Pipe threaded joint and method for manufacturing pipe threaded joint
The Zn-Ni alloy plating layer with graphite enhances seizure resistance and maintains high torque, addressing the loosening issue in threaded pipe joints used in horizontal wells, ensuring their integrity and airtightness.
Patent Information
- Application Number
- JP2018157568
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-08-24
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2038-08-24
AI Technical Summary
Existing threaded pipe joints used in horizontal wells experience high stress and friction, leading to loosening and reduced airtightness due to insufficient seizure resistance and loosening prevention, despite previous technologies improving seizure resistance.
A Zn-Ni alloy plating layer containing graphite is applied to the contact surfaces of the pin and box, enhancing seizure resistance and maintaining high torque during unscrewing, thereby preventing loosening.
The Zn-Ni alloy plating layer with graphite improves seizure resistance and maintains high torque, preventing loosening even in high-stress environments like horizontal wells, ensuring the integrity of oil country tubular goods.
Smart Images

Figure 0007553221000008 
Figure 0007553221000003 
Figure 0007553221000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a tubular threaded joint and a method for manufacturing a tubular threaded joint. [Background technology]
[0002] Oil well tubular goods are used for the extraction of oil fields and natural gas fields. Oil well tubular goods are formed by connecting multiple steel pipes according to the depth of the well. The steel pipes are connected by screwing together pipe thread joints formed on the ends of the steel pipes. The oil well tubular goods are pulled up for inspection, etc., unscrewed, and after inspection, screwed again and used again.
[0003] The threaded joint for pipes comprises a pin and a box. The pin includes a male thread portion and an unthreaded metal contact portion formed on the outer peripheral surface of the end of the steel pipe. The box includes a female thread portion and an unthreaded metal contact portion formed on the inner peripheral surface of the end of the steel pipe. The unthreaded metal contact portions each include a metal seal portion and a shoulder portion. When the steel pipes are screwed together, the male thread portion and the female thread portion, the metal seal portions come into contact with each other, and the shoulder portions come into contact with each other.
[0004] The threaded parts and unthreaded metal contact parts of the pin and box are repeatedly subjected to strong friction when the steel pipe is screwed in and out. If these parts do not have sufficient durability against friction, galling (irreparable seizure) will occur when the pipe is repeatedly screwed in and out. Therefore, pipe threaded joints are required to have sufficient durability against friction, i.e., excellent seizure resistance.
[0005] Conventionally, compound greases containing heavy metals have been used to improve seizure resistance. The seizure resistance of tubular threaded joints can be improved by applying compound grease to the surface of the joint. However, heavy metals such as Pb contained in compound grease may have an adverse effect on the environment. For this reason, there is a demand for the development of tubular threaded joints that do not use compound grease.
[0006] A technology relating to a threaded joint that exhibits excellent seizure resistance is proposed in JP 5-149485 A (Patent Document 1). The threaded joint described in Patent Document 1 is characterized in that a dispersion plating layer is formed on the surface of the pin or box, in which one or more nonmetallic phases or other metallic phases are dispersed and co-deposited in a metal matrix. Patent Document 1 states that this makes it possible to obtain a threaded joint that exhibits excellent seizure resistance even when tightening and loosening using a compound grease that does not contain heavy metal components.
[0007] As in Patent Document 1, studies are being conducted to improve seizure resistance by dispersing nonmetallic materials in the plating layer and to improve sliding properties by lowering the friction coefficient.
[0008] The screw member described in JP 2008-214666 A (Patent Document 2) is characterized in that a low-friction composite coating layer containing a carbon nanomaterial and a zinc component is formed on the surface of the substrate. As a result, the screw member has excellent low-friction characteristics under high loads and excellent fastening characteristics that can withstand harsh environments, as described in Patent Document 2.
[0009] The composite plated non-ferrous metal material described in JP-A-5-331694 (Patent Document 3) has a composite plated layer on the surface. The composite plated layer is made of a plated material made of one or more metals selected from the group consisting of Ni, Fe, Co, Cu, Cr, Mn, Sn, and Zn, or one or more of these metals and P, B, and W. In the plated material, one or more hardening particles selected from the group consisting of SiC, Al2O3, Si3N4, WC, TiC, and TiN, and one or more lubricating particles selected from the group consisting of BN, MoS2, fluorine carbide, graphite, and mica are dispersed. This provides a composite plated non-ferrous metal material that is excellent in wear resistance, seizure resistance, lubricity, and corrosion resistance and is useful as a material for machine structural parts having sliding parts and rolling parts, as described in Patent Document 3. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 5-149485 [Patent Document 2] JP 2008-214666 A [Patent Document 3] Japanese Patent Application Publication No. 5-331694 Summary of the Invention [Problem to be solved by the invention]
[0011] Incidentally, in order to improve the recovery rate of oil and natural gas, it is predicted that in the future, horizontal wells will increase in addition to deep wells. A horizontal well is a well that is drilled vertically to the stratum (oil reservoir) where oil and natural gas are buried, and then drilled horizontally or in a direction inclined from the horizontal along the oil reservoir. In fact, in recent years, the length of the horizontal part of a horizontal well has tended to increase. In a horizontal well, the well path changes from vertical to horizontal in the middle of the well. Therefore, at the bend where the well path changes from vertical to horizontal, high stress is applied to the entire oil well pipe. At the bend, high stress is also applied to the tubular thread joint. Furthermore, in the drilling work of a horizontal well, it is necessary to push the oil well pipe into the well while rotating it in the circumferential direction. If it rotates under high stress, the tubular thread joint is likely to loosen. If the tubular thread joint loosens, the airtightness of the oil well pipe decreases. Therefore, it is required that the tubular thread joint does not loosen easily even when used in a horizontal well.
[0012] The techniques disclosed in Patent Documents 1 to 3 can improve the seizure resistance of tubular threaded joints. However, even when the techniques disclosed in Patent Documents 1 to 3 are used, there are cases where loosening of tubular threaded joints cannot be sufficiently suppressed when used in horizontal wells.
