Method for smelting high-titanium vanadium titano-magnetite through hydrogen-rich carbon circulating oxygen blast furnace
By optimizing the charge structure and air supply parameters, combined with full oxygen air volume and coke oven gas control, the problems of high carbon emissions and low smelting efficiency in hydrogen-rich carbon cycle oxygen blast furnace smelting were solved, and efficient high-titanium vanadium-titanium magnets were realized Ore smelting reduces energy consumption and increases productivity.
Patent Information
- Application Number
- CN202410978303.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
AI Technical Summary
The existing technology has the problems of high carbon emissions and low smelting efficiency in smelting high-titanium vanadium-titanium magnetite in a hydrogen-rich carbon circulating oxygen blast furnace, making it difficult to achieve large-scale industrial application.
By determining the charge structure, distribution system, air supply system, thermal system and slagging system, the proportion and composition of vanadium-titanium sinter and vanadium-titanium pellets are optimized, combined with the control of full oxygen air volume and coke oven gas, to achieve efficient smelting.
It reduces carbon emissions, improves smelting intensity and efficiency, realizes efficient and comprehensive utilization of high-titanium vanadium-titanium magnetite, saves energy consumption and increases productivity.
Smart Images

Figure CN118773386A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of smelting high-titanium vanadium-titanium magnetite, and specifically relates to a method for smelting high-titanium vanadium-titanium magnetite in a hydrogen-rich carbon circulating oxygen blast furnace. Background Art
[0003] The oxygen blast furnace is a new type of blast furnace ironmaking process, which has the advantages of greatly reducing the fuel ratio and reducing CO 2 The oxygen blast furnace has the problem of "cold on top and hot on bottom" because the oxygen combustion in the cyclone zone releases a lot of heat, and the reduction in the fuel ratio leads to a decrease in the amount of furnace gas. The top gas circulation injection can provide the required heat for the upper part of the blast furnace, while increasing the flow of furnace gas, effectively solving the problem of "cold on top and hot on bottom" in the oxygen blast furnace. The blast furnace carbon cycle realizes full oxygen smelting, avoiding N 2 After full oxygen blasting, the concentration of reducing gas is close to 100%; the indirect reduction degree of ore is greatly improved. After full oxygen smelting, the working conditions in the blast furnace change dramatically, the fuel ratio is greatly reduced, and new requirements will be put forward for the performance of the charge.
[0004] In the existing technology, there are many theoretical studies on the blast furnace hydrogen-rich carbon cycle, but relatively few experimental studies. Sweden 9m 3 The experimental blast furnace has been studied, and Japan NKK Company 4Nm 3 The ULCOS project was carried out in 2007 at the 9m 3 The experimental blast furnace was tested for seven consecutive weeks to spray circulating gas in the hearth and the furnace body. The experimental blast furnace used two rows of tuyere at the bottom of the hearth and the furnace body. The circulating gas volume at the hearth tuyere was 550m 3 / t (1250℃), the circulating gas volume at the lower tuyere of the furnace is about 550m 3 / t (1000℃), the coal injection ratio is kept at 170kg / t, the coke ratio is reduced from 400-405 kg / t to 260-265kg / t, and the carbon consumption is reduced by 24%. Japan's COURSE50 low-carbon ironmaking technology project adopts a completely different gas injection and top gas circulation process. In 2015, a 12m2 coal injection furnace was built at the Kimitsu Plant of Nippon Steel & Sumitomo Metal Corporation. 3 The experimental blast furnace has three types of tuyere: hearth tuyere, lower tuyere and upper tuyere. The hearth tuyere and lower tuyere of the furnace body inject coke oven gas or reformed coke oven gas, and the upper tuyere of the furnace body injects top gas heated by partial spontaneous combustion to control the temperature of the furnace charge, thereby controlling the reduction rate of the furnace charge. The process test was successful and achieved the expected purpose.
[0005] Although the technology has shown significant effects in reducing carbon emissions and improving efficiency during the trial phase, most of these technologies are still in the laboratory or small-scale trial phase. The transformation from trial to industrial large-scale application faces many challenges, such as technology maturity, equipment investment cost, safety assessment and operational stability. Summary of the invention
[0006] A technical problem to be solved by the present invention is to provide a method for full oxygen hydrogen-rich carbon cycle based on blast furnace smelting of high-titanium vanadium-titanium magnetite, aiming to further improve the smelting intensity on the basis of reducing carbon emissions and realize the efficient comprehensive utilization of high-titanium vanadium-titanium magnetite.
[0007] In order to solve the above technical problems, on the one hand, the present invention provides a method for smelting high-titanium vanadium-titanium magnetite in a hydrogen-rich carbon cycle oxygen blast furnace, the method comprising: S1. Determine the charge structure; S2. Determine the cloth system; S3. Determine the air supply system; S4. Determine the thermal regime; S5. Determine the slag making system; S6. Smelting high-titanium vanadium-titanium magnetite based on parameters related to S1-S5; The charge structure includes ore, and the ore includes vanadium-titanium sinter and vanadium-titanium pellet. In terms of mass percentage, vanadium-titanium sinter accounts for 10% to 70%, and vanadium-titanium pellet accounts for 90% to 30%. Moreover, the mass percentage of vanadium-titanium magnetite contained in the vanadium-titanium sinter and vanadium-titanium pellet is greater than 65%.
