Induction heating coil, single crystal manufacturing apparatus using the same, and method for manufacturing single crystal
The induction heating coil with a radial step on its upper surface addresses the challenge of uneven heating in larger diameter rods, ensuring uniform heat distribution and stable single crystal growth in the FZ method.
Patent Information
- Application Number
- JP2021083852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-18
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-05-18
AI Technical Summary
In the FZ method for producing single crystals, larger diameter raw material rods are difficult to heat uniformly, leading to uneven melting surfaces that can cause manufacturing disruptions.
An induction heating coil with a radial step on its upper surface, excluding the slit vicinity, to enhance current density and heat distribution uniformly around the raw material rod.
The coil stabilizes the melting surface height, allowing for consistent single crystal growth by reducing variations in heat distribution, thereby improving the success rate of dislocation-free single crystal production.
Smart Images

Figure 0007552498000011 
Figure 0007552498000009 
Figure 0007552498000010
Abstract
Description
[Technical field]
[0001] The present invention relates to an induction heating coil used in the production of single crystals by the FZ method (Floating Zone method), and to a single crystal production apparatus and method using the same. [Background technology]
[0002] The FZ method is known as a method for producing silicon single crystals. In the FZ method, a part of a raw material rod made of polycrystalline silicon is heated to generate a molten zone, and the raw material rod and seed crystal located above and below the molten zone, respectively, are gradually lowered to grow a large single crystal above the seed crystal. The FZ method does not use a quartz crucible as in the CZ method (Czochralski method), so it is possible to produce single crystals with a low oxygen concentration.
[0003] In the FZ method, induction heating is used to heat the polycrystalline silicon raw material. When a magnetic field generated by passing a high-frequency current through an induction heating coil is applied to the silicon raw material, eddy currents flow in the silicon raw material due to electromagnetic induction, and Joule heat is generated by the eddy currents. In the induction heating method, this Joule heat is used to heat the silicon raw material.
[0004] Regarding a method for heating silicon raw material using an induction heating coil, for example, Patent Document 1 describes that on the back side of the induction heating coil, a region of 20 degrees or more and 80 degrees or less from the slit as the center is made flat, and the other region is provided with a tapered shape that becomes thicker from the center toward the periphery.
[0005] Patent Document 2 also describes a method in which a sub-induction heating coil is installed between the main induction heating coil and the raw material and / or single crystal, on the opposite side of the electrode (slit) of the main coil, and the state of the floating zone, which may affect the occurrence of dislocations, is adjusted by moving the position of the sub-induction heating coil while checking the state of the floating zone.
[0006] Patent Document 3 describes arranging auxiliary heaters using halogen lamp heaters above or below the induction heating coil or both sides to surround the raw material or single crystal. The auxiliary heaters allow efficient heating of the raw material. However, heating using halogen lamp heaters also heats the induction heating coil at the same time, which may exceed the cooling limit of the cooling water flowing through the coil and cause the coil to burst due to boiling of the cooling water. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-168345 A [Patent Document 2] JP 2015-218076 A [Patent Document 3] JP 2016-141612 A Summary of the Invention [Problem to be solved by the invention]
[0008] In the FZ method, the diameter of the raw material rod needs to be increased to improve the yield of single crystals. However, as the diameter of the raw material rod increases, it becomes difficult to heat the entire circumferential direction of the raw material rod uniformly, and the amount of melted raw material increases locally in some areas, which increases the circumferential height variation of the melted surface of the raw material rod. This uneven melted surface eventually comes into contact with the coil surface, forcing the manufacturing process to be halted.
[0009] Therefore, an object of the present invention is to provide an induction heating coil capable of stably producing single crystals by suppressing variation in height of the melting surface of a raw material rod, and a single crystal production apparatus and a single crystal production method using the same. [Means for solving the problem]
[0010] In order to solve the above problems, the induction heating coil of the present invention is an induction heating coil for heating a raw material rod in the production of single crystals by the FZ method, and comprises a circular coil conductor having an opening in the center, a slit extending radially from the opening to separate one end and the other end of the coil conductor, and a radial step formed on the upper surface of the coil conductor, the upper surface of the coil conductor having a step-forming region in which the step is arranged in an arc shape in a planar view so as to surround the opening, and a step-free region in which the step is not provided, the step-free region includes a slit vicinity region adjacent to the slit, the step-forming region is a region farther from the slit than the step-free region, and the step is provided near the outer circumferential end of the straight body portion of the raw material rod and radially inward from the outer circumferential end.
