Method for manufacturing a probe suitable for a scanning probe microscope

The self-aligned plasma etching method enhances SPM tip aspect ratios by forming nano-sized tips with a mask layer, addressing the low aspect ratio challenge in current SPM tips, improving resolution and applicability to advanced scanning techniques.

JP7553247B2Active Publication Date: 2024-09-18IMEC VESETWAY +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020031411
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-01
Filing Date
2020-02-27
Publication Date
2024-09-18
Estimated Expiration
2040-02-27

AI Technical Summary

Technical Problem

Current scanning probe microscopy (SPM) tips face challenges with aspect ratios that are too low for sub-10 nm technology nodes, requiring complex fabrication methods to increase resolution.

Method used

A method involving self-aligned plasma etching with a mask layer of irregular thickness, using seed particles, oxycarbide layers, and sputtered particles to form nano-sized tips with higher aspect ratios on a probe tip body, without the need for complex microfabrication.

Benefits of technology

The method produces probes with significantly smaller and more pointed tips, enhancing resolution and suitability for advanced SPM applications, including tiltable SPM heads and 'scalpel AFM' techniques, with a simple and cost-effective manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553247000006
    Figure 0007553247000006
  • Figure 0007553247000008
    Figure 0007553247000008
  • Figure 0007553247000017
    Figure 0007553247000017
Patent Text Reader

Abstract

To manufacture one or more relatively small tips on a relatively large tip body of a probe appropriate for SPM, after manufacturing the probe tip body.SOLUTION: The surface of an Ni core 20 as a probe tip body is coated with a doped diamond layer 21. This diamond layer 21 has an undoped diamond seed particle 3 and an SiOxCy layer 12. When a dry etching process is continued until the diamond layer 21 is removed from a side surface of a pyramid, a diamond having a sufficient thickness remains in a vertex area due to the thickness difference between thicknesses a1 and a2. Thus, one or more sharp tips appear only in the vertex area.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a probe suitable for scanning probe microscopy (SPM) techniques such as atomic force microscopy (AFM) or scanning spreading resistance microscopy (SSRM). [Background technology]

[0002] An SPM probe comprises an elongated strip attached at one end to a holder and carrying a tip at the other end. The strip is referred to as the cantilever of the probe, but the tip may be a pyramidal body placed on the plane of the cantilever, as shown for example in US Pat. No. 5,221,415, so that it points in a direction essentially perpendicular to the cantilever. Alternatively, the tip may extend in the plane of the cantilever, as shown for example in US Pat. No. 8,484,761, or the tip may extend at an angle between 0 and 90 degrees from the cantilever. During SPM acquisition, the tip is placed in contact with or close to a surface and the probe is scanned along a predefined trajectory (usually a series of parallel lines). Depending on the properties of the tip, the interaction between the tip and the surface is converted into topographical, electrical or magnetic data of the surface or into a signal related to the composition of the sample. The probe may be in continuous contact with the surface to be investigated, or an intermittent contact mode may be applied. The surface properties are measured by detecting changes in the impedance (electrical or otherwise) of the probe surface connection. The non-contact mode is equally applicable when the interaction between the probe and the surface is dominated by non-contact forces such as van der Waals forces.

[0003] Various materials have been proposed for the manufacture of tips and cantilevers. Full diamond tips and diamond-coated tips have proven advantageous due to the mechanical and electrical properties of diamond probe material. The dimensions of the apical region of the tip determine the capture resolution. Pyramidal and in-plane tips are available, allowing imaging and characterization of nanoscale surface topography. However, for the new sub-10 nm technology nodes, the aspect ratio of currently available tips becomes too low. It is known, for example from US Pat. No. 6,328,902, to manufacture "tip-on-tip" structures, thereby increasing the aspect ratio of the tip, but the available methods for manufacturing such structures are technically complex. Summary of the Invention

[0004] The present invention aims to provide a technically simple method for manufacturing probe tips with increased aspect ratios. The present invention relates to methods as disclosed in the accompanying claims and to probe tips manufactured by these methods.

[0005] According to the invention, one or more relatively small tips are fabricated on a relatively large tip body of a probe suitable for SPM after fabrication of the probe tip body itself. The relatively small tips are nano-sized tips, but the dimensions of the tip body are on the order of micrometers. The probe tip body can be fabricated by any technique known in the art, for example by filling a mould with a probe material such as diamond. Fabrication of the relatively small tips is achieved by a self-aligned plasma etching process using a mask layer on the outer surface of the probe tip body. The mask layer may comprise nano-sized particles and / or mixtures such as oxides or oxycarbides, which naturally form on the outer surface of the probe tip body or on the outer surface of the mould. The nano-sized particles may be seed particles deposited in the mould before the probe material is deposited in the mould and / or particles generated during the etching process itself, such as particles sputtered from the cantilever or the reaction chamber in which the etching is performed. Alternatively or additionally, masking particles may be intentionally deposited on the probe tip body before the etching process.

[0006] The present invention relates to a method for manufacturing a probe tip, particularly suitable for scanning probe microscopy (SPM), The method comprises: manufacturing a probe tip body having at least one outer layer of probe material; forming a mask layer on the outer layer of probe material during and / or after the manufacturing process of the probe tip body; and subjecting the probe tip body to a plasma etching process, the mask layer acting as an etch mask for etching the probe material, the plasma etching process and the etch mask configured to produce one or more tips formed from the probe material, the one or more tips being significantly smaller and sharper than the probe tip body prior to the plasma etching process.

