Manufacturing method of multi-layer tube
The multilayer PTFE tube design with a low-porosity inner and high-porosity outer layer, integrated through extrusion, addresses durability and flexibility issues, enhancing degassing performance and reducing kinking risks.
Patent Information
- Application Number
- JP2020147752
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-02
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-02
AI Technical Summary
Existing PTFE tubes with a porous outer layer for degassing applications face issues with durability and flexibility due to potential gaps or uneven layers, leading to reduced durability and increased risk of kinking.
A multilayer tube design with an inner layer of low porosity PTFE and an outer layer of high porosity PTFE, integrated through a single extrusion process, ensuring the outer layer is formed continuously with the inner layer, enhancing flexibility and durability while maintaining high degassing performance.
The integrated multilayer structure achieves improved flexibility, durability, and enhanced degassing performance by minimizing gaps and ensuring a continuous interface between the inner and outer layers, thereby reducing the risk of kinking and maintaining effective gas permeability.
Smart Images

Figure 0007553080000006 
Figure 0007553080000007 
Figure 0007553080000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-layer tube and a method for producing the same. [Background technology]
[0002] As a PTFE tube having excellent chemical resistance and heat resistance, a PTFE tube having an inner layer made of solid PTFE and an outer layer made of a PTFE film with a porous structure wound on the inner layer is known. PTFE tubes are sometimes used for degassing gases such as oxygen dissolved in liquids. Such PTFE tubes are manufactured, for example, by winding the outer layer spirally on the inner layer, and therefore may have a portion (step) where an outer layer is laminated on the outer layer in order to laminate the outer layer without gaps.
[0003] A PTFE tube with a porous outer layer has excellent flexibility and is less likely to kink even with a small bending radius. However, if the above-mentioned step exists, that part may have a negative effect on durability. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-001630 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a multi-layer tube which is excellent in flexibility and durability and has high degassing performance, and a method for producing the same. [Means for solving the problem]
[0006] The present invention To According to the multi-layer tube Manufacturing methodThe multi-layer tube includes an inner layer including a first polytetrafluoroethylene and an outer layer including a second polytetrafluoroethylene. The outer layer is formed so as to be integrated with the entire outer peripheral surface of the inner layer. The porosity of the inner layer is lower than the porosity of the outer layer.
[0007] The above A method for producing a multi-layer tube includes preparing a first mixture including a first polytetrafluoroethylene and a second mixture including a second polytetrafluoroethylene having a higher number average molecular weight than the first polytetrafluoroethylene, preforming the first mixture and the second mixture to obtain a tablet, paste extrusion molding the tablet to obtain a green tube, and stretching the green tube while heat treating it.
[0008] The preforming is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder, and includes inserting a pipe between the inner wall of the cylinder and the outer wall of the mandrel, filling the second mixture between the pipe and the inner wall of the cylinder, compressing the second mixture to form a cylindrical second mixture, and then removing the pipe, filling the first mixture between the outer wall of the mandrel and the cylindrical second mixture, and compression-molding the first mixture and the cylindrical second mixture to obtain a tablet.
[0009] or the above A method for producing a multi-layer tube includes preparing a first mixture including a first polytetrafluoroethylene and a second mixture including a second polytetrafluoroethylene having a higher number average molecular weight than the first polytetrafluoroethylene, preforming the first mixture and the second mixture to obtain a tablet, paste extrusion molding the tablet to obtain a green tube, and stretching the green tube while heat treating it.
[0010] The pre-molding is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder, and includes inserting a pipe between the inner wall of the cylinder and the outer wall of the mandrel, filling a first mixture between the outer wall of the mandrel and the pipe, compressing the first mixture to form a cylindrical first mixture, and then removing the pipe, filling a second mixture between the cylindrical first mixture and the inner wall of the cylinder, and compression-molding the cylindrical first mixture and the second mixture to obtain a tablet. Effect of the Invention
[0011] According to the present invention, it is possible to provide a multi-layer tube having excellent flexibility, durability and high degassing performance, and a method for producing the same. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a cross-sectional perspective view illustrating an example of a multi-layer tube according to an embodiment. [Diagram 2] FIG. 1 is a schematic diagram showing an example of an apparatus configuration for performing a degassing test on a multi-layer tube using an internal perfusion method. [Diagram 3] 3A to 3C are process diagrams showing an example of a method for producing a multi-layer tube according to an embodiment. [Figure 4] 1 is a scanning electron microscope (SEM) image showing a cross section of a multilayer tube according to an embodiment. [Diagram 5] 13 is an SEM image showing a cross section of a tube according to a comparative example. [Figure 6] FIG. 2 is a cross-sectional view showing a cross section of a multi-layer tube according to an embodiment, observed using an SEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0014] PTFE tubes are used in various industrial fields such as semiconductor manufacturing, food manufacturing, automobile manufacturing, and medical care to allow fluids to flow through the tube. PTFE tubes have high chemical resistance, so it is possible to minimize contamination of fluids caused by the tube. When flowing liquid through a tube, it may be necessary to degas the gas dissolved in the liquid. To degas the dissolved gas, specifically, the outside of the tube is evacuated, and the partial pressure difference between the gases present inside and outside the tube is used to remove the gas dissolved in the liquid flowing through the tube. Therefore, the PTFE tube used for this purpose is required to have the performance to allow only gas to pass through the tube wall, without allowing liquid to pass through it.
