Anti-fogging resin composition and laminated film

A laminated film with a specific polyvinyl alcohol resin composition addresses the challenge of recyclability in anti-fog films by ensuring easy removal of the antifogging resin layer, maintaining effective antifogging performance and facilitating recycling.

JP7552247B2Active Publication Date: 2024-09-18MITSUBISHI CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020175656
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-19
Publication Date
2024-09-18
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

Existing anti-fog films with polyvinyl alcohol and isobutylene-maleic anhydride copolymer coatings have good antifogging properties but are difficult to peel off, leading to issues in recyclability, as they adhere strongly to the base film.

Method used

A laminated film with an antifogging resin composition containing 90% or more of a polyvinyl alcohol resin with specific saponification and polymerization degrees, allowing for easy removal of the antifogging resin layer after use, while maintaining excellent antifogging performance.

Benefits of technology

The laminated film achieves good antifogging properties during use and facilitates easy recycling by allowing the resin layer to be peeled off, enhancing its recyclability and industrial utility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552247000001
    Figure 0007552247000001
  • Figure 0007552247000002
    Figure 0007552247000002
Patent Text Reader

Abstract

To provide a laminate film that has high anti-fogging performance during its use, and allows an anti-fogging resin layer to be removed for recycling a base film after its use, and an anti-fogging resin composition forming the anti-fogging resin layer.SOLUTION: An anti-fogging resin composition contains a polyvinyl alcohol resin of 90 mass% or more with a degree of saponification of 40-99 mol% and with an average degree of polymerization of 400 or less or 650 or more and 2500 or less. A laminate film has, on at least one side of a base film, an anti-fogging resin layer formed from the anti-fogging resin composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an anti-fogging resin composition and a laminate film having a resin layer formed from the resin composition. [Background technology]

[0002] Polyester films have excellent properties such as mechanical strength, dimensional stability, flatness, heat resistance, chemical resistance, and optical properties, and also have excellent cost performance, so they are used in a variety of applications.

[0003] Anti-fog films, which are made by imparting anti-fog properties to polyester films, have been proposed. Anti-fog films using surfactants are known, but the surfactant system exerts its anti-fog properties by bleeding out, which causes problems in use, such as sticky surfaces of the anti-fog resin layer or easy peeling off when rubbed. In response to this, a biaxially oriented polyester film with an anti-fogging coating has been proposed, which has a coating layer formed from polyvinyl alcohol and an isobutylene-maleic anhydride copolymer (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-310976 Summary of the Invention [Problem to be solved by the invention]

[0005] The anti-fog resin layer described in Patent Document 1 has good anti-fog properties, but the high adhesion of the anti-fog resin layer to the substrate film makes it difficult to peel off the anti-fog resin layer, posing a problem in terms of recyclability. That is, although a moderate level of anti-fog properties is necessary during use, when considering recycling of polyester films, it may be desirable to quickly remove the anti-fog resin layer after use and reuse the film. Therefore, there is a need for a laminated film having an anti-fogging resin layer that has adequate anti-fogging properties during use and is also easily recyclable. The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a laminate film that has good anti-fogging performance during use and that allows the base film to be recycled by peeling off the anti-fogging resin layer after use, and an anti-fogging resin composition that constitutes the anti-fogging resin layer. [Means for solving the problem]

[0006] In view of the above circumstances, the present inventors have conducted extensive research and found that the above problems can be easily solved by using an anti-fog resin composition having a specific composition and a laminate film having an anti-fog resin layer formed from the resin composition, and have thus completed the present invention. That is, the present invention provides the following items [1] to

[18] .

[0007] [1] An anti-fogging resin composition containing 90% by mass or more of a polyvinyl alcohol-based resin having a degree of saponification of 40 to 99% by mole and an average degree of polymerization of 400 or less or 650 or more and 2500 or less. [2] An anti-fogging resin composition containing 90% by mass or more of a modified polyvinyl alcohol-based resin. [3] A laminated film comprising an anti-fogging resin layer formed on at least one surface of a substrate film from the anti-fogging resin composition according to either [1] or [2] above. [4] The laminate film according to the above [3], wherein the difference between the average water droplet contact angle 20 to 60 seconds after a water droplet is dropped on the surface of the anti-fogging resin layer and the average advancing contact angle 20 to 60 seconds after the liquid is discharged by the expansion method (advancing contact angle - water droplet contact angle) is 1° or more. [5] The laminated film according to the above [3] or [4], wherein a water droplet is dropped onto the surface of the anti-fogging resin layer, and the contact angle after 60 seconds is 35° or less. [6] The laminate film according to any one of the above [3] to [4], wherein the anti-fogging resin layer is exposed to a water bath at 40°C for 1 minute and then evaluated for anti-fogging properties as rank 2 or higher. Rank 2: Blurring was visible due to the water film that formed, but visibility through the film was good [7] The laminated film according to any one of the above [3] to [6], which has an anti-fogging property evaluation of rank 2 or higher after water immersion treatment (immersion at 23°C for 1 minute). [8] The laminate film according to any one of the above [3] to [7], wherein the coating remaining rate (%) of the anti-fogging resin layer is 55% or less after immersion in water at 23°C for 1 hour. [9] The laminated film according to any one of the above [3] to [8], wherein the base film is a polyester film.

[10] The laminated film according to any one of the above [3] to [9], wherein the base film is a polyester film that is unstretched or stretched at least uniaxially.

[11] The laminated film according to any one of the above [3] to

[10] , wherein the anti-fogging resin layer has a thickness (after drying) of 0.01 μm to 1 μm.

[12] The laminated film according to any one of the above [3] to

[11] , further comprising a functional layer on the opposite side of the anti-fogging resin layer.

[13] The laminated film according to

[12] above, wherein the functional layer is a visibility improving layer.

[14] The laminated film according to the above

[13] , wherein the visibility-improving layer is a resin layer obtained by curing a resin composition containing a fluorine-containing compound and a crosslinking agent.

[15] A method for using a laminate film, comprising treating the laminate film according to any one of the above [3] to

[14] with water and / or an alcohol-based solvent and then reusing the same.

[16] The anti-fogging resin composition according to [1] or [2] above, which is for a face shield.

[17] The laminated film according to any one of the above [3] to

[14] , which is for a face shield.

[18] The use of the above

[15] as a face shield. [Effects of the Invention]

[0008] According to the present invention, it is possible to provide a laminated film that has good anti-fogging properties and also has good recyclability, and the film is highly useful industrially. DETAILED DESCRIPTION OF THE INVENTION

[0009] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the following embodiment, and can be modified and implemented as desired without departing from the gist of the present invention.

[0010] [Anti-fog resin composition] The anti-fogging resin composition of the present invention is characterized by containing 90% by mass or more of a polyvinyl alcohol-based resin having a degree of saponification of 40 to 99 mol% and an average degree of polymerization of 400 or less, or 650 to 2500. By providing an anti-fogging resin layer formed from such a PVA-based resin on at least one side of a substrate film, it is possible to provide a laminate film that has excellent anti-fogging properties and allows the substrate film to be easily recycled. Note that the polyvinyl alcohol content here means the ratio to the total non-volatile components of the composition.

[0011] (A) Polyvinyl alcohol resin Polyvinyl alcohol resins (hereinafter sometimes abbreviated as "PVA resins") are resins primarily composed of vinyl alcohol structural units, obtained by saponifying polyvinyl ester resins obtained by polymerizing vinyl ester monomers, and are composed of vinyl alcohol structural units and vinyl ester structural units in amounts corresponding to the degree of saponification.

[0012] The saponification degree of the PVA resin in the present invention is 40 to 99 mol%. If the saponification degree of the PVA resin is less than 40 mol%, it is difficult to obtain the desired anti-fogging performance. On the other hand, if the saponification degree exceeds 99 mol%, the stability of the anti-fogging resin composition tends to decrease, and recyclability may be poor due to low water solubility. From the above viewpoints, the saponification degree of the PVA resin is preferably 40 to 95 mol%, more preferably 50 to 80 mol%, and particularly preferably 50 to 70 mol%. The degree of saponification of the PVA resin is measured in accordance with JIS K 6726.