[0008] In some embodiments, in the vanadium-titanium sintered ore, by mass percentage, vanadium-titanium concentrate accounts for 0-45%, imported ore accounts for 5-15%, the total iron content is 49-51%, the titanium dioxide content is 5-7%, the vanadium pentoxide content is 0.2-0.5%, and the remainder is additives and auxiliary agents.
[0009] In some embodiments, in terms of mass percentage, vanadium-titanium concentrate accounts for 95-99% of the vanadium-titanium pellets, and flux and bentonite account for 1-5%; the titanium dioxide content in the vanadium-titanium pellets is 9-11%, and the vanadium pentoxide content is 0.5-0.7%. It should be noted that titanium dioxide in vanadium-titanium pellets refers to the titanium dioxide content in the entire vanadium-titanium pellets, and the vanadium pentoxide content is also the mass percentage of vanadium pentoxide in the vanadium-titanium pellets, which is two evaluation systems with vanadium-titanium concentrate, flux and bentonite. In some embodiments, the basicity of vanadium-titanium sinter is 1.9-2.7, and the basicity of vanadium-titanium pellets is 0.2-1.3.
[0010] In some embodiments, the charge structure also includes coke and coke diced, and S2 includes: the charge structure in S1 has a charge rate of 5~10 batches / h, an ore batch weight of 40~45t / batch, a coke and coke diced batch weight of 5~12t / batch, a coke load of 4.0~5.0t / t, and a charging coke and ore charge line depth of 1.5m~2.1m.
[0011] In some embodiments, S3 includes determining the air inlet area, the air inlet area is 0.2-0.3m 2 .
[0012] In some embodiments, S3 also includes determining the gas injected into the system and its injection amount, specifically including: injecting the gas into the circulation to capture and remove CO 2 The gas after the injection is 400~800m 3 / t molten iron, coke oven gas volume is 50~350Nm 3 / t molten iron.
[0013] In some embodiments, S3 also includes determining air supply parameters, the air supply parameters include: the total oxygen air volume is 15000~20000m 3 / t molten iron, wind temperature 1200~1260℃, wind pressure 370~380kPa, wind speed 250~260m / s, blast kinetic energy 160~180kJ / s, coal injection ratio 80~150kg / t, furnace top temperature 140~170℃, furnace top pressure 190~220kPa.
[0014] In some embodiments, S4 includes determining the system molten iron temperature state and the system element content state, the system molten iron temperature state includes: the molten iron temperature in the system is maintained at 1420~1480℃, the system element content state includes: in terms of mass percentage, the V content in the system is maintained at 0.2~0.6%, the Ti content is 0.10~0.40%, the Si content is 0.10~0.40% and the S content is 0.05~0.20%.
[0015] In some embodiments, S5 includes determining slag parameters, wherein the slag parameters include a binary basicity R2 of 1.0-1.2, a ternary basicity R3 of 1.3-1.5, a CaO content of 23-28% by mass, and a TiO 2 The content is 18~35%, V 2 O 5 The content is 0.2~1.0%, the magnesium-aluminum ratio is 0.5~0.9, and the slag-iron ratio is 510~580kg / t.
[0016] The beneficial effects of the present invention include at least: The present invention can further improve the smelting intensity on the basis of reducing carbon emissions, realize the efficient comprehensive utilization of high-titanium vanadium-titanium magnetite, save energy consumption, improve yield, and further realize the efficient smelting of vanadium-titanium ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] For a more complete understanding of embodiments of the present invention, reference should be made to the embodiments illustrated in more detail in the accompanying drawings and described below by way of example, in which: Figure 1 A flow chart of a method for smelting high-titanium vanadium-titanium magnetite in a hydrogen-carbon cycle oxygen blast furnace provided by some embodiments of the present invention is shown. DETAILED DESCRIPTION
[0018] Embodiments of the present invention are described below. However, it should be understood that the disclosed embodiments are merely examples, and other embodiments may take various alternative forms. The drawings are not necessarily drawn to scale; certain features may be exaggerated or minimized to show the details of a particular component. Therefore, the specific structural and functional details disclosed herein should not be interpreted as limiting, but merely as a representative basis for teaching those skilled in the art to use the present invention in various ways. As will be understood by those skilled in the art, the various features shown and described with reference to any one of the figures may be combined with the features shown in one or more other figures to produce embodiments that are not explicitly shown or described. The combination of features shown provides representative embodiments for typical applications. However, various combinations and modifications of features consistent with the teachings of the present invention may be desirable for certain specific applications or embodiments.
[0019] Furthermore, in this document, the terms "comprises," "comprising," or any other variation thereof, are intended to cover a non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but may also include elements not expressly listed or inherent to such process, method, article, or apparatus.
[0020] One or more embodiments of the present invention will be described below in conjunction with the accompanying drawings. The flowchart illustrates the process performed by the system according to the present invention. It is understood that the execution of the flowchart does not need to be performed in sequence, one or more steps may be omitted, one or more execution steps may be added, and one or more steps may be performed in sequence or in reverse order, and even in some embodiments, one or more steps may be performed simultaneously.
[0021] In the present invention, "content" refers to "mass percentage", such as a [V] content of 0.36% means that the mass of V in the liquid iron accounts for 0.36% of the entire iron, or a CaO content of 25.3% means that the mass of CaO in the slag accounts for 25.3% of the mass of the entire slag, and so on.
