Method for pre-treating lump ore and method for operating a blast furnace
The pretreatment of lump ore by removing adhering powder and controlling SiO2 and Al2O3 content improves high-temperature reduction properties, stabilizing blast furnace operation by reducing residual powder to less than 2%.
Patent Information
- Application Number
- JP2019116162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-06-24
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-06-24
AI Technical Summary
Existing methods for pre-treating lump ore for blast furnaces do not adequately address the improvement of high-temperature reduction properties, which are crucial for stable furnace operation, due to the presence of adhering powder that affects the porosity and reduction reactions.
A pretreatment method for lump ore involves removing adhering powder with a diameter less than 3mm, maintaining SiO2 content at 4.5% by mass or less, Al2O3 content at 3% by mass or less, and a mass ratio A/S of 0.5 or more, followed by drying to reduce moisture content, ensuring less than 2% residual powder remains.
The method enhances the high-temperature reduction properties of lump ore, improving blast furnace operation by preventing softening and shrinkage, thereby stabilizing furnace conditions.
Smart Images

Figure 0007553179000003 
Figure 0007553179000002 
Figure 0007553179000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for pre-treating lump ore to remove adhering fines before charging the lump ore into a blast furnace, and a method for operating a blast furnace in which the lump ore obtained by this pre-treatment method is charged into the blast furnace. [Background technology]
[0002] In Patent Document 1, raw materials (iron raw materials) containing lumpy ores are heat-treated and dried, and before the dried raw materials are charged into a furnace from the top, fine ore adhering to the raw materials is removed by sieving. By removing the fine ore, a decrease in the void ratio inside the furnace due to the fine ore is suppressed, and fluctuations in the furnace pressure are suppressed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Laid-Open No. 2007-039747 Summary of the Invention [Problem to be solved by the invention]
[0004] In Patent Document 1, attention is paid to the porosity of the raw material layer (ore layer) formed in the upper part of a blast furnace, and fine ore adhering to the raw material is removed to prevent a decrease in this porosity. The inventors discovered that, depending on the type of lump ore, removing the adhering powder adhering to the lump ore can improve the high-temperature reduction properties of the lump ore, leading to the completion of the present invention. The high-temperature reduction properties refer to the reduction properties in the lower part of the furnace where softening of the iron raw material begins, and improving the high-temperature reduction properties can improve blast furnace operation. [Means for solving the problem]
[0005] The lump ore pretreatment method of the present invention is a method for pretreating lump ore having a predetermined composition by removing slag from the lump ore before charging it into a blast furnace. Diameter less than 3mmThe lump ore has an SiO2 content of 4.5 mass% or less, an Al2O3 content of 3 mass% or less, and a ratio of the Al2O3 content to the SiO2 content of 0.5 or more.
[0006] The removal of the adhering powder can be carried out until the ratio of the mass of the adhering powder remaining on the lump ore to the mass of the lump ore before the removal of the adhering powder is less than 2 mass %. Furthermore, the lump ore can be dried before the removal of the adhering powder.
[0007] In the method for operating a blast furnace according to the present invention, the lump ore obtained by the above-described pretreatment method is charged into the blast furnace. [Effects of the Invention]
[0008] According to the present invention, by removing the adhering powder from the lump ore having the above-mentioned composition before charging the lump ore into the furnace, the high-temperature reduction properties of the lump ore in the furnace can be improved. [Brief explanation of the drawings]
[0009] [Figure 1] This is an equilibrium phase diagram of FeO-Al2O3-SiO2. [Figure 2] FIG. 1 is a diagram showing the relationship between the amount of adhering fines and the high-temperature reduction rate for four types of lump ore. DETAILED DESCRIPTION OF THE INVENTION
[0010] In the lump ore pretreatment method of this embodiment, fine particles adhering to lump ore having a predetermined composition are removed before the lump ore is charged into a blast furnace. In the blast furnace operation method of this embodiment, the lump ore obtained by the pretreatment method described above is charged into a blast furnace. The lump ore is used as an iron raw material, similar to sintered ore and pellets, and is charged into the furnace from the furnace top alternately with coke. The fine particles are fine ore particles having a diameter of 3 mm or less.