[0007] According to one embodiment, the mask layer includes a layer having a random thickness formed prior to the plasma etching process, the layer having a random thickness acting as an etch mask for etching the probe material.

[0008] The layer of irregular thickness may comprise a compound that forms naturally, for example by oxidation, on the surface of the probe tip after the manufacturing process of the probe tip and before the plasma etching process.

[0009] The layer of irregular thickness may include particles that are intentionally deposited on the probe tip after the fabrication process of the probe tip and before the plasma etching process.

[0010] According to one embodiment, the probe tip body is manufactured by forming a mold on a substrate and depositing the probe material into the mold, seed particles being deposited on the mold prior to depositing the probe material, and the layer having irregular thickness includes the seed particles.

[0011] According to one embodiment, the layer of irregular thickness further comprises a mixture naturally formed on the surface of the mold.

[0012] According to one embodiment, the etch rate of the layer having the irregular thickness is significantly less than the etch rate of the probe material.

[0013] According to one embodiment, the plasma etching process comprises: a first etching step performed for a first short etching time and configured to generate craters in the layer having irregular thickness; a second etching step performed for a second etching time period significantly longer than the first short etching time period and configured to generate the one or more tips; Includes.

[0014] According to one embodiment, the probe tip is attached to a cantilever, particles of material of the cantilever are sputtered and deposited on the probe tip during the plasma etching process, and the sputtered particles from the cantilever contribute to the formation of the mask layer for the remainder of the plasma etching process.

[0015] According to one embodiment, a plasma etching process is performed in an etching chamber, particles from a material in the chamber are sputtered and deposited on the probe tip body during the etching process, and sputtered particles from a material in the chamber contribute to the formation of the mask layer for the remainder of the etching process.

[0016] According to one embodiment, polymer etch residues generated during the etching process are deposited on the probe tip body, and the etch residues contribute to the formation of the mask layer for the remainder of the etching process.

[0017] According to one embodiment, the etching process includes multiple etching steps performed at different plasma conditions for different etching times.

[0018] At the end of the plasma etching process, the tips may be distributed throughout the probe tip body. According to another embodiment, the probe tip body is pyramidal and at the end of the plasma etching process, the one or more tips are present in an apex region of the probe tip body and no tips are present on the sides of the probe tip body; These have the following effects: A higher concentration of masking particles is deposited at the apex region than at the sides during the plasma etching process. The probe tip body includes a core, and the thickness of the layer of probe material on the core is greater at the apex region than at the sides, so that at the end of the plasma etching process the probe material is removed from the sides. This can be done through one or a combination of the following:

[0019] According to one embodiment, the etching step comprises a single etching step using the same plasma gas or the same plasma gas mixture throughout the process.

[0020] The probe material may be diamond. According to another embodiment, the probe material is titanium nitride (TiN).

[0021] The method of the present invention further comprises the steps of: depositing a cap layer over said one or more tips, thereby completely covering said one or more tips. subjecting the tips to a plasma etching process configured to remove the cap layer from a tip region of the one or more tips, the tip region including an apex of the one or more tips while substantially maintaining the cap layer around a side of the one or more tips. It may further include.

[0022] The invention also relates to a probe tip suitable for a scanning probe microscope, comprising a probe tip body including at least one outer layer of a probe material, with a plurality of tips formed from said probe material distributed throughout said probe tip body, said tips being significantly smaller and sharper than said probe tip body.

[0023] According to one embodiment, the tip comprises a cap layer on an outer surface of the tip except for a tip region, the tip region including the apex of the tip.

[0024] The invention also relates to a probe tip suitable for a scanning probe microscope (SPM), comprising a probe tip body having an apex region and comprising one or more tips at the apex region of the probe tip body, the remainder of the probe tip body being free of tips, the tips being significantly smaller and sharper than the probe tip body, the tips comprising a cap layer on an outer surface of the tip except for the tip region, and the tip region including the apex of the tip.

[0025] The invention also relates to a probe comprising a cantilever, a holder attached to the cantilever, and a probe tip attached to the end of the cantilever, the probe tip being the probe tip according to the invention. [Brief description of the drawings]