[0015] In order to increase gas permeability, it is necessary to reduce the thickness of the solid layer in the PTFE tube. However, in the conventional method of manufacturing PTFE tubes by paste extrusion, if the tube thickness is made too thin, defects such as cracks will occur during firing. Therefore, it has been difficult to significantly thin the solid layer by paste extrusion.
[0016] On the other hand, when a thin PTFE tube is manufactured in advance by a method other than paste extrusion, it is necessary to laminate an outer layer having a porous structure in a post-process in order to impart flexibility and kink resistance to the tube. Such laminated products may have problems with durability as described above.
[0017] (First embodiment) According to the first embodiment, a multi-layer tube is provided. The multi-layer tube according to the embodiment is manufactured by a method including, when manufacturing a tablet as a preform used in paste extrusion, forming the inner layer side of the tablet with a PTFE resin that is difficult to make porous, and forming the outer layer side of the tablet with a PTFE resin that is easy to make porous. By using such a tablet containing two types of PTFE resin, a multi-layer tube in which an inner layer that is thin and has a solid structure and an outer layer that has a porous structure are integrated can be manufactured by only one paste extrusion. The inner layer and the outer layer have different porosities, and the porosity of the inner layer is lower than that of the outer layer.
[0018] Unlike a tube whose entire structure is solid, the multilayer tube according to the embodiment has an outer layer having a porous structure. The thickness of the inner layer having a solid structure is reduced by the presence of the outer layer. Therefore, the multilayer tube according to the embodiment has high degassing performance. In addition, the outer layer is not added later on the inner layer, but is extruded together with the inner layer by a single paste extrusion. In other words, there is substantially no boundary between the inner layer and the outer layer, and the inner layer and the outer layer are integrated or formed as a continuous body. Therefore, the multilayer tube has high durability against bending. In addition, since the outer layer has a porous structure, the multilayer tube has excellent flexibility and kink resistance.
[0019] Hereinafter, a multi-layer tube according to an embodiment will be described with reference to the drawings. 1 is a cross-sectional perspective view that illustrates an example of a multi-layer tube. The multi-layer tube may be a two-layer tube having a two-layer structure of an inner layer and an outer layer.
[0020] The multilayer tube 1 includes an inner layer 2 having a solid structure and an outer layer 3 having a porous structure. The inner layer 2, the outer layer 3, and the multilayer tube 1 formed by them all have an annular cylindrical shape. The inner layer 2 and the outer layer 3 both extend from the bottom surface to the top surface of the multilayer tube 1. The inner peripheral surface of the outer layer 3 is in contact with the outer peripheral surface of the inner layer 2. The outer layer 3 is formed so as to be integrated with the entire outer peripheral surface of the inner layer 2. Note that, although the boundary between the inner layer 2 and the outer layer 3 is shown in FIG. 1 for convenience, in reality, this boundary does not clearly exist. This will be described later with reference to FIG. 4 showing a cross-sectional SEM image of a multilayer tube according to an embodiment.
[0021] The porosity of the inner layer 2 is lower than that of the outer layer 3. Therefore, the multi-layer tube 1 has superior degassing performance compared to a case where the entire multi-layer tube 1 is made of a solid PTFE resin.
[0022] The porosity of the inner layer 2 is, for example, less than 1%, and preferably less than 0.1%. The porosity of the inner layer 2 may be 0%. If the porosity of the inner layer is excessively large, when the multilayer tube is used for degassing purposes, liquid may permeate through the tube wall surface or the pressure resistance may decrease, which is not preferable.
[0023] The porosity of the outer layer 3 is, for example, 5% to 80%. The porosity of the outer layer 3 is preferably within the range of 10% to 40%. If the porosity of the outer layer 3 is excessively small, the flexibility and kink resistance may decrease. If the porosity of the outer layer 3 is excessively large, the strength as a support is lost, and strength aspects such as pressure resistance decrease. The porous structure of the outer layer 3 is typically composed of amorphous node parts and fibril parts drawn out from the node parts. Therefore, the pores present in the outer layer 3 are mutually connected. The porous structure composed of nodes and fibrils is formed, for example, when a shear force is applied to the preform during paste extrusion, which will be described later.
[0024] <Porosity measurement method> The porosity of the inner and outer layers is measured by specific gravity measurement using the underwater displacement method. Specifically, first, an air permeability test is performed on the multilayer tube at 0.01 MPa. If no air permeability is observed in the air permeability test, the porosity of the inner layer can be considered to be 0% (specific gravity 2.2). Next, the multilayer tube is cut to a certain length, and the cross-sectional areas of the inner and outer layers are measured using a microscope to measure the volume of each layer. Separately, specific gravity measurement is performed on the multilayer tube using the underwater displacement method to measure the specific gravity of the entire multilayer tube.
[0025] Then, the specific gravity of the outer layer is calculated based on the following formula (1). [Specific gravity measured by underwater displacement method] = (specific gravity of inner layer × volume of inner layer + specific gravity of outer layer × volume of outer layer) ÷ (total volume of multi-layer tube) (1) From the specific gravity of the outer layer thus determined, the porosity of the outer layer can be calculated.