[0011] Furthermore, the single crystal manufacturing apparatus according to the present invention is a single crystal manufacturing apparatus used for manufacturing a single crystal by the FZ method, and is characterized in that it comprises an upper shaft that supports a raw material rod so that it can rotate and rise and fall, a lower shaft that is arranged below the upper shaft and supports a seed crystal so that it can rotate and rise and fall, and an induction heating coil that heats the raw material rod, and the induction heating coil has the above-mentioned characteristics.
[0012] Furthermore, the method for producing a single crystal according to the present invention is characterized in that a single crystal is produced by the FZ method using an induction heating coil having the above-mentioned features.
[0013] According to the present invention, the variation in the amount of heat between the near-slit region and the far-slit region can be reduced, and the entire outer periphery of the raw material rod can be heated uniformly in the circumferential direction. Therefore, the variation in the height of the melting surface of the raw material rod can be suppressed, and a single crystal can be stably grown.
[0014] In the present invention, the difference (Δr=r0-r1) between the radius (r0) of the raw material rod and the radius (r1) of the step is preferably 2 mm or more and 8 mm or less. If the radius difference between the raw material rod and the step is within the range of 2 to 8 mm, the entire circumferential direction of the outer periphery of the raw material rod can be uniformly heated.
[0015] In the present invention, the height (h) of the step is preferably 0.5 mm or more and 1.5 mm or less. If the height of the step is within the range of 0.5 to 1.5 mm, the current density in the vicinity of the step formation region can be increased, resulting in an appropriate increase in the amount of heat generated.
[0016] In the present invention, the non-step region is preferably a substantially sector-shaped region with a central angle of 45 degrees or more and 90 degrees or less extending on both sides of the slit. In this case, the area of the non-step region provided on the one end side of the coil conductor and the area of the non-step region provided on the other end side may be equal to or different from each other. Effect of the Invention
[0017] According to the present invention, there is provided an induction heating coil capable of stably producing single crystals by suppressing the variation in height of the melting surface of a raw material rod, and a single crystal production apparatus and a single crystal production method using the same. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic diagram showing the configuration of a single crystal manufacturing apparatus according to an embodiment of the present invention. [Diagram 2] 2(a) and (b) are diagrams showing the configuration of an induction heating coil according to a first embodiment of the present invention, where (a) is a schematic top view and (b) is a schematic cross-sectional view taken along line XX' in (a). [Diagram 3] FIG. 3 is a diagram illustrating the flow of current in the induction heating coil. [Figure 4] 4(a) and (b) are graphs showing the simulation results of the heat generation distribution of a raw material rod when heated using a conventional induction heating coil, where (a) shows the heat generation distribution in the radial direction and (b) shows the heat generation distribution in the circumferential direction. [Diagram 5] 5(a) to (e) are diagrams for explaining the relationship between the presence or absence of a step on the upper surface of the induction heating coil and the amount of heat generated. [Figure 6] 6(a) and (b) are graphs showing the simulation results of the heat generation amount distribution of a raw material rod when heated using the induction heating coil according to this embodiment, where (a) shows the heat generation amount distribution in the radial direction and (b) shows the heat generation amount distribution in the circumferential direction. [Figure 7] FIG. 6 is a schematic plan view showing the configuration of an induction heating coil according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0020] FIG. 1 is a schematic diagram showing the configuration of a single crystal manufacturing apparatus according to an embodiment of the present invention.
[0021] As shown in FIG. 1, this single crystal manufacturing apparatus 1 is an apparatus for growing a silicon single crystal by the FZ method, and is equipped with a reactor 10 that accommodates a raw material rod 2, a seed crystal 3, and a silicon single crystal 4 growing on the seed crystal 3, an upper shaft 11 that supports the raw material rod 2 so that it can rotate and rise and fall, a lower shaft 12 that supports the seed crystal 3 and the silicon single crystal 4 so that they can rotate and rise and fall, an induction heating coil 20 that heats the lower end of the raw material rod 2, a single crystal weight holder 14 that abuts against a tapered portion 4a of the silicon single crystal 4 that has become larger as the crystal growth progresses and supports the weight of the silicon single crystal 4, and a gas doping device 15 that supplies a doping gas to a molten zone 5 (molten silicon) between the raw material rod 2 and the silicon single crystal 4.
