycerol mono(meth)acrylate are preferred, and glycerol mono(meth)acrylate is more preferred.

[0063] Examples of the isocyanate group-containing monomer include 2-(meth)acryloylethyl isocyanate, 2-(meth)acryloyloxyethyl isocyanate, and 1,1-bis[methacryloyloxy]ethyl isocyanate.

[0064] Monomers that can be used other than the above-mentioned monomers include, in addition to the other monomers exemplified in the above method (i), phosphate ester group-containing monomers, etc.

[0065] The phosphate group-containing monomer is, for example, a compound obtained by reacting the hydroxyl group of a hydroxyl group-containing monomer with a phosphate esterifying agent such as phosphorus pentoxide or polyphosphoric acid.

[0066] The above-mentioned raw materials for the binder resin (B) can be used alone or in combination of two or more kinds. The binder resin (B) can be used alone or in combination of two or more kinds.

[0067] The content of the binder resin (B) is preferably 20 to 400 parts by mass, more preferably 50 to 250 parts by mass, based on 100 parts by mass of the colorant (A). In order to obtain good film-forming properties and various resistances, the content is preferably 20 parts by mass or more, and in order to obtain a high colorant concentration and to obtain good color characteristics, the content is preferably 400 parts by mass or less.

[0068] The weight average molecular weight (Mw) of the binder resin (B) is preferably from 2,000 to 40,000, more preferably from 3,000 to 30,000, and even more preferably from 4,000 to 20,000. The value of Mw / Mn is preferably not more than 10. Here, Mn is the number average molecular weight.

[0069] The acid value of the alkali-soluble resin is preferably 50 to 200 mgKOH / g, more preferably 70 to 180 mgKOH / g, and even more preferably 90 to 170 mgKOH / g. A suitable acid value allows a high level of balance to be achieved among alkali solubility, adhesion, and residue suppression.

[0070] <Polymerizable compound (C)> The polymerizable compound (C) is a monomer or oligomer containing a polymerizable unsaturated group. Examples of the polymerizable compound (C) include an acid group-containing monomer, a urethane bond-containing monomer, and other monomers.

[0071] Examples of the acid group of the acid group-containing monomer include a sulfonic acid group, a carboxyl group, and a phosphoric acid group.

[0072] Examples of the acid group-containing monomer include esters of free hydroxyl group-containing poly(meth)acrylates of polyhydric alcohols and (meth)acrylic acid with dicarboxylic acids; esters of polycarboxylic acids with monohydroxyalkyl (meth)acrylates; and the like. Specific examples include free carboxyl group-containing monoesters of monohydroxy oligoacrylates or monohydroxy oligomethacrylates, such as trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol pentamethacrylate, with dicarboxylic acids, such as malonic acid, succinic acid, glutaric acid, and phthalic acid; and free carboxyl group-containing oligoesters of tricarboxylic acids, such as propane-1,2,3-tricarboxylic acid (tricarballylic acid), butane-1,2,4-tricarboxylic acid, benzene-1,2,3-tricarboxylic acid, benzene-1,3,4-tricarboxylic acid, and benzene-1,3,5-tricarboxylic acid, with monohydroxy monoacrylates or monohydroxy monomethacrylates, such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate.

[0073] (Urethane bond-containing monomer) Examples of the urethane bond-containing monomer include polyfunctional urethane acrylates obtained by reacting a (meth)acrylate having a hydroxyl group with a polyfunctional isocyanate, and polyfunctional urethane acrylates obtained by reacting an alcohol with a polyfunctional isocyanate and further reacting the alcohol with a (meth)acrylate having a hydroxyl group.

[0074] Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol ethylene oxide modified penta(meth)acrylate, dipentaerythritol propylene oxide modified penta(meth)acrylate, dipentaerythritol caprolactone modified penta(meth)acrylate, glycerol acrylate methacrylate, glycerol dimethacrylate, 2-hydroxy-3-acryloylpropyl methacrylate, a reaction product of an epoxy group-containing compound and a carboxy(meth)acrylate, and a hydroxyl group-containing polyol polyacrylate.

[0075] Examples of the polyfunctional isocyanate include tolylene diisocyanate, hexamethylene diisocyanate, diphenylmethylene diisocyanate, isophorone diisocyanate, and polyisocyanate.

[0076] Other monomers include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, β-carboxyethyl (meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, trimethylolpropane PO modified tri(meth)acrylate, trimethylolpropane EO modified tri(meth)acrylate, isocyanuric acid EO modified di(meth)acrylate, isocyanuric acid EO modified tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, Examples of the acrylic acid esters and methacrylic acid esters include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, 1,6-hexanediol diglycidyl ether di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol diglycidyl ether di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tricyclodecanyl (meth)acrylate, (meth)acrylic acid ester of methylolated melamine, epoxy (meth)acrylate, and urethane acrylate, as well as (meth)acrylic acid, styrene, vinyl acetate, hydroxyethyl vinyl ether, ethylene glycol divinyl ether, pentaerythritol trivinyl ether, (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-vinyl formamide, and acrylonitrile.

[0077] The polymerizable compound (C) can be used alone or in combination of two or more kinds.

[0078] The blending amount of the polymerizable compound (C) is preferably 1 to 50 mass %, more preferably 2 to 40 mass parts, based on 100 mass % of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is blended, the curability and developability are further improved.

[0079] <Photopolymerization initiator (D)> The photopolymerization initiator (D) is, for example, 4-phenoxydichloroacetophenone, 4-t-butyl-dichloroacetophenone, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-1-[4-(4-morpholino)phenyl]-2-(phenylmethyl)-1-butanone, or 2-(dimethylamino)-2-[(4- acetophenone compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, or benzil dimethyl ketal; benzophenone, benzoylbenzoic acid, benzoylbenzoic acid methyl, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, or 3,3',4,4'-tetra(t- butylperoxycarbonyl)benzophenone and other benzophenone compounds; thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, 2,4-diethylthioxanthone and other thioxanthone compounds; 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis( triazine-based compounds such as 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, or 2,4-trichloromethyl-(4'-methoxystyryl)-6-triazine;Examples of suitable oxime ester compounds include 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], or ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); phosphine compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide or diphenyl-2,4,6-trimethylbenzoylphosphine oxide; quinone compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate compounds; carbazole compounds; imidazole compounds; or titanocene compounds. Among these, oxime ester compounds are preferred.

[0080] (Oxime ester compounds) The photopolymerization initiator preferably contains an oxime ester compound. In the oxime ester compound, the NO bond of the oxime is cleaved by absorbing ultraviolet light, generating an iminyl radical and an alkyloxy radical. These radicals further decompose to generate highly active radicals, so that a pattern can be formed with a small amount of exposure. When the colorant concentration of the photosensitive coloring composition is high, the ultraviolet transmittance of the coating film may decrease, resulting in a low degree of curing of the coating film, but the oxime ester compound has a high quantum efficiency and can be used suitably.

[0081] Examples of the oxime ester compound include oxime ester photopolymerization initiators described in JP-A-2007-210991, JP-A-2009-179619, JP-A-2010-037223, JP-A-2010-215575, JP-A-2011-020998, and the like.

[0082] The photopolymerization initiator (D) can be used alone or in combination of two or more kinds.

[0083] The content of the photopolymerization initiator (D) is preferably 2 to 50 parts by mass, and more preferably 2 to 30 parts by mass, based on 100 parts by mass of the colorant. When an appropriate amount is added, the photocurability and developability are further improved.

[0084] The photosensitive coloring composition may further contain a sensitizer. Examples of the sensitizer include polymethine dyes such as chalcone derivatives, unsaturated ketones typified by dibenzalacetone, 1,2-diketone derivatives typified by benzil and camphorquinone, benzoin derivatives, fluorene derivatives, naphthoquinone derivatives, anthraquinone derivatives, xanthene derivatives, thioxanthene derivatives, xanthone derivatives, thioxanthone derivatives, coumarin derivatives, ketocoumarin derivatives, cyanine derivatives, merocyanine derivatives, and oxonol derivatives, acridine derivatives, azine derivatives, thiazine derivatives, oxazine derivatives, indoline derivatives, azulene derivatives, azulenium derivatives, squarylium derivatives, porphyrin derivatives, tetraphenylporphyrin derivatives, triarylmethane derivatives, tetrabenzoporphyrin derivatives, and tetrapyrazinoporphyrazine derivatives. , phthalocyanine derivatives, tetraazaporphyrazine derivatives, tetraquinoxalyloporphyrazine derivatives, naphthalocyanine derivatives, subphthalocyanine derivatives, pyrylium derivatives, thiopyrylium derivatives, tetraphylline derivatives, annulene derivatives, spiropyran derivatives, spirooxazine derivatives, thiospiropyran derivatives, metal arene complexes, organic ruthenium complexes, or Michler's ketone derivatives, α-acyloxy esters, acylphosphine oxides, methylphenyl glyoxylates, benzyl, 9,10-phenanthrenequinone, camphorquinone, ethyl anthraquinone, 4,4'-diethylisophthalophenone, 3,3' or 4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 4,4'-bis(diethylamino)benzophenone, and the like. Among these, thioxanthone derivatives, Michler's ketone derivatives, and carbazole derivatives are preferred. Specifically, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-dichlorothioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 1-chloro-4-propoxythioxanthone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(ethylmethylamino)benzophenone, N-ethylcarbazole, 3-benzoyl-N-ethylcarbazole, 3,6-dibenzoyl-N-ethylcarbazole, and the like are more preferred.