[0026] [Figure 1a] FIG. 1a illustrates the method of the invention according to one embodiment, where the probe is manufactured by a molding technique. [Figure 1b] FIG. 1b illustrates the method of the invention according to one embodiment, where the probe is manufactured by a molding technique. [Figure 1c] FIG. 1c illustrates the method of the invention according to one embodiment, where the probe is manufactured by a molding technique. [Figure 1d] FIG. 1d illustrates the method of the invention according to one embodiment, where the probe is manufactured by a molding technique. [Figure 1e] FIG. 1e illustrates the method of the invention according to one embodiment, where the probe is manufactured by a molding technique. [Figure 2a] Figure 2a shows the appearance of the SiOxCy layer formed during the initial stage of diamond growth on a silicon mold. [Figure 2b] Figure 2b shows the appearance of the SiOxCy layer formed during the initial stage of diamond growth on the silicon mold. [Figure 2c] Figure 2c shows the appearance of the SiOxCy layer formed during the initial stage of diamond growth on the silicon mold. [Figure 3a]FIG. 3a shows the result of the method when the tip body is pyramidal in shape and nano-sized tips are distributed throughout the tip body. [Figure 3b] FIG. 3b shows a pyramidal tip with a few or a single nano-sized tip at the apex region of the tip body. [Figure 3c] FIG. 3c shows a pyramidal tip with a few or a single nano-sized tip at the apex region of the tip body. [Figure 4] FIG. 4 shows a pyramidal tip body having a thicker diamond layer in the apex region than on the sides of the tip body. [Figure 5a] FIG. 5a shows how the method of the present invention can be applied to an in-plane probe. [Figure 5b] FIG. 5b shows how the method of the present invention can be applied to an in-plane probe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The method of the invention will be described in detail for the case of a diamond probe tip manufactured by a molding technique. However, the method is also applicable to tips made of other materials and manufactured by other techniques. Figure 1a shows a silicon substrate 1 on which a pyramidal mold 2 has been formed. This is typically done by anisotropic wet etching along the crystal planes of the substrate. This can be achieved, for example, if the substrate 1 is a (100) oriented silicon substrate, by wet etching the substrate with a square opening while protecting the rest of the substrate with a mask. The dimensions of the mold are on the order of micrometers, for example the sides of the mold may be about 5-10 micrometers long and the depth of the mold may be of the same order of magnitude. Nano-sized diamond seed particles 3 are deposited on the mold, as shown diagrammatically in the detailed view of the mold included in Figure 1a. The seed particles allow for the subsequent growth of a diamond layer within the mold. As is known in the art, the deposition of the seed particles may be performed by immersion seeding, where the substrate 1 containing the mold 2 is immersed in a colloidal solution of particles dissolved in a solvent such as ethanol or H2O. The potential of these diamond nanoparticles is adjusted to be opposite to that of the silicon substrate, which attracts and ultimately deposits these diamond nanoparticles onto the surface of the silicon substrate. The detailed view shows the particles evenly distributed in a linear array, but in reality the particles are more randomly distributed.

[0028] According to this particular embodiment of the invention, at least some of these particles are non-doped diamond particles. The density of the particles when deposited in the mold may be according to existing methods, for example 1E10 / cm 2 From 5E10 / cm 2 However, the density can be between 1E9 / cm by adjusting the seeding dispersion chemistry, the particle and substrate potentials, and the seeding time. 2 From 1E11 / cm 2The applied density must allow the growth of a closed (i.e. completely coalesced) diamond layer in the mould. According to one embodiment, the particles consist of a mixture of undoped and doped diamond particles deposited at any of the above densities. Both doped and undoped particles allow the growth of a closed diamond layer, but only the undoped particles act later as a mask to form the nano-sized tips according to the invention. The diameter of the individual particles is typically 3-5 nm, but they often cluster together in a close pack with a size distribution typically of 5-25 nm.

[0029] A doped diamond layer is then deposited, for example by chemical vapor deposition (CVD). The dopant may be boron. As shown in FIG. 1b, the diamond layer is deposited on the surface of the substrate 1 in a mold 2 and patterned to form patches 4 of the diamond layer in and around the mold. Thus, the diamond does not completely fill the mold cavity, but the diamond layer is deposited on the inverted pyramidal surface of the mold. The thickness of the diamond layer depends on the required probe properties. Diamond layers of about 1 micrometer thickness are often used, but thinner layers, for example about 100 nm, are also possible. It is also possible to produce a perfect diamond tip by filling the entire mold with diamond.

[0030] As shown in Figure 1c, the deposition of diamond is followed by the deposition and patterning of a metal layer stack 5. This may be, for example, a composite of TaN (~50 nm) acting as an adhesion and release layer, Cu (~50 nm) as a seed layer for Ni electroplating, and Ni (~5 μm) as the cantilever material. The metal fills the rest of the mold cavity, so that the cavity is finally filled with a solid tip with a metal core formed on top of the diamond layer. The metal is patterned such that the base 6 is formed and the cantilever 7 extends outward from the base 6. To facilitate the release of the probe, lateral arms 8 extending outward on either side of the base 6 may be provided. The cantilever 7 and the tip inside the mold are then underetched and the base 6 is slightly peeled off from the substrate overcoming the adhesion of the release layer. A silicon holder tip 9 is then attached to the base 6 as shown in Figure 1d, and the assembly is removed from the substrate, resulting in the completed probe shown in Figure 1e. The cantilever 7 is terminated with a pyramidal tip body 10. The pyramidal tip body 10 has a Ni core and a diamond layer on the outside and tip of the pyramid. A base surface 11 is also made of diamond and extends around the tip body 10. The base surface 11 is embedded in the material of the cantilever 7. The parameters of the steps of the above-mentioned method are known to those skilled in the art and will not be described in detail here. Any technique known in the art for realizing the above steps is applicable to the method of the present invention. Details of the under-etching and stripping process are described, for example, in US Pat. No. 6,756,584.