[0013] An object of the present invention is to provide a tubular threaded joint that has excellent seizure resistance and is furthermore inhibited from loosening even when used in a horizontal well, and a method for manufacturing the same. [Means for solving the problem]
[0014] The threaded joint for pipes of this embodiment includes a pin, a box, and a Zn-Ni alloy plating layer. The pin has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The box has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The Zn-Ni alloy plating layer is disposed on at least one of the contact surface of the pin and the contact surface of the box. The Zn-Ni alloy plating layer contains graphite.
[0015] The manufacturing method for a tubular threaded joint of this embodiment includes a preparation step and a plating step. In the preparation step, a pin, a box, and a plating solution are prepared. The pin has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The box has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The plating solution contains zinc ions, nickel ions, and graphite. In the plating step, at least one of the contact surface of the pin or the contact surface of the box is brought into contact with the plating solution, and a Zn-Ni alloy plating layer is formed on at least one of the contact surface of the pin or the contact surface of the box by electroplating. Effect of the Invention
[0016] The tubular threaded joint of this embodiment manufactured by the above-described manufacturing method has excellent seizure resistance, and furthermore, loosening is suppressed even when used in a horizontal well. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a diagram showing the results of the Bowden sliding test for test numbers 1, 3 and 7 in the examples. [Diagram 2] FIG. 2 is a diagram showing the configuration of a coupling-type threaded joint for pipes according to the present embodiment. [Diagram 3] FIG. 3 is a diagram showing the configuration of an integral type tubular threaded joint according to the present embodiment. [Figure 4] FIG. 4 is a cross-sectional view of an example of a tubular threaded joint. [Diagram 5] FIG. 5 is a cross-sectional view of an example of a tubular threaded joint according to the present embodiment. [Figure 6] FIG. 6 is a cross-sectional view of an example of a threaded joint for pipes according to another embodiment different from that of FIG. [Figure 7] FIG. 7 is a cross-sectional view of an example of a pipe threaded joint according to another embodiment different from that shown in FIGS. [Figure 8] FIG. 8 is a cross-sectional view of an example of a threaded joint for pipes in which the pin and the box are provided with lubricating coatings. [Figure 9] FIG. 9 is a cross-sectional view of an example of a pipe threaded joint according to another embodiment different from that of FIG. [Figure 10] FIG. 10 is a cross-sectional view of an example of a pipe threaded joint according to another embodiment different from that shown in FIGS. [Figure 11] FIG. 11 is a diagram showing the results of the Bowden sliding test for test numbers 2, 4, and 5 in the examples. [Figure 12] FIG. 12 is a diagram showing the results of the Bowden sliding test for test number 6 and test number 8 in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the present embodiment will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.
[0019] The present inventors have investigated the seizure resistance, friction coefficient, and loosening of tubular threaded joints when used in horizontal wells. As a result, they have obtained the following findings.
[0020] A pipe threaded joint is screwed and unscrewed with a predetermined torque. As described above, the contact surfaces of the pin and the box slide under a high surface pressure of, for example, 1.0 GPa or more when screwing and unscrewing. In other words, the contact surfaces of the pin and the box are subjected to strong friction. If the friction coefficient of the contact surfaces is high, the frictional heat generated during screwing and unscrewing is high, and adhesion and seizure are likely to occur. In the contact between metals, if the friction coefficient exceeds, for example, 0.4, seizure becomes significantly likely. Therefore, in the past, attempts have been made to reduce the friction coefficient of the contact surfaces by applying a lubricant to the contact surfaces or forming a plating layer with a low friction coefficient on the contact surfaces. For example, when a general-purpose API dope is used, the friction coefficient is about 0.05 to 0.2, and seizure is suppressed.
[0021] However, the present inventors have discovered that by increasing the coefficient of friction, the torque can be increased, and thereby loosening of a tubular threaded joint can be suppressed.
[0022] The torque during tightening and unscrewing is proportional to the friction coefficient of the contact surface. In other words, the higher the friction coefficient of the contact surface, the higher the torque during tightening and unscrewing. If a high torque is maintained during unscrewing, a pipe threaded joint that is less likely to come loose can be obtained. Hereinafter, the ability to maintain a high torque during unscrewing is referred to as high torque maintenance characteristic.
[0023] However, as described above, increasing the friction coefficient makes seizure more likely to occur, and therefore it has generally been thought to be difficult to improve both seizure resistance and high torque maintenance characteristics.
[0024] However, the present inventors have discovered that by adding graphite to a specific alloy plating, the seizure resistance is improved and at the same time, the high torque maintaining characteristics are improved.
[0025] FIG. 1 is a diagram showing the results of the Bowden sliding test in the examples. Referring to FIG. 1, the steel plate of test number 7 has a plating layer in which graphite is contained in the conventional Cu plating. When graphite is contained in the conventional Cu plating, the friction coefficient is suppressed to a very low value of about 0.1 up to about 250 sliding cycles due to the lubricating effect of graphite. After that, the Cu plating layer is damaged and peeled off, and the friction coefficient suddenly exceeds 0.4. Therefore, it was found that high torque maintenance characteristics cannot be obtained when graphite is contained in the conventional Cu plating. In addition, the steel plate of test number 1 having a Zn-Ni alloy plating layer not containing graphite had a friction coefficient exceeding 0.4 after two sliding cycles.
[0026] On the other hand, the steel sheet of test number 3 having the graphite-containing Zn-Ni alloy plating layer did not suffer from seizure for a while even after the friction coefficient exceeded 0.2 and reached a high friction coefficient, and the friction coefficient exceeded 0.4 after 100 or more sliding cycles. In other words, if the Zn-Ni alloy plating layer contained graphite, a high friction coefficient of about 0.2 to 0.4 was maintained without seizure. From this, the present inventors found that it is only by including graphite in the Zn-Ni alloy plating layer that it is possible to improve the seizure resistance and the high torque maintenance characteristic at the same time.