[0085] The sensitizers can be used alone or in combination of two or more kinds.

[0086] The content of the sensitizer is preferably 3 to 60 parts by mass, and more preferably 5 to 50 parts by mass, based on 100 parts by mass of the polymerization initiator (E). When an appropriate amount is contained, the photocurability and developability are further improved.

[0087] <Thermosetting compounds> The photosensitive coloring composition can contain a thermosetting compound. When a color filter is produced using the photosensitive coloring composition, the thermosetting compound is thermally cured in the post-baking process to increase the crosslink density of the coating, thereby improving heat resistance. This suppresses pigment aggregation in the post-baking process, improving the contrast ratio.

[0088] The thermosetting compound may be a low molecular weight compound or a high molecular weight compound such as a resin. Examples of the thermosetting compound include epoxy compounds, oxetane compounds, benzoguanamine compounds, rosin-modified maleic acid compounds, rosin-modified fumaric acid compounds, melamine compounds, urea compounds, and phenol compounds. Among these, epoxy compounds and oxetane compounds are preferred.

[0089] <Thiol-based chain transfer agent> The photosensitive coloring composition can contain a chain transfer agent. The chain transfer agent is preferably a thiol-based chain transfer agent. When the thiol-based chain transfer agent is used in combination with a photopolymerization initiator, a thiyl radical that is not easily inhibited by oxygen during radical polymerization after irradiation with light is generated, and the sensitivity of the photosensitive coloring composition is improved.

[0090] The thiol chain transfer agent is preferably a polyfunctional thiol having two or more thiol groups (SH groups). It is more preferable that the thiol chain transfer agent has four or more SH groups. As the number of functional groups increases, the coating becomes easier to photocure from the surface to the deepest part.

[0091] Examples of polyfunctional thiols include hexanedithiol, decanedithiol, 1,4-butanediol bisthiopropionate, 1,4-butanediol bisthioglycolate, ethylene glycol bisthioglycolate, ethylene glycol bisthiopropionate, trimethylolpropane tristhioglycolate, trimethylolpropane tristhiopropionate, trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakisthioglycolate, pentaerythritol tetrakisthioglycolate, and ethylene glycol bisthiopropionate. Examples of the thiopropionate include erythritol tetrakisthiopropionate, trimercaptopropionic acid tris(2-hydroxyethyl)isocyanurate, 1,4-dimethylmercaptobenzene, 2,4,6-trimercapto-s-triazine, 2-(N,N-dibutylamino)-4,6-dimercapto-s-triazine, and preferably, ethylene glycol bisthiopropionate, trimethylolpropane tristhiopropionate, and pentaerythritol tetrakisthiopropionate.

[0092] The thiol chain transfer agents can be used alone or in combination of two or more kinds.

[0093] The content of the thiol-based chain transfer agent is preferably 0.1 to 10 mass%, more preferably 0.1 to 5 mass%, based on 100 mass% of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the photosensitivity and taper shape are improved, and wrinkles are less likely to occur on the coating surface.

[0094] <Polymerization inhibitor> The photosensitive coloring composition may contain a polymerization inhibitor, which can suppress photosensitivity due to diffracted light from a mask during exposure in a photolithography method, making it easier to obtain a pattern of a desired shape.

[0095] Examples of the polymerization inhibitor include alkyl catechol compounds such as catechol, resorcinol, 1,4-hydroquinone, 2-methyl catechol, 3-methyl catechol, 4-methyl catechol, 2-ethyl catechol, 3-ethyl catechol, 4-ethyl catechol, 2-propyl catechol, 3-propyl catechol, 4-propyl catechol, 2-n-butyl catechol, 3-n-butyl catechol, 4-n-butyl catechol, 2-tert-butyl catechol, 3-tert-butyl catechol, 4-tert-butyl catechol, and 3,5-di-tert-butyl catechol; 2-methyl resorcinol, 4-methyl resorcinol, 2-ethyl resorcinol, 4-ethyl resorcinol, 2-propyl resorcinol, 4-propyl resorcinol, and 2-n-butyl catechol. Examples of the alkyl resorcinol include alkyl resorcinol compounds such as ethylresorcinol, 4-n-butylresorcinol, 2-tert-butylresorcinol, and 4-tert-butylresorcinol; alkylhydroquinone compounds such as methylhydroquinone, ethylhydroquinone, propylhydroquinone, tert-butylhydroquinone, and 2,5-di-tert-butylhydroquinone; phosphine compounds such as tributylphosphine, trioctylphosphine, tricyclohexylphosphine, triphenylphosphine, and tribenzylphosphine; phosphine oxide compounds such as trioctylphosphine oxide and triphenylphosphine oxide; phosphite compounds such as triphenylphosphite and trisnonylphenylphosphite; pyrogallol; and phloroglucinone.

[0096] The polymerization inhibitors can be used alone or in combination of two or more kinds.

[0097] The content of the polymerization inhibitor is preferably 0.01 to 0.4 parts by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition. Within this range, the effect of the polymerization inhibitor is increased, and the linearity of the taper, wrinkles in the coating film, pattern resolution, etc. are improved.

[0098] <Ultraviolet absorbing agent> The photosensitive coloring composition may contain an ultraviolet absorbing agent. Examples of the ultraviolet absorbing agent include benzotriazole-based compounds, triazine-based compounds, benzophenone-based compounds, salicylic acid ester-based compounds, cyanoacrylate-based compounds, and salicylate-based compounds. The ultraviolet absorbing agent may be an oligomer or a polymer.

[0099] Benzotriazole compounds include, for example, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α, α-Dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 5% 2-methoxy-1-methylethyl acetate and 95% benzenepropanoic acid, 3-(2H-benzotriazol-2-yl)-(1,1-dimethylethyl)-4-hydroxy, C7-9 side and linear alkyl ester mixture, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, methyl 3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 reaction products, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-t- Butyl-4-methylphenol, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, octyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate.

[0100] Examples of triazine compounds include 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol, and the reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine with (2-ethylhexyl)-glycidic acid ester. Examples of the compound include 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)phenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine.

[0101] Examples of benzophenone compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid-3H2O, 2-hydroxy-4-n-octoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0102] Examples of the salicylate ester compounds include phenyl salicylate, p-octylphenyl salicylate, and p-tert-butylphenyl salicylate.

[0103] The ultraviolet absorbents can be used alone or in combination of two or more kinds.

[0104] The content of the ultraviolet absorber is preferably 5 to 70% by mass relative to 100% by mass of the total of the photopolymerization initiator and the ultraviolet absorber. When an appropriate amount is contained, the resolution after development is further improved.

[0105] The total content of the photopolymerization initiator and the ultraviolet absorber is preferably 1 to 20% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the adhesion between the substrate and the coating is further improved, and good resolution can be obtained.

[0106] <Antioxidants> The photosensitive coloring composition can contain an antioxidant. The antioxidant can prevent the coating film formed from the photosensitive coloring composition from yellowing due to oxidation during the thermal process of heat curing or ITO annealing, and suppress the decrease in the transmittance of the coating film. In particular, when the colorant concentration of the photosensitive coloring composition is high, the content of the photopolymerizable compound (D) is relatively reduced, so that the coating film is likely to yellow when the amount of the photopolymerization initiator is increased or a thermosetting compound is blended. Therefore, by including an antioxidant, yellowing due to oxidation during the heating process can be prevented, and the decrease in the transmittance of the coating film can be suppressed.

[0107] Examples of the antioxidant include hindered phenol-based, hindered amine-based, phosphorus-based, sulfur-based, and hydroxylamine-based compounds. In this specification, the antioxidant is preferably a compound that does not contain a halogen atom.

[0108] Among these, from the viewpoint of achieving both the transmittance and the sensitivity of the coating film, hindered phenol-based antioxidants, hindered amine-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants are preferred.

