Method for evaluating SiC substrates, method for manufacturing SiC epitaxial wafers, and method for manufacturing SiC devices
The photoluminescence-based evaluation method for SiC substrates effectively identifies through-hole defects by positional and signal-to-noise ratio comparison, enhancing production efficiency and reducing defects in SiC epitaxial wafers and devices.
Patent Information
- Application Number
- JP2020175604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-10-19
AI Technical Summary
Existing methods struggle to efficiently identify small through-hole defects in SiC substrates, which are crucial for SiC epitaxial wafers and devices, due to their size and the potential for inaccurate defect coordinate positioning, leading to breakdown voltage failures.
A method involving photoluminescence imaging and comparative analysis of SiC substrates cut from the same ingot, using a reference wafer to determine through defects by positional and signal-to-noise ratio criteria, allowing for efficient and cost-effective identification.
This method enables accurate detection of through-hole defects without destroying the substrates, improving yield and throughput in SiC epitaxial wafer and device production.
Smart Images

Figure 0007552246000002 
Figure 0007552246000001 
Figure 0007552246000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for evaluating a SiC substrate, a method for manufacturing a SiC epitaxial wafer, and a method for manufacturing a SiC device. [Background technology]
[0002] Silicon carbide (SiC) has an electric breakdown field one order of magnitude larger than silicon (Si) and a band gap three times larger. Silicon carbide (SiC) also has properties such as a thermal conductivity about three times higher than silicon (Si). For this reason, silicon carbide (SiC) is expected to be applied to power devices, high-frequency devices, high-temperature operating devices, and the like. For this reason, SiC epitaxial wafers have come to be used in the above-mentioned semiconductor devices in recent years.
[0003] SiC epitaxial wafers are manufactured by growing a SiC epitaxial film, which will become the active region of a SiC device, on a SiC substrate by chemical vapor deposition (CVD).
[0004] SiC substrates are produced by cutting out SiC ingots. Defects in SiC substrates have adverse effects on SiC epitaxial wafers and SiC devices. Threading defects are one of the defects that have a large impact on SiC epitaxial wafers and SiC devices. In addition, SiC devices with threading defects may cause voltage failure.
[0005] Patent Document 1 describes a method for identifying a micropipe, which is a type of through defect, from the coordinate position of the defect. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2020-31076 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, some through defects are small in size and cannot be detected by surface images taken with an optical microscope. Also, the coordinate positions may coincide by chance, so the accuracy of identifying through defects is low.
[0008] The present invention has been made in consideration of the above problems, and has an object to provide a method for evaluating SiC substrates that can identify penetrating defects efficiently and at low cost. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides the following means.
[0010] (1) A method for evaluating a SiC substrate according to a first aspect includes an image acquiring step of acquiring photoluminescence images of two or more SiC substrates among a plurality of SiC substrates cut from an ingot grown from the same seed crystal, an extraction step of extracting positions of defects in each of the two or more SiC substrates, and a determination step of comparing positions of the defects and S / N ratios of the defects in the photoluminescence images between the two or more SiC substrates to determine whether the defects are through-hole defects, the determination step including a first determination step of determining whether a substrate among the two or more SiC substrates closest to the seed crystal is a reference wafer and whether a position of a defect in the comparison wafer to be compared is within a predetermined range with respect to a position of a defect in the reference wafer, and a second determination step of determining whether an S / N ratio of a defect in the comparison wafer is equal to or less than an S / N ratio of the reference wafer, for a defect in the reference wafer and a defect in the comparison wafer whose position is determined to be within the predetermined range in the first determination step.
[0011] (2) In the method for evaluating a SiC substrate according to the above aspect, the seed crystal may have no offset angle, and the first determination step may determine whether or not a position of a defect in a comparison wafer to be compared coincides with a position of a defect in the reference wafer.
[0012] (3) In the image acquiring step of the method for evaluating a SiC substrate according to the above aspect, each of the two or more SiC substrates may be irradiated with excitation light having a wavelength of 200 nm or more and 380 nm or less to acquire the photoluminescence image.
[0013] (4) In the image acquiring step of the method for evaluating a SiC substrate according to the above aspect, the photoluminescence image may be acquired through a long-pass filter that passes wavelengths of 600 nm or more.
[0014] (5) The method for evaluating a SiC substrate according to the above aspect may further include an estimation step of estimating positions of penetrating defects in other SiC substrates of an ingot grown from the same seed crystal, based on positions of the defects in the reference wafer or the comparison wafer that are determined to be penetrating defects in the determination step.