[0022] In the present invention, the total iron content (TFe) in the vanadium-titanium sinter refers to the content of iron in the vanadium-titanium concentrate, imported ore and other additives of the vanadium-titanium sinter, and the content is by mass.
[0023] In the present invention, the imported ore is the imported ore conventionally used in the art, such as South African ore, etc., which will not be described in detail here.
[0024] In the art, sintered ore contains not only iron but also silicon dioxide (SiO 2 ), calcium oxide (CaO), magnesium oxide (MgO), aluminum oxide (Al 2 O 3 ), vanadium pentoxide (V 2 O 5 ), titanium dioxide (TiO 2 ) and other ingredients.
[0025] The high-titanium vanadium-titanium magnetite in the present invention refers to titanium dioxide (TiO 2 ) content range is about 10% or more vanadium-titanium magnetite concentrate.
[0026] In this field, additives and auxiliary agents are generally fluxes such as limestone and activated ash, etc., containing oxides of elements such as Ca, Si, and Mg.
[0027] like Figure 1 As shown, the present invention provides a method for smelting high-titanium vanadium-titanium magnetite in a hydrogen-rich carbon circulating oxygen blast furnace, comprising: S1. Determine the charge structure; S2. Determine the cloth system; S3. Determine the air supply system; S4. Determine the thermal regime; S5. Determine the slag making system; S6. Smelting high-titanium vanadium-titanium magnetite based on parameters related to S1-S5; The charge structure includes ore, and the ore includes vanadium-titanium sinter and vanadium-titanium pellet. In terms of mass percentage, vanadium-titanium sinter accounts for 10% to 70%, and vanadium-titanium pellet accounts for 90% to 30%. Moreover, the mass percentage of vanadium-titanium magnetite contained in the vanadium-titanium sinter and vanadium-titanium pellet is greater than 65%.
[0028] The present invention realizes the effective recovery and utilization of vanadium, titanium and other elements in high-titanium vanadium-titanium magnetite by limiting the ratio of specific vanadium-titanium sintered ore and vanadium-titanium pellets, so that the content of titanium dioxide in the slag is higher than 18%. At the same time, the chemical reaction balance in the furnace is optimized, the overall efficiency of the smelting process and product quality are improved, and energy consumption is reduced.
[0029] In some embodiments, in the vanadium-titanium sintered ore, by mass percentage, vanadium-titanium concentrate accounts for 0-45%, imported ore accounts for 5-15%, the total iron content is 49-51%, the titanium dioxide content is 5-7%, the vanadium pentoxide content is 0.2-0.5%, and the remainder is additives and auxiliary agents.
[0030] By precisely controlling the proportions of various components in vanadium-titanium sintered ore, especially the contents of vanadium-titanium concentrate and imported ore, the present invention not only ensures the appropriate reduction performance of the charge, but also promotes the efficient extraction of elements such as vanadium and titanium, reduces the residual harmful impurities, and improves the comprehensive utilization rate of resources.
[0031] In some embodiments, by mass percentage, the vanadium-titanium concentrate accounts for 95-99% of the vanadium-titanium pellets, and the flux and bentonite account for 1-5%; the titanium dioxide content in the vanadium-titanium pellets is 9-11%, and the vanadium pentoxide content is 0.5-0.7%.
[0032] By strictly regulating the composition of vanadium-titanium pellets, the present invention ensures good reducibility and fluidity of the pellets in the blast furnace, improves the reactivity of the pellets, thereby enhancing the heat utilization efficiency and uniformity of chemical reactions in the blast furnace, and helps to increase molten iron production.
[0033] In some embodiments, the basicity of the vanadium-titanium sintered ore is 1.9-2.7, and the basicity of the vanadium-titanium pelletized ore is 0.2-1.3.
[0034] In some embodiments, the basicity of the vanadium-titanium sintered ore is 1.9-2.55, and the basicity of the vanadium-titanium pelletized ore is 0.2-1.27.
[0035] The purpose of limiting the basicity range of vanadium-titanium sinter and vanadium-titanium pellets is to optimize the physical and chemical properties of the slag, ensure that the slag has good fluidity, desulfurization and dephosphorization capabilities, and protection of the furnace lining. It is also conducive to maintaining stable operating conditions in the furnace, reducing energy consumption and improving production stability.
[0036] In some embodiments, the charge structure also includes coke and coke diced, and S2 includes: the charge structure in S1 has a charge rate of 5~10 batches / h, an ore batch weight of 40~45t / batch, a coke and coke diced batch weight of 5~12t / batch, a coke load of 4.0~5.0t / t, and a charging coke and ore charge line depth of 1.5m~2.1m.
[0037] Through the carefully designed charge structure and charge distribution system, including charge rate, batch weight, coke load and charge line depth, the present invention not only optimizes the gas distribution and heat exchange in the furnace, but also ensures the uniform descent of the charge, improves the thermal energy utilization efficiency and reduces the production cost.
[0038] In some embodiments, the air supply system in S3 includes determining the air inlet area, and the air inlet area is 0.2~0.3m 2 .
[0039] By precisely controlling the air inlet area, the present invention can effectively adjust the airflow distribution in the furnace, increase combustion efficiency, reduce local overheating or cooling problems, and provide a guarantee for the stable and efficient operation of the blast furnace.