[0011] The lump ore targeted by this embodiment has an SiO2 content of 4.5 mass% or less, an Al2O3 content of 3 mass% or less, and a mass ratio of the Al2O3 content to the SiO2 content (i.e., the value obtained by dividing the Al2O3 content by the SiO2 content, hereinafter referred to as the mass ratio A / S) of 0.5 [-] or more. An example of a lump ore satisfying this composition is Pilbara blend ore. By removing the adhering powder from this lump ore before charging it into a blast furnace, the reduction properties of the lump ore at high temperatures (1100°C to 1200°C) can be improved.
[0012] It has been found that the high-temperature reduction properties of lump ore depend on the reducibility of the lump ore itself (excluding the attached fines) and the amount of attached fines. Focusing on the relationship between the reducibility of the lump ore itself and the amount of attached fines, it has been found that for lump ores satisfying the above-mentioned composition, removing the attached fines is very important in improving the high-temperature reduction properties of the lump ore. The significance of the above-mentioned lump ore composition will be explained below.
[0013] The reducibility of lump ore itself depends on the SiO2 and Al2O3 contents. In the FeO-Al2O3-SiO2 equilibrium phase diagram shown in Figure 1, when the mass ratio A / S is less than 0.5, there is a region at 1200°C where a 2FeO·SiO2 melt is generated. If a 2FeO·SiO2 melt is generated at a low temperature, the reduction reaction is delayed due to the softening and shrinkage of the lump ore. On the other hand, if the mass ratio A / S is 0.5 or more, there is no region in the equilibrium phase diagram shown in Figure 1 where a 2FeO·SiO2 melt is generated. Therefore, the mass ratio A / S must be 0.5 or more.
[0014] Furthermore, even if the mass ratio A / S is 0.5 or more, if the SiO2 content increases, the amount of 2FeO·SiO2-based melt produced increases, which makes the lump ore more likely to soften and shrink, and the reduction reaction is more likely to be delayed. In consideration of this point, in this embodiment, the SiO2 content is set to 4.5 mass% or less. Here, the SiO2 content is preferably 4.0 mass% or less, and more preferably 3.5 mass% or less. The SiO2 content can be measured in accordance with the provisions of JIS M8214.
[0015] Furthermore, even if the mass ratio A / S is 0.5 or more, an increase in the Al2O3 content increases the amount of 2FeO·SiO2-Al2O3-based melt produced, which makes the lump ore more likely to soften and shrink, and the reduction reaction more likely to be delayed. In consideration of this point, in this embodiment, the Al2O3 content is set to 3 mass% or less. Here, the Al2O3 content is preferably 2.5 mass% or less. The Al2O3 content can be measured in accordance with the provisions of JIS M8856.
[0016] A known process can be appropriately adopted as a process for removing the adhering fines from the lump ore (hereinafter referred to as the removal process). In this removal process, it is sufficient to remove at least a portion of the adhering fines from the lump ore. For example, the adhering fines can be removed by washing the lump ore with water or by vibrating the lump ore. When removing the adhering fines by vibration, it is preferable to dry the lump ore in advance by a heat treatment or the like. Drying the lump ore facilitates the removal of the adhering fines. Furthermore, if the lump ore to be charged into a blast furnace is dried by a heat treatment or the like until its moisture content is reduced to a predetermined amount or less, the heat of evaporation of the moisture can be reduced when the lump ore is charged into the blast furnace, thereby preventing a decrease in the furnace temperature. Therefore, for stable operation of the blast furnace, it is preferable to charge lump ore that has been dried into the blast furnace.
[0017] The following index is used to quantitatively express the operation of removing adhering fines from lump ore. Mass of lump ore before removal process (including adhering powder) Wt Mass of adhering powder removed by removal process Wpd Mass of powder remaining on lump ore after removal treatment Wpr Total mass of adhering powder (=Wpd+Wpr) Wpt
[0018] After the removal treatment, the remaining ratio Rpr of the adhering powder that remains attached to the lump ore is preferably less than 2 mass %.