[0109] The antioxidants can be used alone or in combination of two or more kinds.

[0110] The content of the antioxidant is preferably 0.5 to 5.0% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition, which leads to further improvements in transmittance, spectral characteristics, and sensitivity.

[0111] <Leveling agent> The photosensitive coloring composition can contain a leveling agent. This improves the wettability of the transparent substrate during film formation and the drying property of the film. Examples of the leveling agent include silicone surfactants, fluorine surfactants, nonionic surfactants, cationic surfactants, and anionic surfactants.

[0112] The surfactants can be used alone or in combination of two or more.

[0113] The content of the surfactant is preferably 0.001 to 2.0% by mass, more preferably 0.005 to 1.0% by mass, based on the non-volatile content of the photosensitive coloring composition. By being within this range, the balance between the coatability, pattern adhesion, and transmittance of the photosensitive coloring composition is further improved.

[0114] <Storage stabilizer> The photosensitive coloring composition can contain a storage stabilizer to stabilize the viscosity of the composition over time. Examples of the storage stabilizer include quaternary ammonium chlorides such as benzyl trimethyl chloride and diethylhydroxyamine, organic acids such as lactic acid and oxalic acid and their methyl ethers, organic phosphines such as t-butylpyrocatechol, tetraethylphosphine and tetraphenylphosphine, and phosphites.

[0115] The content of the storage stabilizer is preferably 0.1 to 10% by mass based on 100 parts by mass of the colorant (A).

[0116] <Adhesion improver> The photosensitive coloring composition can contain an adhesion improver. This improves the adhesion between the coating and the substrate. In addition, it becomes easier to form a narrow pattern by photolithography. Examples of the adhesion improver include a silane coupling agent.

[0117] Examples of the silane coupling agent include vinyl silanes such as vinyl trimethoxy silane and vinyl triethoxy silane, (meth)acrylic silanes such as 3-methacryloxypropyl methyl dimethoxy silane, 3-methacryloxypropyl trimethoxy silane, 3-methacryloxypropyl methyl diethoxy silane, 3-methacryloxypropyl triethoxy silane and 3-acryloxypropyl trimethoxy silane, epoxy silanes such as 2-(3,4-epoxycyclohexyl) ethyl trimethoxy silane, 3-glycidoxypropyl methyl dimethoxy silane, 3-glycidoxypropyl trimethoxy silane, 3-glycidoxypropyl methyl diethoxy silane and 3-glycidoxypropyl triethoxy silane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxy silane, N-2-( aminosilanes such as N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride; mercaptos such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; styryls such as p-styryltrimethoxysilane; ureidos such as 3-ureidopropyltriethoxysilane; sulfides such as bis(triethoxysilylpropyl)tetrasulfide; and isocyanates such as 3-isocyanatepropyltriethoxysilane.

[0118] The content of the adhesion improver is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the colorant (A). When an appropriate amount is contained, the photosensitivity of the photosensitive coloring composition is improved, the adhesion of the coating is further improved, and the resolution of the pattern is further improved.

[0119] <Method for producing photosensitive coloring composition> The photosensitive coloring composition is prepared by dispersing an organic pigment, a resin-type dispersant, a solvent, etc., for example. When a dispersing aid such as a dye derivative is used during the dispersing process, the organic pigment can be dispersed more finely, and when the pigment has high solubility in the solvent, the dispersing process may not be necessary. Since at least three types of pigments are used in this specification, a dispersion can be prepared for each pigment and then mixed. Also, a dispersion can be prepared by using two or more types of pigments at once. Next, the binder resin (B), the polymerizable compound (C), and the photopolymerization initiator (D) are blended into the dispersion and mixed to obtain a photosensitive coloring composition. It goes without saying that the timing of blending each material is arbitrary. Also, the above-mentioned production is one example, and it goes without saying that other methods can be used for production.

[0120] The dispersion treatment can be carried out using, for example, a kneader, a two-roll mill, a three-roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, or the like.

[0121] The photosensitive coloring composition is preferably prepared as a so-called resist material. The resist material may be of a solvent development type or an alkali development type, with the alkali development type being preferred.

[0122] <Solvent> The photosensitive coloring composition can contain a solvent. This makes it easier to adjust the viscosity of the photosensitive coloring composition, making it easier to form a coating with a smooth surface. The solvent may be appropriately selected according to the purpose of use, and may be contained in an appropriate amount.

[0123] Examples of the solvent include ester solvents (solvents containing -COO- but not -O- in the molecule), ether solvents (solvents containing -O- but not -COO- in the molecule), ether ester solvents (solvents containing -COO- and -O- in the molecule), ketone solvents (solvents containing -CO- but not -COO- in the molecule), alcohol solvents (solvents containing OH in the molecule and not containing -O-, -CO- or -COO-), aromatic hydrocarbon solvents, amide solvents, dimethyl sulfoxide, and the like.

[0124] Of the above solvents, from the viewpoint of coatability and drying property, it is preferable to include an organic solvent having a boiling point at 1 atm of 120° C. or more and 180° C. or less. Among them, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, propylene glycol monomethyl ether, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone, N,N-dimethylformamide, N-methylpyrrolidone, etc. are preferred, and propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, ethyl 3-ethoxypropionate, etc. are more preferred.

[0125] <Removal of large particles> In this specification, it is preferable to remove the contained coarse particles at the stage of the colorant dispersion or after the photosensitive coloring composition is prepared, which makes it easier to form a fine pattern since foreign matter can be removed from the coating. The removal of coarse particles is preferably carried out by centrifuging the photosensitive coloring composition at a gravitational acceleration of 3000 to 25000 G, filtering the photosensitive coloring composition with a sintered filter or a membrane filter, or the like, to remove coarse particles of 5 μm or more, preferably coarse particles of 1 μm or more, more preferably coarse particles of 0.5 μm or more, and mixed dust. In this way, it is preferable that the coloring composition does not substantially contain particles of 0.5 μm or more. More preferably, the particles are 0.3 μm or less.

[0126] <Color filters> In this specification, the color filter comprises a base material (also referred to as a transparent substrate) and a filter segment formed from a photosensitive coloring composition. The color filter can have a red filter segment, a green filter segment, and a blue filter segment by appropriately selecting the type of colorant (A) used. In addition, the color filter can have a magenta filter segment, a cyan filter segment, and a yellow filter segment as necessary. Note that a reflective substrate can be used instead of the transparent substrate. Examples of the transparent substrate include a glass substrate. Examples of the reflective substrate include a substrate using an aluminum electrode or a thin metal film as a reflective surface. A transparent electrode such as an ITO film can also be formed on the substrate.

[0127] <Manufacturing method for color filters> It is preferable to form a color filter by first forming a black matrix on a substrate and then forming filter segments. It is also possible to form a thin film transistor (TFT) on the substrate before forming the black matrix. Examples of the black matrix include a multilayer film of chromium or chromium / chromium oxide, an inorganic film such as titanium nitride, and a resin film with a light-shielding agent dispersed therein.

[0128] The filter segments can be formed by, for example, a printing method, an electrodeposition method, a transfer method, an inkjet method, a photolithography method, etc. In this specification, the most preferred method is the photolithography method.

[0129] In the photolithography method, for example, a photosensitive coloring composition containing a colorant of a certain color tone is applied onto a transparent substrate so that the dry film thickness is about 0.2 to 5 μm to form a coating. The obtained coating (hereinafter referred to as the first coating) is exposed (irradiated with light) through a mask having a predetermined pattern. Then, the coating is developed by immersing in a solvent or an alkaline developer or spraying the developer with a spray or the like, and the uncured parts are removed to obtain a desired pattern. This process can be similarly carried out using a photosensitive coloring composition containing a colorant of another color tone to produce a color filter having filter segments of each color. In addition, a second coating (oxygen barrier film) can be formed on the first coating before exposure using polyvinyl alcohol or a water-soluble acrylic resin. This prevents the first coating from coming into contact with oxygen, thereby further improving the exposure sensitivity. In addition, the color filter can be heated to cure the uncured photopolymerizable compound in the filter segment.

[0130] Examples of the coating device include a spray coater, a spin coater, a slit coater, and a roll coater. A drying step can be carried out during coating. Examples of the drying device include a hot air oven and an infrared heater.

[0131] The developer may be an alkaline developer, for example, an inorganic alkali such as sodium carbonate or sodium hydroxide, or an organic alkali such as dimethylbenzylamine or triethanolamine. A defoaming agent or a surfactant may be added to the developer.