[0040] In some embodiments, S3 also includes determining the gas injected into the system and its injection amount, specifically including: injecting the gas into the circulation to capture and remove CO 2 The gas after the injection is 400~800m 3 / t molten iron, coke oven gas volume is 50~350Nm 3 / t molten iron.
[0041] In some embodiments, the coke oven gas volume is 70-100 Nm 3 / t molten iron.
[0042] By finely controlling the type and amount of gas injected into the system, the present invention not only significantly improves oxygen utilization and promotes more thorough combustion and reduction reactions, but also effectively controls carbon emissions during the smelting process by introducing coke oven gas and other means, laying the foundation for achieving green and low-carbon production.
[0043] In some embodiments, S3 also includes determining air supply parameters, which include: total oxygen air volume of 15000~20000m3 / t molten iron, wind temperature of 1200~1260℃, wind pressure of 370~380kPa, wind speed of 250~260m / s, blast kinetic energy of 160~180kJ / s, coal injection ratio of 80~150kg / t, furnace top temperature of 140~170℃, and furnace top pressure of 190~220kPa.
[0044] By setting scientific air supply parameters, the present invention ensures high efficiency and low energy consumption in a full oxygen smelting environment, while maintaining appropriate furnace top temperature and pressure, creating good conditions for stable operation and optimizing furnace reactions.
[0045] In some embodiments, S4 includes determining the system molten iron temperature state and the system element content state, the system molten iron temperature state includes: the molten iron temperature in the system is maintained at 1420~1480℃, the system element content state includes: in terms of mass percentage, the V content in the system is maintained at 0.2~0.6%, the Ti content is 0.10~0.40%, the Si content is 0.10~0.40% and the S content is 0.05~0.20%.
[0046] By precisely controlling the temperature state and element content of molten iron, the present invention not only ensures the quality of molten iron and meets subsequent processing requirements, but also effectively controls the content of harmful elements, reduces post-processing costs, and improves the economic benefits and environmental protection level of the entire steel production chain.
[0047] In some embodiments, S5 includes determining slag parameters, the slag parameters including slag binary basicity R 2 is 1.0~1.2, ternary basicity R 3 is 1.3~1.5, in terms of mass percentage, the CaO content is 23~28%, and the TiO 2 The content is 18~35%, V 2 O 5 The content is 0.2~1.0%, the magnesium-aluminum ratio is 0.5~0.9, and the slag-iron ratio is 510~580kg / t.
[0048] In some embodiments, the dibasic basicity R 2 is 1.0~1.1, ternary basicity R 3 It is 1.45~1.5.
[0049] By optimizing the slag parameters, the present invention not only improves the recycling rate of resources, but also ensures the environmental friendliness of the slag, which meets the requirements of green and sustainable development of the modern steel industry.
[0050] In some specific embodiments, the method of smelting high-titanium vanadium-titanium magnetite in a hydrogen-rich carbon cycle oxygen blast furnace of the present invention is as follows: S1. Determine the charge structure In some embodiments, the charge structure that can be smelted in the present invention can be specifically the following: ① The charge structure is 70% vanadium-titanium sintered ore + 30% vanadium-titanium pelletized ore, of which vanadium-titanium concentrate accounts for 35-45% of the vanadium-titanium sintered ore, imported ore accounts for 5-10%, TFe content is 49-50%, TiO 2 The content is 5~7%, V 2 O 5 The content is 0.2~0.5%, the basicity is 2.0~2.3, and the drum index is 75~80%. The vanadium titanium concentrate accounts for 95~99% of the vanadium titanium pellets. 2 The content is 9~11%, V 2 O 5 The content is 0.5~0.7%, the basicity is 0.2~0.3. The proportion of vanadium-titanium magnetite entering the furnace is 65.10%.
[0051] ② The charge structure is 50% vanadium-titanium sintered ore + 50% vanadium-titanium pelletized ore, of which vanadium-titanium concentrate accounts for 20-25% of the vanadium-titanium sintered ore, imported ore accounts for 5-10%, TFe content is 49.5-50.5%, TiO 2The content is 2.8~3.0%, V 2 O 5 The content is 0.1~0.2%, the basicity is 1.9~2.1, and the drum index is 75~80%. The vanadium titanium concentrate accounts for 95~99% of the vanadium titanium pellets. 2 The content is 9~11%, V 2 O 5 The content is 0.5~0.7%, the basicity is 0.2~0.3. The proportion of vanadium-titanium magnetite entering the furnace is 65.44%.
[0052] ③ 45% vanadium-titanium sintered ore + 55% vanadium-titanium pelletized ore, of which vanadium-titanium concentrate accounts for 10-20% of the vanadium-titanium sintered ore, imported ore accounts for 5-10%, TFe content is 50.0-51.0%, TiO 2 The content is 1.9~2.1%, V 2 O 5 The content is 0.1~0.2%, the basicity is 2.1~2.3, and the drum index is 75~80%. The vanadium titanium concentrate accounts for 95~99% of the vanadium titanium pellets. 2 The content is 9~11%, V 2 O 5 The content is 0.5~0.7%, the basicity is 0.2~0.3. The proportion of vanadium-titanium magnetite entering the furnace is 65.42%.