[0022] The raw material rod 2 is made of high-purity polycrystalline silicon obtained by refining a silicon raw material such as monosilane or trichlorosilane, and the upper end of the raw material rod 2 is attached to the lower end of an upper shaft 11 via a raw material holder 16. The lower end of the seed crystal 3 is attached to the upper end of a lower shaft 12 via a seed crystal holder 17. The upper shaft 11 and the lower shaft 12 are each rotated and raised and lowered by a driving mechanism (not shown).
[0023] Generally, the diameter R1 of the silicon single crystal 4 grown by the FZ method is larger than the diameter R0 of the raw material rod 2. For example, when growing a silicon single crystal 4 with a diameter R1=200 mm, a raw material rod 2 with a diameter R0=150 to 160 mm is preferably used. The diameter R1 of the silicon single crystal 4 is the diameter of the straight body portion 4b of the silicon single crystal 4, and is the maximum diameter of the silicon single crystal 4. The diameter R0 of the raw material rod 2 is also the diameter of the straight body portion of the raw material rod 2, and is the maximum diameter of the raw material rod 2.
[0024] The induction heating coil 20 is a high-frequency coil with approximately one turn surrounding the molten zone 5 or the raw material rod 2, and is connected to a high-frequency oscillator (not shown). The induction heating coil 20 is preferably made mainly of copper or silver. By passing a high-frequency current through the induction heating coil 20, the lower end of the raw material rod 2 is induction heated and the molten zone 5 is generated. After the seed crystal 3 is fused to the molten zone 5 thus generated, the raw material rod 2 and the silicon single crystal 4 are lowered while being rotated, whereby the silicon single crystal 4 can be grown from the molten zone 5.
[0025] 2(a) and (b) are diagrams showing the configuration of an induction heating coil 20 according to a first embodiment of the present invention, where (a) is a schematic top view and (b) is a schematic cross-sectional view taken along line XX' in (a).
[0026] 2(a) and (b), the induction heating coil 20 includes a substantially flattened circular coil conductor 21, an opening 22 provided in the center of the coil conductor 21, a slit 23 extending radially from the opening 22 toward the outer circumferential end to separate one end and the other end of the coil conductor 21, and a pair of terminal electrodes 24A, 24B connected to the one end and the other end of the coil conductor 21, respectively. The coil conductor 21 is connected to a high-frequency oscillator via the pair of terminal electrodes 24A, 24B.
[0027] Typically, the outer diameter Ra of the coil conductor 21 is larger than the diameter R0=2×r0 of the raw material rod 2, and the inner diameter Rb (diameter of the opening 22) of the coil conductor 21 is smaller than the diameter R0 of the raw material rod 2. For example, when a raw material rod 2 with a diameter R0=160 mm is used, the outer diameter Ra of the coil conductor 21 is larger than 160 mm, and the inner diameter Rb of the coil conductor 21 is smaller than 160 mm.
[0028] The upper surface 21A of the coil conductor 21 may be an upward inclined surface from the inner periphery side to the outer periphery side, or may be a horizontal surface. The lower surface 21B of the coil conductor 21 is preferably an upward inclined surface from the inner periphery side to the outer periphery side, but may be a horizontal surface.
[0029] The upper surface 21A of the coil conductor 21 is provided with a step 25 having a radius corresponding to the radius of the raw material rod 2. The region radially inward from the step 25 is a lower step surface 26A, and the region radially outward from the step 25 is an upper step surface 26B that is higher than the lower step surface 26A. The shape of the lower surface 21B of the coil conductor 21 is not particularly limited, and may be a flat surface without a step.