[0019] Here, the remaining ratio Rpr is defined by the following formula (1). Rpr = 100 × (Wpr / Wt) (1)
[0020] Here, since Wpr = Wpt - Wpd, Rpr can be calculated using the following equation (2). Rpr=100×((Wpt-Wpd) / Wt) ···(2)
[0021] The mass W0 of the lump ore excluding the adhering powder (Wt-Wpd or Wt-Wpt) can be used instead of the mass Wt to determine the residual ratio Rpr (Rpr=100×(Wpr / W0)).
[0022] The mass Wpd of the adhering powder removed from the lump ore depends on the removal process time. That is, the longer the removal process time, the greater the mass Wpd, and so a predetermined correlation exists between the removal process time and the mass Wpd. If this correlation is determined in advance, the mass Wpd can be adjusted by adjusting the removal process time. If the masses Wt and Wpt are measured in advance, the remaining ratio Rpr can be adjusted by adjusting the removal process time using the above formula (2). Therefore, by determining in advance the removal process time until the remaining ratio Rpr becomes less than 2% by mass and performing the removal process for this time, the remaining ratio Rpr can be made less than 2% by mass.
[0023] For lump ore having the above-mentioned composition, the lower the residual ratio Rpr, the easier it is to improve the high-temperature reduction properties. 1100In order to further increase the high-temperature reduction rate R, it is preferable to set the residual ratio Rpr to less than 2 mass%. 1100 is a value that serves as an index of the reducibility of the iron raw material, and is the reduction rate of the iron raw material at 1100°C. [Example]
[0024] The residual ratio Rpr and high-temperature reduction ratio R for four types of lump ore: A (Pilbara Blend), B (Robe), C (Gore), and D (Yandi). 1100 The relationship between the above was investigated. Each lump ore A to D was adjusted to a particle size of 10 to 15 mm in diameter by sieving. Table 1 below shows the chemical components, mass ratio A / S, and total attached powder ratio Rpt for each lump ore A to D.
[0025] Here, total iron T.Fe was measured in accordance with the standard of JIS M8212, and water of crystallization CW was measured by the Karl Fischer method.
[0026] [Table 1]
[0027] The total adhered powder ratio Rpt is the ratio of the mass of the powder removed by the water washing treatment to the mass Wt of the lump ore before the water washing treatment (Rpt = 100 × (Wpd / Wt)), assuming that the mass Wpt of the total adhered powder is the mass of the powder removed by the water washing treatment (Wpt = Wpd, Wpr = 0).
[0028] In measuring the total adhered fine ratio Rpt, first, the mass Wt of the lump ore (including the adhered fine) is measured before the water washing process. Next, all the adhered fines adhering to the lump ore are removed by the water washing process, and the mass Wpd (=Wpt) of the removed adhered fines is measured. From this, the total adhered fine ratio Rpt is calculated.
[0029] Residual ratio Rpr and high-temperature reduction rate R 1100 Regarding the relationship between the high-temperature reduction rate R and the residual ratio R, the residual ratio R was varied. 1100The high-temperature reduction rate R 1100 The measurement was performed based on the measurement method described in the paper "Development of a method for evaluating the softening and melting properties of sintered ore" (Hosoya et al., Iron and Steel, Vol. 83 (1997), 97-102), and from the results, the reduction rate at the time when the temperature reached 1100°C was determined as the high-temperature reduction rate R 1100 In this paper, sintered ore is used, but lump ore is used instead of sintered ore, and the high-temperature reduction rate R 1100 The reduction rate R can be measured. 1100 The measurement conditions are as described in the above paper, and the high-temperature reduction rate R 1100 The calculation method is also well known, so a detailed explanation will be omitted here.
[0030] The process of making the remaining ratios Rpr of the lump ores A to D different will be described below.
[0031] First, each lump ore A to D was placed in a dryer and left in an atmosphere at 110°C for one day. After this drying process, each lump ore A to D was shaken using a rotary shaker equipped with a sieve with 2.7 mm mesh to remove the adhering fine particles from each lump ore A to D. Then, the removal rate Rpd of the adhering fine particles removed from each lump ore A to D was measured.
[0032] The removal rate Rpd is the ratio of the mass Wpd of the adhering fines removed by shaking to the mass of the lump ore before shaking with the rotary shaker (corresponding to the mass Wt described above) (Rpd = 100 × (Wpd / Wt)). The removal rate Rpd can be determined by measuring the mass Wt of the lump ore before shaking and the mass Wpd of the adhering fines removed by shaking.