[0013] The average degree of polymerization of the PVA-based resin is 650 to 2500, preferably 800 to 2300, and particularly preferably 1000 to 2200. If the average degree of polymerization of the PVA-based resin is below the lower limit, it is difficult to form a continuous anti-fogging resin layer. On the other hand, if the average degree of polymerization is above the upper limit, the viscosity of the anti-fogging resin composition is high, and coating streaks, coating unevenness, etc. tend to occur easily. The average degree of polymerization of the PVA resin is measured in accordance with JIS K 6726. In another embodiment of the present invention, the scope of the present invention also includes a PVA-based resin having an average degree of polymerization of 400 or less, preferably 300 or less, and more preferably 250 or less. In such a system having a low average degree of polymerization, the PVA-based resin is preferably a modified polyvinyl alcohol-based resin, which will be described in detail later.

[0014] The PVA resin can be obtained, for example, by saponifying a polyvinyl ester polymer obtained by polymerizing a vinyl ester monomer. Examples of vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate, with vinyl acetate being preferred. The PVA resin may be an unmodified polyvinyl alcohol resin or a modified polyvinyl alcohol resin, but a modified polyvinyl alcohol resin is preferred.

[0015] Also within the scope of the present invention is an anti-fogging resin composition containing 90% by mass or more of a modified polyvinyl alcohol-based resin. The average polymerization degree of the modified polyvinyl alcohol-based resin is not particularly limited, but is preferably from 100 to 2500, more preferably from 150 to 2300, and even more preferably from 180 to 2200. The saponification degree is also not particularly limited, but is preferably from 40 to 99 mol%, more preferably from 50 to 80 mol%, and even more preferably from 50 to 70 mol%.

[0016] (Modified polyvinyl alcohol resin) In the present invention, the modified polyvinyl alcohol resin may be obtained by copolymerizing the vinyl ester monomer with a copolymerizable monomer. Examples of the copolymerizable monomer include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, α-octadecene, etc.; hydroxyl group-containing α-olefins such as 3-butene-1-ol, 4-pentene-1-ol, 5-hexene-1-ol, 3,4-dihydroxy-1-butene, etc., and their acylated derivatives; acetoacetyl group-containing monomers such as vinyl acetoacetate and acetoacetoxyalkyl (meth)acrylate; acrylic acid, methacrylic acid, crotonic acid, maleic acid, Unsaturated acids such as carboxylic acids such as maleic anhydride, itaconic acid, and undecylenic acid, their salts (sodium salts, potassium salts, etc.), monoesters, or dialkyl esters; polyoxyethylene (meth)allyl ether, polyoxyethylene (meth)acrylamide, polyoxypropylene (meth)acrylamide, polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, Polyoxyalkylene group-containing monomers such as polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, and polyoxypropylene vinylamine; cationic group-containing monomers such as N-acrylamidomethyltrimethylammonium chloride, N-acrylamidoethyltrimethylammonium chloride, N-acrylamidopropyltrimethylammonium chloride, 2-acryloxyethyltrimethylammonium chloride, 2-methacryloxyethyltrimethylammonium chloride, 2-hydroxy-3-methacryloyloxypropyltrimethylammonium chloride, allyltrimethylammonium chloride, methallyltrimethylammonium chloride, 3-butenetrimethylammonium chloride, dimethyldiallylammonium chloride, and diethyldiallylammonium chloride; nitriles such as acrylonitrile and methacrylonitrile;olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, or their salts; alkyl vinyl ethers; vinyl compounds such as dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, and glycerin monoallyl ether; substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate; and hydroxymethyl vinylidene diacetates such as vinylidene chloride, 1,4-diacetoxy-2-butene, 1,4-dihydroxy-2-butene, vinylene carbonate, 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyronyloxy-2-methylenepropane. The content of such copolymerizable monomers is usually 10 mol % or less, preferably 5 mol % or less, and particularly preferably 1 mol % or less, based on the total amount of the polymer. Among these copolymerizable monomers, from the viewpoint of improving anti-fogging properties, preferred monomers copolymerizable with vinyl ester-based monomers are acetoacetyl group-containing monomers, unsaturated acids such as carboxylic acids, polyoxyalkylene group-containing monomers, and cationic group-containing monomers.

[0017] Furthermore, from the viewpoint of improving the anti-fogging properties before and after the water immersion treatment described in detail below, modified polyvinyl alcohols composed of a combination of vinyl alcohol structural units and ethylene oxide group-containing structural units, or vinyl alcohol structural units and acetoacetyl group-containing structural units, are more preferred, and modified polyvinyl alcohols composed of a combination of vinyl alcohol structural units and ethylene oxide group-containing structural units are particularly preferred.

[0018] The method for polymerizing the vinyl ester monomer and the copolymerizable monomer is not particularly limited, and any conventionally known method can be used, such as bulk polymerization, solution polymerization, suspension polymerization, dispersion polymerization, or emulsion polymerization.

[0019] ((B) Other optional ingredients) When forming the anti-fogging resin layer, various conventionally known polymers such as polyester resins, acrylic resins, and urethane resins may be used in combination with the anti-fogging resin composition as a binder in order to improve the coating appearance, transparency, film-forming properties, and the like. Furthermore, within the scope of the present invention, particles for improving blocking properties or slip properties, a material having antibacterial properties for antibacterial or antiviral properties, or an ultraviolet absorber for weather resistance may also be used in combination. Among these, it is preferable to use a material having antibacterial properties in combination from the viewpoint of hygiene.

[0020] Materials with antibacterial properties are agents that have an MIC (minimum inhibitory concentration) against bacteria and fungi, and include inorganic antibacterial agents and organic antibacterial agents.

[0021] Examples of inorganic antibacterial agents include silver-based antibacterial agents, zinc-based antibacterial agents, and copper-based antibacterial agents. These are formed by supporting one or more ions selected from silver ions, zinc ions, and copper ions on an inorganic compound, and examples of inorganic compounds include zeolite, glass, talc, silica gel, silicates, mica, and sepiolite. When multiple ion species are used, each ion may be supported on the same inorganic compound. Specific examples include inorganic antibacterial agents in which silver ions and zinc ions are supported on glass. Furthermore, when multiple ion species are used, each ion may be supported on a different inorganic compound. Specific examples include inorganic antibacterial agents in which silver ions are supported on glass and inorganic antibacterial agents in which zinc ions are supported on zeolite.