[0132] The color filter of the present invention is laminated to an opposing substrate using a sealant, liquid crystal is injected through an injection port provided in the sealing part, the injection port is sealed, and a polarizing film or a retardation film is laminated to the outside of the substrate as necessary, to produce a color liquid crystal display device. This color liquid crystal display device can be used in liquid crystal display modes that use color filters such as twisted nematic (TN), super twisted nematic (STN), in-plane switching (IPS), vertically aligned (VA), and optically convencive bend (OCB).

[0133] The color filter in this specification can be used for applications such as solid-state imaging devices, organic EL displays, quantum dot displays, electronic paper, and head-mounted displays, in addition to liquid crystal displays.

[0134] <Image display device> An image display device equipped with the color filter of the present invention will be described. The image display device of the present invention comprises the color filter of the present invention and a light source. Examples of light sources include cold cathode fluorescent lamps (CCFL) and white LEDs, but in the present invention, it is preferable to use a white LED because it broadens the red reproduction range. Fig. 1 is a schematic cross-sectional view of an image display device 10 equipped with the color filter of the present invention. The device 10 shown in Fig. 1 comprises a pair of transparent substrates 11 and 21 arranged to face each other at a distance, with liquid crystal LC sealed between them.

[0135] The liquid crystal LC is aligned according to a driving mode such as TN (Twisted Nematic), STN (Super Twisted Nematic), IPS (In-Plane switching), VA (Vertical Alignment), OCB (Optically Compensated Bifefringence), etc. A TFT (Thin Film Transistor) array 12 is formed on the inner surface of the first transparent substrate 11, and a transparent electrode layer 13 made of, for example, ITO is formed thereon. An alignment layer 14 is provided on the transparent electrode layer 13. In addition, a polarizing plate 15 is formed on the outer surface of the transparent substrate 11.

[0136] On the other hand, a color filter 22 of the present invention is formed on the inner surface of the second transparent substrate 21. Red, green and blue filter segments constituting the color filter 22 are separated by a black matrix (not shown).

[0137] A transparent protective film (not shown) is formed as necessary to cover the color filter 22, and a transparent electrode layer 23 made of, for example, ITO is formed on top of the transparent protective film. An alignment layer 24 is provided to cover the transparent electrode layer 23.

[0138] In addition, a polarizing plate 25 is formed on the outer surface of the transparent substrate 21. Below the polarizing plate 25, a backlight unit 30 is provided.

[0139] The white LED light source may be one in which a fluorescent filter is formed on the surface of a blue LED, or one in which a fluorescent material is contained in the resin package of a blue LED, and has a wavelength (λ3) in the range of 430 nm to 485 nm at which the emission intensity is maximized, a wavelength (λ4) in the range of 530 nm to 580 nm at which the emission intensity is maximized, and a wavelength (λ5) in the range of 600 nm to 650 nm at which the emission intensity is maximized, and the ratio (I4 / I3) of the emission intensity I3 at wavelength λ3 to the emission intensity I4 at wavelength λ4 is 0.2 or more and 0.4 or less. In particular, a white LED light source (LED1) having spectral characteristics in which the ratio (I5 / I3) of the emission intensity I3 at wavelength λ3 to the emission intensity I5 at wavelength λ5 is 0.1 or more and 1.3 or less, or a white LED light source (LED2) having a wavelength (λ1) at which the emission intensity is maximum within the range of 430 nm to 485 nm, a peak wavelength (λ2) of the second emission intensity within the range of 530 nm to 580 nm, and a ratio (I2 / I1) of the emission intensity I1 at wavelength λ1 to the emission intensity I2 at wavelength λ2 is 0.2 or more and 0.7 or less is preferred.

[0140] Specific examples of the LED 1 include NSSW306D-HG-V1 (manufactured by Nichia Chemical Industries, Ltd.) and NSSW304D-HG-V1 (manufactured by Nichia Chemical Industries, Ltd.).

[0141] Specific examples of the LED 2 include NSSW440 (manufactured by Nichia Chemical Industries, Ltd.) and NSSW304D (manufactured by Nichia Chemical Industries, Ltd.). EXAMPLES

[0142] The present invention will be described below with reference to examples. However, the present invention is not limited to these. In addition, "parts" means "parts by mass" and "%" means "% by mass".

[0143] Before going into the examples, the method of calculating the average molecular weight of the resin and the method of measuring the acid value of the resin will be described. Propylene glycol monomethyl ether acetate (hereinafter, PGMAc)

[0144] (Average molecular weight of resin) The number average molecular weight (Mn) and mass average molecular weight (Mw) of the resin were measured by gel permeation chromatography (GPC) equipped with an RI detector. The instrument used was an HLC-8220GPC (manufactured by Tosoh Corporation), with two separation columns connected in series, and both packings were "TSK-GEL SUPER HZM-N" connected in series. The oven temperature was 40°C, THF solution was used as the eluent, and the flow rate was 0.35 ml / min. The sample was dissolved in a solvent consisting of 1 wt% of the above eluent, and 20 microliters were injected. All molecular weights are polystyrene equivalent values.

[0145] (Acid value of resin) 80 ml of acetone and 10 ml of water were added to 0.5 to 1 g of resin solution, and the solution was stirred to dissolve uniformly. The solution was titrated using an automatic titrator ("COM-555" manufactured by Hiranuma Sangyo Co., Ltd.) with a 0.1 mol / L KOH aqueous solution as the titrant, and the acid value (mgKOH / g) of the resin solution was measured. The acid value per unit of non-volatile content of the resin was calculated from the acid value of the resin solution and the concentration of non-volatile content of the resin solution.

[0146] <Production of resin-type dispersant solution 1> In the first stage synthesis, 90 parts of methyl methacrylate, 60 parts of ethyl acrylate, 40 parts of t-butyl acrylate, 10 parts of methacrylic acid, and 40 parts of propylene glycol monomethyl ether acetate (hereinafter referred to as PGMAC) were charged into a reaction vessel equipped with a gas inlet tube, a condenser, an agitator, and a thermometer, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 80°C, 12 parts of 3-mercapto-1,2-propanediol was added, and then 0.2 parts of 2,2'-azobisisobutyronitrile were added in 20 portions every 30 minutes, and the reaction was continued for 12 hours at 80°C, and it was confirmed that 95% had reacted by measuring the non-volatile content. Next, in the second stage synthesis, 18 parts of pyromellitic anhydride, 190 parts of PGMAC, and 0.4 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added, and the reaction was continued for 7 hours at 120°C. The reaction was terminated when it was confirmed by titration that 98% or more of the acid anhydride had been half-esterified. In this way, a resin-type dispersant solution with an acid value of 42 mgKOH / g per non-volatile content and a weight average molecular weight of 9,800 was obtained. After cooling to room temperature, about 2 g of the resin solution was sampled and dried by heating at 180°C for 20 minutes to measure the non-volatile content, and PGMAC was added so that the non-volatile content became 40% by mass, thereby obtaining a resin-type dispersant solution 1.

[0147] <Method for producing halogenated zinc phthalocyanine pigment (A1)> (Halogenated zinc phthalocyanine pigment (A1-1)) In a 300 mL flask, 91 parts of sulfuryl chloride, 109 parts of aluminum chloride, 15 parts of sodium chloride, 30 parts of zinc phthalocyanine, and 74 parts of bromine were charged. The mixture was heated to 130°C over 40 hours, taken out in water, and filtered to obtain a green crude pigment. 20 parts of the obtained green crude pigment, 140 parts of pulverized sodium chloride, 32 parts of diethylene glycol, and 1.8 parts of xylene were charged in a 1 L double-arm kneader and kneaded at 100°C for 6 hours. After kneading, the mixture was taken out in 2 kg of water at 80°C, stirred for 1 hour, filtered, washed with hot water, dried, and pulverized to obtain a halogenated zinc phthalocyanine pigment (A1-1). The obtained halogenated zinc phthalocyanine pigment (A1-1) was found to have an average of 13.97 halogen atoms per molecule according to fluorescent X-ray analysis using a Rigaku ZSX100E, of which the average number of bromine atoms was 11.46 and the average number of chlorine atoms was 2.51.

[0148] (Halogenated zinc phthalocyanine pigment (A1-2)) In a 300 mL flask, 91 parts of sulfuryl chloride, 109 parts of aluminum chloride, 15 parts of sodium chloride, 30 parts of zinc phthalocyanine, and 59 parts of bromine were charged. The mixture was heated to 130°C over 40 hours, taken out in water, and then filtered to obtain a green crude pigment. 20 parts of the obtained green crude pigment, 140 parts of pulverized sodium chloride, 32 parts of diethylene glycol, and 1.8 parts of xylene were charged in a 1 L double-arm kneader and kneaded at 100°C for 6 hours. After kneading, the mixture was taken out in 2 kg of water at 80°C, stirred for 1 hour, filtered, washed with hot water, dried, and pulverized to obtain a halogenated zinc phthalocyanine pigment (A1-2). The obtained halogenated zinc phthalocyanine pigment (A1-2) was found to have an average of 12.71 halogen atoms per molecule from fluorescent X-ray analysis, of which the average number of bromine atoms was 10.22 and the average number of chlorine atoms was 2.49.