[0026] The wall thickness (total thickness) of the multi-layer tube is, for example, within the range of 0.2 mm to 2 mm, and preferably within the range of 0.5 mm to 1 mm. The wall thickness of the multi-layer tube is the sum of the thickness of the inner layer and the thickness of the outer layer. There is no limit to the wall thickness of the multi-layer tube as long as the multi-layer tube has excellent degassing performance. However, an excessively large wall thickness is undesirable because it impairs the flexibility of the multi-layer tube. The degassing performance of the multi-layer tube is largely dependent on the thickness of the inner layer, which will be described later. Since the outer layer has a porous structure, typically, gas can easily permeate through the outer layer even without creating a vacuum on the outside of the multi-layer tube.
[0027] The thickness of the inner layer is, for example, in the range of 0.01 mm to 0.1 mm, and preferably in the range of 0.02 mm to 0.05 mm. In order to improve the degassing performance of the multi-layer tube, it is preferable that the thickness of the inner layer is as thin as possible. As the thickness of the inner layer increases, the degassing performance tends to deteriorate.
[0028] The thickness of the outer layer is, for example, in the range of 0.1 mm to 1 mm, and preferably in the range of 0.2 mm to 0.5 mm. If the thickness of the outer layer is too small, the multilayer tube tends to have poor flexibility or kink resistance. There is no problem even if the thickness of the outer layer is large as long as the desired degassing performance can be achieved, but if the thickness is too large, the handleability of the multilayer tube may be reduced.
[0029] The ratio of the thickness of the inner layer to the total thickness of the multilayer tube is, for example, in the range of 1% to 25%, and preferably in the range of 15% to 25%. If this ratio is too small, the strength of the inner layer is weakened and it may break when bent, and the inner layer also tends to become porous during processing, which is not preferable. If this ratio is too large, the degassing performance may be reduced. If this ratio is in the range of 15% to 25%, not only is the degassing performance excellent, but the kink resistance performance is also excellent, which is preferable.
[0030] <Measurements of various dimensions> The thickness of the inner layer, the thickness of the outer layer, and the wall thickness of the multilayer tube can be determined by measuring these thicknesses at eight points on the SEM image obtained in the above-mentioned porosity measurement and calculating the average value of the eight points for each thickness. From the calculated values of the thickness of the inner layer, the thickness of the outer layer, and the wall thickness of the multilayer tube, the proportion of the inner layer in the thickness of the multilayer tube can be calculated.
[0031] The inner diameter of the multi-layer tube is not particularly limited, but is, for example, within the range of 0.5 mm to 10 mm. The outer diameter of the multi-layer tube is not particularly limited, but is, for example, within the range of 1 mm to 20 mm. The inner and outer diameters of the multi-layer tube can be measured using a pin gauge and a vernier caliper having an accuracy of 1 / 1000 mm.
[0032] In order to improve the degassing performance of the multi-layer tube, it is advantageous for the multi-layer tube to have a large inner surface area. The inner surface area can also be called the surface area of the inner wall of the multi-layer tube. If the surface area of the inner wall of the tube is large, the contact area between the liquid present in the tube and the inner wall of the tube increases. In other words, the area of the liquid exposed to the vacuum increases, making it easier to degas the gas dissolved in the liquid.
[0033] The internal surface area per unit length of a multi-layer tube is, for example, 1.57 mm 2 / mm~31.4mm 2 / mm, preferably 2.51 mm 2 / mm~18.84mm 2 / mm. If the thickness of the inner layer is constant, the degassing performance tends to be high when the inner diameter surface area per unit length is large.
[0034] The inside surface area of the multi-layer tube can be calculated from the inside diameter measured using a pin gauge with an accuracy of 1 / 1000 mm.
[0035] <Degassing test> The degassing performance of a multi-layer tube can be roughly estimated from parameters such as the thickness of the inner layer, the porosity of the inner layer, and the inner diameter surface area, but the degassing rate can also be specifically evaluated based on the degassing test described below. Figure 2 is a schematic diagram showing the configuration of a degassing test device used in the degassing test. Here, the degassing rate of oxygen is measured. The configuration of the degassing test device shown in Figure 2 shows the case where the degassing test is performed by the internal perfusion method.
[0036] The degassing test apparatus 100 includes a degassing module 110, a dissolved oxygen meter 120, and a circulation pump 130. As the degassing module, for example, a product name (SEPAREL) manufactured by DIC Corporation can be used. Alternatively, a degassing module having equivalent functions may be used. A multilayer tube to be measured is set inside the degassing module 110.
[0037] The degassing module 110, the dissolved oxygen meter 120, and the circulation pump 130 are connected to one another by a tube 101 such as a rubber tube. The degassing module 110 is separately connected to a vacuum pump 140 via the tube 101. The inside of the degassing module 110 can be made to be at a lower pressure than atmospheric pressure by operating the vacuum pump 140.