[0027] When the Zn-Ni alloy plating layer contains graphite, the reason why it shows high torque retention property instead of conventionally known lubricity is unclear. However, in the examples, peeling of the plating layer was confirmed after the test in the steel plate of test number 7 having the Cu plating containing graphite and the steel plate of test number 1 having the Zn-Ni alloy plating layer not containing graphite. On the other hand, it was confirmed that more plating layers remained after the test in the steel plates of test numbers 2 to 5 having the Zn-Ni alloy plating layer containing graphite. Therefore, when graphite is contained in the Zn-Ni alloy plating layer, it is possible that it suppresses peeling of the Zn-Ni alloy plating layer. In addition, the Zn-Ni alloy plating has a higher hardness than the conventional Cu plating. If the hardness is high, the resistance to the stress applied when sliding at a significantly high surface pressure (for example, 1.0 GPa or more) during screw tightening is high. Therefore, it is possible that the high friction coefficient was maintained by sliding with more of the Zn-Ni alloy plating layer remaining, which has a higher resistance to sliding.
[0028] The present embodiment of a threaded joint for pipes, which has been completed based on the above findings, comprises a pin, a box, and a Zn-Ni alloy plating layer. The pin has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The box has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The Zn-Ni alloy plating layer is disposed on at least one of the contact surface of the pin or the contact surface of the box. The Zn-Ni alloy plating layer contains graphite.
[0029] The tubular threaded joint of this embodiment is provided with a Zn-Ni alloy plating layer. Therefore, the tubular threaded joint has excellent galling resistance. Furthermore, the Zn-Ni alloy plating layer contains graphite. Therefore, the high torque retention characteristics are improved, and the tubular threaded joint is less likely to loosen even when used in a horizontal well. In this specification, a plating layer consisting of a Zn-Ni alloy, graphite, and impurities is referred to as a Zn-Ni alloy plating layer.
[0030] Preferably, the Zn-Ni alloy plating layer contains 5 to 35 at % of Ni, assuming that the entire chemical composition of the Zn-Ni alloy plating layer is 100 at %.
[0031] In this case, the hardness of the Zn-Ni alloy plating layer is increased.
[0032] Preferably, the Zn-Ni alloy plating layer contains 30 to 60 at % of graphite when the entire chemical composition of the Zn-Ni alloy plating layer is taken as 100 at %.
[0033] In this case, the high torque retention characteristics are further improved, making the tubular threaded joint even more resistant to loosening.
[0034] The Zn-Ni alloy plating layer may have a thickness of 1 to 50 μm.
[0035] The above-mentioned threaded joint for pipes may further comprise a lubricating coating on at least one selected from the group consisting of a contact surface of the pin, a contact surface of the box, and a Zn-Ni alloy plating layer.
[0036] In this case, the lubricity of the tubular threaded joint is improved.
[0037] The manufacturing method for a tubular threaded joint of this embodiment includes a preparation step and a plating step. In the preparation step, a pin, a box, and a plating solution are prepared. The pin has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The box has a contact surface including a threaded portion, a metal seal portion, and a shoulder portion. The plating solution contains zinc ions, nickel ions, and graphite. In the plating step, at least one of the contact surface of the pin or the contact surface of the box is brought into contact with the plating solution, and a Zn-Ni alloy plating layer is formed on at least one of the contact surface of the pin or the contact surface of the box by electroplating.
[0038] The threaded joint for pipes and the method for producing the same according to the present embodiment will be described in detail below. In the following description, at % refers to atomic composition percentage.
[0039] [Pipe threaded joints] The tubular threaded joint comprises a pin and a box. Fig. 2 is a diagram showing the configuration of a coupling-type tubular threaded joint according to this embodiment. Referring to Fig. 2, the tubular threaded joint comprises a steel pipe 1 and a coupling 2. At both ends of the steel pipe 1, a pin 3 having a male thread portion on its outer surface is formed. At both ends of the coupling 2, a box 4 having a female thread portion on its inner surface is formed. The coupling 2 is attached to the end of the steel pipe 1 by screwing the pin 3 and the box 4 together.
[0040] On the other hand, an integral type oil well pipe threaded joint may be used in which a pin 3 is provided at one end of a steel pipe 1 and a box 4 is provided at the other end without using a coupling 2. FIG. 3 is a diagram showing the configuration of an integral type tubular threaded joint according to this embodiment. Referring to FIG. 3, the tubular threaded joint includes a steel pipe 1. A pin 3 having a male thread portion on its outer surface is formed at one end of the steel pipe 1. A box 4 having a female thread portion on its inner surface is formed at the other end of the steel pipe 1. The steel pipes 1 can be connected to each other by screwing the pin 3 and the box 4 together. The tubular threaded joint of this embodiment can be used for both coupling type and integral type tubular threaded joints.
[0041] The pin 3 and the box 4 each have a contact surface having a threaded portion, a metal seal portion, and a shoulder portion. FIG. 4 is a cross-sectional view of a pipe threaded joint. Referring to FIG. 4, the pin 3 has a male threaded portion 31, a metal seal portion 32, and a shoulder portion 33. The box 4 has a female threaded portion 41, a metal seal portion 42, and a shoulder portion 43. The portions that come into contact when the pin 3 and the box 4 are screwed together are called the contact surfaces 34 and 44. Specifically, when the pin 3 and the box 4 are screwed together, the threaded portions (the male threaded portion 31 and the female threaded portion 41), the metal seal portions (the metal seal portions 32 and 42), and the shoulder portions (the shoulder portions 33 and 43) come into contact with each other. That is, the contact surface 34 includes the threaded portion 31, the metal seal portion 32, and the shoulder portion 33. The contact surface 44 includes the threaded portion 41, the metal seal portion 42, and the shoulder portion 43.