[0053] ④40% vanadium-titanium sintered ore + 60% vanadium-titanium pelletized ore, of which vanadium-titanium concentrate accounts for 1~6% of vanadium-titanium sintered ore, imported ore accounts for 10~15%, TFe content is 49.0~51.0%, TiO 2 The content is 0.7~1.2%, V 2 O 5 The content is 0.1~0.2%, the basicity is 2.2~2.5, and the drum index is 75~80%. The vanadium titanium concentrate accounts for 95~99% of the vanadium titanium pellets. 2 The content is 9~11%, V 2 O 5 The content is 0.5~0.7%, the basicity is 0.2~0.3. The proportion of vanadium-titanium magnetite entering the furnace is 66.03%.
[0054] ⑤10% sintered ore + 90% vanadium-titanium pellets, of which vanadium-titanium concentrate accounts for 0% in the sintered ore, imported ore accounts for 5-10%, TFe content is 49.0-51.0%, TiO 2 The content is 0~0.1%, V 2 O 5 The content is 0%, the basicity is 2.4~2.7, and the drum index is 75~80%. The vanadium titanium concentrate accounts for 95~99% of the vanadium titanium pellets, and TiO 2 The content is 9~11%, V 2 O5 The content is 0.5~0.7%, and the pellets change from acidic to alkaline. The proportion of vanadium-titanium magnetite entering the furnace is >90%.
[0055] The change of charge structure must ensure that the charging grade, slag making system and thermal system remain basically unchanged without affecting the stable operation of the blast furnace. The proportion of vanadium-titanium concentrate in the sintered ore decreases with the increase of the proportion of pelletized ore charging into the furnace.
[0056] S2. Determine the fabric system The S1 material rate is 5~10 batches / h, the ore batch weight is 40~45t / batch, the coke batch weight is 5~12t / batch, and the coke load is 4.0~5.0t / t.
[0057] The cloth matrix is: It is suitable for the charge structure of 70~50% vanadium-titanium sintered ore + 30~50% vanadium-titanium pelletized ore. As the proportion of pellets increases, the maximum ore distribution angle can be slightly reduced, and the depth of coke and ore feed lines is between 1.5m and 2.1m.
[0058] The cloth matrix is: It is suitable for the charge structure of 50~10% vanadium-titanium sintered ore + 50~90% vanadium-titanium pelletized ore. As the proportion of pellets increases, the maximum ore distribution angle can be slightly reduced, and the depth of coke and ore feed lines is between 1.5m and 2.1m.
[0059] S3. Determine the air supply system Air outlet layout: 24 air outlets, air outlet length: 450mm*20+500mm*4, air outlet diameter 120mm*24, air inlet area 0.2~0.3m 2 .
[0060] Cyclic capture and removal of CO 2 The gas is then blown in through the tuyere, with a blowing volume of 400~800m 3 / t molten iron, coke oven gas injection volume 50~350Nm 3 / t molten iron, the composition of coke oven gas is shown in Table 1.
[0061] Air supply parameters: Full oxygen air volume is 15000~20000m 3 / t molten iron, wind temperature 1200~1260℃, wind pressure 370~380kPa, wind speed 250~260m / s, blast kinetic energy 160~180kJ / s, coal injection ratio 80~150kg / t, furnace top temperature 140~170℃, furnace top pressure 190~220kPa, theoretical combustion temperature 1600~2300℃.
[0062] S4. Determine the slag making system Slag binary basicity R2 is 1.0~1.2, ternary basicity R 3 is 1.3~1.5, in terms of mass percentage, the CaO content is 23~28%, and the TiO 2 The content is 18~35%, the V2O5 content is 0.2~1.0%, the magnesium-aluminum ratio is 0.5~0.9, and the slag-iron ratio is 510~580kg / t (content is mass percentage).
[0063] S5. Determine the thermal regime The molten iron temperature is maintained at 1420~1480℃, the [V] content is 0.2~0.6%, the [Ti] content is 0.10~0.40%, the [Si] content is 0.10~0.40%, and the [S] content is 0.05~0.20%.
[0064] S6. Smelting of high-titanium vanadium-titanium magnetite based on parameters related to S1~S5.
[0065] The present invention will be described in detail below by way of examples, but the scope of protection of the present invention is not limited thereto: In the present invention, the coke oven gas composition includes the components shown in Table 1: wherein CmHn is other alkanes except methane, and the remainder is other gases: Table 1. Composition of coke oven gas (volume content, %)
[0066] Unless otherwise specified, the contents of Examples 1 to 3 in the present invention are all in mass percentage.