[0038] When performing a degassing test, first, pure water is introduced into the degassing module 110, the dissolved oxygen meter 120, and the circulation pump 130. The degassing test apparatus 100 can repeatedly circulate the pure water inside the degassing module 110, the dissolved oxygen meter 120, and the circulation pump 130 in this order. The symbol D in Fig. 2 indicates the direction in which the pure water circulates.
[0039] Before operating the vacuum pump 140, the amount of dissolved oxygen [ml / L] in the pure water before degassing is measured. Then, the vacuum pump 140 is operated and the pressure in the vacuum section is set to 0.08 MPa. In this state, the dissolved oxygen is degassed for 24 hours, and the amount of dissolved oxygen in the pure water after 24 hours (after degassing) is measured. Then, the amount of dissolved oxygen before degassing (A 1 Dissolved oxygen amount after degassing (A 2 ) ratio multiplied by 100 (A 2 / A 1 × 100) and calculate the degassing rate (%).
[0040] The degassing rate of the multi-layer tube measured by the above-mentioned degassing test (internal perfusion method) is, for example, 5% or more, preferably 10% or more. The higher the degassing rate, the more desirable it is, but in one example, it may be 25% or less.
[0041] The degassing rate varies depending on the amount of pure water circulating in the degassing test device, and the inner diameter and length of the multi-layer tube to be measured. As an example, the inner diameter of the tube is 4.0 mm to 4.5 mm, and the length of the tube is 145 mm to 155 mm.
[0042] Although the above describes a case where the degassing test is performed by the internal perfusion method, in another embodiment, the degassing test may be performed by the external perfusion method. That is, it is also possible to degas the dissolved oxygen by placing the liquid to be degassed on the outside of the multi-layer tube and creating a vacuum inside the multi-layer tube. In the case of the external perfusion method, the liquid flows randomly (turbulent flow) on the outside of the multi-layer tube, so that the frequency of contact between the dissolved oxygen and the multi-layer tube can be increased.
[0043] In this example, the degassing of oxygen dissolved in pure water is shown as an example of measuring the degassing rate of a multi-layer tube. However, if there is no need to measure the degassing rate of dissolved oxygen, there is no limitation on the type of liquid to be degassed and the type of gas to be degassed.
[0044] If the degassing rate is high despite the small inner surface area, the degassing performance of such a multi-layer tube can be said to be excellent. 2 The ratio of the degassing rate [%] to the inner diameter surface area per unit length [mm 2 The ratio of the degassing rate [%] to the air gap [mm] is in the range of 0.5 to 1.5, and preferably in the range of 0.8 to 1.5.
[0045] The inner layer includes a first polytetrafluoroethylene. The inner layer may be made of the first polytetrafluoroethylene. The inner layer has a solid structure. The first polytetrafluoroethylene is polytetrafluoroethylene (PTFE) having a lower number average molecular weight than the second polytetrafluoroethylene included in the outer layer, which will be described later. The number average molecular weight of the first polytetrafluoroethylene is, for example, 1 million or more and 5 million or less. The first polytetrafluoroethylene preferably includes a modified monomer unit. The inner layer may include additives such as auxiliary agents in addition to the first polytetrafluoroethylene. Examples of the auxiliary agents include petroleum-based auxiliary agents.
[0046] The outer layer includes a second polytetrafluoroethylene. The outer layer may be made of the second polytetrafluoroethylene. The outer layer has a porous structure. The second polytetrafluoroethylene is a PTFE having a larger number average molecular weight than the first polytetrafluoroethylene. The number average molecular weight of the second polytetrafluoroethylene is, for example, 6 million or more and 15 million or less, and preferably 10 million or more and 15 million or less. The second polytetrafluoroethylene preferably does not contain a modified monomer unit. The second polytetrafluoroethylene may be a virgin type PTFE resin.
[0047] PTFE having a high number average molecular weight is easily made porous by paste extrusion. In the multilayer tube according to the embodiment, the second polytetrafluoroethylene contained in the outer layer preferably contains PTFE having a number average molecular weight larger than that of the first polytetrafluoroethylene contained in the inner layer. This makes it easy to manufacture a multilayer tube in which the porosity of the inner layer is lower than that of the outer layer.
[0048] In addition, PTFE resins containing modified monomer units tend to maintain a solid structure even when paste extruded. Virgin PTFE resins tend to be porous when paste extruded, as fibrils are pulled out from the nodes. In other words, the first polytetrafluoroethylene contained in the inner layer contains modified monomer units, making it easier to manufacture a multi-layer tube in which the porosity of the inner layer is lower than that of the outer layer.
[0049] Whether or not the inner layer contains a modified monomer unit can be confirmed by differential scanning calorimetry (DSC).
[0050] The specific gravity of the inner layer having a solid structure is close to the specific gravity inherent to PTFE, and is within the range of, for example, 2.12 to 2.25. On the other hand, the specific gravity of the outer layer having a porous structure is within the range of, for example, 1.00 to 2.0. The specific gravity of the entire multilayer tube including the inner layer and the outer layer is within the range of, for example, 1.60 to 2.0.
[0051] Second embodiment According to a second embodiment, a method for producing a multi-layer tube is provided. A multi-layer tube in which an outer layer is integrally formed over the entire outer peripheral surface of an inner layer can be produced, for example, by paste extrusion as described below.