[0031] The method steps characterizing this embodiment of the method of the invention are steps added to the above-mentioned fabrication. The probe shown in FIG. 1e is subjected to a plasma etching process. This may be a reactive ion etching (RIE) or an inductively coupled plasma (ICP) etching, and may be configured such that the undoped diamond nanoparticles 3 have a lower etching rate than the doped diamond of the tip body 10. This means that the particles are etched slower than the doped diamond layer, i.e. they act as an etching mask for etching the doped diamond. A suitable etching process with this effect is plasma etching using O2 as plasma gas, hereafter referred to as O2 plasma, which is well known in the art (examples of suitable parameters are given below). Furthermore, at the beginning of the process of growing diamond on a silicon mold, a thin (usually 1-5 nm thick) silicon oxycarbide layer is formed naturally with a non-uniform thickness. Silicon oxycarbide is a SiOxCy mixture with x<2 and y>0. As with the undoped particles 3, the SiOxCy layer is etched slower than the doped diamond by O2 plasma etching. That is, SiOxCy also functions as an etching mask.

[0032] As shown in FIG. 2a, a SiOxCy layer 12 forms on the mold surface 13 in the spaces between adjacent seed particles 3 and grows thicker until the spaces between the growing doped diamond islands 14 close to form a fully coalesced diamond film 4. FIG. 2b shows the outer surface of the probe after removal from the mold. As shown by the bold lines in FIG. 2b, the SiOxCy layer 12 forms a layer 16 with the nanoparticles 3 that has an irregular thickness. When the tip is subjected to O2 plasma etching, the SiOxCy layer 12 and the nanoparticles 3 are slowly etched away until parts of the doped diamond layer 4 are exposed. This occurs locally due to the irregular thickness of the layer 16. At these places, the doped diamond is etched faster than the SiOxCy layer 12 and the seed particles 3. As the O2 etching process continues, sharp nano-sized doped diamond tips 15 (hereafter also referred to as nanotips) form in the diamond layer 4, resulting in the "hedgehog" tip structure shown in FIG. 3a. The nanotips 15 are distributed throughout the pyramidal tip body 10 and on the diamond base surface 11 around the tip body.

[0033] According to another etching process that can achieve the structure shown in Fig. 3a, the tip is first subjected to a short plasma etch, for example for about 20 seconds, using SF6 or a mixture of SF6 and O2 as plasma gas. This short "flash" etch creates a crater 17 in the SiOxCy layer 12 as shown in Fig. 2c. This step is followed by the O2 plasma etch described above. If part of the SiOxCy layer is pre-removed, the doped diamond layer 4 is exposed more quickly, so that the "hedgehog" structure of Fig. 3a is achieved in a shorter overall time.

[0034] Apart from the SiOxCy layer 12 and the seed particles 3 acting as an etching mask, a third masking effect may occur during the plasma etching process itself. The energy of the plasma may cause particles to be ejected from the material in the etching chamber by sputtering and / or from the cantilever. Said particles may be deposited on the tip and also serve as an etching mask for a given etching recipe. Also, a masking effect may be exerted by polymer etching residues deposited on the tip during the etching process. In the particular case of a diamond tip formed by the above-mentioned shaping technique on a Ni cantilever, the sputtering of Ni particles from the cantilever may contribute significantly to the formation of the nanotip 15. The Ni particles are ejected from the cantilever by sputtering under the effect of ion bombardment generated by O2, SF6 or SF6 / O2 plasma. Also, due to the ion bombardment from the plasma, the pyramid acquires an electrostatic charge, which results in an electric field that attracts the Ni particles. This causes Ni particles to be deposited on the pyramids, but as Ni is essentially not etched by either SF6 or O2 plasma, they also act as an etching mask, just like the seed particles 3 and the SiOxCy layer 12. As the electric field is stronger where the surface is sharper, i.e. at the edges and mainly at the apex of the pyramid plane, the concentration of Ni particles is higher in these regions, which can be exploited to generate specific tip structures (more on this later). When the dry etching is terminated early enough, i.e. before the nanotip 15 itself is etched away, the three masking effects mentioned above, the SiOxCy layer 12, the seed particles 3, and the Ni particles, have a combined effect to generate the "hedgehog" structure shown in Figure 3a. The effect of the SiOxCy layer and the seed particles is more important at the beginning of the etching process and can be the dominant process in the case of a thin diamond layer, for example about 100 nm. In the case of a thicker diamond layer, for example 1 micrometer, or a complete diamond tip, all three effects contribute to the formation of the nanotip 15, and the effect of Ni sputtering becomes dominant after the SiOxCy layer and the seed particles are etched away.

[0035] As mentioned above, all three masking effects (seed particles 3, SiOxCy layer 12, and sputtering particles or etching residues) may contribute to the formation of the "hedgehog" structure in the case of a diamond tip produced in a silicon mold on a Ni cantilever. For tips produced in other materials and / or in other molds or by manufacturing techniques other than molding techniques, not all of the above effects necessarily occur simultaneously. In the method of the invention, any one of the above masking effects may occur alone or in combination with the others. If the cantilever material does not provide a suitable etching mask, the sputtering effect is less important. Also, a layer similar to the SiOxCy layer may not be formed or may not have a masking effect. The presence of seed particles in the mold is not always necessary, as in the case of TiN probe tips, but this will be discussed later. On the other hand, particles that will act as a mask in the etching step may be deposited on the tip body 10 after the probe manufacturing step and before the etching step. For example, undoped diamond particles may be deposited on the diamond tip by colloidal deposition. This may be done in addition to one or more of the masking effects mentioned above, or when these effects are not applicable, for example when the seed particles are not suitable as a chemical mask for the particular etch or when the probe is not manufactured by molding techniques. The masking effect may also be due solely to particles deposited on the tip during the etching process, such as sputtered particles from the cantilever or the etch chamber. This may be the case when there are no seed particles and compounds such as naturally formed oxides do not provide a masking effect.