[0149] (Halogenated zinc phthalocyanine pigment (A1-3)) In a 300 mL flask, 91 parts of sulfuryl chloride, 109 parts of aluminum chloride, 15 parts of sodium chloride, 30 parts of zinc phthalocyanine, and 44 parts of bromine were charged. The mixture was heated to 130°C over 40 hours, taken out in water, and then filtered to obtain a green crude pigment. 20 parts of the obtained green crude pigment, 140 parts of pulverized sodium chloride, 32 parts of diethylene glycol, and 1.8 parts of xylene were charged in a 1 L double-arm kneader and kneaded at 100°C for 6 hours. After kneading, the mixture was taken out in 2 kg of water at 80°C, stirred for 1 hour, filtered, washed with hot water, dried, and pulverized to obtain a halogenated zinc phthalocyanine pigment (A1-3). The obtained halogenated zinc phthalocyanine pigment (A1-3) was found to have an average of 11.98 halogen atoms per molecule from fluorescent X-ray analysis, of which the average number of bromine atoms was 9.00 and the average number of chlorine atoms was 2.98.

[0150] (Halogenated zinc phthalocyanine pigment (A1-4)) In a 300 mL flask, 109 parts of sulfuryl chloride, 131 parts of aluminum chloride, 18 parts of sodium chloride, 30 parts of zinc phthalocyanine, and 52 parts of bromine were charged. The mixture was heated to 130°C over 40 hours, taken out in water, and then filtered to obtain a green crude pigment. 20 parts of the obtained green crude pigment, 140 parts of pulverized sodium chloride, 32 parts of diethylene glycol, and 1.8 parts of xylene were charged in a 1 L double-arm kneader and kneaded at 100°C for 6 hours. After kneading, the mixture was taken out in 2 kg of water at 80°C, stirred for 1 hour, filtered, washed with hot water, dried, and pulverized to obtain a halogenated zinc phthalocyanine pigment (A1-4). The obtained halogenated zinc phthalocyanine pigment (A1-4) was found to have an average of 12.69 halogen atoms per molecule from fluorescent X-ray analysis, of which the average number of bromine atoms was 8.54 and the average number of chlorine atoms was 4.16.

[0151] (Halogenated zinc phthalocyanine pigment (A1-5)) Commercially available CI Pigment Green 58 (FASTOGEN Green A110 manufactured by DIC Corporation) was used as is. X-ray fluorescence analysis revealed that the average number of halogen atoms per molecule was 15.46, of which the average number of bromine atoms was 14.75 and the average number of chlorine atoms was 0.71, making this a halogenated zinc phthalocyanine pigment.

[0152] (Halogenated zinc phthalocyanine pigment (A1-6)) In a 300 mL flask, 91 parts of sulfuryl chloride, 72 parts of aluminum chloride, 15 parts of sodium chloride, 30 parts of zinc phthalocyanine, and 29 parts of bromine were charged. The mixture was heated to 130°C over 40 hours, taken out in water, and filtered to obtain a green crude pigment. 20 parts of the obtained green crude pigment, 140 parts of pulverized sodium chloride, 32 parts of diethylene glycol, and 1.8 parts of xylene were charged in a 1 L double-arm kneader and kneaded at 100°C for 6 hours. After kneading, the mixture was taken out in 2 kg of water at 80°C, stirred for 1 hour, filtered, washed with hot water, dried, and pulverized to obtain a halogenated zinc phthalocyanine pigment (A1-6). The obtained halogenated zinc phthalocyanine pigment (A1-6) was found to have an average of 8.88 halogen atoms per molecule from fluorescent X-ray analysis, of which the average number of bromine atoms was 6.90 and the average number of chlorine atoms was 1.98.

[0153] <Method of manufacturing the finely processed yellow pigment> The azobarbituric acid precursor was prepared according to the synthesis method described in JP 2017-171915 A. (Instruction 1) 46.2 g of diazobarbituric acid and 38.4 g of barbituric acid were introduced into 1100 g of distilled water at 85° C. The pH was then adjusted to about pH 5 with an aqueous potassium hydroxide solution and stirring was continued for 90 minutes. (Yellow pigment (Y-1)) Azobarbituric acid (0.3 moles) prepared in instruction 1 was mixed with 1500 parts of distilled water at 82°C. 10 parts of 30% strength hydrochloric acid were then added dropwise to adjust the pH to 2-2.5. Afterwards, 79.4 parts of melamine (0. 63 moles) were introduced. 0.3 moles of about 25% strength nickel chloride solution were then added dropwise. After 3 hours at 82°C, the pH was adjusted to about 5.5 with KOH. This was followed by dilution with about 100 parts of distilled water at 90°C. 21 parts of 30% strength hydrochloric acid were then added dropwise and the temperature was kept at 90°C for 12 hours. The pH was then adjusted to about 5 with aqueous potassium hydroxide solution. The pigment was then isolated on a suction filter, washed, dried at 80°C in a vacuum drying cabinet and ground in a standard laboratory mill for 2 minutes. (Yellow pigment (Y-1) = adduct of nickel azobarbituric acid and melamine).

[0154] (Yellow pigment (Y-2)) Yellow pigment (Y-2) was obtained in the same manner as yellow pigment (Y-1), except that "0.3 moles of approximately 25% strength nickel chloride solution" in the preparation example of yellow pigment (Y-1) was replaced by "0.225 moles of a mixed solution of 25% strength nickel chloride + 0.075 moles of a 25% strength copper (II) chloride". (Yellow pigment (Y-2) = melamine adduct of copper / nickel azobarbituric acid, a hybrid compound with 25 mole % copper and 75 mole % nickel components)

[0155] (Yellow pigment (Y-3)) Yellow pigment (Y-3) was obtained in the same manner as yellow pigment (Y-2), except that "0.3 moles of approximately 25% strength nickel chloride solution" in the preparation example of yellow pigment (Y-1) was replaced by "0.150 moles of a mixed solution of 25% strength nickel chloride + 0.150 moles of 25% strength zinc chloride". (Yellow pigment (Y-3) = melamine adduct of zinc / nickel azobarbituric acid, a hybrid compound with the components 25 mole % Zn and 75 mole % Nickel).

[0156] (Yellow pigment (Y-4)) Yellow pigment (Y-4) was obtained in the same manner as yellow pigment (Y-2), except that "0.3 moles of approximately 25% strength nickel chloride solution" in the preparation example of yellow pigment (Y-1) was replaced by "a mixed solution of 0.075 moles of 25% strength nickel chloride + 0.225 moles of 25% strength zinc chloride". (Yellow pigment (Y-4) = melamine adduct of zinc / nickel azobarbituric acid, a hybrid compound with the components 50 mole % Zn and 50 mole % Nickel).

[0157] (Yellow finely processed pigment (A2-1)) 100 parts of yellow pigment (Y-1), 10 parts of dye derivative (d-1), 1000 parts of sodium chloride, and 120 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho) and kneaded for 8 hours at 70° C. This mixture was poured into 2000 parts of warm water, heated to about 80° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, which was filtered and washed repeatedly with water to remove salt and the solvent, and then dried at 80° C. for 24 hours to obtain a yellow finely treated pigment (A2-1).

[0158] (Yellow finely processed pigment (A2-2)) A yellow finely divided pigment (A2-2) was obtained in the same manner as in the production of the yellow finely divided pigment (A2-1), except that the yellow pigment (Y-1) was changed to the yellow pigment (Y-2).

[0159] (Yellow finely processed pigment (A2-3)) A yellow finely divided pigment (A2-3) was obtained in the same manner as in the production of the yellow finely divided pigment (A2-1), except that the yellow pigment (Y-1) was changed to the yellow pigment (Y-3).

[0160] (Yellow finely processed pigment (A2-4)) A yellow finely divided pigment (A2-4) was obtained in the same manner as in the production of the yellow finely divided pigment (A2-1), except that the yellow pigment (Y-1) was changed to the yellow pigment (Y-4).