[0022] Examples of organic antibacterial agents include, but are not limited to, pyridine antibacterial agents such as zinc pyrithione (bis(2-pyridithio-1-oxide)zinc), densil (2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine), and copper pyrithione (bis(2-pyridithio-1-oxide)copper); OIT (2-n-octyl-4-isothiazolin-3-one), MIT (2-methyl-4-isothiazolin-3-one), CMI (5-chloro-2-methyl-4-isothiazolin-3-one), BIT (1,2-benzisothiazolone), and n Thiazoline antibacterial agents such as Nn-butyl-1,2-benzisothiazolone-3; triazine antibacterial agents such as hexahydro-1,3,5-trimethyl-1,3,5-triazine and 2,4-dichloro-6-methoxy-1,3,5-triazine; imidazole antibacterial agents such as thiabendazole (2-(4-thiazolyl)-benzimidazole) and carbendazim (methyl-2-benzimidazole carbamate); tebuconazole ((±)-α-[2-(4-chlorophenyl)ethyl]-α-(1,1-dimethylethyl)-1H-1,2, triazole-based antibacterial agents such as 4-triazole-1-ethanol; iodine-based antibacterial agents such as diiodomethyl-paratolyl sulfone, polyvinylpyrrolidone iodine, and 3-iodo-2-propynyl butylcarbamate; arsenic-based antibacterial agents such as 10,10'-oxybis-10H-phenoxyarsine; ether-based antibacterial agents such as triclosan; triclocarban (3,4,4'-trichlorocarbanilide), halocarban (4,4-dichloro-3-(3-fluoromethyl)-carbanilide), and chlorothalonil (2,4,5,6-tetrachloroisophthalonitride) Organochlorine antibacterial agents such as chloroisocyanuric acid, dichloroisocyanuric acid, and trichloroisocyanuric acid; biguanide antibacterial agents such as chlorhexidine gluconate, chlorhexidine hydrochloride, polybiguanide hydrochloride, polyaminopropyl biguanide, and polyhexamethylene biguanide; sulfamide antibacterial agents such as dichlofluanid and trifluanid; quaternary ammonium chlorine antibacterial agents such as benzothonium chloride, cetylpyridinium chloride, and diallyldimethylammonium chloride; aldehyde antibacterial agents such as BCA (α-bromocinnamaldehyde);Examples of antibacterial agents include carboxylic acid-based antibacterial agents such as magnesium dihydrogen bismonoperoxyphthalate and zinc undecylenate; ester-based antibacterial agents such as lauricidin (glycerol laurate); phenol-based antibacterial agents such as butylparaben (butyl-p-hydroxybenzoate) and sodium orthophenylphenol; and carbamate-based antibacterial agents such as sodium N-methyldithiocarbamate.

[0023] The anti-fogging resin layer described below is composed of the above-mentioned anti-fogging resin composition, but it can be assumed that unreacted compounds of the various compounds in the anti-fogging resin composition, reacted compounds, or a mixture thereof may be present.

[0024] The proportion of the (A) PVA resin in the total nonvolatile components of the anti-fogging resin composition is usually 90 to 100 mass %, preferably 95 to 100 mass %. If the content of the (A) PVA resin is less than 90 mass %, the anti-fogging performance will be insufficient.

[0025] [Laminated film] The laminated film of the present invention has an anti-fog resin layer on at least one surface of a substrate film, and the anti-fog resin layer is formed from the anti-fog resin composition of the present invention. The anti-fog resin layer may be formed by applying the anti-fog resin composition and drying or curing it.

[0026] <Base film> The substrate film is not particularly limited as long as it can achieve the effects of the present invention, but a polyester film having excellent properties such as mechanical strength, dimensional stability, flatness, heat resistance, chemical resistance, and optical properties is preferred. The polyester film constituting the base film may have a single-layer structure or a multi-layer structure. In the case of a multi-layer structure, it may have a two-layer structure, a three-layer structure, or may have four or more layers without departing from the gist of the present invention, and the number of layers is not particularly limited. Furthermore, as the polyester film, a non-stretched film or a polyester film stretched at least in one direction is preferred, a biaxially stretched polyester film or a non-stretched polyester film is more preferred, and a biaxially stretched polyester film is even more preferred.

[0027] The polyester used may be a homopolyester or a copolymer polyester. In the case of a homopolyester, it is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of aromatic dicarboxylic acids include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and examples of aliphatic glycols include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol. A typical example of a polyester is polyethylene terephthalate. On the other hand, examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, and oxycarboxylic acid, and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 4-cyclohexanedimethanol, and neopentyl glycol.

[0028] The polyester polymerization catalyst is not particularly limited, and any conventionally known compound can be used, such as a titanium compound, a germanium compound, an antimony compound, a manganese compound, an aluminum compound, a magnesium compound, and a calcium compound.

[0029] In order to suppress the amount of oligomer component precipitation, the film may be produced using a polyester having a low content of oligomer components as the raw material. Various known methods can be used to produce polyesters having a low content of oligomer components, such as a method of solid-state polymerization after polyester production. Furthermore, the amount of oligomer component precipitation may be suppressed by forming a polyester film having three or more layers, with the outermost layer of the polyester film being a layer made from a polyester raw material having a low content of oligomer components. Alternatively, the polyester may be obtained by carrying out an esterification or transesterification reaction, followed by melt polycondensation at a higher reaction temperature under reduced pressure.

[0030] In order to improve the weather resistance of the polyester film, an ultraviolet absorber may be contained in the polyester film. The ultraviolet absorber is a compound that absorbs ultraviolet light and is not particularly limited as long as it can withstand the heat applied in the polyester film production process.

[0031] The ultraviolet absorber includes organic ultraviolet absorbers and inorganic ultraviolet absorbers, and organic ultraviolet absorbers are preferred from the viewpoint of transparency.The organic ultraviolet absorbers are not particularly limited, but examples thereof include cyclic iminoesters, benzotriazoles, and benzophenones.From the viewpoint of durability, cyclic iminoesters and benzotriazoles are more preferred.In addition, two or more types of ultraviolet absorbers can be used in combination.

[0032] Particles can be incorporated into the polyester layer of the film, primarily for the purposes of imparting lubricity and preventing scratches during each process. The type of particles to be incorporated is not particularly limited as long as they are capable of imparting lubricity. Specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide; and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a portion of a metal compound such as a catalyst during the polyester production process can also be used.

[0033] On the other hand, the shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. Furthermore, there are no particular limitations on the hardness, specific gravity, color, etc. Two or more types of these particles may be used in combination as needed.

[0034] The average particle size of the particles used is usually 5 μm or less, preferably in the range of 0.01 to 3 μm. If the particle size is 5 μm or less, the surface roughness of the film will not be too rough, and problems will not occur when various surface functional layers are formed in subsequent processes. In addition, the transparency of the film will be good.

[0035] Furthermore, the particle content in the polyester layer is usually less than 5% by mass, preferably in the range of 0.0003 to 3% by mass. When there are no particles or only a small amount of particles, the film becomes highly transparent, resulting in a film that is excellent in terms of transparency. On the other hand, when particles are contained in the above range, the film also becomes excellent in terms of slipperiness.

[0036] The method for adding particles to the polyester layer is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage in the production of the polyester constituting each layer, but it is preferable to add the particles after the completion of the esterification or transesterification reaction.

[0037] In addition to the above-mentioned particles, conventionally known antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to the polyester film as needed.

[0038] The thickness of the substrate film is not particularly limited as long as it can be formed into a film, but is usually in the range of 25 to 1000 μm, preferably 30 to 800 μm, more preferably 35 to 600 μm, and even more preferably 40 to 400 μm.

[0039] Next, examples of producing polyester films will be specifically described, but the present invention is not limited to these examples.

[0040] (unstretched polyester film) A preferred method is to extrude the dried pellets of the polyester raw material described above from a die using an extruder as a molten sheet, and then cool and solidify it on a cooling roll to obtain an unstretched sheet. In this case, it is preferable to increase the adhesion between the sheet and the rotating cooling drum to improve the flatness of the sheet, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably used. In this way, an unstretched polyester film is obtained.

[0041] (biaxially oriented polyester film) The unstretched sheet obtained by the above method is then biaxially stretched. In this case, the unstretched sheet is first stretched in one direction using a roll or tenter-type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3 to 6 times. Next, the sheet is stretched in a direction perpendicular to the first-stage stretching direction. In this case, the stretching temperature is usually 70 to 170°C, and the stretching ratio is usually 3 to 7 times, preferably 3.5 to 6 times. Subsequently, the sheet is heat-treated at a temperature of 180 to 270°C under tension or relaxation of 30% or less to obtain a biaxially oriented film. In the above stretching, a method in which unidirectional stretching is performed in two or more stages can also be used. In this case, it is preferable to perform the stretching so that the final stretching ratios in both directions are each within the above range.

[0042] A simultaneous biaxial stretching method can also be used to produce polyester films. In this method, the unstretched sheet is simultaneously stretched and oriented in both the machine direction and the width direction under temperature control, typically at 70 to 120°C, preferably 80 to 110°C, with an areal stretch ratio of 4 to 50, preferably 7 to 35, and more preferably 10 to 25. The sheet is then subsequently heat-treated at 170 to 250°C under tension or relaxation of 30% or less to obtain a stretched and oriented film. Regarding the simultaneous biaxial stretching apparatus used in the above-described stretching method, any conventionally known stretching method, such as a screw method, a pantograph method, or a linear drive method, can be used.