[0015] (6) A method for producing a SiC epitaxial wafer according to a second aspect includes the method for evaluating a SiC substrate according to the above aspect.
[0016] (7) A method for producing a SiC device according to a third aspect includes the method for evaluating a SiC substrate according to the above aspect. Effect of the Invention
[0017] The SiC substrate evaluation method, SiC epitaxial wafer manufacturing method, and SiC device manufacturing method according to the above aspects can identify threading defects efficiently and at low cost. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a flow diagram of an evaluation method for a SiC substrate according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram of an ingot grown from a seed crystal. [Diagram 3] 1 shows an example of a coordinate system for extracting the position of a defect from a SiC substrate. [Figure 4]This is an enlarged image of a defect in a photoluminescence image. [Diagram 5] This is a photoluminescence image of a threading defect identical to that in FIG. 4, but located farther from the seed crystal than the defect in FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.
[0020] 1 is a flow diagram of a method for evaluating a SiC substrate according to the present embodiment. The method for evaluating a SiC substrate includes, for example, a preparation step S0, an image acquisition step S1, an extraction step S2, and a determination step S3. The method for evaluating a SiC substrate is performed, for example, in the order of the preparation step S0, the image acquisition step S1, the extraction step S2, and the determination step S3. The order of the image acquisition step S1 and the extraction step S2 may be reversed.
[0021] In the preparation step S0, an ingot is first prepared. Figure 2 is a schematic diagram of an ingot Ig grown from a seed crystal. In Figure 2, the height direction of the ingot Ig is called the z direction, one direction perpendicular to the z direction is called the x direction, and a direction perpendicular to the x direction and z direction is called the y direction. The ingot Ig is a SiC single crystal grown from the same seed crystal.
[0022] The seed crystal may or may not have an offset angle on the growth surface facing the raw material with respect to the crystal surface. If the seed crystal has an offset angle, the offset angle is, for example, 2° to 6°. The ingot is grown on the growth surface of the seed crystal by, for example, sublimation.
[0023] The ingot Ig may have penetrating defects 1 therein. The penetrating defects 1 are defects that extend in the crystal growth direction of the ingot Ig. After the SiC substrate W is cut out from the ingot Ig, the penetrating defects 1 penetrate from the front surface to the back surface of the SiC substrate W. There are two types of penetrating defects 1: penetrating defects originating from the seed crystal that originate from the interface with the seed crystal, and penetrating defects originating from bulk growth that originate from a point inside the SiC ingot (a point other than the interface with the seed crystal), with the proportion of penetrating defects originating from the seed crystal being higher.
[0024] The threading defect 1 is often formed along the crystal growth direction. For example, when a seed crystal having an offset angle is used, the threading defect 1 is often inclined with respect to the z direction of the ingot Ig. The inclination angle θ of the threading defect 1 with respect to the z direction of the ingot Ig is, for example, equal to the offset angle. When the seed crystal does not have an offset angle, the inclination angle θ is, for example, 0°.
[0025] Next, the SiC substrates W are cut out from the ingot Ig. The SiC substrates W may be cut out parallel to the xy plane or inclined with respect to the xy plane. For example, the SiC substrates W may be cut out so as to be perpendicular to the threading defects 1. By cutting out the ingot Ig, a plurality of SiC substrates W are obtained.
[0026] Next, an image acquiring step S1 is performed. In the image acquiring step S1, a photoluminescence inspection is performed on two or more SiC substrates W out of the cut out SiC substrates. By performing the photoluminescence inspection, a photoluminescence image is obtained. The photoluminescence inspection may be performed on all the cut out SiC substrates, or may be performed on some of the cut out SiC substrates.
[0027] The photoluminescence method is a method in which a substance is irradiated with excitation light and light emitted when excited electrons return to the ground state is measured. The first surface of the SiC substrate W is irradiated with excitation light having energy greater than the band gap of SiC, and the intensity of photoluminescence emitted from the SiC substrate W is measured. By applying the photoluminescence method to the SiC substrate W, defects, locations of agglomeration of impurities, etc. in the SiC substrate W can be identified. The photoluminescence inspection can be performed, for example, using SICA88 manufactured by Lasertec Corporation.
[0028] In the photoluminescence inspection, the excitation light irradiated to the SiC substrate has, for example, a wavelength of 200 nm or more and 380 nm or less, preferably a wavelength of 313 nm. When obtaining a photoluminescence image, it is preferable to detect the light emitted from the SiC substrate W through a long-pass filter that passes wavelengths of 600 nm or more.