[0052] First, a first powder containing a first polytetrafluoroethylene and a second powder containing a second polytetrafluoroethylene are prepared. The second polytetrafluoroethylene is a PTFE having a higher number average molecular weight than the first polytetrafluoroethylene. As the first polytetrafluoroethylene and the second polytetrafluoroethylene, those described in the first embodiment can be used. The first polytetrafluoroethylene preferably contains a modified monomer unit. This makes it possible to suppress cracking of the inner layer during firing after the paste extrusion described later.
[0053] The first powder and the second powder are preferably fine powders. Fine powders are obtained by coagulating and drying an aqueous dispersion obtained by emulsion polymerization. The fine powders may be mainly composed of, for example, primary particles produced by polymerization that have aggregated to form secondary particles having a particle size of about 100 μm. The average particle diameter (D 50 ) is, for example, in the range of 300 μm to 800 μm.
[0054] Next, a petroleum-based auxiliary is added to the first powder and stirred to obtain a mixture of the first powder and the auxiliary. The amount of the petroleum-based auxiliary added is, for example, within the range of 10% by mass to 30% by mass relative to the mass of the first powder. The obtained mixture is aged, for example, for 8 hours or more in a temperature environment of 10°C or higher. The temperature during aging is preferably within the range of 30°C to 35°C. The aging time is preferably within the range of 24 hours to 96 hours. By aging the mixture, the auxiliary penetrates into the surface irregularities of the fine powder (here, the first powder), and in the paste extrusion process described later, the fluidity is improved and the mixture can be extruded at a low pressure. In this way, a first mixture is obtained.
[0055] Similarly, the petroleum-based auxiliary is added to the second powder and stirred to obtain a mixture of the second powder and the auxiliary. The conditions for aging the obtained mixture are the same as those for the mixture of the first powder and the auxiliary. Thus, a second admixture is obtained.
[0056] Next, the first mixture and the second mixture are subjected to a preforming step. The preforming is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder. The preforming is performed, for example, using a preforming machine having at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder. An example of the preforming will be described with reference to FIG. 3. Each of FIG. 3(a) to FIG. 3(g) is a schematic plan view showing one step in a method for producing a tablet as a preformed body for a multilayer tube.
[0057] 3(a) to 3(g) are schematic diagrams showing a pre-forming machine including a cylinder and a mandrel, as viewed from above. The pre-forming machine 10 includes a cylinder 11 and a mandrel 12. The cylinder 11 has a cylindrical shape with a bottom. The mandrel 12 has a cylindrical shape and a smaller diameter than the cylinder 11. The mandrel 12 passes through the bottom of the cylinder 11. The inside of the mandrel 12 is hollow.
[0058] 3(a) shows the process of inserting pipe 13 from above cylinder 11 between the inner wall of cylinder 11 and the outer wall of mandrel 12. Pipe 13 is inserted until it contacts the bottom surface of cylinder 11. Pipe 13 serves to divide the space within cylinder 11 into two spaces: an inner layer side 20 space excluding mandrel 12, and an outer layer side 30 space. Pipe 13 can be a resin pipe made of, for example, polyvinyl chloride or the like.
[0059] 3(b) shows a process of filling the second mixture between the pipe 13 and the inner wall of the cylinder 11. Specifically, first, the lid 14 is placed so as to close the inner layer side 20, and then the second mixture 31 is poured into the outer layer side 30.
[0060] 3(c) shows a process of preliminarily compressing the second mixture 31 filled in the outer layer side 30. First, the lid 14 placed in the previous process is removed, and the lid 15 is placed so as to close the outer layer side 30. Then, the second mixture 31 filled in the outer layer side 30 is compressed with a force of 500N to 1000N to form a cylindrical second mixture 32.
[0061] FIG. 3(d) shows the process of removing the pipe 13. After removing the lid 15 installed on the outer layer side 30 in the process of FIG. 3(c), the pipe 13 is removed. The preliminarily compressed second mixture 31 forms a cylindrical second mixture 32. Therefore, even after the pipe 13 is removed, the cylindrical second mixture 32 does not penetrate into the inner layer side 20. In the figure, the symbol 25 indicates a virtual boundary (virtual line) between the inner layer side 20 and the outer layer side 30.
[0062] 3(e) shows a process of filling the first mixture 21 between the outer wall of the mandrel 12 and the cylindrical second mixture 32. Thus, the inside of the cylinder 11 is filled with the first mixture 21 and the cylindrical second mixture 32.
[0063] Fig. 3(f) shows a process of subjecting the first mixture 21 and the cylindrical second mixture 32 to compression molding together. As shown in Fig. 3(f), the compression molding is performed with the lid 16 placed over the entire cylinder 11. The first mixture 21 is compressed by compression molding to become the first molded body 22 shown in Fig. 3(g). The cylindrical second mixture 32 is compressed by compression molding to become the second molded body 33 shown in Fig. 3(g).