[0030] 2(a), the step 25 is formed in an arc shape in a plan view so as to surround the opening 22, and is provided radially inward from the outer circumferential end 2e of the straight body of the raw material rod 2. When the radius of the straight body of the raw material rod 2 is r0 and the radius of the step 25 is r1, the difference between r0 and r1, Δr=r0-r1, is preferably 2 mm or more and 8 mm or less. This is because if the position of the step 25 is too close to the outer circumferential end 2e of the raw material rod 2 or is located outside the outer circumferential end 2e of the raw material rod 2, the effect of compensating for the amount of heat generated is small, and if the step 25 is located too far to the inner circumferential side of the raw material rod 2, the effect on the minimum position of the amount of heat generated is small.
[0031] For example, when a raw material rod 2 with a diameter of 160 mm is used, the step 25 is provided within a range of 72 to 78 mm in the radial direction from the center of the coil conductor 21. When a raw material rod 2 with a diameter of 150 mm is used, the step 25 is provided within a range of 67 to 73 mm in the radial direction from the center of the coil conductor 21. When the step 25 is provided within a range of 72 to 73 mm in the radial direction from the center of the coil conductor 21, it can be widely used for raw material rods 2 with diameters of 150 to 160 mm.
[0032] The height h of the step 25 is preferably 0.5 mm or more and 1.5 mm or less. If the height h of the step 25 is too low, the effect of the step 25 is not observed, and if the height h of the step 25 is too high, the effect of increasing the current density in the vicinity of the formation position of the step 25 is weakened.
[0033] The step 25 is provided over the entire circumferential direction of the coil conductor 21 except for the slit vicinity region 27A of the upper surface 21A of the coil conductor 21, and is not provided in the slit vicinity region 27A. Here, the slit vicinity region 27A is defined as a sector-shaped region extending on both sides of the slit 23 with a central angle θ of 45 degrees or more and 90 degrees or less (±22.5 degrees or more and ±45 degrees or less).
[0034] 2(a), the end portion of the step 25, which is arc-shaped in a plan view, is extended and terminated at the outer circumferential end of the coil conductor 21. The radially extending portion of the step 25 does not contribute to the adjustment of the heating distribution of the raw material rod 2, so the step surface may be gently inclined.
[0035] The upper surface 21A of the coil conductor 21 is roughly divided into a slit vicinity region 27A adjacent to the slit 23 and a slit far region 27B which is a region farther from the slit 23 than the slit vicinity region 27A, and the step 25 is provided in the slit far region 27B. That is, a step formation region 28 in which the step 25 is provided so as to surround the opening 22 is provided in the slit far region 27B. The slit vicinity region 27A also constitutes a step non-formed region 29 without the step 25. The step formation region 28 is made up of a lower step surface 26A and an upper step surface 26B, whereas the step non-formed region 29 is made up of only the lower step surface 26A, and the entire surface is a flat surface.
[0036] As shown by the arrows in Fig. 3, the current flowing through the induction heating coil 20 flows through a path that provides the shortest distance between the pair of terminal electrodes 24A, 24B. As a result, the current density is high in the slit vicinity region 27A, and the amount of heat generated is large. On the other hand, in the slit distant region 27B, the current flows mostly near the inner circumferential end (opening 22) of the coil conductor 21, and the amount of heat generated near the outer circumferential end of the raw material rod 2 is small. As a result, heating in the circumferential direction becomes non-uniform at the outer circumferential portion of the raw material rod 2, making it difficult to melt the raw material rod 2 uniformly in the circumferential direction.
[0037] However, when a radial step 25 is provided on the upper surface 21A of the coil conductor 21 excluding the slit vicinity region 27A, the current density near the position where the step 25 is formed can be increased to increase the amount of heat generated, thereby making it possible to heat the outer periphery of the raw material rod 2 uniformly in the circumferential direction. This makes it possible to prevent a part of the melting surface from sagging.
[0038] 4(a) and (b) are graphs showing the simulation results of the heat generation distribution of a raw material rod when heated using a conventional induction heating coil, where (a) shows the heat generation distribution in the radial direction and (b) shows the heat generation distribution in the circumferential direction.
[0039] As shown in Fig. 4(a), when induction heating coil 20 is heated on the side opposite the slit (0 degree position), the radial variation in the amount of heat generated is small, but when it is heated on the slit side (180 degree position), the difference in the amount of heat generated between the inside and outside in the radial direction becomes very large. Also, as shown in Fig. 4(b), the distribution of heat generated in the circumferential direction of the induction heating coil is maximum near the slit, and is less at the position opposite the slit than near the slit.