[0036] From the above description it is clear that the "mask layer" referred to in the attached claim 1 can be composed of various components. The mask layer may comprise a layer with irregular thickness formed before the etching process, such as layer 16 in FIG. 2b. The mask layer may also consist of or comprise particles that contribute to the formation of this layer during the etching process itself. The claimed "layer with irregular thickness" may also have various compositions depending on the material of the probe tip and the manufacturing process. This layer may consist only of seed particles, or only of particles deposited on the tip body after the probe manufacturing process, or only of mixtures that naturally form on the tip body, such as oxides formed on TiN probe tips, as will be described below. This layer can be closed so that none of the probe material is initially exposed to the plasma, but this probe material will only be exposed when the mask layer is locally etched away. This necessarily occurs locally due to the irregular thickness of the layer. The layer with irregular thickness may be a layer that locally exposes the underlying probe material from the beginning of the etching process, for example a layer consisting of only seed particles with a thickness of zero between the seed particles.

[0037] The above etching process is terminated when the nanotip 15 has the desired shape and aspect ratio. In the case of the above O2 plasma etching of the diamond tip, the O2 etching time determines the shape of the nanotip. Initially, the nanotip is a conical pillar, as shown in Figure 3a. If the etching process is applied longer, the nanotip becomes more needle-like due to the slight isotropy of the dry etching process. Thus, the etching time can be controlled to obtain the desired shape. Even after the etching process is terminated, some of the seed particle and / or SiOxCy layer and / or sputtered particles may remain on the nanotip. In some applications, these remaining etch masks are not a problem and may remain. If not, these remaining residues may be burned off by a slight oxygen overetch, or may be removed by applying a high bias voltage or high scanning force for a short period of time if the tip is to be used in electrical SPM measurements.

[0038] FIG. 3a is a schematic diagram. In practice, the number of nanotips 15 may be much higher, or the nanotips may be more randomly distributed across the diamond surface. The dimensions of the nanotip are on the order of nanometers, for example about 50-100 nm in height. The radius of the apex region of the nanotip ranges from less than 1 nm to several nanometers, which is comparable or better than the radius of a standard pyramidal tip, but the nanotip is significantly smaller and sharper than the tip body 10 before the etching process. In other words, the aspect ratio of the nanotip 15 is significantly larger compared to the aspect ratio of the apex region of the tip body 10 before the etching process. The aspect ratio of the apex region can be determined by approximating the apex region as a sphere and defining the aspect ratio as the ratio of the average diameter of the surface to its height. The aspect ratio of the nanotip may be calculated according to commonly established definitions depending on the shape of the nanotip, for example as the ratio of the average width of a conical tip to the height of the tip. Thus, the method of the present invention provides a method for producing probes with increased aspect ratios at the tips that actually contact the surface without the need for complex micromachining or other manufacturing methods. The etching process is self-aligning and does not require a lithographic mask other than particles, SiOxCy layers, or other contributors to the mask layer referred to in claim 1 below.

[0039] When the probe tip shown in FIG. 3a is used for probing a sample by SPM, the nanotip that contacts the sample may be the outermost nanotip at the top of the pyramid or one of the nanotips adjacent to it, depending on the angular position of the probe. This type of probe is therefore very suitable for use in combination with tiltable SPM heads known per se in the art. The presence of multiple nanotips 15 ensures contact of at least one of these tips with the sample. The presence of multiple sharp nanotips also makes the probe tip of the invention suitable for scratching the surface and removing material from it, as applied for example in the known "scalpel AFM" technique. Another application of the probe tip with multiple sharp nanotips produced according to the invention is the attachment of nano / micro objects such as biological cells to the sharp nanotips. This is made possible by the known fact that multiple closely spaced nanotips can affect the wettability of a surface.

[0040] The present invention is not limited to the above-mentioned "hedgehog" type structure. According to one embodiment, the dry etching process is continued until the nano-tips 15 on the sides of the pyramid are etched away. However, one or more nano-tips 15 are still formed in the apex region of the tip body 10, as shown diagrammatically in Fig. 3b and Fig. 3c. This tip structure, also referred to hereafter as "tip-on-tip morphology", may be realized by utilizing one or more effects that may occur simultaneously. In the case of the above-mentioned diamond-coated tip / silicon mold / Ni cantilever set, sputtering of Ni particles from the cantilever during the etching process is one of the effects that contribute to this kind of tip structure. As mentioned above, the electric field generated by the ion bombardment is stronger where the surface is sharper, i.e., at the edges of the pyramid plane and mainly at the apex. Since the electric field attracts the Ni particles, there are more etch mask particles on the apex than on the sidewall. As a result, the diamond layer on the sidewall is completely etched away, but one or more sharp diamond tips 15 remain in the apex region. Thus, after the etching step, the tip body is made entirely of Ni, except for the sharp diamond tip 15 in the apex region.