[0029] Next, an extraction step S2 is performed. In the extraction step S2, the positions of defects in each of the two or more SiC substrates W are extracted. The positions of the defects are measured, for example, by a confocal microscope. In the extraction step S2, for example, the positions of the defects may be extracted from the photoluminescence image detected in the image acquisition step S1, or the positions of the defects may be extracted by a defect measurement performed separately from the photoluminescence (for example, a surface inspection using a microscope). The positions of the defects may also be extracted by combining the photoluminescence image with the results of a defect inspection other than photoluminescence. When the photoluminescence image is not used in the extraction step S2, the order of the image acquisition step S1 and the extraction step S2 can be reversed.
[0030] FIG. 3 shows an example of a coordinate system for extracting the position of a defect from a SiC substrate W. The SiC substrate W shown in FIG. 3 has an orientation flat OF. For example, the position of a defect D is extracted by taking the direction parallel to the orientation flat OF as the x direction and the direction perpendicular to the x direction as the y direction. The x direction is, for example, [11-20], and the y direction is, for example, [1-100]. When [11-20] and [1-100] are different from the main surface direction of the SiC substrate W, the x component may be the orthogonal projection direction component of [11-20], and the y component may be the orthogonal projection direction component of [1-100].
[0031] Next, a determination step S3 is performed. In the determination step S3, the positions of defects and the S / N ratios of the defects in the photoluminescence images of different SiC substrates W are compared. The determination step includes, for example, a first determination step S3a and a second determination step S3b.
[0032] In the first judgment step S3a, the positional relationship of defects in different SiC substrates W is compared. First, the SiC substrate closest to the seed crystal among the multiple SiC substrates W for which defect positions are compared is set as the reference wafer W1 (see FIG. 2). As described above, the rate of seed crystal-derived penetrating defects that originate from the interface with the seed crystal is high, and they may also be blocked during growth. By setting the SiC substrate W closer to the seed crystal as the reference wafer W1, the probability of overlooking penetrating defects present in the ingot Ig can be reduced. In addition, since the seed crystal-derived penetrating defects are connected across the seed crystal and the ingot Ig, it is easy to predict the position where the penetrating defects are likely to exist in the SiC substrate W closer to the seed crystal.
[0033] A SiC substrate W cut from the reference wafer W1 at a position away from the seed crystal is used as a comparison wafer W2. In a first determination step S3a, the positions of defects in the reference wafer W1 and the comparison wafer W2 are compared to determine whether they are within a predetermined range.
[0034] 2, the threading defect 1 is continuous in the crystal growth direction. Therefore, when the defect whose position is identified in the extraction step S2 is the threading defect 1, the defect position in the reference wafer W1 and the defect position in the comparative wafer W2 substantially coincide with each other.
[0035] When the seed crystal has an offset angle and the penetrating defect 1 has a tilt angle θ with respect to the z direction, the position of the penetrating defect in the reference wafer W1 is slightly shifted from the position of the penetrating defect in the comparative wafer W2. When the seed crystal does not have an offset angle and the tilt angle θ of the penetrating defect 1 with respect to the z direction of the ingot Ig is 0°, the defect position in the reference wafer W1 coincides with the defect position in the comparative wafer W2.
[0036] The amount of deviation between the two defects is a value obtained by multiplying the distance h in the z direction between the reference wafer W1 and the comparative wafer W2 in the ingot Ig by tan θ. The direction in which the defect positions are shifted is, for example, the [11-20] direction.
[0037] When the amount of deviation between a defect in the reference wafer W1 and a defect in the comparison wafer W2 is htanθ or more, it is highly likely that these defects are not interconnected through-hole defects 1. Regardless of the positional relationship between the reference wafer W1 and the comparison wafer W2 in the z direction, when the amount of deviation between the positions of the two defects is 0.6 mm or more, it is statistically highly likely that these defects are not interconnected through-hole defects 1. In this case, the "predetermined range" is, for example, htanθ or 0.6 mm.
[0038] In contrast, when the amount of deviation between a defect in the reference wafer W1 and a defect in the comparison wafer W2 is htanθ or less, these defects are likely to be interconnected through-hole defects 1. Regardless of the positional relationship between the reference wafer W1 and the comparison wafer W2 in the z direction, when the amount of deviation between the positions of the two defects is 0.2 mm or less, it is statistically highly likely that these defects are interconnected through-hole defects 1. In this case, the "predetermined range" is, for example, htanθ or 0.2 mm.
[0039] For example, when the positions of two defects are outside a predetermined range, the first determination step S3a determines that these defects are not associated with the same penetrating defect 1. The first determination step S3a roughly screens for defects associated with the same penetrating defect 1 and defects that are not associated with the same penetrating defect 1.