[0042] In FIG. 4, in the pin 3, the shoulder portion 33, the metal seal portion 32, and the male thread portion 31 are arranged in this order from the end of the steel pipe 1. In addition, in the box 4, the female thread portion 41, the metal seal portion 42, and the shoulder portion 43 are arranged in this order from the end of the steel pipe 1 or the coupling 2. However, the arrangement of the thread portions 31 and 41, the metal seal portions 32 and 42, and the shoulder portions 33 and 43 is not limited to the arrangement in FIG. 4 and can be changed as appropriate. For example, as shown in FIG. 3, in the pin 3, the male thread portion 31, the metal seal portion 32, the shoulder portion 33, the metal seal portion 32, and the male thread portion 31 may be arranged in this order from the end of the steel pipe 1. In the box 4, the female thread portion 41, the metal seal portion 42, the shoulder portion 43, the metal seal portion 42, and the female thread portion 41 may be arranged in this order from the end of the steel pipe 1 or the coupling 2. In addition, the contact surfaces 34 and 44 may not have the shoulder portions 33 and 43.
[0043] [Zn-Ni alloy plating layer] The Zn-Ni alloy plating layer 100 is disposed on at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4. The Zn-Ni alloy plating layer 100 is composed of a Zn-Ni alloy, graphite, and impurities. The Zn-Ni alloy contains zinc (Zn) and nickel (Ni). The Zn-Ni alloy may contain impurities. Here, the impurities in the Zn-Ni alloy plating layer 100 and the impurities in the Zn-Ni alloy include substances other than Zn, Ni, and graphite that are contained in the Zn-Ni alloy plating layer 100 or the Zn-Ni alloy during the manufacture of a tubular threaded joint, etc., and include substances contained in an amount that does not affect the effects of the present invention.
[0044] The Ni content in the Zn-Ni alloy plating layer 100 is not particularly limited. However, when the entire chemical composition of the Zn-Ni alloy plating layer 100 is taken as 100 at%, if the Ni content in the Zn-Ni alloy plating layer 100 is 5 to 35 at%, the hardness of the Zn-Ni alloy plating layer 100 is increased. Therefore, when the entire chemical composition of the Zn-Ni alloy plating layer 100 is taken as 100 at%, the Zn-Ni alloy plating layer 100 preferably contains 5 to 35 at% Ni. The lower limit of the Ni content in the Zn-Ni alloy plating layer 100 is more preferably 10 at%. The upper limit of the Ni content in the Zn-Ni alloy plating layer 100 is more preferably 30 at%.
[0045] Zinc (Zn) contained in the Zn-Ni alloy plating layer 100 is a less noble metal than iron (Fe), the main component of steel pipes, and therefore has a sacrificial corrosion protection effect, enhancing the corrosion resistance of the tubular threaded joint.
[0046] [Graphite] Graphite is a material formed by laminating sheets (graphene) in which carbon atoms are bonded in a hexagonal lattice pattern. Graphite contains carbon (C), with the remainder being impurities. Since the bonding strength between graphene layers is weak, graphene is easily peeled off from between the layers. For this reason, graphite is generally used as a lubricant. However, in this embodiment, if the Zn-Ni alloy plating layer 100 contains graphite, the high torque retention characteristics are improved and loosening of the tubular threaded joint is suppressed.
[0047] [Graphite content] The graphite content in the Zn-Ni alloy plating layer 100 is not particularly limited. However, when the entire chemical composition of the Zn-Ni alloy plating layer 100 is taken as 100 at%, if the graphite content is 30 at% or more, the high torque retention characteristic of the Zn-Ni alloy plating layer 100 is further improved. In this case, the loosening of the tubular threaded joint is further suppressed even when used in a horizontal well. On the other hand, when the entire chemical composition of the Zn-Ni alloy plating layer 100 is taken as 100 at%, if the graphite content is 60 at% or less, a normal Zn-Ni alloy plating layer 100 is stably formed. Therefore, the graphite content in the Zn-Ni alloy plating layer 100 is preferably 30 to 60 at% when the entire chemical composition of the Zn-Ni alloy plating layer 100 is taken as 100 at%. The lower limit of the graphite content in the Zn-Ni alloy plating layer 100 is more preferably 40 at%. The upper limit of the graphite content in the Zn-Ni alloy plating layer 100 is more preferably 55 at %.
[0048] [Method for measuring Ni content and graphite content in Zn-Ni alloy plating layer] The Ni content and graphite content of the Zn-Ni alloy plating layer 100 are measured by the following method. First, a sample of a pipe threaded joint on which the Zn-Ni alloy plating layer 100 is formed is prepared. An electron beam microanalyzer (FE-EPMA, JXA-8530F manufactured by JEOL Ltd.) is used to perform elemental analysis by EDS (energy dispersive X-ray spectroscopy) on the surface of the Zn-Ni alloy plating layer 100 of the sample. An electron beam is irradiated at a measurement magnification of 1500 to 5000 times, an acceleration voltage of 15 to 30 kV, and a maximum irradiation current of 1 nA, and the X-ray intensities of C-kα rays, Zn-kα rays, and Ni-kα rays are measured. The C content (at%), Zn content (at%), and Ni content (at%) are calculated based on the X-ray intensity of each element. The Ni content (at%) is calculated by dividing the Ni content by the total content of C, Zn, and Ni. The graphite content (at%) is calculated by dividing the C content by the total content of C, Zn, and Ni. The content is measured at three arbitrary points on the surface of the Zn-Ni alloy plating layer 100, and the average content is used.
[0049] [Thickness of Zn-Ni alloy plating layer] The thickness of the Zn-Ni alloy plating layer 100 is not particularly limited. The thickness of the Zn-Ni alloy plating layer 100 is, for example, 1 to 50 μm. If the thickness of the Zn-Ni alloy plating layer 100 is 1 μm or more, sufficient seizure resistance can be stably obtained. Even if the thickness of the Zn-Ni alloy plating layer 100 exceeds 50 μm, the above effect is saturated. The upper limit of the thickness is preferably 20 μm.
[0050] [Method for measuring the thickness of Zn-Ni alloy plating layer] The thickness of the Zn-Ni alloy plating layer 100 is measured by the following method. The thickness of the Zn-Ni alloy plating layer 100 is measured at four points on the contact surface 34 or 44 on which the Zn-Ni alloy plating layer 100 is formed, using an eddy current phase-type thickness gauge PHASCOPE PMP910 manufactured by Helmut Fischer GmbH. The measurement is performed by a method conforming to ISO (International Organization for Standardization) 21968 (2005). The measurement points are four points (0°, 90°, 180°, and 270°) in the pipe circumferential direction of the pipe threaded joint. The arithmetic average of the measurement results is taken as the thickness of the Zn-Ni alloy plating layer 100.