[0064] FIG. 3(g) shows a tablet 40 obtained after the first mixture 21 and the cylindrical second mixture 32 are compressed together. The tablet 40 is composed of a first molded body 22 and a second molded body 33. As shown in the step of FIG. 3(e), the first mixture 21 and the cylindrical second mixture 32 are in contact with each other at the imaginary line 25. In addition, the first mixture 21 and the cylindrical second mixture 32 are both mixtures containing PTFE having similar properties. Therefore, by subjecting these to compression molding together, a tablet 40 in which the first molded body 22 and the second molded body 33 are integrated at the imaginary line 25 can be obtained. The tablet 40 has an annular cylindrical shape. This ring is formed because the mixture is not filled in the mandrel 12. By performing paste extrusion molding using the tablet 40 in which the first molded body 22 and the second molded body 33 are integrated, a multi-layer tube in which the outer layer is formed to be integrated with the outer circumferential surface of the inner layer can be manufactured.
[0065] In the above-described preforming process with reference to FIG. 3, the second mixture 31 is filled first on the outer layer side 30, and then the first mixture 21 is filled on the inner layer side 20. However, the order of filling the first mixture 21 and the second mixture 31 into the cylinder 11 may be reversed. That is, the first mixture 21 may be filled first on the inner layer side 20, and then the second mixture 31 may be filled on the outer layer side 30, and the tablet may be obtained through compression molding.
[0066] When the tablet is subjected to paste extrusion molding, for example, the following procedure is followed. First, the tablet is put into a paste extruder and extruded to obtain an unsintered tube. Next, the unsintered tube is stretched while being heat-treated to obtain a multi-layer tube. The heat treatment includes, for example, drying and sintering the unsintered tube. The unsintered tube extruded from the paste extruder is first dried in a drying furnace. By drying at a temperature equal to or higher than the boiling point of the petroleum-based auxiliary used earlier, the auxiliary can be volatilized. Next, the dried tube is heated and sintered at a temperature equal to or higher than the melting point of PTFE, for example, at a temperature equal to or higher than 330°C.
[0067] In a series of steps from the step of obtaining an unsintered tube by paste extrusion to the step of drying and firing, the tube is stretched by setting a speed difference between the extrusion speed of the tube and the take-up speed of the fired tube. By this stretching, the first molded body part constituting the tablet changes to an inner layer having a lower porosity than the outer layer, and the second molded body part changes to an outer layer having a higher porosity than the inner layer. The stretching ratio is, for example, 1.1 times or more, and preferably 1.5 times or more and 1.8 times or less. By changing the stretching ratio, the porosity of the inner layer and the porosity of the outer layer can be adjusted. In this way, the multilayer tube according to the embodiment can be obtained. As described above, the inner layer has, for example, a solid structure, and the outer layer has, for example, a porous structure.
[0068] The thickness of the inner layer and the outer layer of the multi-layer tube can be changed, for example, by changing the diameter of the cylinder and / or the pipe used in preforming. By appropriately changing these diameters and adjusting the thickness of the first mixture and / or the second mixture to be filled, the total thickness of the inner layer, the outer layer and the multi-layer tube can be adjusted.
[0069] In the above-mentioned manufacturing method, in order to make the outer layer porous, a PTFE resin having a higher number average molecular weight than the first polytetrafluoroethylene is used as the second polytetrafluoroethylene contained in the second admixture. On the other hand, a PTFE resin having a lower number average molecular weight than the second polytetrafluoroethylene is used as the first admixture filled on the inner layer side. This makes it possible to manufacture a multi-layer tube in which the porosity of the outer layer is higher than that of the inner layer. However, the manufacturing method of a multi-layer tube in which the porosity of the outer layer is lower than that of the inner layer is not limited to this. Specifically, as another method, a method of adding a pore-forming material to the second admixture before the preforming step can be mentioned.
[0070] By adding no pore-forming material to the first mixture but only to the second mixture, and then performing the preforming step and paste extrusion with firing according to the above-mentioned procedure, a multi-layer tube having a higher porosity in the outer layer than in the inner layer can be obtained. The pore-forming material added to the second mixture sublimes during firing, so that pores can be formed only in the outer layer. In the multi-layer tube thus obtained, the outer layer is formed so as to be integrated with the entire outer peripheral surface of the inner layer.
[0071] When a multi-layer tube is manufactured by adding a pore-forming material to the second mixture, the first polytetrafluoroethylene and the second polytetrafluoroethylene may be the same type of PTFE resin, or in this case, the first polytetrafluoroethylene and the second polytetrafluoroethylene may have the same number average molecular weight.
[0072] The ratio of the pore-forming material to the mass of the second mixture is, for example, within the range of 10% by mass to 50% by mass. By adjusting this ratio, the porosity of the outer layer of the resulting multi-layer tube can be adjusted.
[0073] An example of the pore-forming material is at least one selected from the group consisting of cross-linked acrylic resins and cross-linked styrene resins.
[0074] [Example] Examples will be described below, but the embodiments are not limited to the examples described below.
[0075] Example 1 As the first powder, a first polytetrafluoroethylene (F-302, manufactured by Daikin Industries) having a number average molecular weight of about 5.7 million was prepared. The first powder was a PTFE fine powder having an average particle diameter of 500 μm. The first polytetrafluoroethylene contained perfluoropropyl vinyl ether (PPVE) as a modified monomer unit. As the second powder, a second polytetrafluoroethylene (F-106, manufactured by Daikin Industries) having a number average molecular weight of about 8.1 million was prepared. The second powder was a PTFE fine powder having an average particle diameter of 550 μm.