[0040] Next, a second judgment step S3b is performed on the defects whose positional relationship is determined to be within a predetermined range in the first judgment step S3a. The second judgment step S3b compares the S / N ratio of the defect on the reference wafer W1 in the photoluminescence image with the S / N ratio of the defect on the comparison wafer W2. The defects whose S / N ratios are compared are the defects whose positional relationship is determined to be within a predetermined range in the first judgment step S3a.
[0041] FIG. 4 is an enlarged image of a defect in a photoluminescence image. FIG. 5 is a photoluminescence image of a threading defect that is the same as the defect in FIG. 4, but is located farther from the seed crystal than the defect in FIG. 4. A threading defect appears in a photoluminescence image as a point that has a different brightness compared to its surroundings. The brightness of the defect may be higher than the brightness of the surroundings, or may be lower than the brightness of the surroundings. The ratio of the brightness of the defect bright spot to the brightness of the surroundings (S / N ratio) is, for example, 1.5 or more, or 0.75 or less. In the extraction step S2, the S / N ratio of the defect whose position has been extracted is measured. The S / N ratio is the ratio of brightness between the center of the defect and the surroundings of the defect.
[0042] The S / N ratio of a defect caused by threading defect 1 tends to be larger in the early stages of crystal growth (closer to the seed crystal) and smaller in the later stages of crystal growth (farther from the seed crystal). The defect shown in Figure 5 is caused by the same threading defect as the defect shown in Figure 4, but the S / N ratio of the defect is different because the cutting position of the SiC substrate W is different. When the defect is threading defect 1, the S / N ratio of the defect in the comparison wafer W2 is equal to or lower than the S / N ratio of the defect in the reference wafer W1.
[0043] For example, when the S / N ratio of the defect in the comparison wafer W2 is equal to or lower than the S / N ratio of the defect in the reference wafer W1, the second determination step S3b determines that the defect is associated with the same penetrating defect 1. Conversely, for example, when the S / N ratio of the defect in the comparison wafer W2 is greater than the S / N ratio of the defect in the reference wafer W1, the second determination step S3b determines that the defect is not associated with the same penetrating defect 1.
[0044] As described above, according to the method for evaluating a SiC substrate according to the present embodiment, the threading defect 1, which is one of the killer defects, can be easily estimated without destroying the SiC substrate W.
[0045] The SiC substrate evaluation method according to the present embodiment can be incorporated as one step in a method for manufacturing a SiC epitaxial wafer and a method for manufacturing a SiC device. Specifically, an evaluation step using the evaluation method is performed after cutting out a SiC substrate W from an ingot Ig and before forming an epitaxial film. By performing the evaluation step, a SiC substrate W that may become a defective product can be evaluated early, and the product yield can be increased.
[0046] In addition, the positions of the threading defects in other SiC substrates of the ingot grown from the same seed crystal can be estimated from the results obtained by comparing the reference wafer W1 and the comparative wafer W2. Hereinafter, this step is referred to as the estimation step.
[0047] In the estimation step, the positions of the threading defects in other SiC substrates of the ingot grown from the same seed crystal are estimated based on the positions of the defects in the reference wafer W1 or the comparative wafer W2 that have been determined to be threading defects in the determination step.
[0048] In the estimation step, the position of the penetrating defect in the other SiC substrate is estimated based on the position of the penetrating defect in the reference wafer W1 or the comparative wafer W2, the step flow direction, and the offset angle of the SiC substrate. The position of the penetrating defect in the other SiC substrate can be estimated to be shifted by Htanθ from the position of the penetrating defect in the reference wafer W1 or the comparative wafer W2, for example, based on the distance H in the thickness direction between the other SiC substrate and the reference wafer W1 or the comparative wafer W2 and the offset angle θ of the seed crystal.
[0049] For example, when the seed crystal does not have an offset angle and the inclination angle θ of the penetrating defect 1 with respect to the z direction of the ingot Ig is 0°, it can be estimated that the penetrating defect in the other SiC substrate is located at a position that approximately coincides with the position of the penetrating defect in the reference wafer W1 and the comparative wafer W2. S / N ratio of the penetrating defect Although the S / N ratio tends to decrease toward the crystal growth direction, even when the S / N ratio approaches 1 and detection in the image acquisition step S1 becomes difficult, the position of the penetrating defect can be estimated by the estimation step.