[0051] [Vickers hardness of Zn-Ni alloy plating layer] The higher the hardness of the Zn-Ni alloy plating layer 100, the higher the seizure resistance of the tubular threaded joint. Therefore, the lower limit of the Vickers hardness Hv of the Zn-Ni alloy plating layer 100 is preferably 150, and more preferably 250. The higher the upper limit of the Vickers hardness Hv of the Zn-Ni alloy plating layer 100, the more preferable. The upper limit of the Vickers hardness Hv of the Zn-Ni alloy plating layer 100 is, for example, 600.
[0052] [Method for measuring Vickers hardness of Zn-Ni alloy plating layer] The Vickers hardness of the Zn-Ni alloy plating layer 100 is measured by the following method. A pin 3 or box 4 with the Zn-Ni alloy plating layer 100 is prepared. The pin 3 or box 4 with the Zn-Ni alloy plating layer 100 is cut perpendicularly to the axial direction. The Vickers hardness is measured at any five points on the cross section of the Zn-Ni alloy plating layer 100 according to the method of JIS Z2244 (2009). A microhardness tester Fischer scope HM2000 manufactured by Fischer Instruments Co., Ltd. is used for the measurement. The test temperature is room temperature (25°C), and the test force (F) is 5 to 100 mN. The arithmetic average of three points excluding the maximum and minimum values among the five measurement results obtained is taken as the Vickers hardness Hv of the Zn-Ni alloy plating layer 100.
[0053] [Zn-Ni alloy plating layer arrangement] The Zn-Ni alloy plating layer 100 may be disposed on at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4. In FIG. 5, the Zn-Ni alloy plating layer 100 is disposed on both the contact surface 34 of the pin 3 and the contact surface 44 of the box 4. However, the arrangement of the Zn-Ni alloy plating layer 100 is not limited to FIG. 5. As shown in FIG. 6, the Zn-Ni alloy plating layer 100 may be disposed only on the contact surface 44 of the box 4. Also, as shown in FIG. 7, the Zn-Ni alloy plating layer 100 may be disposed only on the contact surface 34 of the pin 3.
[0054] The Zn-Ni alloy plating layer 100 may be disposed entirely on at least one of the contact surfaces 34 and 44, or may be disposed only partially. The metal seal portions 32 and 42 and the shoulder portions 33 and 43 are subjected to particularly high surface pressure in the final stage of screw fastening. Therefore, when the Zn-Ni alloy plating layer 100 is disposed partially on at least one of the contact surfaces 34 and 44, it may be disposed at at least one of the metal seal portion 32, the metal seal portion 42, the shoulder portion 33 and the shoulder portion 43. On the other hand, if the Zn-Ni alloy plating layer 100 is disposed entirely on at least one of the contact surfaces 34 and 44, the production efficiency of the tubular threaded joint is improved.
[0055] [Lubricating film] The tubular threaded joint of this embodiment exhibits excellent seizure resistance and excellent high torque maintenance characteristics even without lubricating oil, and loosening is suppressed. However, the tubular threaded joint may further include a lubricating coating 200 on at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100. In this case, the lubricity of the tubular threaded joint is improved. As shown in FIG. 8, the lubricating coating 200 may be disposed on both the Zn-Ni alloy plating layer 100 on the contact surface 34 of the pin 3 and the Zn-Ni alloy plating layer 100 on the contact surface 44 of the box 4. However, the arrangement of the lubricating coating 200 is not limited to FIG. 8. The lubricating coating 200 may be disposed only on the Zn-Ni alloy plating layer 100 on the contact surface 34 of the pin 3, or may be disposed only on the Zn-Ni alloy plating layer 100 on the contact surface 44 of the box 4. Also, the lubricating coating 200 may be disposed directly on the contact surface 34 of the pin 3 or on the contact surface 44 of the box 4. For example, as shown in Fig. 9 and Fig. 10, when the Zn-Ni alloy plating layer 100 is not disposed on the contact surface 34 of the pin 3 or on the contact surface 44 of the box 4, the lubricating coating 200 may be disposed directly on the contact surface 34 of the pin 3 or on the contact surface 44 of the box 4.
[0056] The lubricating coating 200 may also be disposed over the entirety of at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100. The lubricating coating 200 may also be disposed over only a portion of at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100.
[0057] The lubricant coating 200 may be in a solid, semi-solid, or liquid state. The lubricant coating 200 may use any known lubricant. The lubricant coating 200 may contain, for example, lubricating particles and a binder. The lubricant coating 200 may contain a lubricant, a solvent, and other ingredients as necessary.
[0058] The lubricating particles are not particularly limited as long as they have lubricity. For example, the lubricating particles may be one or more selected from the group consisting of graphite, MoS2 (molybdenum disulfide), WS2 (tungsten disulfide), BN (boron nitride), PTFE (polytetrafluoroethylene), CFx (graphite fluoride), and CaCO3 (calcium carbonate).
[0059] The binder is, for example, one or two types selected from the group consisting of organic binders and inorganic binders. The organic binder is, for example, one or two types selected from the group consisting of thermosetting resins and thermoplastic resins. The thermosetting resin is, for example, one or more types selected from the group consisting of polyethylene resins, polyimide resins, and polyamideimide resins. The inorganic binder is, for example, one or two types selected from the group consisting of alkoxysilanes and compounds containing siloxane bonds.
[0060] The lubricant is, for example, SEAL-GUARD (trademark) ECF (trademark) manufactured by JET-LUBE Co., Ltd. Other lubricants include, for example, lubricants containing rosin, metal soap, wax, and lubricating powder. The chemical composition of the lubricating coating 200 disposed on the contact surface 34 of the pin 3, the chemical composition of the lubricating coating 200 disposed on the contact surface 44 of the box 4, and the chemical composition of the lubricating coating 200 disposed on the Zn-Ni alloy plating layer 100 may be the same or different.