[0161] (Yellow finely processed pigment (A2-5)) 100 parts of quinophthalone-based yellow pigment CI Pigment Yellow 138 (PY138) (BASF Japan "Paliotol Yellow K0960-HD"), 700 parts of sodium chloride, and 180 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho) and kneaded for 6 hours at 80° C. This mixture was poured into 2000 parts of warm water, heated to 80° C. and stirred for 1 hour to form a slurry, filtered and washed repeatedly to remove salt and solvent, and then dried at 80° C. overnight to obtain 95 parts of a yellow finely treated pigment (A2-5).

[0162] (Blue micronized pigment (A3-1)) 90 parts of crude copper phthalocyanine synthesized by a known method and 10 parts of dye derivative (d-3) were added to 1000 parts of 98% sulfuric acid, and the mixture was stirred at 30°C for 2 hours, and then mixed with 5000 parts of water using an aspirator to obtain an aqueous solution in which copper phthalocyanine particles were precipitated. The aqueous solution obtained was stirred for 30 minutes, filtered, washed with water, dried, and pulverized to obtain 95 parts of blue finely treated pigment (A3-1). When the X-ray diffraction pattern of the obtained blue finely treated pigment (A3-1) was confirmed from 2θ=5 to 35° using an X-ray diffractometer (RIGAKU RINT2000), peaks characteristic of α-type copper phthalocyanine were confirmed at around 6.94° and 9.76°, and peaks characteristic of β-type copper phthalocyanine were not confirmed at around 6.9°, 9.0°, and 12.4°, so it was confirmed to be α-type copper phthalocyanine.

[0163] (Blue finely processed pigment (A3-2)) 85 parts of crude copper phthalocyanine synthesized by a known method, 15 parts of dye derivative (d-3), 1000 parts of sodium chloride, and 280 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader manufactured by Inoue Seisakusho Co., Ltd., and kneaded for 8 hours at 70°C. After kneading, the mixture was taken out into 20,000 parts of an aqueous buffer solution of acetic acid-sodium acetate (pH 4.0) at 45°C, and after keeping the mixture warm and stirring for 1 hour, it was filtered, washed with water, dried, and pulverized to obtain 96 parts of a blue finely treated pigment (A3-2). The X-ray diffraction pattern of the obtained blue finely treated pigment (A3-2) was confirmed from 2θ=5 to 35° using an X-ray diffractometer (RIGAKU RINT2000). Peaks characteristic of β-type copper phthalocyanine were confirmed at around 6.9°, 9.0°, and 12.4°, while peaks characteristic of α-type copper phthalocyanine were not confirmed at around 6.94° and 9.76°. Furthermore, peaks characteristic of ε-type copper phthalocyanine were not confirmed at around 7.5° and 9.1°, confirming that the pigment was β-type copper phthalocyanine.

[0164] (Blue micronized pigment (A3-3)) 95 parts of Toyocolor ε-type copper phthalocyanine pigment "LIONOL BLUE E", 5 parts of dye derivative (d-3), 1000 parts of sodium chloride, and 280 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader manufactured by Inoue Seisakusho, and kneaded for 10 hours at 80°C. After kneading, the mixture was taken out into 20,000 parts of acetic acid-sodium acetate buffer solution (pH 4.0) at 30°C, kept warm and stirred for 1 hour, then filtered, washed with water, dried, and pulverized to obtain 96 parts of blue finely treated pigment (A3-3). The X-ray diffraction pattern of the obtained blue finely treated pigment (A3-3) was confirmed from 2θ=5 to 35° using an X-ray diffractometer (RIGAKU RINT2000). Peaks characteristic of ε-type copper phthalocyanine were confirmed at around 7.5° and 9.1°, peaks characteristic of α-type copper phthalocyanine were not confirmed at around 6.94° and 9.76°, and peaks characteristic of β-type copper phthalocyanine were not confirmed at around 6.9°, 9.0°, and 12.4°, confirming that it was ε-type copper phthalocyanine.

[0165] <Method of manufacturing pigment dispersion> (Pigment Dispersion (PG-1)) The mixture below was stirred and mixed until homogeneous, and then dispersed in an Eiger mill (Eiger Japan, "Mini Model M-250 MKII") using zirconia beads with a diameter of 0.5 mm for 5 hours. The mixture was then filtered through a 5.0 μm filter to prepare a yellow pigment dispersion (PG-1). Halogenated zinc phthalocyanine pigment (A1-1): 14.0 parts Resin-type dispersant solution 1: 15.0 parts PGMAC: 71.0 copies

[0166] (Pigment Dispersion (PG-2~6, DY-1~5, DB-1~3)) The following pigment dispersions (PG-2 to 6, DY-1 to 5, DB-1 to 3) were prepared in the same manner as for the pigment dispersion (PG-1), except that the types and blending amounts (parts by mass) of the finely divided pigment, dye derivative, resin-type dispersant solution, and solvent were changed to those shown in Table 1.

[0167] [Table 1]

[0168] The dye derivatives in Table 1 are shown in Table 2.

[0169] [Table 2]

[0170] The abbreviations in Table 2 are as follows: Et: Ethyl group

[0171] <Preparation of binder resin (B) solution> (Preparation of binder resin solution (B1-1)) A separable 4-neck flask was fitted with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer. 196 parts of cyclohexanone was charged into the reaction vessel, which was then heated to 80°C and substituted with nitrogen in the reaction vessel. From the dropping tube, a mixture of 37.2 parts of n-butyl methacrylate, 12.9 parts of 2-hydroxyethyl methacrylate, 12.0 parts of methacrylic acid, 20.7 parts of paracumylphenol ethylene oxide modified acrylate ("Aronix M110" manufactured by Toagosei Co., Ltd.), and 1.1 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours. After the dropwise addition was completed, the reaction was continued for another 3 hours to obtain an acrylic resin solution. After cooling to room temperature, approximately 2 parts of the resin solution was sampled and dried at 180°C for 20 minutes to measure the non-volatile content, and PGMAc was added to the previously synthesized resin solution so that the non-volatile content was 20%, to prepare a non-photosensitive binder resin solution (B1-1). The weight average molecular weight (Mw) was 26,000.

[0172] (Preparation of binder resin solution (B1-2)) A reaction vessel equipped with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer was charged with 207 parts of cyclohexanone, heated to 80°C and substituted with nitrogen in the reaction vessel. From the dropping tube, a mixture of 20 parts of methacrylic acid, 20 parts of paracumylphenol ethylene oxide modified acrylate (Aronix M110 manufactured by Toagosei Co., Ltd.), 45 parts of methyl methacrylate, 8.5 parts of 2-hydroxyethyl methacrylate and 1.33 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours. After the dropping was completed, the reaction was continued for another 3 hours to obtain a copolymer resin solution. Next, the total amount of the copolymer solution obtained was stirred while stopping the nitrogen gas and injecting dry air for 1 hour, and then cooled to room temperature, and a mixture of 6.5 parts of 2-methacryloyloxyethyl isocyanate (Karens MOI manufactured by Showa Denko K.K.), 0.08 parts of dibutyltin laurate, and 26 parts of cyclohexanone was dropped at 70 ° C. for 3 hours. After the dropwise addition, the reaction was continued for another hour to obtain an acrylic resin solution. After cooling to room temperature, about 2 parts of the resin solution was sampled and dried by heating at 180 ° C. for 20 minutes to measure the non-volatile content, and cyclohexanone was added to the previously synthesized resin solution so that the non-volatile content was 20% to prepare a photosensitive binder resin solution (B1-2). The weight average molecular weight (Mw) was 18,000.

[0173] (Preparation of binder resin solution (B1-3)) A separable 4-neck flask equipped with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer was charged with 370 parts of cyclohexanone, heated to 80°C, and the atmosphere in the flask was replaced with nitrogen, and then a mixture of 18 parts of dicyclopentanyl methacrylate, 10 parts of benzyl methacrylate, 18.2 parts of glycidyl methacrylate, 25 parts of methyl methacrylate and 2.0 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours from the dropping tube. After the dropwise addition, the mixture was reacted at 100°C for another 3 hours, and then a solution of 1.0 part of azobisisobutyronitrile in 50 parts of cyclohexanone was added, and the reaction was continued at 100°C for another 1 hour. Next, the inside of the vessel was replaced with air, and 9.3 parts of acrylic acid (100% of glycidyl groups) was added to the vessel along with 0.5 parts of trisdimethylaminophenol and 0.1 parts of hydroquinone, and the reaction was continued for 6 hours at 120°C, and the reaction was terminated when the non-volatile acid value reached 0.5, to obtain an acrylic resin solution. Furthermore, 19.5 parts of tetrahydrophthalic anhydride (100% of the generated hydroxyl groups) and 0.5 parts of triethylamine were added and the reaction was continued for 3.5 hours at 120°C, to obtain an acrylic resin solution. After cooling to room temperature, about 2 g of the resin solution was sampled and dried at 180°C for 20 minutes to measure the non-volatile content, and PGMAc was added to the previously synthesized resin solution so that the non-volatile content was 20 mass%, to prepare binder resin solution (B1-3) (I). The weight average molecular weight (Mw) was 19,000.