[0041] A second contribution to this "tip on tip" morphology is that the diamond layer can be thicker near the apex region compared to the sides of the pyramid. This is illustrated in FIG. 4, which shows a cross section of a diamond coated probe tip body with a Ni core 20 and a doped diamond layer 21. It also shows the presence of an undoped diamond seed particle 3 and a SiOxCy layer 12 in a schematic manner. It can be seen that the thickness of the diamond layer measured in a direction perpendicular to the base of the pyramid is greater at the apex region (thickness a1) than at the sides of the pyramid (thickness a2). This can be a result of the deposition process applied to form the diamond layer. If the dry etching process is continued until the diamond layer 21 is removed from the sides of the pyramid, a sufficient thickness of diamond remains at the apex region due to the thickness difference between thicknesses a1 and a2. This results in one or more sharp tips 15 appearing only at the apex region, as shown in FIG. 3b and FIG. 3c. The number of tips that appear depends on the exact distribution of the particles near the apex region. Thus, the present embodiment provides a simple method for producing a "tip on tip" probe without requiring complex micromachining or similar methods. The difference between thicknesses a1 and a2 may not necessarily occur or may not be sufficient to obtain the above-mentioned effect. This may depend on the average thickness of the layer 21 of probe material (diamond or other) and / or the specific parameters applied when producing this layer.

[0042] The present invention can be used to manufacture any type of probe suitable for SPM scanning, manufactured by any known technique and formed from any known material, for example, a silicon-silicon mixture tip or a metal-metal alloy tip. The method can be used equally well for diamond tips other than boron-doped diamond tips, for example, phosphorus-doped diamond, undoped diamond, NV (nitrogen vacancy) diamond. The inventors have manufactured a "hedgehog" probe tip comprising a nanotip 15 formed of TiN on a Ni cantilever. The probe was manufactured by a molding technique similar to that described above. However, instead of a diamond CVD layer, a TiN layer of about 150 nm thickness was deposited on a silicon mold by sputtering of TiN. No seed particles were deposited on the mold. The layer with irregular thickness formed on the TiN layer is an oxide layer that initially forms naturally on the outer surface of the TiN pyramid after it is removed from the mold. The oxide acts as an etch mask for a plasma etching process under a SF6 / O2 mixture in the same way as the combined action of the seed particles and SiOxCy described above. That is, the oxide etches at a slower rate, thereby locally exposing the TiN layer underneath, which is then etched at a faster rate. As the etching process progresses, the sputtered Ni particles contribute to the mask layer in the same manner as above. By exposing the tip to plasma etching in this environment, we have produced a "hedgehog" structure with a TiN nanotip15. Details of suitable etching parameters are given below.

[0043] The invention is not limited to pyramidal tips. The nanotip 15 may be produced with other tip shapes as well. Figure 5a shows an in-plane probe, known for example from US Pat. No. 8,484,761. This figure shows a cantilever 7 with a diamond tip body 10 extending outwards from the cantilever and lying in the plane of the cantilever. Figure 5b shows a side view of the same probe and a detail of the tip region after applying an etching treatment according to the invention. The nanotip 15 extends in a direction perpendicular to the plane of the cantilever 7 and the tip body 10. The particles with the masking effect mentioned above may be deposited in a separate deposition step. And / or, if the cantilever material is suitable for this purpose, the masking particles may be deposited by sputtering of the cantilever material and / or material in the etching chamber during the etching step itself and / or by the masking effect of etching residues.

[0044] After completion of the method according to any of the above embodiments, several additional method steps may be performed. These additional method steps include the following steps: depositing a capping layer onto the one or more nanotips 15, thereby completely covering the one or more nanotips with the capping layer. subjecting the cap layer to a plasma etching process to remove the cap layer from a tip region of the nanotip while maintaining the cap layer on sides of the nanotip, the tip region including the apex of at least one nanotip.

[0045] In other words, after these additional processes, the cap layer forms a sleeve around the nano tip while leaving the apex of the nano tip exposed, so that the function of the nano tip in an SPM apparatus or other applications is not inhibited. The cap layer reinforces the nano tip. That is, while increasing the mechanical resistance of the nano tip, the nano tip maintains its function execution ability. This embodiment is particularly beneficial in high-load applications, and the cap layer helps prevent damage to the nano tip. In the case of the tip of the above diamond or the tip of the diamond coating, the cap layer may be a hamster-type probe as shown in FIG. 3a, or a SiOx layer (1 <x <2) deposited on the "tip on tip" as shown in FIGS. 3b and 3c. The SiOx layer may be deposited by plasma-enhanced chemical vapor deposition (PECVD). The thickness of the SiOx layer may be on the order of several tens of nanometers, for example, about 50 nm. The etching process for removing the SiOx layer from the apex region may be plasma etching using a mixture of SF6 and O2. The etching process ends when at least the apex of the nano tip is exposed. A more detailed description of appropriate parameters will be described later.

[0046] The additional processes described in the previous paragraph for generating a cap layer on one or more nano tips 15 are also applicable to the "tip on tip" probe described in the prior art, that is, a probe tip including a nano tip in the apex region of the tip body. However, the nano tip is manufactured by a method other than the above method including the manufacture of these nano tips by a self-aligned etching process. For example, the cap layer may be manufactured by the same process as described above on a probe tip manufactured by the method described in U.S. Patent No. 6328902. Accordingly, the present invention is similarly related to a method for manufacturing a probe tip suitable for a scanning probe microscope (SPM), which includes the following steps. A step of manufacturing a probe tip body (10) having an apex region and one or more tip portions that are significantly smaller and sharper than the tip body in the apex region, and no tip portions in the remaining portion of the probe tip body A step of depositing a cap layer on one or more tip portions (15), thereby completely covering the one or more tip portions subjecting the tips to a plasma etching process configured to remove the cap layer from a tip region of the one or more tips, the tip region including the apex of the one or more tips while substantially maintaining the cap layer around a side of the one or more tips (15).