[0043] <Anti-fogging resin layer> The anti-fogging resin layer is a layer formed from the above-mentioned anti-fogging resin composition. The thickness of the anti-fogging resin layer (after drying) is preferably 0.01 μm to 1 μm, more preferably 0.02 μm to 0.5 μm, even more preferably 0.02 μm to 0.1 μm, and particularly preferably 0.02 μm to 0.08 μm. If the thickness of the anti-fogging resin layer is within the above range, good anti-fogging properties can be imparted.

[0044] The method for forming the anti-fogging resin layer is not particularly limited, and may be in-line coating, off-line coating, or the like. Preferably, the anti-fogging resin layer is formed by in-line coating, which treats the surface of a base film such as a polyester film during the film-forming process.

[0045] In-line coating is a method of coating within the production process of a base film. Specifically, when the base film is a polyester film, coating is performed at any stage from melt extrusion of the polyester to stretching, heat setting, and winding up. Usually, coating is performed on any of the following: an unstretched sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, or a film after heat setting and before winding up. Although not limited to the following, for example, in sequential biaxial stretching, a particularly advantageous method is to coat a uniaxially stretched film that has been stretched in the longitudinal direction (machine direction) and then stretch it in the transverse direction. This method offers advantages in terms of production costs, since film formation and the formation of the anti-fogging resin layer can be carried out simultaneously. Furthermore, because stretching is carried out after coating, the thickness of the anti-fogging resin layer can be changed by adjusting the stretch ratio, and thin-film coating can be carried out more easily than with offline coating of films.

[0046] Furthermore, by providing an anti-fog resin layer on the film before stretching, the anti-fog resin layer can be stretched together with the polyester film, thereby firmly adhering the anti-fog resin layer to the polyester film. Furthermore, in the production of biaxially stretched polyester films, by stretching while holding the film edges with clips or the like, the film can be restrained in both the longitudinal and transverse directions, and high temperatures can be applied in the heat setting step while maintaining flatness and preventing wrinkles. Therefore, the heat treatment performed after coating can be performed at a high temperature that cannot be achieved by other methods, improving the film-forming properties of the anti-fog resin layer and enabling stronger adhesion between the anti-fog resin layer and the polyester film, resulting in a stronger anti-fog resin layer.

[0047] When the anti-fogging resin layer is formed by in-line coating, it is preferable to produce a laminated film by coating a polyester film with an anti-fogging resin composition prepared by preparing an aqueous solution or dispersion of the above-mentioned compounds so that the solid content is approximately 0.1 to 50% by mass. The anti-fogging resin composition may contain a small amount of organic solvent to improve dispersibility in water, film-forming properties, etc., within the scope of the present invention. Only one type of organic solvent may be used, or two or more types may be used as appropriate.

[0048] The anti-fogging resin layer can be provided by a conventional coating method such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, curtain coating, or the like.

[0049] The drying and curing conditions when forming an anti-fog resin layer on a polyester film are not particularly limited. For example, when the anti-fog resin layer is formed by offline coating, the heat treatment is usually carried out at 80 to 200°C for 3 to 40 seconds, preferably at 100 to 180°C for 3 to 40 seconds. On the other hand, when the anti-fogging resin layer is provided by in-line coating, it is generally recommended to carry out heat treatment at 70 to 280° C. for 3 to 200 seconds.

[0050] Regardless of whether off-line coating or in-line coating is used, heat treatment and irradiation with active energy rays such as ultraviolet radiation may be used in combination as necessary. The polyester film (substrate film) constituting the laminated polyester film of the present invention may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment.

[0051] The components in the anti-fogging resin layer can be analyzed by, for example, TOF-SIMS, ESCA, fluorescent X-ray analysis, or the like.

[0052] <Functional layer> The laminate film of the present invention is characterized by having an anti-fogging resin layer on at least one side of a substrate film. The anti-fogging resin layer may be provided on one or both sides of the substrate film. Alternatively, an anti-fogging resin layer may be formed on one side of the substrate film and a different functional layer may be provided on the other side. Examples of functional layers include a visibility improving layer having functions such as low reflection and improved transmittance, a hard coat layer for preventing scratches, and an antibacterial layer for maintaining cleanliness. The functional layer may be formed by preparing a functional layer-forming composition (resin layer-forming composition) and applying it to the substrate film.

[0053] <Visibility improvement layer> The visibility-improving layer is a layer designed for low reflectivity and is a functional layer that can improve total light transmittance. By designing the functional layer for low reflectivity, it becomes possible to prevent light and objects from being reflected. Furthermore, reflectivity and total light transmittance are interrelated properties, and polyester films with low light absorption and high transparency exhibit high total light transmittance by having low reflectivity, making it possible to improve visibility.

[0054] The visibility-improving layer preferably has one minimum absolute reflectance value in the wavelength range of 300 to 800 nm, and the minimum value is 3.0% or less. The wavelength of the minimum value is more preferably in the range of 400 to 700 nm, and even more preferably in the range of 450 to 650 nm. The minimum value is also preferably 2.5% or less, and even more preferably 2.0% or less.

[0055] The visibility improving layer preferably contains a resin having a low refractive index, such as a fluorine-containing compound or an acrylic resin.

[0056] (Fluorine-containing compounds) As the fluorine-containing compound, from the viewpoint of increasing the strength of the coating film, it is preferable to use a fluorine-containing resin.Specific examples of the fluorine-containing resin include: fluoroolefin copolymer resins with vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, hexafluoropropylene, chlorotrifluoroethylene, etc. as monomers; fluorine-containing copolymer resins obtained by polymerizing compounds having polyalkylene ether groups (such as fluoromethylene ether groups, difluoromethylene ether groups, fluoroethylene ether groups, difluoroethylene ether groups, tetrafluoroethylene ether groups, hexafluoropropylene ether groups) in which part or all of hydrogen atoms are substituted with fluorine atoms, such as fluoromethylene ether groups, difluoromethylene ether groups, tetrafluoroethylene ether groups, hexafluoropropylene ether groups, etc., with other monomers; fluorine-containing copolymer resins obtained by graft polymerization of hydroxyl-containing fluororesin copolymers with (meth)acrylic acid ester compounds or other monomers; vinyl polymers having perfluoroalkyl groups, etc. Among these, from the viewpoint of low refractive index and more effectively suppressing reflection and improving transmittance, fluoroolefin copolymer resins and fluororesin copolymers containing polyalkylene ether groups in which some or all of the hydrogen atoms are fluorinated are preferred, and from the viewpoint of recyclability, fluororesin copolymers containing polyalkylene ether groups in which some or all of the hydrogen atoms are fluorinated are preferred.

[0057] Examples of fluorine-based copolymer resins obtained by polymerizing a compound having a polyalkylene ether group in which some or all of the hydrogen atoms have been substituted with fluorine atoms with other monomers include urethane resins having a polyfluoroalkylene ether group, polyester resins having a polyfluoroalkylene ether group, and acrylic resins having a polyfluoroalkylene ether group. Other monomers constituting the urethane resin having a polyfluoroalkylene ether group include isocyanate compounds. Examples of the isocyanate compound include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate; aliphatic diisocyanates having an aromatic ring such as α,α,α',α'-tetramethylxylylene diisocyanate; aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic diisocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and isopropylidenedicyclohexyl diisocyanate.

[0058] Other monomers constituting the urethane resin include polyols not containing fluorine atoms, and polyols having a carboxy group such as dimethylolpropanoic acid, dimethylolbutanoic acid, bis-(2-hydroxyethyl)propionic acid, and bis-(2-hydroxyethyl)butanoic acid. Among these, it is preferable to include a polyol having a carboxy group, from the viewpoint of being able to self-emulsify when water is used as the dispersion solvent, and among these, dimethylolpropanoic acid is more preferable.