[0076] A first mixture was obtained by adding 22 parts by mass of a petroleum-based auxiliary to 100 parts by mass of the first powder, mixing uniformly, and aging for 48 hours at a temperature of 24° C. Similarly, a second mixture was obtained by adding 22 parts by mass of a petroleum-based auxiliary to 100 parts by mass of the second powder, mixing uniformly, and aging for 48 hours at a temperature of 24° C.
[0077] The first and second mixtures thus obtained were preformed according to the method described with reference to Figs. 3(a) to 3(g) to prepare tablets.
[0078] The prepared tablet was put into a paste extruder and extruded to obtain an unsintered tube. The extruded unsintered tube was transported to a drying furnace and dried in a temperature environment of 130°C to 190°C to volatilize the auxiliary. The dried unsintered tube was transported to a firing furnace and fired for 120 seconds in a temperature environment of 380°C to 450°C. In a series of steps from extrusion to obtain an unsintered tube, drying and firing, the tube was stretched 1.5 times to produce a two-layer tube.
[0079] Comparative Example 1 A tube was produced in the same manner as in Example 1, except that only the first powder was used as the raw material powder and no pipe was used to separate the inner layer side and the outer layer side when producing a tablet as a preformed body. That is, during preformation, only the first mixture was filled in a cylinder and compressed to obtain a tablet. The obtained tube did not have a two-layer structure, but had a solid structure as a whole.
[0080] For the tubes obtained in Example 1 and Comparative Example 1, SEM images were taken according to the method described in the first embodiment, and specific gravity measurements were performed using the underwater displacement method to measure various dimensions and porosity. In addition, a degassing test was performed using the internal perfusion method described in the first embodiment to measure the degassing rate. These results are shown in Table 1 below. In Table 1, the "specific gravity" column shows the specific gravity of the entire tube.
[0081] [Table 1]
[0082] In general, the larger the contact area between the degassing part (the inner wall of the tube) and water, the more advantageous the degassing performance. In other words, the larger the inner diameter surface area per unit length of the tube, the higher the degassing performance tends to be. Comparing Example 1 with Comparative Example 1, the two-layer tube of Example 1 has a better degassing rate, even though the tube of Comparative Example 1 has a larger inner diameter surface area per unit length. Therefore, it can be seen that the two-layer tube of Example 1 has better degassing performance.
[0083] Fig. 4 shows an SEM image showing an example of a cross section of the two-layer tube according to Example 1. The SEM image shown in Fig. 4 was obtained by observing and photographing the two-layer tube according to Example 1 from the observation direction X shown in Fig. 6. As shown in Fig. 6, the multi-layer tube 1 (here, the two-layer tube) was cut along the diameter direction, and the exposed cross section was observed. During the SEM observation, the observed portion 17 was observed from the observation direction X at a magnification of 500 times.
[0084] In Fig. 4, the region indicated by reference numeral 3 is the outer layer, and the region indicated by reference numeral 2 is the inner layer. The region indicated by reference numeral 4 is the region in which the inner diameter surface of the two-layer tube is reflected. The region indicated by reference numeral 5 is the background image, and is the region in which nothing is reflected. From Fig. 4, it can be seen that in the two-layer tube of Example 1, there is substantially no boundary between the inner layer 2 having a solid structure and the outer layer 3 having a porous structure, and they are formed integrally.
[0085] FIG. 5 shows an SEM image showing an example of a cross section of the tube according to Comparative Example 1. The SEM image shown in FIG. 6 is also an image obtained by observing the tube from the observation direction X shown in FIG. 6. In FIG. 5, the region indicated by reference numeral 6 is a single solid layer. In region 6, there are parts with different colors due to the influence of minute steps formed by cutting the tube to be observed with a razor, but as described above, region 6 is a single solid layer. In addition, the region indicated by reference numeral 7 is a skin layer. Reference numeral 4 is a region in which the inner diameter surface of the tube is reflected. From FIG. 5, it can be seen that the tube according to Comparative Example 1 has a solid structure over the entire radial direction.