[0174] (Preparation of binder resin solution (B1-4)) 333g of PGMAc was introduced into a 1L flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a gas inlet tube. Nitrogen gas was then introduced into the flask through the gas inlet tube. The solution in the flask was then heated to 100°C, and a mixture consisting of 22.0g of dicyclopentanyl methacrylate, 70.5g of benzyl methacrylate, 43.0g of methacrylic acid, 3.6g of azobisisobutyronitrile and 164g of PGMAc was added dropwise to the flask using a dropping funnel over 2 hours, and after the dropping was completed, stirring was continued for another 5 hours at 100°C. After the stirring was completed, air was introduced into the flask through the gas inlet tube, and 35.5g of glycidyl methacrylate, 0.9g of trisdimethylaminomethylphenol and 0.145g of hydroquinone were added into the flask, and the reaction was continued at 110°C for 6 hours to obtain a resin solution with a non-volatile content and an acid value of 80mgKOH / g. After cooling to room temperature, approximately 2 g of the resin solution was sampled and dried by heating at 180°C for 20 minutes to measure the non-volatile content. PGMAc was then added to the resin solution previously synthesized so that the non-volatile content was 20 mass %, to prepare binder resin solution (B1-4) (II).

[0175] <Method for producing photosensitive coloring composition for color filters> [Example 1] (Photosensitive Coloring Composition (R-1) The following mixture was stirred and mixed to be homogeneous, and then filtered through a 1.0 μm filter to prepare a photosensitive coloring composition for color filters (R-1). Pigment dispersion (PG-1): 26.42 parts Pigment dispersion (PY-2): 11.57 parts Pigment dispersion (PB-1): 0.58 parts Binder resin solution (B1-1): 30.64 parts Photopolymerizable compound (C-1): 2.70 parts Photopolymerization initiator (D-1): 0.31 parts Thermosetting compound (E-1): 0.05 part Sensitizer (F): 0.14 parts Thiol chain transfer agent (G): 0.18 parts Polymerization inhibitor (H): 0.18 parts Ultraviolet absorber (I): 0.18 parts Antioxidant (J): 0.18 parts Leveling agent (K: non-volatile content 3%): 0.30 parts Storage stabilizer (L): 0.09 parts Silane coupling agent (M): 0.18 parts Solvent (N): 26.31 parts

[0176] [Examples 2 to 32, Comparative Examples 1 to 4] (Photosensitive coloring composition (R-2~32) The following photosensitive materials were used except that the pigment dispersion, alkali-soluble resin solution, photopolymerizable compound, photopolymerization initiator, chain transfer agent, UV absorber, and solvent were changed to the types and amounts (parts by mass) shown in Table 3. Coloring Photosensitive coloring compositions for color filters (R-2 to 36) were prepared in the same manner as for the composition (R-1). In this specification, Examples 5 to 32 are reference examples.

[0177] [Table 3-1]

[0178] [Table 3-2]

[0179] [Table 3-3]

[0180] <Photopolymerizable compound (C)> (C-1) Trimethylolpropane triacrylate [Aronix M309 (manufactured by Toagosei)] (C-2) Dipentaerythritol penta- and hexaacrylate [Aronix M402 (manufactured by Toagosei)] (C-3) Polybasic acidic acrylic oligomer [Aronix M520 (manufactured by Toagosei)] (C-4) Caprolactone-modified dipentaerythritol hexaacrylate [KAYARAD DPCA-30 (manufactured by Nippon Kayaku)]

[0181] (C-5) Multifunctional urethane acrylate Pentaerythritol triacrylate (432 parts) and hexamethylene diisocyanate (84 parts) were charged into a 1 liter, five-necked reaction vessel and reacted at 60°C for 8 hours to obtain a product containing a multifunctional urethane acrylate (C-5) having a (meth)acryloyl group. The proportion of the multifunctional urethane acrylate (C-5) in the product was 70 mass%, with the remainder being other photopolymerizable monomers. It was confirmed by IR analysis that no isocyanate groups were present in the reaction product.

[0182] (C-6) Bifunctional bisphenol A (meth)acrylate [ABE-300 (manufactured by Shin-Nakamura Chemical Co., Ltd.)] (C-7) Ethoxylated isocyanuric acid triacrylate [A-9300 (manufactured by Shin-Nakamura Chemical Co., Ltd.)] The above (C-1) to (C-7) were mixed in equal amounts to obtain a photopolymerizable compound (C).

[0183] <Photopolymerization initiator (D)> (D-1) 2-Methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one [Omnirad 907 (IGM Resins)] (D-2) 2-(Dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone [Omnirad 379EG (IGM Resins)] (D-3) 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide [Omnirad TPO (manufactured by IGM Resins)] (D-4) 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetraphenyl-1,2'-biimidazole [Biimidazole (Kurokane Chemicals)] (D-5) p-Dimethylaminoacetophenone [DMA (manufactured by Daikifine)] (D-6) Ethan-1-one, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl], 1-(O-acetyloxime) [Irgacure OXE02 (manufactured by BASF Japan)] (D-7) 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one [Omnirad 2959 (IGM Resins)] (D-8) Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide [Omnirad 819 (IGM Resins)] The above (D-1) to (D-8) were mixed in equal amounts to prepare a photopolymerization initiator (D).

[0184] <Thermosetting compound (E)> Epoxy compounds (E-1) (E-1-1) 1,2-2,2'-bis(hydroxymethyl)-1-butanol Epoxy-4-(2-oxiranyl)cyclohexane adduct [EHPE-3150 (manufactured by Daicel)], (E-1-2) Glycidyl etherified epoxy compound of sorbitol [Denacol EX611 (manufactured by Nagase ChemteX Corporation)], (E-1-3) Triglycidyl isocyanurate Equal amounts of (E-1-1) to (E-1-3) were mixed to obtain epoxy compound (E-1). Oxetane compounds (E-2): 3-Ethyl-3-[(3-ethyloxetan-3-yl)methoxymethyl]oxetane [Aron Oxetane OXT-221 (manufactured by Toagosei)]

[0185] <Sensitizer (F)> (F-1) 2,4-Diethylthioxanthone [Kayacure DETX-S (manufactured by Nippon Kayaku)] (F-2) 4,4'-Bis(diethylamino)benzophenone [CHEMARK DEABP (manufactured by Chemark Chemical)] The above (F-1) and (F-2) were mixed in equal amounts to prepare sensitizer (F).

[0186] <Thiol-based chain transfer agent (G)> (G-1) Trimethylolethane tris(3-mercaptobutyrate) [TEMB (Showa Denko)] (G-2) Trimethylolpropane tris(3-mercaptobutyrate) [TPMB (Showa Denko)] (G-3) Pentaerythritol tetrakis(3-mercaptopropionate) [PEMP (Sakai Chemical Industry Co., Ltd.)] (G-4) Trimethylolpropane tris(3-mercaptopropionate) [TMMP (manufactured by Sakai Chemical Industry Co., Ltd.)] (G-5) Tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate [TEMPIC (manufactured by Sakai Chemical Industry Co., Ltd.)] The above (G-1) to (G-5) were mixed in equal amounts to prepare a thiol-based chain transfer agent (G).

[0187] <Polymerization inhibitor (H)> (H-1) 3-Methylcatechol (H-2) Methylhydroquinone (H-3) t-Butylhydroquinone The above (H-1) to (H-3) were mixed in equal amounts to prepare a polymerization inhibitor (H).

[0188] <Ultraviolet absorber (I)> (I-1) 2-[4-[(2-hydroxy-3-(dodecyl and tridecyl)oxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine [TINUVIN400 (BASF Japan)] (I-2) 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol [TINUVIN900 (manufactured by BASF Japan)] The above (I-1) and (I-2) were mixed in equal amounts to prepare an ultraviolet absorber (I).

[0189] <Antioxidants (J)> (J-1) Pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (J-2) Dioctadecyl 3,3'-thiodipropanoate (J-3) Tris[2,4-di-(t)-butylphenyl]phosphine (J-4) Bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate (J-5) p-Octylphenyl Salicylate The above (J-1) to (J-5) were mixed in equal amounts to prepare antioxidant (J).

[0190] <Leveling agent (K)> 1 copy of "BYK-330" manufactured by BYK Chemical Co., Ltd. One copy of DIC's "Megafac F-551" and A mixed solution of 1 part of Kao Corporation's "Emulgen 103" dissolved in 97 parts of PGMAc.