[0059] The visibility-improving layer is preferably formed from a resin layer-forming composition containing a fluorine-containing compound. The resin layer-forming composition may contain the fluorine-containing compound as a non-volatile component, or may contain other components. Furthermore, the visibility improving layer is more preferably formed by curing a resin layer forming composition containing a fluorine-containing compound and a crosslinking agent. By curing the resin layer forming composition containing a crosslinking agent in this manner, the strength of the visibility improving layer is improved. Details of the crosslinking agent will be described later. The content of the fluorine-containing compound in the visibility-improving layer-forming composition is preferably 30 to 100% by mass, more preferably 40 to 98% by mass, and even more preferably 50 to 95% by mass, based on the non-volatile components in the resin layer-forming composition. By making it 30% by mass or more, it becomes possible to effectively lower the refractive index of the visibility-improving layer, suppress the reflectance, and improve the total light transmittance.

[0060] (acrylic resin) Acrylic resins are polymers made from polymerizable monomers, including acrylic and methacrylic monomers. These may be homopolymers or copolymers, or even copolymers with polymerizable monomers other than acrylic and methacrylic monomers. Also included are copolymers of these polymers with other polymers (e.g., polyesters, polyurethanes, etc.). Examples include block copolymers and graft copolymers. Also included are polymers (and in some cases, polymer mixtures) obtained by polymerizing polymerizable monomers in polyester solutions or polyester dispersions. Similarly, polymers (and in some cases, polymer mixtures) obtained by polymerizing polymerizable monomers in polyurethane solutions or polyurethane dispersions are also included. Similarly, polymers (and in some cases, polymer mixtures) obtained by polymerizing polymerizable monomers in other polymer solutions or dispersions are also included. Hydroxy groups or amino groups may also be included to further improve adhesion to substrates.

[0061] The polymerizable monomer is not particularly limited, but particularly representative compounds include various carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, and citraconic acid, and salts thereof; various hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, monobutylhydroxyfumarate, and monobutylhydroxyitaconate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Examples of the polymerizable monomer include various (meth)acrylic acid esters such as cyclohexyl (meth)acrylate and lauryl (meth)acrylate; various nitrogen-containing compounds such as (meth)acrylamide, diacetone acrylamide, N-methylolacrylamide, and (meth)acrylonitrile; various styrene derivatives such as styrene, α-methylstyrene, divinylbenzene, and vinyltoluene; various vinyl esters such as vinyl propionate; various silicon-containing polymerizable monomers such as γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane; phosphorus-containing vinyl monomers; various vinyl halides such as vinyl chloride and vinylidene chloride; and various conjugated dienes such as butadiene.

[0062] <Hard coat layer> The hard coat layer preferably has a pencil hardness of F or more. A pencil hardness of F or more can protect the surface of the laminate film from scratches, stains, etc. From the above viewpoints, the pencil hardness is more preferably H or more, and even more preferably 2H or more. The hard coat layer can be formed using various hard coat agents, and is not limited as long as it can obtain the above-mentioned pencil hardness. For example, a layer formed using a hard coat agent containing an active energy ray-curable resin composition or a thermosetting resin composition can be used. Specifically, the composition may contain a polymerizable monomer or a polymerizable oligomer that forms a cured product upon irradiation with active energy rays.

[0063] Examples of the polymerizable monomer include a (meth)acrylate monomer having a radically polymerizable unsaturated group in the molecule, and a (meth)acrylate oligomer having a radically polymerizable unsaturated group in the molecule. More specifically, examples of the polymerizable monomers include (meth)acrylic derivatives of polyfunctional alcohols such as dipentaerythritol hexa(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, tetramethylolmethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,6-bis(3-acryloyloxy-2-hydroxypropyloxy)hexane; and monomers or oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, epoxy (meth)acrylate, melamine (meth)acrylate, polyfluoroalkyl (meth)acrylate, and silicone (meth)acrylate. These polymerizable monomers or oligomers may be used alone or in combination of two or more. Among these, (meth)acrylic derivatives of polyfunctional alcohols and urethane (meth)acrylate are preferred because they provide high surface hardness.

[0064] <Antibacterial layer> The antibacterial layer is a functional layer having an inhibitory effect against bacteria and fungi, and suppresses the growth of bacteria on the surface of the antibacterial layer, thereby keeping the film clean. Examples of the antibacterial layer include a layer containing an antibacterial agent such as the inorganic antibacterial agent or organic antibacterial agent described above, and the antibacterial layer may have the same composition as the antifogging resin layer or a different composition.

[0065] The antibacterial layer preferably contains various polymers in combination to retain the antibacterial agent on the film surface. Specific examples of polymers include polyester resins, acrylic resins, urethane resins, polyvinyls (such as polyvinyl alcohol and vinyl chloride-vinyl acetate copolymers), polyalkylene glycols, polyalkyleneimines, methyl cellulose, hydroxycellulose, and starches. Among these, polyester resins and urethane resins are preferred, and polyester resins are more preferred, in terms of their excellent adhesion to polyester films.

[0066] (polyester resin) The polyester resin may be composed of, for example, the following polycarboxylic acids and polyhydroxy compounds as main constituents. That is, as the polycarboxylic acids, terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, p-hydroxybenzoic acid, trimellitic acid monopotassium salt, and ester-forming derivatives thereof can be used. Examples of the oxy compound that can be used include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of these compounds can be appropriately selected and used to synthesize the polyester resin by conventional polycondensation reaction.

[0067] (Crosslinking agent) The functional layer-forming composition may further contain a crosslinking agent from the viewpoint of improving the strength of the coating film. The crosslinking agent is preferably used when the functional layer is a visibility improving layer as described above. As the crosslinking agent, various known crosslinking agents can be used, such as melamine compounds, oxazoline compounds, epoxy compounds, isocyanate compounds, carbodiimide compounds, and silane coupling compounds. Among these, melamine compounds are preferably used from the viewpoint of improving the durability of the resin layer. The crosslinking agents may be used alone or in combination of two or more.

[0068] The melamine compound refers to a compound having a melamine skeleton within the compound, and examples thereof include alkylolated melamine derivatives, compounds obtained by reacting alkylolated melamine derivatives with alcohol to partially or completely etherify them, and mixtures thereof. Examples of alkylolation include methylolation, ethylolation, isopropylolation, n-butylolation, and isobutyrolation. Among these, methylolation is preferred from the viewpoint of reactivity. Examples of alcohols used for etherification include methanol, ethanol, isopropanol, n-butanol, and isobutanol, and among these, methanol is more preferred. The melamine compound may be a monomer or a dimer or higher polymer, or a mixture thereof. Furthermore, a melamine compound partially co-condensed with urea or the like may also be used. Furthermore, a catalyst may be further blended into the resin layer-forming composition to increase the reactivity of the melamine compound.

[0069] The crosslinking agent may be designed to react during the drying process or film-forming process to improve the performance of the resin layer. It is assumed that the formed resin layer contains unreacted crosslinking agent, reacted compound, or a mixture thereof.

[0070] The content of the crosslinking agent in the functional layer is preferably 1 to 50% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 30% by mass, based on the non-volatile components in the functional layer-forming composition. By making the content 1% by mass or more, the effect of blending the crosslinking agent can be more easily exerted. Furthermore, by making the content 50% by mass or less, the refractive index can be kept low, and transparency can be maintained.

[0071] The thickness of the functional layer (after drying) is preferably 0.04 μm to 0.15 μm, more preferably 0.06 μm to 0.13 μm. If the thickness of the functional layer is within the above range, the total light transmittance is high and visibility can be improved.

[0072] The method for providing the functional layer is the same as that for forming the antifogging resin layer, and any conventionally known coating method such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, curtain coating, etc. can be used.