[0050] By performing the estimation process, it is possible to identify the positions where device killer defects may exist in SiC substrates obtained from the same SiC ingot without checking each SiC substrate, SiC epitaxial wafer, SiC chip, etc. Screening in the estimation process improves the throughput of manufacturing SiC epitaxial wafers. In the SiC substrate evaluation method according to this embodiment, from the viewpoint of performing the estimation process with high accuracy, the more SiC substrates are used, the more preferable it is. On the other hand, considering the labor required for observation, the closer to two SiC substrates are used, the more preferable it is.
[0051] Although an example of the present embodiment has been illustrated above, the present invention is not limited to these embodiments. For example, the characteristic configurations of the respective embodiments may be combined, or other configurations may be added. EXAMPLES
[0052] Example 1 Ten SiC ingots with different seed crystals were prepared, and the above-mentioned evaluation method was applied to each of the ingots. There were 63 defects whose defect positions were within the specified range and whose S / N ratios of the defects on the comparison wafer were equal to or lower than that of the reference wafer. When X-ray topography was used to examine whether each of the extracted defects was a penetrating defect, 60 penetrating defects were confirmed, and the proportion of penetrating defects was 95%.
[0053] Comparative Example 1 In Comparative Example 1, the ingot was judged without screening based on the S / N ratio. There were 75 defects whose defect positions were within the specified range, i.e., the rate of through defects was 80%.
[0054] As described above, Example 1 was able to extract penetrating defects with a higher probability than Comparative Example 1. [Explanation of symbols]
[0055] S0: preparation step, S1: image acquisition step, S2: extraction step, S3: judgment step, S3a: first judgment step, S3b: second judgment step, Ig: ingot, 1: through defect, W: SiC substrate, W1: reference wafer, W2: comparison wafer, D: defect, OF: orientation flat
Claims
1. an image acquiring step of acquiring photoluminescence images of two or more SiC substrates among a plurality of SiC substrates cut from an ingot grown from the same seed crystal; An extraction step of extracting positions of defects in each of the two or more SiC substrates; and a determination step of comparing positions of defects and S / N ratios of the defects in the photoluminescence images between the two or more SiC substrates to determine whether the defects are penetrating defects; The determination step includes: a first determination step of determining whether a position of a defect in a comparison wafer to be compared is within a predetermined range with respect to a position of a defect in the reference wafer, the first determination step being a reference wafer among the two or more SiC substrates that is closest to the seed crystal; a second determination step of determining whether an S / N ratio of the defect in the comparison wafer, the position of which is determined to be within the predetermined range in the first determination step, is equal to or lower than an S / N ratio of the defect in the reference wafer, a signal-to-noise ratio (S / N ratio) of the defect that appears in the photoluminescence image as a point with higher brightness than its surroundings is 1.5 or more, and a signal-to-noise ratio (S / N ratio) of the defect that appears in the photoluminescence image as a point with lower brightness than its surroundings is 0.75 or less.
2. The seed crystal has no offset angle; 2. The method for evaluating a SiC substrate according to claim 1, wherein the first determination step determines whether or not a defect in a comparison wafer matches a defect in the reference wafer.
3. 3. The method for evaluating a SiC substrate according to claim 1, wherein in the image acquisition step, the photoluminescence image is acquired by irradiating each of the two or more SiC substrates with excitation light having a wavelength of 200 nm or more and 380 nm or less.
4. The method for evaluating a SiC substrate according to any one of claims 1 to 3, wherein in the image acquisition step, the photoluminescence image is acquired through a long-pass filter that passes wavelengths of 600 nm or more.
5. The method for evaluating a SiC substrate according to any one of claims 1 to 4, further comprising an estimation step of estimating positions of threading defects in other SiC substrates of an ingot grown from the same seed crystal, based on positions of the defects in the reference wafer or the comparative wafer determined to be threading defects in the determination step.
6. A method for manufacturing a SiC epitaxial wafer using the method for evaluating a SiC substrate according to any one of claims 1 to 5.
7. A method for manufacturing a SiC device using the method for evaluating a SiC substrate according to any one of claims 1 to 5.
Citation Information
Patent Citations
Semiconductor substrate
JP2018131350A
Method of manufacturing silicon carbide semiconductor device
JP2020031076A
EVALUATION METHOD OF SiC SUBSTRATE, MANUFACTURING METHOD OF SiC EPITAXIAL WAFER, AND SiC EPITAXIAL WAFER
JP2020040853A
Sic epitaxial wafer
JP2020063186A
METHOD FOR EVALUATING SiC INGOT, METHOD FOR MANUFACTURING SiC DEVICE AND METHOD FOR EVALUATING SiC SEED CRYSTAL
JP2021038106A