[0040] As described above, since the heat generation amount distribution of the raw material rod is not uniform in the circumferential direction, the raw material rod cannot be melted uniformly in the circumferential direction, and part of the melted surface may droop or icicle-like unmelted residue may remain, which may pose a risk of contact with the induction heating coil 20 or discharge.
[0041] Therefore, in this embodiment, a step is provided on the upper surface of the induction heating coil located directly below the vicinity of the outer periphery of the raw material rod 2. If there is a step on the upper surface of the induction heating coil, current flows along the side of the step, and the current density increases near the position where the step 25 is formed, thereby increasing the heating effect around the step. However, no step is provided in the slit vicinity region 27A because it is not desired to increase the heat generation effect. Therefore, the coil shape is as shown in FIG. 2.
[0042] 5(a) to (e) are diagrams illustrating the relationship between the step shape of the upper surface 21A of the induction heating coil 20 and the amount of heat generated.
[0043] Fig. 5(a) shows the positional relationship between the raw material rod 2 and the induction heating coil 20, and Figs. 5(b) to (d) show enlarged views of the coil shape near the outer periphery of the raw material rod 2 surrounded by the dashed line E in Fig. 5(a). Shape 1 in Fig. 5(b) is when the top surface of the coil is flat and far from the raw material rod, Shape 2 in Fig. 5(c) is when the top surface of the coil is flat and close to the raw material rod, and Shape 3 in Fig. 5(d) is when a step is provided on the top surface of the coil. Furthermore, Fig. 5(e) is a graph showing the distribution of heat generation in the radial direction of the raw material rod 2 when coils of Shapes 1 to 3 shown in Figs. 5(b) to (d) are used, with the horizontal axis showing the distance (mm) from the center of the raw material rod and the vertical axis showing the heat generation (standard value).
[0044] When the top surface of the coil is flat as in Figures 5(b) and (c), the radial heat generation amount distribution in the vicinity of the outer periphery of the material rod is minimum at a position 75 mm inside the outer periphery (80 mm) of the material rod. In the case of Shape 1 in which the distance between the material rod and the top surface of the coil is large as in Figure 5(b), such a heat generation amount distribution is generally low, whereas in the case of Shape 2 in which the distance between the material rod and the top surface of the coil is small as in Figure 5(c), such a heat generation amount distribution is generally high. Therefore, the variation in the heat generation amount cannot be reduced by changing the distance between the material rod and the top surface of the coil.
[0045] However, when a step is provided at the 75 mm position where the amount of heat generated is minimal, as in shape 3 in Figure 5(d), the amount of heat generated at that position increases locally, making it possible to reduce the deviation in the distribution of the amount of heat generated, as shown in Figure 5(e).
[0046] 6(a) and (b) are graphs showing the simulation results of the heat generation amount distribution of a raw material rod when heated using the induction heating coil according to this embodiment, where (a) shows the heat generation amount distribution in the radial direction and (b) shows the heat generation amount distribution in the circumferential direction.
[0047] As is clear from a comparison of Fig. 6(a) with Fig. 4(a), when induction heating coil 20 according to this embodiment is used, the difference in the amount of heat generated on the inside and outside in the radial direction when heating is performed on the slit side (180 degree position) is small. Also, as is clear from a comparison of Fig. 6(b) with Fig. 4(b), the circumferential heat generation distribution of the induction heating coil suppresses the steep peaks on both sides of the slit, and the variation in the amount of heat generated is reduced.
[0048] As described above, the induction heating coil 20 according to this embodiment has radial steps 25 in the region excluding the vicinity of the slits on the upper surface 21A of the coil conductor 21, and the radial position of the steps 25 is set slightly inside the outer circumferential end of the raw material rod 2, thereby making it possible to uniform the heat generation distribution in the circumferential direction of the raw material rod 2. Therefore, it is possible to reduce the circumferential height variation of the melting surface of the raw material rod, and to improve the success rate of dislocation-free single crystals.
[0049] FIG. 7 is a schematic top view showing the configuration of an induction heating coil according to the second embodiment of the present invention.