[0067] Embodiment 1: 1750m 3 Take the charge structure of high-titanium vanadium-titanium magnetite blast furnace smelting 70% vanadium-titanium sintered ore + 30% vanadium-titanium pelletized ore as an example: The vanadium-titanium concentrate accounts for 35%, the imported ore accounts for 8%, the TFe content is 49.6%, and the TiO 2 The content is 6.3%, V 2 O 5 The content of vanadium-titanium sinter and vanadium-titanium concentrate is 0.36%, the basicity is 2.01, and the drum index is 77.5%, accounting for 98%. 2 The content is 9.75%, V 2 O 5 The vanadium-titanium pellets with a content of 0.56% and a basicity of 0.22 are mixed with coke and coke dicing in a furnace structure of 70% vanadium-titanium sintered ore + 30% vanadium-titanium pellets and are placed in a 1750m 3 Blast furnace, hydrogen-rich carbon cycle oxygen blast furnace smelting process coke ratio is 350kg / t. The furnace grade is 51.6%, and the distribution matrix is , the material rate is 8.5 batches / h, the ore batch weight is 44.450t / batch, the coke batch weight is 9.2t / batch, and the coke load is 4.59t / t. The fan-shaped distribution method is realized through the blast furnace distribution chute, the material surface shape is controlled, and the edge and center two airflow patterns are formed. Since the pellet ore has good rolling properties and the natural stack angle is only 24~27°, in the blast furnace distribution process, it is necessary to realize the circular, fixed-point, fan-shaped and other distribution methods through the distribution chute, control the reasonable material surface shape, develop reasonable edge and center two airflow patterns, and control the blast furnace gas utilization rate above 44%.
[0068] 16500m 3 / t of full oxygen air is heated to 1210℃ by the hot blast furnace and sent to the blast furnace through the hot blast duct. The air pressure is 380kPa, the wind speed is 252m / s, and the air inlet area is 0.2714m 2 , kinetic energy of air blowing is 170kJ / s. Circular capture and removal of CO 2 The gas is then blown in through the tuyere, with a blowing volume of 400m 3 / t, and inject (the injection method is to inject the furnace body and the furnace at the same time) coke oven gas, the coke oven gas volume is 70Nm 3 / t. Pulverized coal is injected through the tuyere at a coal injection ratio of 100kg / t. The furnace top temperature is controlled at 140°C, the furnace top pressure is controlled at 210kPa, the pressure difference is controlled at 160kPa, and the average throat temperature is controlled at 130°C. The combustion of coke and pulverized coal participates in the indirect reduction reaction of the high-titanium vanadium-titanium magnetite inside the blast furnace.
[0069] High-titanium vanadium-titanium magnetite undergoes indirect and direct reduction reactions in the blast furnace block zone, soft melting zone, dripping zone, tuyere combustion zone and furnace hearth in turn, generating liquid iron that is discharged from the furnace through the taphole. The temperature of the molten iron is 1450°C, the [V] content is 0.36%, the [Ti] content is 0.24%, the [Si] content is 0.22%, and the [S] content is 0.11%. Slag binary basicity R 2 is 1.07, ternary basicity R 3 is 1.48, CaO content is 25.3%, TiO 2 The content is 21.5%, V 2 O 5 The content is 0.38%, the magnesium-aluminum ratio is 0.62, and the slag-iron ratio is 530kg / t.
[0070] Embodiment 2: 1750m 3 Take the charge structure of high-titanium vanadium-titanium magnetite blast furnace smelting 50% vanadium-titanium sintered ore + 50% vanadium-titanium pelletized ore as an example: The vanadium-titanium concentrate accounts for 21%, the imported ore accounts for 8%, the TFe content is 49.5%, and the TiO 2 The content is 2.9%, V2 O 5 The content of vanadium-titanium sinter and vanadium-titanium concentrate is 0.15%, the basicity is 1.98, and the drum index is 78%, accounting for 98%. 2 The content is 9.75%, V 2 O 5 The vanadium-titanium pellets with a content of 0.56% and a basicity of 0.22 are mixed with coke and coke dicing in a charge structure of 50% vanadium-titanium sintered ore + 50% vanadium-titanium pellets and are placed in a 1750m 3 Blast furnace, hydrogen-rich carbon cycle oxygen blast furnace smelting process coke ratio is 330kg / t. The furnace grade is 51.8%, and the distribution matrix is , the material rate is 8.5 batches / h, the ore batch weight is 44.40t / batch, the coke batch weight is 9t / batch, and the coke load is 4.58t / t. The fan-shaped distribution mode is realized through the blast furnace distribution chute, the material surface shape is controlled, and the edge and center two-way airflow patterns are formed. Develop reasonable edge and center two-way airflow patterns, and the blast furnace gas utilization rate is controlled at more than 44%.
[0071] 16000m 3 / t of full oxygen air is heated to 1210℃ by the hot blast furnace and sent to the blast furnace through the hot blast duct. The air pressure is 380kPa, the wind speed is 252m / s, and the air inlet area is 0.2714m 2 , kinetic energy of air blowing is 170kJ / s. Circular capture and removal of CO 2 The gas is then blown in through the tuyere, with a blowing volume of 500m 3 / t, and inject (the injection method is to inject the furnace body and furnace at the same time) coke oven gas, the coke oven gas volume is 80Nm 3 / t. Pulverized coal is injected through the tuyere at a coal injection ratio of 90kg / t. The furnace top temperature is controlled at 140℃, the furnace top pressure is controlled at 210kPa, the pressure difference is controlled at 160kPa, and the average throat temperature is controlled at 130℃. The combustion of coke and pulverized coal participates in the indirect reduction reaction of the high-titanium vanadium-titanium magnetite inside the blast furnace.
[0072] High-titanium vanadium-titanium magnetite undergoes indirect and direct reduction reactions in the blast furnace block zone, soft melting zone, dripping zone, tuyere combustion zone and furnace hearth in turn, generating liquid iron that is discharged from the furnace through the taphole. The temperature of the iron is 1450°C, the [V] content is 0.32%, the [Ti] content is 0.22%, the [Si] content is 0.21%, and the [S] content is 0.05%. Slag binary basicity R 2 is 1.06, ternary alkalinity R 3 is 1.45, CaO content is 25.5%, TiO 2 The content is 22%, V 2 O 5 The content is 0.35%, the magnesium-aluminum ratio is 0.60, and the slag-iron ratio is 525kg / t.