[0047] In view of the foregoing, the present invention also relates to a probe tip suitable for a scanning probe microscope (SPM), comprising a probe tip body having an apex region and including one or more tips on the apex region of the tip body, the remainder of the tip body being free of tips, the tips being significantly smaller and sharper than the tip body. The tip has a cap layer on an outer surface, except for the tip region of the tip. The tip region includes the apex of the tip.

[0048] The examples of suitable parameters for producing the cap layer described below are applicable to "tip on tip" type diamond probe tips manufactured by the self-aligned etching process method, the method of U.S. Pat. No. 6,328,902, or other methods known in the art.

[0049] (Example) We have fabricated diamond "full hedgehog" tips on probes that include a tip body fabricated by the molding technique described above: a silicon mold, undoped seed particles (density approx. 1E10 / cm) deposited on the mold, and 2 ), Ni cantilever, diamond layer (thickness about 800 nm) on Ni core. The following etching parameters were applied:

[0050] [Table 1] *The gas flow rate was 294K and 3 atm. Under these conditions, 1sccm is approximately 9.09E-9m 3 Equivalent to / s. ※※1 Torr = 133,322 Pa

[0051] A diamond “tip-on-tip” probe as shown in FIG. 3c was fabricated in the same way, i.e., in the same ICP reactor, applying the same RF and ICP powers and the same chamber pressure, but by the following sequence of etching steps. O2 / SF6 mixed plasma etching for 20 seconds; gas flow rates 50 sccm (O2) and 2.5 sccm (SF6) 5 min O2 plasma etching; O2 gas flow 50 sccm

[0052] [Table 2] *Gas was supplied at 294K and 3 atm.

[0053] A SiOx layer was deposited by PECVD to a thickness of about 50 nm on the diamond-tipped "full hedgehog" tip obtained with the parameters in Table 1. The tip was then subjected to SF6 / O2 plasma etching with the parameters shown in Table 3.

[0054] [Table 3] *Gas was supplied at 294K and 3 atm.

[0055] As a result, the SiOx layer was removed from the apex of the nanotip, while a reinforcing cap layer was formed around the sides of the nanotip.

[0056] While the present invention has been illustrated and described in detail in the drawings and the foregoing description, such illustration and description are to be considered as schematic or exemplary and not restrictive. Other variations to the disclosed embodiments can be understood and effected by those skilled in the art of practicing the present invention, in view of the drawings, the disclosure, and the appended claims. In the claims, the term "comprising" does not exclude other elements or steps, and the indefinite article "a" or "an" does not exclude a plurality. The mere fact that certain methods are recited in mutually different dependent claims does not indicate that a combination of these methods cannot be used to advantage. Reference signs in the claims are not to be construed as limiting the scope. The following items 1 to 15 are within the scope of the disclosure of this application. [Item 1] manufacturing a probe tip body (10) having an outer layer (21) of at least one probe material; forming a mask layer on the outer layer of probe material during and / or after the manufacturing process of the probe tip body; subjecting the probe tip body (10) to a plasma etching process, the mask layer acting as an etch mask for etching the probe material, the plasma etching process and the etch mask configured to produce one or more tips (15) formed from the probe material, the one or more tips being significantly smaller and sharper than the probe tip body (10) prior to the plasma etching process. A method for manufacturing a probe tip suitable for a scanning probe microscope, comprising: [Item 2] 2. The method of claim 1, wherein the mask layer comprises a layer of irregular thickness (16) formed prior to the plasma etching process, the layer of irregular thickness acting as an etch mask for etching the probe material. [Item 3] 3. The method of claim 2, wherein the layer (16) having irregular thickness comprises a compound that forms naturally, for example by oxidation, on the surface of the probe tip body (10) after the manufacturing step of the probe tip body and before the plasma etching process. [Item 4] 4. The method of claim 2 or 3, wherein the layer of irregular thickness (16) comprises particles that are intentionally deposited on the probe tip after the fabrication step of the probe tip and before the plasma etching process. [Item 5] 5. The method according to any one of claims 2 to 4, wherein the probe tip body (10) is manufactured by forming a mold (2) on a substrate (1) and by depositing the probe material in the mold, seed particles (3) are deposited on the mold (2) before depositing the probe material, and the layer (16) having irregular thickness includes the seed particles (3). [Item 6] 6. The method according to claim 5, wherein the layer (16) having irregular thickness further comprises a mixture (12) naturally formed on the surface of the mold (2). [Item 7] The plasma etching process includes: a first etching step carried out for a first short etching time and configured to generate craters (17) in said layer (16) of irregular thickness; a second etching step performed for a second etching time period significantly longer than the first short etching time period and configured to generate the one or more tips (15); The method according to any one of items 2 to 6, comprising: [Item 8] 8. The method according to any one of claims 1 to 7, wherein the probe tip body (10) is attached to a cantilever (7), particles of material of the cantilever are sputtered and deposited on the probe tip body (10) during the plasma etching process, and the sputtered particles from the cantilever contribute to the formation of the mask layer for the remainder of the plasma etching process. [Item 9] 9. The method according to any one of claims 1 to 8, wherein at the end of the plasma etching process, the tip (15) is distributed throughout the probe tip body (10). [Item 10] the probe tip body (10) is pyramidal, and at the end of the plasma etching process the one or more tips (15) are present at an apex region of the probe tip body and no tips are present at the sides of the probe tip body; These have the following effects: A higher concentration of masking particles is deposited at the apex region than at the sides during the plasma etching process. The probe tip body (10) includes a core (20) and the thickness of the layer (21) of probe material on the core is greater in the apex region than on the sides, so that at the end of the plasma etching process the probe material is removed from the sides. The method according to any one of items 1 to 8, wherein the method is carried out through one or a combination of the following: [Item 11] 11. The method of any one of claims 1 to 10, wherein the probe material is diamond. [Item 12] The following steps are carried out after the plasma etching process: depositing a cap layer onto said one or more tips (15), thereby completely covering said one or more tips. subjecting the tips to a plasma etching process configured to remove the cap layer from a tip region of the one or more tips, the tip region including the apex of the one or more tips while substantially maintaining the cap layer around a side of the one or more tips (15). 12. The method according to any one of items 1 to 11, further comprising: [Item 13] The probe tip body (10) includes at least one outer layer (21) of a probe material; A probe tip suitable for a scanning probe microscope, wherein a plurality of tip portions (15) formed from the probe material are distributed throughout the probe tip body, and the tip portions are significantly smaller and sharper than the probe tip body. [Item 14] Item 14. The probe tip of item 13, wherein the tip comprises a cap layer on an outer surface of the tip except for a tip region, the tip region including an apex of the tip. [Item 15] A cantilever (7); A holder (9) attached to the cantilever; a probe tip attached to the end of the cantilever; Equipped with The probe tip is the probe tip according to item 13 or 14. [Explanation of symbols]