[0050] As shown in Fig. 7, the induction heating coil 20 according to this embodiment is characterized in that the non-step region 29 provided near the slit 23 is formed asymmetrically with respect to the slit 23. The other configurations are the same as those of the first embodiment. In this embodiment, the non-step region 29 extending toward one end side (first terminal electrode 24A side) of the coil conductor 21 is set to be wider than the non-step region 29 extending toward the other end side (second terminal electrode 24B side), but the opposite is also possible.
[0051] As shown in FIG. 6(b), when a radial step 25 is provided in the region of the upper surface 21A of the coil conductor 21 excluding the vicinity of the slit, the circumferential heat distribution can be improved, but the amount of heat generated near the slit is still large. However, as shown in FIG. 7, when the stepless region 29 upstream of the slit in the rotation direction of the raw material rod is narrowed, the amount of melted raw material can be increased in the region near the slit upstream of the slit. As a result, the amount of heat generated near the slit can be reduced compared to when the stepless region 29 is the same on the upstream and downstream sides. Therefore, excessive melting of the raw material near the slit can be avoided.
[0052] In this way, in the induction heating coil 20 according to the present embodiment, the areas of the stepless regions 29 extending on both sides of the slit 23 are asymmetrical, but the same effects as those of the first embodiment can be achieved.
[0053] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present invention, and it goes without saying that these modifications are also included within the scope of the present invention.
[0054] For example, in the above embodiment, one step is provided, but two or more steps may be provided. Also, a groove or protrusion consisting of a combination of a downward step and an upward step may be provided.
[0055] Furthermore, while the above embodiment has been described with respect to the case of producing a silicon single crystal, the present invention can be applied to the production of various single crystals produced by the FZ method. EXAMPLES
[0056] The coil shape was investigated to improve the yield of silicon single crystals produced by the FZ method. A silicon polycrystal with a diameter of 160 mm was used as the raw material rod for growing silicon single crystals, and a silicon single crystal with a diameter of 200 mm was grown.
[0057] <Consideration of coil step height> The height h of the step formed on the top surface of the induction heating coil was investigated. The step was provided on the top surface of the coil conductor in an area excluding the area near the slit, and the radial position of the step was set to 75 mm from the center of the coil. The area near the slit was defined as a sector-shaped area with a central angle of 60 degrees (±30 degrees) on both sides of the slit, and this area near the slit was defined as the area without a step. The height h of the step was set to five different values: 0 mm (no step), 0.5 mm, 1.0 mm, 2.0 mm, and 4.0 mm, and five crystals were grown using each coil. The results are shown in Table 1.
[0058] [Table 1]
[0059] As shown in Table 1, the number of successful attempts to eliminate dislocations with the conventional coil with a flat top surface without any steps was three. In contrast, the number of successful attempts to eliminate dislocations was four or more with step heights h = 0.5 mm, 1.0 mm, and 1.5 mm, demonstrating an improved success rate for eliminating dislocations compared to the conventional coil with a flat top surface. In particular, the number of successful attempts to eliminate dislocations with step height h = 1.0 mm was five, the best result.
[0060] On the other hand, when the step height h = 2.0 mm, the number of successful dislocation-free runs was 3, which was the same as the number of successful dislocation-free runs for conventional coils without steps. When h = 2.0 mm, the amount of melted raw material increased at the position opposite the slit, and compared to h = 1.0 mm, there was circumferential non-uniformity in the way the raw material melted. When the step height h = 4.0 mm, the circumferential non-uniformity in the way the raw material melted became even greater, and the growth process was stopped due to the risk of contact between the raw material and the coil, and growth was terminated after two runs. As a result, the number of successful dislocation-free runs was 0.
[0061] From the above results, it was found that the step height h should be within the range of 0.5 to 1.5 mm, and 1.0 mm is preferable.
[0062] <Consideration of the size of the step-free area> The width of the non-step region near the slit was examined. The crystal growth conditions were the same as those in the examination of the step height of the coil described above, and the step height h was set to 1.0 mm.
[0063] The sector-shaped region with a central angle θ extending from the slit to both sides was defined as the step-free region. The central angle θ was set to 0 degrees (there is a step around the entire circumference of the coil), 45 degrees, 60 degrees, 90 degrees, and 180 degrees, and five crystals were grown using each coil. The results are shown in Table 2.