[0073] Embodiment 3: 1750m 3 Take the charge structure of 10% vanadium-titanium sintered ore + 90% vanadium-titanium pelletized ore in a high-titanium vanadium-titanium magnetite blast furnace as an example: The vanadium-titanium concentrate accounts for 0%, the imported ore accounts for 10%, the TFe content is 49.8%, and the TiO 2 The content is 0.03%, V 2 O 5 The content of vanadium-titanium sinter and vanadium-titanium concentrate is 0%, the basicity is 2.55, and the drum index is 80%, accounting for 98%. 2 The content is 11.0%, V 2 O 5 The vanadium-titanium pellets with a content of 0.68% and a basicity of 1.27 are mixed with coke and coke dicing in a furnace structure of 10% vanadium-titanium sintered ore + 90% vanadium-titanium pellets and are placed in a 1750m 3 Blast furnace, hydrogen-rich carbon cycle oxygen blast furnace smelting process coke ratio is 260kg / t. The furnace grade is 52.82%, and the distribution matrix is , the material rate is 8 batches / h, the ore batch weight is 44.10t / batch, the coke batch weight is 9t / batch, and the coke load is 4.88t / t. The fan-shaped distribution mode is realized through the blast furnace distribution chute, the material surface shape is controlled, and the edge and center two-way airflow patterns are formed. Develop reasonable edge and center two-way airflow patterns, and the blast furnace gas utilization rate is controlled at more than 44%.
[0074] 19000m 3 / t of full oxygen air is heated to 1210℃ by the hot blast furnace and sent to the blast furnace through the hot blast duct. The air pressure is 378kPa, the wind speed is 255m / s, and the air inlet area is 0.2714m 2 , kinetic energy of air blowing is 177kJ / s. Circular capture and removal of CO 2 The gas is then blown in through the tuyere, with a blowing volume of 600m 3 / t, and inject (the injection method is to inject the furnace body and furnace cylinder at the same time) coke oven gas, the coke oven gas volume is 100Nm 3 / t. Pulverized coal is injected through the tuyere at a coal injection ratio of 80kg / t. The furnace top temperature is controlled at 140℃, the furnace top pressure is controlled at 210kPa, the pressure difference is controlled at 160kPa, and the average throat temperature is controlled at 130℃. The combustion of coke and pulverized coal participates in the indirect reduction reaction of high-titanium vanadium-titanium magnetite inside the blast furnace.
[0075] High-titanium vanadium-titanium magnetite undergoes indirect and direct reduction reactions in the blast furnace block zone, soft melting zone, dripping zone, tuyere combustion zone and furnace hearth in turn, generating liquid iron that is discharged from the furnace through the taphole. The temperature of the molten iron is 1450°C, the [V] content is 0.46%, the [Ti] content is 0.23%, the [Si] content is 0.15%, and the [S] content is 0.06%. Slag binary basicity R 2 is 1.01, ternary basicity R 3 is 1.50, CaO content is 20.7%, TiO 2 The content is 31.2%, V 2 O 5 The content is 0.57%, the magnesium-aluminum ratio is 0.75, and the slag-iron ratio is 520kg / t.
[0076] Other iron ores with a charge structure of 70-10% vanadium-titanium sintered ore + 30-90% vanadium-titanium pellets enter the blast furnace. The smelting process is the same as in Example 1. Due to the increase in the pellet ratio, in order to ensure the smooth progress of blast furnace smelting, the coke batch weight and the amount of coal injection are adjusted to achieve the maximum distribution angle of the ore during the smelting process, the air volume is increased, and the furnace grade, slag making system, and thermal system are kept unchanged. In the hydrogen-rich carbon cycle oxygen blast furnace smelting under the condition of increasing the proportion of vanadium-titanium pellets entering the furnace, the position of the soft melting zone moves downward, the softening interval becomes wider, and the melting interval becomes narrower. On the whole, the thinning of the soft melting zone thickness will cause a large change in the permeability of the blast furnace charge column, which is very different from the traditional blast furnace smelting of a large proportion of sintered ore, and affects the indirect reduction and direct reduction of the blast furnace charge, and it is necessary to control a reasonable air supply system and thermal system.
[0077] Experimental results analysis: From the data of the above embodiments 1 to 3, it can be concluded that the furnace body and furnace cylinder of the present invention simultaneously spray to remove CO 2 The circulating coal gas can save more than 20% of the carbon in oxygen blast furnaces; the all-oxygen blast furnace coke oven gas injection ironmaking process can save 43% coke, increase 33% coal, and reduce the total fuel ratio by 20% compared with the traditional blast furnace ironmaking process.
[0078] A comprehensive mathematical model of an oxygen blast furnace was established, and calculations were performed based on actual domestic blast furnace operation data. The results showed that compared with traditional blast furnaces, the process fuel consumption rate of the present invention was reduced by 24.7%, the direct reduction degree of the oxygen blast furnace was 0.16, and that of the traditional blast furnace was 0.5.