[0061] The thickness of the lubricating coating 200 is not particularly limited. The thickness of the lubricating coating 200 is, for example, 30 to 300 μm. If the thickness of the lubricating coating 200 is 30 μm or more, the effect of reducing the torque value when the shoulder portions 33 and 43 come into contact with each other during tightening of a tubular threaded joint is enhanced. This makes it easier to adjust the torque value during tightening. Even if the thickness of the lubricating coating 200 exceeds 300 μm, the excess lubricating coating 200 is removed from the contact surfaces 34 and 44 during tightening, so the above effect becomes saturated.
[0062] When the lubricating coating 200 is a solid, the thickness of the lubricating coating 200 is measured by the following method. A pin 3 or box 4 equipped with the lubricating coating 200 is prepared. The pin 3 or box 4 is cut perpendicular to the axial direction of the tube. The cross section including the lubricating coating 200 is observed under a microscope. The magnification of the microscope observation is 500 times. In this way, the thickness of the lubricating coating 200 is determined.
[0063] When the lubricating coating 200 is liquid or semi-solid, the thickness of the lubricating coating 200 is measured by the following method. Any measurement location (area: 5 mm × 20 mm) on the metal seal portion 32 or 42 of a tubular threaded joint is wiped with absorbent cotton soaked in ethanol. The amount of lubricant applied is calculated from the difference in weight of the absorbent cotton before and after wiping. The average film thickness of the lubricating coating 200 is calculated from the amount of lubricant applied, the density of the lubricant, and the area of the measurement location.
[0064] [Arrangement of Zn-Ni alloy plating layer and lubricating coating] As long as the Zn-Ni alloy plating layer 100 is disposed on at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4, and the lubricating coating 200 is disposed on at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100, the combination is not particularly limited. The case where only the Zn-Ni alloy plating layer 100 is provided is called pattern 1. The case where the Zn-Ni alloy plating layer 100 is provided and further the lubricating coating 200 is provided thereon is called pattern 2. The case where only the lubricating coating 200 is provided is called pattern 3. The case where neither the Zn-Ni alloy plating layer 100 nor the lubricating coating 200 is provided is called pattern 4. If the above conditions are satisfied, the contact surface 34 of the pin 3 and the contact surface 44 of the box 4 may be any of the patterns 1 to 4. Specifically, when the contact surface 34 of the pin 3 is pattern 1 or pattern 2, the contact surface 44 of the box 4 may be any of the patterns 1 to 4. Furthermore, when contact surface 34 of pin 3 is pattern 3 or pattern 4, contact surface 44 of box 4 is either pattern 1 or pattern 2. Conversely, when contact surface 44 of box 4 is pattern 1 or pattern 2, contact surface 34 of pin 3 may be any of patterns 1 to 4. Furthermore, when contact surface 44 of box 4 is pattern 3 or pattern 4, contact surface 34 of pin 3 is either pattern 1 or pattern 2.
[0065] [Base material for pipe thread joints] The chemical composition of the base material of the tubular threaded joint is not particularly limited. The base material is, for example, carbon steel, stainless steel, alloy steel, etc. Among alloy steels, high alloy steels such as duplex stainless steel and Ni alloys containing alloy elements such as Cr, Ni, and Mo have high corrosion resistance. Therefore, if these high alloy steels are used as the base material, the corrosion resistance of the tubular threaded joint is increased.
[0066] [Manufacturing method] A method for manufacturing a tubular threaded joint according to the present embodiment is a method for manufacturing the above-described tubular threaded joint. The method for manufacturing a tubular threaded joint includes a preparation step and a plating layer formation step.
[0067] [Preparation process] In the preparation step, the pin 3, the box 4, and the plating solution are prepared. As described above, the pin 3 has a contact surface 34 including the threaded portion 31, the metal seal portion 32, and the shoulder portion 33. As described above, the box 4 has a contact surface 44 including the threaded portion 41, the metal seal portion 42, and the shoulder portion 43. At least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4 may be subjected to a well-known pretreatment. For example, the pretreatment is degreasing. By degreasing, oil and oily dirt adhering to at least one of the contact surfaces 34 and 44 are removed. For example, the degreasing is solvent degreasing, alkaline degreasing, and electrolytic degreasing. As a pretreatment, pickling may be further performed. By pickling, rust on at least one of the contact surfaces 34 and 44 and oxide coatings formed during processing can be removed.
[0068] The plating solution contains zinc ions, nickel ions, and graphite. Zinc ions are contained in the plating solution by dissolving zinc ions and a salt of an anion (e.g., zinc sulfate) in the plating solution. Nickel ions are contained in the plating solution by dissolving nickel ions and a salt of an anion (e.g., nickel sulfate) in the plating solution. The anion is, for example, one or more selected from the group consisting of sulfate ions, chloride ions, and pyrophosphate ions. The plating solution preferably contains 1 to 100 g / L of zinc ions and 1 to 100 g / L of nickel ions.
[0069] The plating solution further contains graphite. In this case, the Zn-Ni alloy plating layer 100 contains graphite. As a result, the high torque retention characteristic of the Zn-Ni alloy plating layer 100 is enhanced, and even when used in a horizontal well, loosening of the tubular threaded joint is suppressed. In the manufacturing method of this embodiment, it is preferable to use powdered graphite. The particle size of the graphite is not particularly limited. The particle size of the graphite is, for example, 0.01 to 30 μm. In consideration of the balance with the dispersibility in the plating solution and the plating film thickness, the more preferable particle size of the graphite particles is 0.01 to 10 μm. The particle size of the graphite particles can be appropriately set within a range in which the graphite particles can be dispersed in the plating solution and the graphite is incorporated into the Zn-Ni alloy plating layer 100.
[0070] When the graphite content in the plating solution is 3 g / L or more, the graphite can be stably incorporated into the Zn-Ni alloy plating layer 100. Therefore, the high torque maintenance characteristic of the Zn-Ni alloy plating layer 100 can be stably improved. On the other hand, when the graphite content in the plating solution is 20 g / L or less, the precipitation of graphite in the plating tank can be suppressed. Therefore, the graphite content in the plating solution is preferably 3 to 20 g / L. The lower limit of the graphite content in the plating solution is more preferably 5 g / L. The upper limit of the graphite content in the plating solution is more preferably 10 g / L.