[0064] [Table 2]
[0065] As shown in Table 2, when the central angle θ was 45 degrees, 60 degrees, and 90 degrees, the number of successful attempts to eliminate dislocations was 4 or more, indicating an improvement in the success rate of eliminating dislocations compared to the conventional method. In particular, when the central angle θ was 60 degrees, the number of successful attempts to eliminate dislocations was 5, which was the best result.
[0066] On the other hand, when the central angle θ = 180 degrees, the number of successful cases of no dislocation was 3, which was the same as the conventional coil without steps. When the central angle θ = 0 degrees, the number of successful cases of no dislocation was 1. When the central angle θ = 0 degrees, that is, when steps are provided around the entire circumference of the coil, the amount of heat generated near the slits was emphasized, and unstable melting of the raw material was observed.
[0067] <Investigation of the radial position of the coil step (raw material diameter 160 mm)> We investigated the best radial position of the step for a raw material rod with a diameter of 160 mm. Based on the above results, we set the step height h to 1.0 mm and the central angle θ of the step-free region to 60 degrees.
[0068] The radial distance L from the center of the coil conductor to the position where the step is formed, i.e., the radius r1 of the arc-shaped step (see Figure 2(a)), was set to six values: 70mm, 72mm, 75mm, 78mm, 80mm, and 82mm, and five silicon single crystals were grown for each. The distance L from the outer edge of the raw material rod to the position where these steps are formed was set to six values: -10mm, -8mm, -5mm, -2mm, 0mm, and +2mm, and five crystals were grown using each coil. The results are shown in Table 3.
[0069] [Table 3]
[0070] As shown in Table 3, when the distance L to the step was 72 mm, 75 mm, and 78 mm, the number of successful attempts to eliminate dislocation was 4 or more, indicating an improvement in the success rate of eliminating dislocation compared to the conventional method. In particular, when the distance L was 75 mm, the number of successful attempts to eliminate dislocation was 5, which was the best result.
[0071] On the other hand, when the distance L to the step was 80 mm and 82 mm, the number of successful attempts to eliminate dislocations was 3, which was the same as for a conventional coil without a step. When the position of the step was at the same level as or further outwards from the outer periphery of the raw material rod, no effect of the step was obtained.
[0072] When the distance L to the step was 70 mm, i.e., when the step was provided 10 mm inward from the outer edge of the raw material rod, the step had no effect and the number of successful dislocation-free results worsened. This is thought to be because heat was concentrated on the inner side of the raw material rod rather than on the outer edge, further worsening the heat distribution.
[0073] From the above results, it was found that the radial position of the step is preferably within a range of 2 to 8 mm inward from the outer circumferential end of the raw material rod, and preferably 5 mm.
[0074] <Investigation of the radial position of the coil step (raw material diameter 150 mm)> We also investigated the radial position of the step suitable for a raw material rod with a diameter of 150 mm. As in the case of using a raw material rod with a diameter of 160 mm, the step height was set to 1.0 mm and the central angle θ of the step-free region was set to 60 degrees.
[0075] The radial distance L from the center of the coil conductor to the position where the step is formed was set to five different values: 65mm, 67mm, 70mm, 73mm, and 75mm, and five silicon single crystals were grown for each. The distances from the outer circumferential edge of the raw material rod to the position where these steps are formed were -10mm, -8mm, -5mm, -2mm, and 0mm, respectively. In addition, a coil with a flat top surface without any steps was also evaluated. The results are shown in Table 4.
[0076] [Table 4]
[0077] As shown in Table 4, the success rate of eliminating dislocations when a conventional coil with a flat top surface and no steps was used for a 150 mm diameter raw material rod was higher than when a conventional coil with no steps was used for a 160 mm diameter raw material rod, with four successes out of five (80%). On the other hand, when the step was located at 65 mm, in other words, when the step was located 10 mm inward from the outer circumferential edge of the raw material rod, the number of successful attempts to eliminate dislocations was three, and the success rate of eliminating dislocations worsened.