[0079] A two-dimensional CFD model of a top gas circulating oxygen blast furnace was established to evaluate the effect of circulating gas on the capacity of the oxygen blast furnace. Taking the process of Example 3 as an example, the results showed that when the top gas circulation rate was increased from 300m 3 / tHM increased to 600m 3 / tHM (i.e. the injection volume in Example 3 is 600m 3 / t), the productivity of oxygen blast furnace is 5.3%~35.3% higher than that of traditional blast furnace.
[0080] Because the present invention has industry universality, the blast furnace used in the present invention is not limited to the above-mentioned blast furnace volume, and all volume iron-making blast furnaces are agreed to be within the patent scope of the present invention.
[0081] The present invention document is intended to illustrate how to use the disclosed technology and various embodiments, and is not intended to limit the scope and spirit to which it is actually directed and equivalent. Moreover, the above description is not intended to be exhaustive of all possibilities or to limit the scope of protection to the precise form disclosed. According to the above teachings, changes and variations are possible. The selected and illustrated embodiments provide the best description of the principles of the technology and its practical application, and enable those skilled in the art to use the disclosed technology for various changes in various conceivable specific applications. Therefore, without substantially departing from the spirit and principles of the technology described herein, various changes and modifications made to the above embodiments are intended to be included in the scope of the present invention.
Claims
1. A method for smelting high-titanium vanadium-titanium magnetite in a hydrogen-rich carbon cycle oxygen blast furnace, characterized in that: Methods include: S1. Determine the charge structure; S2. Determine the cloth system; S3. Determine the air supply system; S4. Determine the thermal regime; S5. Determine the slag making system; S6. Smelting high-titanium vanadium-titanium magnetite based on parameters related to S1-S5; The charge structure includes ore, and the ore includes vanadium-titanium sinter and vanadium-titanium pellets, wherein, in terms of mass percentage, the vanadium-titanium sinter accounts for 10% to 70%, and the vanadium-titanium pellets account for 90% to 30%, and the mass percentage of vanadium-titanium magnetite contained in the vanadium-titanium sinter and vanadium-titanium pellets is greater than 65%.
2. The method according to claim 1, characterized in that: In terms of mass percentage, the vanadium-titanium concentrate accounts for 0-45% of the vanadium-titanium sintered ore, the imported ore accounts for 5-15%, the total iron content is 49-51%, the titanium dioxide content is 5-7%, the vanadium pentoxide content is 0.2-0.5%, and the remainder is additives and auxiliary agents.
3. The method according to claim 1, characterized in that In terms of mass percentage, the vanadium-titanium concentrate accounts for 95-99% of the vanadium-titanium pellet, and the flux and bentonite account for 1-5%; the titanium dioxide content in the vanadium-titanium pellet is 9-11%, and the vanadium pentoxide content is 0.5-0.7%.
4. The method according to claim 1, characterized in that The basicity of the vanadium-titanium sintered ore is 1.9-2.7, and the basicity of the vanadium-titanium pelletized ore is 0.2-1.
3.
5. The method according to claim 1, characterized in that The charge structure also includes coke and coke diced, and S2 includes: the charge structure in S1 has a charge rate of 5 to 10 batches / h, the ore batch weight is 40 to 45 t / batch, the coke and coke diced batch weight is 5 to 12 t / batch, the coke load is 4.0 to 5.0 t / t, and the charging coke and ore material line depth is 1.5 m to 2.1 m.
6. The method according to claim 1, characterized in that S3 includes determining the air inlet area, wherein the air inlet area is 0.2-0.3m 2 .
7. The method according to claim 6, characterized in that S3 also includes determining the gas injected into the system and its injection amount, specifically including: injecting the gas after the CO2 is removed by cyclic capture, the gas includes oxygen and coke oven gas, and the injection amount of the gas is 400-800m 3 / t molten iron, the coke oven gas volume is 50~350Nm 3 / t molten iron.
8. The method according to claim 7, characterized in that The step S3 also includes determining air supply parameters, which include: the total oxygen air volume is 15000-20000m 3 / t molten iron, wind temperature 1200~1260℃, wind pressure 370~380kPa, wind speed 250~260m / s, blast kinetic energy 160~180kJ / s, coal injection ratio 80~150kg / t, furnace top temperature 140~170℃, furnace top pressure 190~220kPa.
9. The method according to claim 1, characterized in that: The S4 includes determining the system molten iron temperature state and the system element content state, the system molten iron temperature state includes: the molten iron temperature in the system is maintained at 1420~1480℃, the system element content state includes: in terms of mass percentage, the V content in the system is maintained at 0.2~0.6%, the Ti content is 0.10~0.40%, the Si content is 0.10~0.40% and the S content is 0.05~0.20%.
10. The method according to claim 1, characterized in that The S5 includes determining the slag parameters, which include a binary basicity R2 of 1.0-1.2, a ternary basicity R3 of 1.3-1.5, a CaO content of 23-28%, a TiO2 content of 18-35%, a V2O5 content of 0.2-1.0%, a magnesium-aluminum ratio of 0.5-0.9, and a slag-iron ratio of 510-580 kg / t.
Citation Information
Cited By
Method for smelting vanadium titano-magnetite in blast furnace
CN121555707A
Method for smelting high-titanium vanadium-titanium magnetite by means of hydrogen-enriched carbon-recycling oxygen blast furnace