[0071] [Dispersant] Preferably, the plating solution further contains a dispersant. The dispersant improves the dispersibility of graphite in the plating solution. Preferably, the dispersant is one or two selected from the group consisting of polyacrylic acid and 1-butyl-1-methylpyrrolidinium chloride.
[0072] Polyacrylic acid is a polymer of acrylic acid. The plating solution contains polyacrylic acid by dissolving polyacrylic acid or a salt of polyacrylic acid (e.g., sodium polyacrylate) in the plating solution. The polyacrylic acid is preferably one having a low molecular weight. This can further increase the dispersibility of graphite. The upper limit of the molecular weight of polyacrylic acid is preferably 10,000, more preferably 2,000, in terms of weight average molecular weight. The lower limit of the molecular weight of polyacrylic acid is not particularly limited. The lower limit of the molecular weight of polyacrylic acid is, for example, 1,000, in terms of weight average molecular weight.
[0073] 1-Butyl-1-methylpyrrolidinium chloride (BMP) has the chemical formula CH 20 It is represented by ClN and is classified as a quaternary ammonium ion. + The ionic liquid contains a heterocyclic compound.
[0074] The content of the dispersant in the plating solution is not particularly limited. If a small amount of the dispersant is contained in the plating solution, the dispersibility of the graphite is improved. For example, the content of the dispersant in the plating solution is 1×10 -6 ~1×10 -4 mol / L. If the plating solution contains both polyacrylic acid and 1-butyl-1-methylpyrrolidinium chloride, the respective contents are 1×10 -6 ~1×10 -4 The content (mol / L) of polyacrylic acid refers to the molar concentration relative to the weight average molecular weight.
[0075] The plating solution may contain, as necessary, one or more additives selected from the group consisting of conductive salts, anode dissolution promoters, complexing agents, pH buffers, surfactants, reducing agents, stabilizers, and other additives.
[0076] [Plating layer formation process] In the plating layer forming step, at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4 is brought into contact with the above-mentioned plating solution to form the Zn—Ni alloy plating layer 100 by electroplating.
[0077] The plating device includes, for example, a plating tank, an agitator, a filter, a temperature regulator, an anode plate, and a water washing device. The plating solution is poured into the plating tank, and at least one of the pin 3 and the box 4 and the anode plate are immersed therein. Here, the entire steel pipe 1 or the coupling 2 may be immersed in the plating solution. The entire pin 3 may be immersed in the plating solution, or only the contact surface 34 of the pin 3 may be immersed in the plating solution. The entire box 4 may be immersed in the plating solution, or only the contact surface 44 of the box 4 may be immersed in the plating solution. By passing a current between at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4 and the anode plate, a Zn-Ni alloy plating layer 100 is formed on at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4.
[0078] The conditions in the plating tank, such as temperature, current density, pH, and stirring speed, can be set appropriately. For example, the electroplating conditions are pH of the plating solution: 1 to 10, temperature of the plating solution: 10 to 60° C., current density: 1 to 100 A / dm 2 The stirring speed is 0.1 to 1 m / sec, and the treatment time is 1 to 100 minutes. After the plating step is completed, at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4 is washed with water and dried as necessary. The method of washing with water and drying is not particularly limited.
[0079] [Film forming process] A film-forming step may be carried out after the above-mentioned Zn-Ni alloy plating layer 100 is formed on at least one of the contact surface 34 of the pin 3 and the contact surface 44 of the box 4. In the film-forming step, a lubricating coating 200 is formed on at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100.
[0080] The lubricating coating 200 can be formed by applying the above-mentioned lubricant to at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100. The application method is not particularly limited. Examples of application methods include spray application, brush application, and immersion. When spray application is adopted, the lubricant may be heated and sprayed in a state of increasing fluidity. The lubricating coating 200 may be formed on a part of at least one selected from the group consisting of the contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100. However, it is preferable that the lubricating coating 200 is uniformly formed over the entire contact surface 34 of the pin 3, the contact surface 44 of the box 4, and the Zn-Ni alloy plating layer 100.
[0081] The pipe threaded joint of this embodiment can be manufactured by the above steps. EXAMPLES
[0082] Examples will be described below. In the examples, % means % by mass.
[0083] [Preparation process] In this example, a commercially available cold-rolled steel sheet was used as the base material for the threaded joint. The cold-rolled steel sheet was 150 mm long x 100 mm wide (the plated surface was 100 mm long x 100 mm wide). The steel type was ultra-low carbon steel. The chemical composition of the steel sheet was C: 0.19%, Si: 0.25%, Mn: 0.8%, P: 0.02%, S: 0.01%, Cu: 0.04%, Ni: 0.1%, Cr: 13%, Mo: 0.04%, and the balance: Fe and impurities.
[0084] The plating baths for Test Nos. 1 to 5 had the following compositions. Plating solution: Dynejin Alloy (manufactured by Daiwa Kasei Co., Ltd.) Graphite: TIMREX (trademark) KS6 (IMERYS GRAPHITE & CARBON) 1-10g / L, particle size <100nm (D90) Polyacrylic acid (Sigma-Aldrich), 2 x 10 -5mol / L, molecular weight (Mw) 1800 1-Butyl-1-methylpyrrolidinium chloride (Merck) 2 x 10 -5 mol / L
[0085] The compositions of the plating baths for Test Nos. 6 to 8 were as follows: Plating solution: Copper sulfate pentahydrate 200g / L, sulfuric acid 50g / L (Kishida Chemical Co., Ltd.) Graphite: TIMREX (trademark) KS6 (IMERYS GRAPHITE & CARBON) 1-10g / L, particle size <100nm (D90) Polyacrylic acid (Sigma-Aldrich), 2 x 10 -5 mol / L, molecular weight (Mw) 1800 1-Butyl-1-methylpyrrolidinium chloride (Merck) 2 x 10 -5 mol / L
[0086] [Plating layer formation process] A plating layer was formed on the surface of the steel sheet having each test number under the following conditions. - Plating bath temperature: 25℃ Plating current density: 2A / dm 2 Plating thickness: 5~10μm Stirring speed: 0.4m / sec Plating anode (counter electrode): Insoluble anode (iridium oxide coated Ti plate)
[0087] [Measuring test of plating layer composition] The Ni content (at%) and graphite content (at%) of the steel sheets with each test number on which a plating layer was formed were measured by the method described above. For test numbers 6 to 8, composition analysis was performed by EDX, and the total content of Cu and C was taken as 100 at%, and the percentage of the C content was taken as the graphite content (at%). The results are shown in Table 1.