[0073] The drying and curing conditions when forming a functional layer on a polyester film are the same as those for forming an anti-fogging resin layer. For example, when forming a functional layer by offline coating, the heat treatment is usually carried out at 80 to 200°C for 3 to 40 seconds, preferably at 100 to 180°C for 3 to 40 seconds. On the other hand, when the functional layer is provided by in-line coating, it is usually preferable to carry out heat treatment at 70 to 280° C. for 3 to 200 seconds.

[0074] Regardless of whether off-line coating or in-line coating is used, heat treatment and irradiation with active energy rays such as ultraviolet radiation may be used in combination as needed, and the polyester film constituting the base film may be previously subjected to a surface treatment such as corona treatment or plasma treatment, as in the case of forming the anti-fogging resin layer.

[0075] The analysis of various components in the functional layer can be carried out by, for example, TOF-SIMS, ESCA, fluorescent X-ray analysis, etc., in the same manner as the analysis of the anti-fogging resin layer.

[0076] [Properties of laminated film] 1) Difference between water droplet contact angle and advancing expansion angle The laminate film of the present invention has a difference (advancing contact angle - water droplet contact angle) of 1° or more between the average water droplet contact angle 20 to 60 seconds after a water droplet is dropped onto the surface of the anti-fogging resin layer and the average advancing contact angle 20 to 60 seconds after the liquid is ejected by the expansion method. More specifically, the difference between the average water droplet contact angle 20 to 60 seconds after the drop of water is dropped and the average advancing contact angle 20 to 60 seconds after the liquid is ejected by the expansion method, measured using an automatic contact angle meter (DataPhysics, model OCA20), is 1° or more, preferably 3° or more, more preferably 4° or more, and even more preferably 5° or more. It is believed that when a water droplet comes into contact with the surface of the anti-fogging resin layer, some of the components derived from the anti-fogging resin layer are dissolved into the water droplet and spread across the surface of the resin layer. Therefore, when the difference between the advancing contact angle and the water droplet contact angle is less than 1°, the newly contacting water droplet spreads across the surface of the anti-fogging resin layer faster than the rate at which the anti-fogging resin layer components are dissolved into the water droplet, and the viscosity difference of the water film formed on the surface of the resin layer increases depending on the position of the landing water droplet, causing bleeding, and it is presumed that this results in poor visibility and reduced visibility even when trying to see the scenery on the other side through the film.

[0077] 2) Water droplet contact angle In the laminate film of the present invention, it is preferable that a water droplet is dropped onto the surface of the anti-fogging resin layer, and the contact angle after 60 seconds has elapsed is 35° or less. More specifically, the anti-fogging resin layer in the laminate film of the present invention preferably has a contact angle of 35° or less, more preferably 30° or less, even more preferably 25° or less, and particularly preferably 20° or less, measured 60 seconds after a water droplet is dropped thereon using an automatic contact angle meter (manufactured by DataPhysics, Model OCA20). When the contact angle is within the above range, the anti-fogging performance is excellent.

[0078] 3) Thickness of the anti-fogging resin layer The surface of the anti-fogging resin layer was stained with RuO4 and embedded in epoxy resin. Then, sections prepared by ultrathin sectioning were stained with RuO4, and the cross-section of the anti-fogging resin layer was measured using a transmission electron microscope (TEM) (Hitachi High-Technologies Corporation, H-7650, accelerating voltage 100 kV).

[0079] 4) Anti-fog properties (initial stage) The laminate film of the present invention preferably has an anti-fogging evaluation of rank 2 or higher after exposing the anti-fogging resin layer to a water bath at 40° C. for 1 minute. The rank is based on the following criteria, with the higher the value, the better the result. (Judgment criteria) Rank 1: Water droplets formed on the film surface, causing it to become cloudy and reducing visibility through the film. Rank 2: The water film formed on the surface of the film was smudged, but this did not affect visibility through the film. Rank 3: No obvious changes were observed on the film surface, and visibility through the film was good.

[0080] 5) Anti-fogging properties after water immersion treatment The laminated film of the present invention preferably has an anti-fogging property evaluation of rank 2 or higher after immersion in water at 23° C. for 1 minute. The ranks are the same as those described above.

[0081] 6) Residual rate of anti-fogging resin layer The laminate film of the present invention preferably has a coating film remaining rate of 70% or less, more preferably 55% or less, and even more preferably 50% or less of the anti-fog resin layer after immersion in water at 23° C. for 1 hour. A smaller remaining rate of the anti-fog coating means higher recyclability. After immersion in water at 23°C for 1 hour, the thickness of the anti-fogging resin layer after immersion was measured in the same manner as in 3) Anti-fogging resin layer thickness above. The coating film remaining rate was calculated from the thicknesses of the anti-fogging resin layer before and after immersion.

[0082] 7) Total light transmittance Measurement was carried out in accordance with JIS K 7361 using a haze meter HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd. The total light transmittance is preferably 90% or more, more preferably 93% or more, and even more preferably 95% or more.

[0083] [Recycling laminated film] The laminate film of the present invention is characterized by its design taking into consideration recyclability, that is, it can be reused after its use for a certain period of time has been completed. That is, the laminate film of the present invention can be used in such a way that the anti-fogging resin layer or the functional layer in addition to the anti-fogging resin layer is dissolved in a solvent or the like, or peeled off, and the substrate film (laminate film) is reused. More specifically, the anti-fogging resin layer or functional layer constituting the laminate film is removed using a cleaning agent. Examples of removal methods include an immersion method in which the film is immersed in a cleaning tank containing a cleaning agent, a coating method in which the cleaning agent is applied, and a spraying method in which a vaporized cleaning agent is sprayed. Among these, the immersion method is preferred because of the penetration of the cleaning agent into the functional layer. As the cleaning agent, from the viewpoint of ease of handling, it is preferable to use an aqueous cleaning agent such as water or alcohols, and it is particularly preferable to use water. Here, the aqueous cleaning agent means water, alcohols, and mixtures thereof. Since the anti-fogging resin layer of the present invention contains a polyvinyl alcohol-based resin as a main component, it can be easily removed with a cleaning solution using an aqueous cleaning agent. The detergent may also contain additives that are commonly used in detergents.

[0084] Examples of alcohols include monohydric alcohols such as methyl alcohol, ethyl alcohol, propyl alcohol, butyl alcohol, benzyl alcohol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; dihydric alcohols such as ethylene glycol, diethylene glycol, and propylene glycol; and polyhydric alcohols such as glycerin. From the viewpoint of cleaning properties, methyl alcohol, ethyl alcohol, propyl alcohol, and benzyl alcohol are more preferred.

[0085] From the viewpoint of cleaning properties, the acidity constant (pKa) of the alcohol is preferably in the range of 10.0 or more and 20.0 or less, more preferably 10.0 or more and 18.0 or less, even more preferably 12.0 or more and 16.0 or less, particularly preferably 14.0 or more and 15.6 or less, and most preferably 14.0 or more and 15.4 or less. The acidity constants (pKa) of some alcohols are as follows: benzyl alcohol (pKa = 15.4), methanol (pKa = 15.5), ethanol (pKa = 16.0), 1-propanol (pKa = 16.1), 2-propanol (pKa = 17.1), 1-butanol (pKa = 16.1), tert-butanol (pKa = 18.0). From the values ​​of the acidity constants (pKa) of alcohols shown above, alcohols with an acidity constant (pKa) of 15.4 or less can be said to be alcohols with an acidity constant (pKa) smaller than that of methanol.

[0086] The temperature of the cleaner in the immersion method is preferably room temperature (20°C) or higher. At room temperature (20°C) or higher, the viscosity of the cleaner is low and it easily penetrates into the functional layer, resulting in good cleaning properties. From the above perspectives, the temperature of the cleaner in the immersion method is more preferably 40°C or higher, even more preferably 50°C or higher, and particularly preferably 60°C or higher. The upper limit of the temperature of the cleaning agent is preferably a temperature equal to or lower than the boiling point when the cleaning agent is used in a solution state. In the case of an aqueous cleaning agent, which is a preferred embodiment of the present application, the upper limit is preferably 100°C or lower, more preferably 80°C or lower.