[0191] <Storage stabilizer (L)> (L-1) 2,6-bis(1,1-dimethylethyl)-4-methylphenol (Honshu Chemical Industry Co., Ltd. "BHT") (L-2) Triphenylphosphine (“TPP” manufactured by Hokuko Chemical Industry Co., Ltd.) The above (L-1) and (L-2) were mixed in equal amounts to prepare a storage stabilizer (L).

[0192] <Adhesion improver (M)> (M-1) 3-Glycidoxypropyltriethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.)] (M-2) 3-Methacryloxypropyltriethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBE-503 (manufactured by Shin-Etsu Chemical Co., Ltd.)] (M-3) N-2-(aminoethyl)-3-aminopropyltrimethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBM-603 (manufactured by Shin-Etsu Chemical Co., Ltd.)] (M-4) 3-Mercaptopropyltrimethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBM-803 (manufactured by Shin-Etsu Chemical Co., Ltd.)] The above (M-1) to (M-4) were mixed in equal amounts to prepare a silane coupling agent (M).

[0193] <Evaluation of Photosensitive Coloring Composition> The resulting photosensitive coloring compositions (R-1 to R-36) were evaluated for developability, film thickness, pattern adhesion, pattern shape, and chemical resistance by the following methods. The results are shown in Tables 4 and 5.

[0194] (developability) The photosensitive coloring composition obtained was applied to a glass substrate of 100 mm length x 100 mm width and 0.7 mm thickness at a rotation speed so that the film thickness after drying was 2.0 μm using a spin coater. Then, the substrate was dried at 90° C. for 90 seconds to remove the solvent, and a coating substrate was obtained. Then, the substrate was spray-developed with an alkaline developer consisting of a 0.2% by mass aqueous solution of sodium carbonate, and the time until the coating film was completely dissolved was defined as the development dissolution time, which was evaluated according to the following criteria. ○: The development dissolution time is 20 seconds or more and less than 40 seconds, and is good. △: Development dissolution time is 40 seconds or more and less than 60 seconds, and it is practical. ×: The development dissolution time is 60 seconds or more, and it is not practical.

[0195] <Formation of filter segments> A black matrix was patterned on a glass substrate measuring 100 mm long x 100 mm wide and 0.7 mm thick. The resulting photosensitive coloring composition was then applied to the coating after baking (after heating at 230°C for 20 minutes) at a rotation speed such that y in the XYZ color system would be 0.597 when a C light source was used as a backlight, and the coating was dried at 90°C for 90 seconds to remove the solvent, yielding a coating substrate. The coating was then irradiated with 100 mJ / cm2 of light using an ultra-high pressure mercury lamp through a mask having a stripe pattern with a width of 10 to 50 μm and a pattern of 400 μm x 400 μm. 2 The coated substrate was irradiated with ultraviolet light of 1000 nm. The uncured portions were then removed by spray development using an alkaline developer consisting of a 0.2% by mass aqueous solution of sodium carbonate, to form the desired pattern. The coated substrate was then heated in an oven at 230°C for 20 minutes to form filter segments. The transmission spectrum was measured using a microspectrophotometer (OSP-SP100 manufactured by Olympus Optical Co., Ltd.) to calculate x.

[0196] (Film thickness) The film thickness of the patterned portion of the obtained filter segment, which was 400 μm×400 μm, was measured using Dektak 3030 (manufactured by Japan Vacuum Engineering Co., Ltd.) The evaluation was performed according to the following criteria. ◯: The thickness was less than 2.2 μm when y was 0.597, which was a good film thickness. △: When y is 0.597, the thickness is 2.2 μm or more and less than 2.6 μm, which is a practical thickness. ×: When y becomes 0.597, the thickness is 2.7 μm or more, which is not practical.

[0197] (Pattern adhesion) The obtained filter segments were checked for the presence or absence of loss of the 10 μm to 50 μm pattern in transmission mode using an optical microscope (Nikon ECLIPSE LV100POL Model). The pattern adhesion was evaluated according to the following criteria, based on how fine the pattern remained on the glass substrate. ◯: All patterns of 10 μm or more remain, and the pattern adhesion is good. △: All patterns of 50 μm or more remain, and the pattern adhesion is sufficient for practical use. ×: Pattern adhesion of 50 μm or more was lost in some places, making the pattern adhesion impractical.

[0198] (Pattern cross-sectional shape) The cross-sectional shape of the pattern of the obtained filter segment was confirmed by a scanning electron microscope (Hitachi High-Tech Corporation's "S-3000H") The evaluation was performed by taking SEM images of a 50 μm-wide stripe pattern and evaluating them as follows. 〇: Good cross-sectional shape with taper angle of 60° or more and less than 70° △: Cross-sectional shape with taper angle of 30° or more and less than 60°, or 70° or more and less than 90°, which is acceptable for practical use ×: The taper angle is 90° or more, there is a reverse taper, and the cross-sectional shape is not practical.

[0199] (Chemical resistance) The chromaticity ([L*(1), a*(1), b*(1)]) of the obtained filter segment pattern with 400 μm×400 μm under Illuminant C was measured using a microspectrophotometer (Olympus Optical Co., Ltd., OSP-SP100). After that, the filter segment was immersed in N-methylpyrrolidone for 30 minutes, washed with ion-exchanged water, and air-dried. Next, the chromaticity ([L*(2), a*(2), b*(2)]) of the 400 μm×400 μm pattern under Illuminant C was measured, and the color difference ΔE*a*b* was calculated using the following formula. ΔE*a*b* = {(L*(2)-L*(1)) 2 +(b*(2)-b*(1)) 2 +(a*(2)-a*(1)) 2} 0.5 The evaluation criteria are as follows: ○: ΔE*a*b* is less than 2.0, and the chemical resistance is extremely good. △: ΔE*a*b* is 2.0 or more and less than 3.0, indicating practical chemical resistance. ×: ΔE*a*b* is 3.0 or more, and the chemical resistance is not suitable for practical use.

[0200] [Table 4]

Claims

1. A photosensitive coloring composition comprising a colorant (A), a binder resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), The colorant (A) includes a green pigment, a yellow pigment, and a blue pigment, the green pigment contains a halogenated zinc phthalocyanine pigment (A1) having an average of 10 to 16 halogen atoms in one molecule, of which the average is 8 to 12 bromine atoms and the average is 2 to 5 chlorine atoms; The yellow pigment comprises a metal azo pigment (A2) containing compounds represented by the following (a) and (b): the blue pigment comprises at least one selected from the group consisting of α-type copper phthalocyanine, β-type copper phthalocyanine, and ε-type copper phthalocyanine, The photosensitive coloring composition, wherein the mass ratio of the green pigment, the yellow pigment, and the blue pigment is 1:0.05 to 1:0.001 to 0.

10. (a) a compound of formula (I) or a tautomeric form thereof 【Chemistry 1】 [In formula (I), R 1 and R 2 is OH, R 3 and R 4 are each independently =O, Me is Ni 2+ , Zn 2+ , Cu 2+ are two or more divalent metal ions selected from the following series: Cu based on 1 mole of the total of the compounds (a) 2+ , Zn 2+ and Ni 2+ the total amount of ions is 95 to 100 mol %, And the Cu 2+ , Zn 2+ and Ni 2+ Based on the total amount of ions, Ni 2+ The amount of ions is 10 to 95 mol %. (b) a compound represented by formula (II) 【Chemistry 2】 [In formula (II), R 6 is a hydrogen atom.

2. The photosensitive coloring composition according to claim 1, wherein the total amount of the colorant (A) is 10 to 50% by weight based on 100% by weight of the nonvolatile content of the photosensitive coloring composition.

3. The photosensitive coloring composition according to claim 1 or 2, wherein the photopolymerization initiator (D) contains an oxime ester compound.

4. The photosensitive coloring composition according to any one of claims 1 to 3, further comprising a thermosetting compound.

5. A color filter comprising a substrate and a filter segment formed from the photosensitive coloring composition according to any one of claims 1 to 4.

6. An image display device comprising the color filter according to claim 5 .

Citation Information

Patent Citations

  • Color photosensitive composition, color filter, and liquid crystal display device

    JP2010175878A

  • Colored curing composition, color filter and method of manufacturing color filter

    JP2011084726A

  • Color filter colorant dispersion liquid, color filter photosensitive coloring resin composition, color filter, and display device

    JP2017004009A

  • Coloring material dispersion liquid for color filter, photosensitive coloring resin composition for color filter, color filter, and display device

    JP2017016132A

  • Coloring resin composition, color filter, and image display device

    JP2017142480A