[0088] [Plating layer thickness measurement test] The thickness of the plating layer was measured for each steel sheet having each test number using the method described above. The results are shown in Table 1.
[0089] [Vickers hardness measurement test for plating layer] For each steel sheet having a coating layer formed thereon, the Vickers hardness (Hv0.005) of the coating layer was measured by the method described above. The results are shown in Table 1.
[0090] [Bowden sliding test] A Bowden sliding test was carried out under the following conditions for the steel sheets with each test number on which a plating layer was formed. The number of sliding cycles at which the friction coefficient (μ) was maintained at 0.2 to 0.4 without causing seizure was counted. The number of sliding cycles is shown in Table 1. The change in the friction coefficient during the test is also shown in Figure 1. ·Steel ball: 3 / 16” SUJ2 Load: 3kgf (Hertz surface pressure: ave.1.5GPa) ·Sliding width: 10mm ·Sliding speed 4mm / s Lubricant: None (unlubricated) Test temperature: Room temperature (25℃)
[0091] [Table 1]
[0092] [Evaluation Results] Figures 11 and 12 are diagrams showing the results of the Bowden sliding test in the examples. With reference to Table 1, Figure 1, Figure 11 and Figure 12, the steel plates of Test Nos. 2 to 5 having a Zn-Ni alloy plating layer containing graphite were subjected to 60 or more sliding cycles while maintaining a high friction coefficient of 0.2 to 0.4 without seizing, exhibiting excellent seizing resistance, and furthermore, exhibiting excellent high torque maintenance characteristics. Therefore, it can be said that the tubular threaded joint has excellent seizing resistance, and is also unlikely to loosen even when used in a horizontal well.
[0093] Furthermore, the steel plates of test numbers 3 to 5, which had a graphite content of 30 to 60 at%, had a higher number of sliding strokes and exhibited even better high torque retention characteristics than the steel plate of test number 2, which had a graphite content of 2.7 at%. In this case, it can be said that the tubular threaded joint is even more difficult to loosen.
[0094] On the other hand, the Zn-Ni alloy plating layer of the steel sheet of test number 1 did not contain graphite, and therefore the number of sliding cycles was only 12, and the high torque retention characteristics and seizure resistance were poor.
[0095] The plating layer of the steel sheet of test number 6 was Cu plating and did not contain graphite, so the number of sliding cycles of the steel sheet of test number 6 was only two, and the high torque retention property and seizure resistance were poor.
[0096] The plating layers of the steel sheets of test numbers 7 and 8 were Cu plating. Therefore, the number of sliding cycles of the steel sheets of test numbers 7 and 8 was low at less than 60, and the high torque retention characteristics and seizure resistance were poor.
[0097] The above describes the embodiments of the present invention. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention. [Explanation of symbols]
[0098] 1 Steel pipe 2 Coupling 3-pin 4. Box 31, 41 Threaded part 32, 42 Metal seal part 33, 43 Shoulder section 34, 44 contact surfaces 100 Zn-Ni alloy plating layer 200 Lubricant coating
Claims
1. A pipe threaded joint, comprising: a pin having a contact surface including a threaded portion, a metal seal portion, and a shoulder portion; a box having a contact surface including a threaded portion, a metal seal portion, and a shoulder portion; a Zn—Ni alloy plating layer disposed on at least one of the contact surface of the pin or the contact surface of the box; The Zn-Ni alloy plating layer contains graphite, When the entire chemical composition of the Zn-Ni alloy plating layer is taken as 100 at%, the Ni content in the Zn-Ni alloy plating layer is 5 to 35 at%, A threaded joint for pipes, wherein the graphite content in the Zn-Ni alloy plating layer is 60 at % or less when the entire chemical composition of the Zn-Ni alloy plating layer is taken as 100 at %.
2. A tubular threaded joint according to claim 1, The Zn-Ni alloy plating layer contains 30 to 60 at % of graphite when the entire chemical composition of the Zn-Ni alloy plating layer is taken as 100 at %.
3. A tubular threaded joint according to claim 1 or 2, A threaded joint for pipes, wherein the Zn-Ni alloy plating layer has a thickness of 1 to 50 μm.
4. A tubular threaded joint according to any one of claims 1 to 3, further comprising: A threaded joint for pipes, comprising a lubricating coating on at least one selected from the group consisting of the contact surface of the pin, the contact surface of the box, and the Zn-Ni alloy plating layer.
5. A method for manufacturing a tubular threaded joint as claimed in claim 1, comprising: Providing a pin having a contact surface including a threaded portion, a metal seal portion, and a shoulder portion, a box having a contact surface including a threaded portion, a metal seal portion, and a shoulder portion, and a plating solution containing zinc ions, nickel ions, and graphite; A method for manufacturing a tubular threaded joint, comprising the step of contacting at least one of the contact surfaces of the pin and the contact surface of the box with the plating solution and forming a Zn-Ni alloy plating layer on at least one of the contact surfaces of the pin and the contact surface of the box by electroplating.
Citation Information
Patent Citations
Threaded joint excellent in seizing resistant property
JP1993149485A
Composite plated nonferrous metallic material for machine structure
JP1993331694A
Screw joint excellent in seizuer resistance
JP1994272791A
Corrosion resisting sliding contact member and its production
JP1994322557A
Screw member and method for manufacturing the same
JP2008214666A