[0087] When the laminate film is composed of only an anti-fogging resin layer, water or warm water is used, and when the laminate film is provided with an anti-fogging resin layer and a functional layer, an alcohol alone or a combination of water and an alcohol is used, and by appropriately using water or an alcohol solvent, the anti-fogging resin layer or the functional layer of the laminate film can be efficiently removed.

[0088] <Explanation of terms> In this specification, when "X to Y" (X and Y are any numbers) is expressed, unless otherwise specified, it means "X or more and Y or less," and also includes the meaning "preferably greater than X" or "preferably smaller than Y." Furthermore, when "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning "preferably greater than X" or "preferably less than Y." [Example]

[0089] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples within the scope of the present invention. The measurement and evaluation methods used in the present invention are as follows.

[0090] (1) Intrinsic viscosity of polyester 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and measured at 30°C.

[0091] (2) Average particle size The coating layer was observed using a TEM (H-7650 manufactured by Hitachi, accelerating voltage 100 V), and the average particle size of 10 particles was taken as the average particle size.

[0092] (3) Thickness of the anti-fogging resin layer The surface of the anti-fogging resin layer was stained with RuO4 and embedded in epoxy resin. Then, sections prepared by ultrathin sectioning were stained with RuO4, and the cross-section of the anti-fogging resin layer was measured using a transmission electron microscope (TEM) (Hitachi High-Technologies Corporation, H-7650, accelerating voltage 100 kV).

[0093] (4) Water droplet contact angle The contact angle of the anti-fog layer surface of a film sample that had been conditioned for more than 24 hours in an environment of 23°C and 50% RH was measured using an automatic contact angle meter (DataPhysics, model OCA20) by contacting a 2 μL water droplet with the anti-fog layer surface, measuring the water droplet contact angle 60 seconds later and the average water droplet contact angle 20 to 60 seconds later.

[0094] (5) Advancing contact angle by the expansion method The contact angle of the anti-fog resin layer surface of a film sample that had been conditioned for more than 24 hours in an environment of 23°C and 50% RH was measured using an automatic contact angle meter (DataPhysics, model OCA20) by contacting a 2 μL water droplet with the anti-fog layer surface, then contacting the tip of a water supply syringe with the center of the resulting droplet and supplying water at a flow rate of 0.06 μL / sec. The average advancing contact angle of the droplet after 20 to 60 seconds was measured.

[0095] (6) Anti-fog properties (initial) The anti-fogging resin layer was exposed to a water bath at 40° C. for 1 minute, and then the anti-fogging properties were evaluated according to the following criteria. (Judgment criteria) Rank 1: Water droplets formed and clouded the view through the film. Rank 2: A water film formed, causing blurring, but visibility through the film was good. Rank 3: Visibility through the film was not affected.

[0096] (7) Evaluation of anti-fogging properties after water immersion treatment The sample film was immersed in water at 23°C for 1 minute, and then evaluated according to the same criteria as for anti-fogging property (initial).

[0097] (8) Residual rate of anti-fogging resin layer After immersion in water at 23°C for 1 hour, the thickness of the anti-fogging resin layer after immersion was measured in the same manner as in (3) Anti-fogging resin layer thickness above. The coating film remaining rate was calculated from the thickness of the anti-fogging resin layer before and after immersion. The smaller the coating film remaining rate, the easier it is to remove the anti-fogging resin layer, and the better the recyclability.

[0098] (9) Total light transmittance Measurement was carried out using a haze meter HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd. in accordance with JIS K 7361. Evaluation was made according to the following criteria. ◎: Total light transmittance is 95% or more 〇: Total light transmittance is 93% or more but less than 95% △: Total light transmittance is 90% or more but less than 93% ×: Total light transmittance is less than 90%

[0099] (10) Method for measuring the absolute minimum reflectance from the functional layer First, black tape (Vinyl tape VT-50 manufactured by Nichiban Co., Ltd.) was attached to the back surface of the functional layer to be measured (the surface of the anti-fogging resin layer), and the absolute reflectance of the functional layer surface was measured in the wavelength range of 300 to 800 nm using a spectrophotometer (UV-Visible Spectrophotometer V-670 manufactured by JASCO Corporation and Automatic Absolute Reflectance Measurement Device ARMN-735) in synchronous mode, with an incident angle of 5°, N polarization, fast response, data acquisition interval of 1.0 nm, bandwidth of 10 nm, and a scanning speed of 1000 m / min, and the wavelength at the minimum value (bottom wavelength) and absolute reflectance were evaluated.

[0100] (11) Overall rating The anti-fogging properties (initial and after water immersion treatment) and the remaining rate of the anti-fogging resin coating were evaluated comprehensively. A: Anti-fogging performance is rank 3, and the remaining coating rate is 30% or less. B: Anti-fogging property (initial) is rank 3, anti-fogging property (after water immersion treatment) is rank 2, and the coating film remaining rate is 30% or less C: Anti-fogging properties are both ranked 2, and the remaining coating film is 30% or less, or the initial anti-fogging properties are ranked 3, and the post-water immersion anti-fogging properties are ranked 2, and the remaining coating film is greater than 30%. D: Anti-fogging performance is rank 2, and the coating film remaining rate is greater than 30%. E: At least one of the anti-fogging properties is rank 1

[0101] The polyester raw materials used in the examples and comparative examples are as follows:

[0102] <Method for producing polyester (1)> Using 100 parts by mass of dimethyl terephthalate and 55 parts by mass of ethylene glycol as starting materials and 0.04 parts by mass of magnesium acetate tetrahydrate as a catalyst, the reactor was charged with the reaction starting temperature of 150°C. As methanol was distilled off, the reaction temperature was gradually increased to 230°C after 3 hours. After 4 hours, the transesterification reaction was essentially complete. 0.02 parts by mass of ethyl acid phosphate was added to the reaction mixture, followed by 0.04 parts by mass of antimony trioxide, and the polycondensation reaction was carried out for 4 hours. The temperature was gradually increased from 230°C to 280°C. Meanwhile, the pressure was gradually reduced from atmospheric pressure to a final value of 0.3 mmHg. After the start of the reaction, the reaction was terminated at a point corresponding to an intrinsic viscosity of 0.65 due to changes in the stirring power of the reactor. The polymer was discharged under nitrogen pressure, yielding polyester (1) with an intrinsic viscosity of 0.65.

[0103] <Method for producing polyester (2)> The starting materials were 100 parts by mass of dimethyl terephthalate and 45 parts by mass of ethylene glycol. 0.06 parts by mass of magnesium acetate tetrahydrate was added to the reactor as a catalyst. The reaction was initiated at 150°C and gradually increased to 230°C after 3 hours as methanol was distilled off. After 4 hours, the transesterification reaction was essentially complete. 0.03 parts by mass of ethyl acid phosphate was added to the reaction mixture, followed by 0.3 parts by mass of silica particles with an average particle size of 2.7 μm dispersed in ethylene glycol and 0.03 parts by mass of antimony trioxide. The polycondensation reaction was carried out for 4 hours. The temperature was gradually increased from 230°C to 280°C. Meanwhile, the pressure was gradually reduced from atmospheric pressure to a final value of 0.3 mmHg. Due to changes in the stirring power of the reactor, the reaction was terminated at a point corresponding to an intrinsic viscosity of 0.65. The polymer was discharged under nitrogen pressure, yielding polyester (2) with an intrinsic viscosity of 0.65.