[0086] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention. The invention as originally claimed in the present application is set forth below. [1] An inner layer having a solid structure and comprising a first polytetrafluoroethylene; and an outer layer having a porous structure and comprising a second polytetrafluoroethylene; The outer layer is formed so as to be integrated with the entire outer peripheral surface of the inner layer, A multi-layer tube, wherein the porosity of the inner layer is lower than the porosity of the outer layer. [2] The multilayer tube according to [1], wherein the porosity of the inner layer is less than 1%, and the porosity of the outer layer is 5% to 80%. [3] The multilayer tube according to [1] or [2], wherein the first polytetrafluoroethylene contains a modified monomer unit. [4] The degassing rate measured by an internal perfusion method is 5% or more; The degassing test includes measuring the amount of dissolved oxygen in the pure water before degassing, and measuring the amount of dissolved oxygen in the pure water after degassing at 0.08 MPa for 24 hours. The multilayer tube according to any one of [1] to [3], wherein the degassing rate is a percentage calculated by multiplying the ratio of the amount of dissolved oxygen after the degassing to the amount of dissolved oxygen before the degassing by 100. [5] Providing a first mixture comprising a first polytetrafluoroethylene and a second mixture comprising a second polytetrafluoroethylene having a higher number average molecular weight compared to the first polytetrafluoroethylene; preforming said first blend and said second blend to obtain a tablet; paste extrusion of said tablet to obtain a green tube; stretching the green tube while heat treating it; A method for producing a multi-layer tube comprising the steps of: The preforming is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder; inserting a pipe between an inner wall of the cylinder and an outer wall of the mandrel; Filling the second mixture between the pipe and the inner wall of the cylinder; compressing the second mixture to form a cylindrical second mixture, and then removing the pipe; Filling the first mixture between the outer wall of the mandrel and the cylindrical second mixture; compressing the first mixture and the cylindrical second mixture to obtain the tablet; A method for producing a multi-layer tube comprising the steps of: [6] Providing a first mixture comprising a first polytetrafluoroethylene and a second mixture comprising a second polytetrafluoroethylene having a higher number average molecular weight compared to the first polytetrafluoroethylene; preforming said first blend and said second blend to obtain a tablet; paste extrusion of said tablet to obtain a green tube; stretching the green tube while heat treating it; A method for producing a multi-layer tube comprising the steps of: The preforming is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder; inserting a pipe between an inner wall of the cylinder and an outer wall of the mandrel; filling the first admixture between the outer wall of the mandrel and the pipe; compressing the first mixture to form a cylindrical first mixture, and then removing the pipe; Filling the second mixture between the cylindrical first mixture and the inner wall of the cylinder; compressing the cylindrical first mixture and the second mixture to obtain the tablet; A method for producing a multi-layer tube comprising the steps of: [7] The method for producing a multilayer tube according to [5] or [6], wherein the first polytetrafluoroethylene contains a modified monomer unit. [Explanation of symbols]
[0087] 1...multilayer tube, 2...inner layer, 3...outer layer, 10...pre-forming machine, 11...cylinder, 12...mandrel, 13...pipe, 14, 15, 16...lid, 20...inner layer side, 21...first mixture, 22...first molded body, 25...virtual line, 30...outer layer side, 31...second mixture, 32...cylindrical second mixture, 33...second molded body, 40...tablet, 100...degassing test apparatus, 101...tube, 110...degassing module, 120...dissolved oxygen meter, 130...circulation pump, 140...vacuum pump, D...circulation direction.
Claims
1. Providing a first blend comprising a first polytetrafluoroethylene and a second blend comprising a second polytetrafluoroethylene having a higher number average molecular weight compared to the first polytetrafluoroethylene; preforming said first blend and said second blend to obtain a tablet; paste extrusion of said tablet to obtain a green tube; stretching the green tube while heat treating it; A method for producing a multi-layer tube comprising the steps of: The preforming is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder; inserting a pipe between an inner wall of the cylinder and an outer wall of the mandrel; filling the second mixture between the pipe and the inner wall of the cylinder; compressing the second mixture to form a cylindrical second mixture, and then removing the pipe; Filling the first mixture between the outer wall of the mandrel and the cylindrical second mixture; compressing the first mixture and the cylindrical second mixture to obtain the tablet; Including, An inner layer having a solid structure and including the first polytetrafluoroethylene; and an outer layer having a porous structure and comprising the second polytetrafluoroethylene; The outer layer is formed so as to be integrated with the entire outer peripheral surface of the inner layer, A method for manufacturing a multi-layer tube, wherein the porosity of the inner layer is lower than the porosity of the outer layer.
2. Providing a first blend comprising a first polytetrafluoroethylene and a second blend comprising a second polytetrafluoroethylene having a higher number average molecular weight compared to the first polytetrafluoroethylene; preforming said first blend and said second blend to obtain a tablet; paste extrusion of said tablet to obtain a green tube; stretching the green tube while heat treating it; A method for producing a multi-layer tube comprising the steps of: The preforming is performed using at least a cylinder having a bottom and a mandrel penetrating the bottom of the cylinder; inserting a pipe between an inner wall of the cylinder and an outer wall of the mandrel; filling the first admixture between the outer wall of the mandrel and the pipe; compressing the first mixture to form a cylindrical first mixture, and then removing the pipe; Filling the second mixture between the cylindrical first mixture and the inner wall of the cylinder; compressing the cylindrical first mixture and the second mixture to obtain the tablet; Including, An inner layer having a solid structure and including the first polytetrafluoroethylene; and an outer layer having a porous structure and comprising the second polytetrafluoroethylene; The outer layer is formed so as to be integrated with the entire outer peripheral surface of the inner layer, A method for manufacturing a multi-layer tube, wherein the porosity of the inner layer is lower than the porosity of the outer layer.
3. The method for producing a multi-layer tube according to claim 1 or 2, wherein the first polytetrafluoroethylene contains a modified monomer unit.
Citation Information
Patent Citations
Method and apparatus for sintering tubes made of ethylene tetrafluoride resin
JP1977077181A
Production of porous polytetrafluoroethylene article
JP1983145735A
Porous highly expansible fluoropolymers and production thereof
JP1988041544A
JP1989096593U