[0033] As described above, the mass Wpd (in other words, the removal rate Rpd) depends on the shaking time of the rotary tap shaker (the above-mentioned removal processing time), so the mass Wpd (removal rate Rpd) can be adjusted by adjusting the shaking time. By adjusting the removal rate Rpd, the remaining rate Rpr of the adhering fines that remain attached to the lump ore can be adjusted. As can be seen from the above formula (2), the remaining rate Rpr is the value obtained by subtracting the removal rate Rpd from the total adhering fines rate Rpt. A plurality of remaining rates Rpr are set for each of the lump ores A to D, and the high-temperature reduction rate R of each of the lump ores A to D is calculated for each remaining rate Rpr. 1100 By measuring the residual ratio Rpr and high-temperature reduction rate R 1100 The following relationship is obtained.
[0034] Figure 2 shows the residual ratio Rpr and high-temperature reduction rate R for each lump ore A to D. 1100 As can be seen from Figure 2, the lower the residual ratio Rpr, the higher the high-temperature reduction rate R 1100 Here, the high-temperature reduction rate R 1100 It was found that the rate of increase in the amount of the sintering, in other words, the gradient of each approximation line shown in FIG. 2, differs depending on the type of lump ore A to D.
[0035] According to Figure 2, for lump ore A, the high-temperature reduction rate R 1100 Among the lump ores A to D, only the lump ore A satisfies the composition described in the embodiment. This shows that performing the removal treatment on the lump ore A is effective in improving the high-temperature reduction properties of the lump ore.
[0036] High-temperature reduction rate R versus decrease in residual ratio Rpr 1100 When only the rate of increase in the high-temperature reduction rate R is considered, lump ores A and D show similar behavior. 1100 When we focus on the high-temperature reduction rate R of lump ore A, 1100 is the high-temperature reduction rate R of lump ore D 1100Therefore, in terms of high-temperature reduction properties, lump ore A is superior to lump ore D. In addition, if the residual ratio Rpr of lump ore A is set to less than 2 mass%, the high-temperature reduction ratio R 1100 This shows that when removing the adhering fines from the lump ore A, it is preferable to set the remaining ratio Rpr to less than 2 mass %.
[0037] The preferable residual ratio Rpr of lump ore A, which is set to less than 2% by mass, is a numerical value expressed by the ratio (the above formula (1)) of the mass Wpr of the adhered fine remaining on lump ore A after the adhered fine removal process to the mass Wt of lump ore A before the adhered fine removal process. When the residual ratio Rpr is defined relative to the mass Wo of the lump ore excluding the adhered fine (i.e., Wt-Wpt), the total adhered fine ratio Rpt of lump ore A is 8.9% by mass, and therefore the residual ratio Rpr is preferably less than 2.2% by mass (=2% by mass / (1-(8.9 / 100))).
Claims
1. SiO 2 The content of Al is 4.5 mass% or less. 2 O 3 The content of is 3% by weight or less, and SiO 2 Al content relative to 2 O 3 The present invention relates to a method for pre-treating lump ore, the method comprising the steps of: removing, from lump ore having a ratio of the content of 0.5 or more, adhering powder having a diameter of 3 mm or less by vibration using a sieve, the adhering powder having a diameter of 3 mm or less, which is subjected to drying treatment by heating before being charged into a blast furnace.
2. 2. The method for pretreating lump ore according to claim 1, further comprising the step of removing the adhering powder until a ratio of the mass of the adhering powder remaining on the lump ore to a mass of the lump ore before the removal of the adhering powder is less than 2 mass%.
3. A method for operating a blast furnace, comprising charging lump ore obtained by the pretreatment method according to claim 1 or 2 into the blast furnace.
Citation Information
Patent Citations
Treatment of washing ore with water and apparatus therefor
JP1995113127A
Method for operating blast furnace
JP2006291255A
Blast furnace operating method
JP2007039747A
Method for manufacturing sintered ore
JP2008261016A
Method for removing powder adhering to lump ore
JP2009149969A