[0104] The following anti-fogging resin composition was used. (A) Polyvinyl alcohol resin A1: PVA with a saponification degree of 99 mol%, an average polymerization degree of 1100, and an acetoacetyl group A2: PVA with a saponification degree of 87 mol%, an average polymerization degree of 1600, and a quaternary ammonium salt group A3: PVA with a saponification degree of 99 mol%, an average polymerization degree of 1800, and a sodium carboxylate group A4: PVA with a saponification degree of 50 mol%, an average polymerization degree of 200, and a polyethylene oxide group A5: PVA with a saponification degree of 93 mol% and an average polymerization degree of 700 A6: PVA with a saponification degree of 80 mol% and an average polymerization degree of 2200 A7: PVA with a saponification degree of 99 mol% and an average polymerization degree of 500 A8: PVA with a saponification degree of 80 mol% and an average polymerization degree of 500

[0105] (B) Other ingredients A9: Sucrose fatty acid ester (Rikemal A, manufactured by Riken Vitamin Co., Ltd.)

[0106] (Functional layer forming composition B1) A composition of fluorine-containing compound:melamine compound=80:20 (mass%) Fluorine-containing compound: Aqueous dispersion of fluorine-based polyether urethane resin, in which isophorone diisocyanate / dimethylolpropanoic acid / perfluoroether glycol (copolymer of difluoroethylene oxide: difluoromethylene oxide: tetrafluoroethylene oxide = 5:43:52 (mol%)) = 49 / 28 / 23 (mol%) Melamine compound: hexamethoxymethylolmelamine

[0107] Example 1 A 92 / 8 blend of polyester (1) and polyester (2) by mass was used as the raw material for Layer A, and polyester (1) alone was used as the raw material for Layer B. These were fed into an extruder, heated and melted at 285°C, and coextruded to a thickness ratio of A / B / A = 5 / 90 / 5, with Layer A split into two outer layers (surface layers) and Layer B as the middle layer. The resulting extrusion was then cooled and solidified while in close contact with a mirror-finished cooling drum at a surface temperature of 40-50°C to produce an unstretched polyethylene terephthalate film. This film was stretched 3.7 times in the longitudinal direction while passing through a group of heated rolls at 85°C to produce a uniaxially oriented film (uniaxially stretched film). An anti-fog resin composition A1 shown in Table 1 below was applied to one side of this uniaxially stretched film, and then the film was introduced into a tenter stretching machine and stretched 4.3 times in the width direction at 100°C. After further heat treatment at 230°C, the film was subjected to a 2% relaxation treatment in the width direction to obtain a 50 μm thick biaxially oriented polyester film having an anti-fog resin layer with a film thickness (after drying) of 0.07 μm.

[0108] Examples 2 to 6 and Comparative Examples 1 to 2 The same procedure as in Example 1 was carried out except that the anti-fogging resin composition was changed as shown in Tables 1 and 2, to obtain a laminated film.

[0109] Example 7 A laminate film was obtained in the same manner as in Example 4, except that anti-fog resin composition A4 was applied to one surface of a uniaxially stretched film and also to the other surface of the uniaxially stretched film to form an anti-fog resin layer with a film thickness (after drying) of 0.09 μm. The anti-fog resin layer formed on the other surface had a minimum value of absolute reflectance at a wavelength of 560 nm, and the absolute reflectance at that minimum value was 1.9%.

[0110] Example 8 A laminated film was obtained in the same manner as in Example 7, except that the functional layer was changed to the following functional layer composition B1. The obtained functional layer had a minimum value of absolute reflectance at a wavelength of 510 nm, and the absolute reflectance at that minimum value was 1.0%.

[0111] Reference example 1 The same procedure as in Example 1 was carried out except that the anti-fogging resin composition was changed as shown in Tables 1 and 2, to obtain a laminated film.

[0112] [Table 1]

[0113] [Table 2]

[0114] The anti-fog resin composition and laminate film of the present invention maintain good anti-fog performance while exhibiting good recyclability. They are suitable for a variety of applications requiring anti-fog properties, such as agricultural, medical, and packaging applications. Among these, they are particularly suitable for face shields. Furthermore, they are particularly suitable for disposable applications, and can be recovered and recycled.

Claims

1. A method for using a laminate film, comprising treating the laminate film, on at least one surface of a substrate film, with water and / or an alcohol, and then reusing the laminate film, wherein the anti-fogging resin composition contains a polyvinyl alcohol-based resin having a degree of saponification of 40 to 99 mol% and an average degree of polymerization of 400 or less, or 650 or more and 2500 or less, and the proportion of the polyvinyl alcohol-based resin in the total non-volatile components of the anti-fogging resin composition is 90 mass% or more.

2. The method for using the laminated film according to claim 1 , wherein the polyvinyl alcohol-based resin comprises a modified polyvinyl alcohol-based resin.

3. 3. The method for using the laminate film according to claim 2, wherein the modified polyvinyl alcohol resin is a modified polyvinyl alcohol composed of a combination of a vinyl alcohol structural unit and an ethylene oxide group-containing structural unit or a combination of a vinyl alcohol structural unit and an acetoacetyl group-containing structural unit.

4. 4. The method for using the laminate film according to claim 1, wherein the difference between the average water droplet contact angle 20 to 60 seconds after a water droplet is dropped on the anti-fogging resin layer surface of the laminate film and the average advancing contact angle 20 to 60 seconds after a liquid is discharged by an expansion method (advancing contact angle - water droplet contact angle) is 1° or more.

5. 5. The method for using the laminate film according to claim 1, wherein a contact angle of water dropped on the surface of the anti-fogging resin layer after 60 seconds is 35° or less.

6. The method for using the laminate film according to any one of claims 1 to 5, wherein the anti-fogging resin layer is exposed to a water bath at 40°C for 1 minute and then evaluated for anti-fogging properties as rank 2 or higher. Rank 2: A water film formed and blurred the image, but visibility through the film was good.

7. 7. A method for using the laminate film according to claim 1, wherein the anti-fogging property evaluation after a water immersion treatment (immersion at 23° C. for 1 minute) is rank 2 or higher. Rank 2: A water film formed and blurred the image, but visibility through the film was good.

8. 8. The method for using the laminate film according to claim 1, wherein after immersion in water at 23° C. for 1 hour, the coating film remaining rate (%) of the anti-fogging resin layer is 55% or less.

9. The method for using the laminated film according to any one of claims 1 to 8, wherein the base film is a polyester film.

10. The method for using the laminated film according to any one of claims 1 to 9, wherein the base film is a polyester film that is unstretched or stretched at least uniaxially.

11. The method for using the laminate film according to any one of claims 1 to 10, wherein the anti-fogging resin layer has a thickness (after drying) of 0.01 µm or more and 1 µm or less.

12. A method for using the laminate film according to any one of claims 1 to 11, further comprising providing a functional layer on the opposite surface of the anti-fogging resin layer.

13. The method for using the laminated film according to claim 12, wherein the functional layer is a visibility improving layer.

14. The method for using the laminate film according to claim 13, wherein the visibility improving layer is a resin layer obtained by curing a resin composition containing a fluorine-containing compound and a crosslinking agent.

15. The method for using the laminated film according to any one of claims 1 to 14, wherein the alcohol has an acidity constant (pKa) of 10.0 or more and 20.0 or less.

16. The method for using the laminate film according to any one of claims 1 to 15, wherein the anti-fogging resin layer is removed by immersing the layer in a cleaning bath containing water and / or alcohol.

17. The method for using the laminated film according to any one of claims 1 to 16, wherein the alcohol comprises at least one selected from the group consisting of methyl alcohol, ethyl alcohol, propyl alcohol and benzyl alcohol.

18. Use of the laminate film according to any one of claims 1 to 17 as a face shield.

Citation Information

Patent Citations

  • Method of antiistatic and anticlouding treatment of surface of synthetic resin

    JP1978014771A

  • Easy-to-adhere polyester film and method for producing the same

    JP1993310976A

  • Defogging film

    JP1997174750A

  • Hygroscopic Anti-fogging film and method of manufacturing the same

    JP2001145982A

  • Aqueous Anti-clouding coating agent and material improved in Anti-clouding property