[0078] When a raw material rod with a diameter of 150 mm is used, the effect of the step is difficult to see because the success rate of eliminating dislocations is originally high, but the results were the same as when a raw material rod with a diameter of 160 mm was used, showing that a range of 2 to 8 mm inward from the outer edge of the raw material rod was best, with 5 mm being the best. [Explanation of symbols]
[0079] 1. Single crystal manufacturing equipment 2 Raw material rod 2e Outer end of raw material rod 3 seed crystals 4. Silicon single crystal 4a Tapered part of silicon single crystal 4b Silicon single crystal straight body 5. Melting Zone 10 Reactor 11 Upper shaft 12 Lower axis 14 Single crystal weight holder 15 Gas doping device 16 Raw material holder 17 Seed crystal holder 20 Induction heating coil 21 Coil conductor 21A Top surface of coil conductor 21B Bottom surface of coil conductor 22 Opening 23 Slit 24A First terminal electrode 4B Second terminal electrode 25 steps 26A Lower side 26B Upper surface 27A Slit vicinity area 27B Slit far region 28 Step formation area 29 Non-step area R0 raw material rod diameter R1 Silicon single crystal diameter Ra Outer diameter of coil conductor Rb Inner diameter of coil conductor r0 Radius of raw material rod r1 Step radius Δr radius difference θ Central angle of the area near the slit (area without step)
Claims
1. An induction heating coil for heating a raw material rod in the production of a single crystal by the FZ method, a ring-shaped coil conductor having an opening at its center; a slit extending radially from the opening and separating one end and the other end of the coil conductor; a radial step formed on an upper surface of the coil conductor; the upper surface of the coil conductor has a step-forming region in which the step is provided in an arc shape in a plan view so as to surround the opening, and a step-free region in which the step is not provided, the non-step region includes a slit vicinity region adjacent to the slit, the step region is a region farther from the slit than the step non-forming region, the step is provided in the vicinity of an outer circumferential end of the straight body portion of the raw material rod and radially inward from the outer circumferential end, An induction heating coil, characterized in that the difference between the radius of the raw material rod and the radius of the step is 2 mm or more and 8 mm or less.
2. The induction heating coil according to claim 1 , wherein the height of the step is 0.5 mm or more and 1.5 mm or less.
3. 3. The induction heating coil according to claim 1, wherein the non-step region is a sector-shaped region extending on both sides of the slit and having a central angle of 45 degrees or more and 90 degrees or less.
4. 4. The induction heating coil according to claim 1, wherein an area of the non-step region provided on the one end side of the coil conductor is different from an area of the non-step region provided on the other end side of the coil conductor.
5. An induction heating coil for heating a raw material rod in the production of a single crystal by the FZ method, a ring-shaped coil conductor having an opening at its center; a slit extending radially from the opening and separating one end and the other end of the coil conductor; a radial step formed on an upper surface of the coil conductor; the upper surface of the coil conductor has a step-forming region in which the step is provided in an arc shape in a plan view so as to surround the opening, and a step-free region in which the step is not provided, the non-step region includes a slit vicinity region adjacent to the slit, the step region is a region farther from the slit than the step non-forming region, the step is provided in the vicinity of an outer circumferential end of the straight body portion of the raw material rod and radially inward from the outer circumferential end, An induction heating coil, characterized in that the area of the non-step region provided on one end side of the coil conductor is different from the area of the non-step region provided on the other end side.
6. The induction heating coil according to claim 5 , wherein the height of the step is not less than 0.5 mm and not more than 1.5 mm.
7. 7. The induction heating coil according to claim 5, wherein the non-step region is a sector-shaped region extending on both sides of the slit and having a central angle of 45 degrees or more and 90 degrees or less.
8. A single crystal manufacturing apparatus used for manufacturing a single crystal by the FZ method, an upper shaft that supports the raw material rod so as to be rotatable and vertically movable; a lower shaft disposed below the upper shaft and configured to support a seed crystal rotatably and vertically; 8. An apparatus for producing a single crystal, comprising: an induction heating coil for heating the raw material rod according to claim 1 .
9. A method for producing a single crystal, comprising producing a single crystal by an FZ method using an induction heating coil described in any one of claims 1 to 7.
Citation Information
Patent Citations
Boss coil for preparing zone melting single-crystal
CN105154967A
Engine starter
JP1994002636A
Induction heating coil and method for manufacturing monocrystal using the same
JP2013168345A
Manufacturing method for single crystal and single crystal manufacturing apparatus
JP2015218076A
Device and method for manufacturing semiconductor single crystal
JP2016141612A