[0057] 1 Board Type 2 3 types of particles (nanoparticles) 4 Patch (Diamond Layer, Diamond Film) 5 Metal Layer Stack 6 base 7 Cantilever 8 Lateral Arm 9 Holder 10 Probe tip body (tip body) 11 Base 12 SiOxCy layer 13 type surface 14 Diamond Islands 15 Tip (nano tip, diamond tip) 16 Layers of irregular thickness 17 Crater 20 cores 21 Diamond layer (outer layer)

Claims

1. A process for manufacturing a probe tip body (10) by depositing seed particles (3) on a mold (2) formed on a substrate (1), and then depositing a probe material within the mold to grow an outer layer (21) consisting of at least one probe material, wherein as the outer layer (21) grows, it thickens in the spaces between adjacent seed particles (3) to naturally form a layer (16) having an irregular thickness, and the layer (16) functions as a mask layer; subjecting the probe tip body (10) to a plasma etching process, the mask layer acting as an etch mask for etching the probe material, the plasma etching process and the etch mask configured to produce one or more tips (15) formed from the probe material, the one or more tips being significantly smaller and sharper than the probe tip body (10) prior to the plasma etching process. A method for manufacturing a probe tip suitable for a scanning probe microscope, comprising:

2. 2. The method of claim 1, wherein the layer of irregular thickness (16) comprises particles that are intentionally deposited on the probe tip after the fabrication step of the probe tip and before the plasma etching process.

3. The method of claim 1 , wherein the layer (16) having irregular thickness further comprises a mixture (12) naturally formed on the surface of the mold (2).

4. A process for manufacturing a probe tip body (10) by depositing seed particles (3) on a mold (2) formed on a substrate (1), and then depositing a probe material within the mold to grow an outer layer (21) consisting of at least one probe material, wherein as the outer layer (21) grows, a silicon oxycarbide layer (12) thickens in the spaces between adjacent seed particles (3), naturally forming a layer (16) having an irregular thickness including the seed particles (3) and the silicon oxycarbide layer (12), and the layer (16) functions as a mask layer; subjecting the probe tip body (10) to a plasma etching process, the mask layer acting as an etch mask for etching the probe material, the plasma etching process and the etch mask configured to produce one or more tips (15) formed from the probe material, the one or more tips being significantly smaller and sharper than the probe tip body (10) prior to the plasma etching process. Including, The plasma etching process includes: a first etching step carried out for a first short etching time and configured to generate craters (17) in said layer of irregular thickness (16); a second etching step performed for a second etching time significantly longer than the first short etching time and configured to generate the one or more tips (15); A method for manufacturing a probe tip suitable for a scanning probe microscope, comprising:

5. The method according to any one of claims 1 to 4, wherein at the end of the plasma etching process, the tips (15) are distributed throughout the probe tip body (10).

6. The method of any one of claims 1 to 5, wherein the probe material is diamond.

7. The following steps are carried out after the plasma etching process: depositing a cap layer onto said one or more tips (15), thereby completely covering said one or more tips. subjecting the tips to a plasma etching process configured to remove the cap layer from a tip region of the one or more tips, the tip region including the apex of the one or more tips while substantially maintaining the cap layer around a side of the one or more tips (15). The method of any one of claims 1 to 6, further comprising:

Citation Information

Patent Citations

  • Method for manufacturing a measuring tip for a scanning probe microscope and measuring probe with a measuring tip manufactured according to this method

    DE102010035931A1

  • Diamond probe and its forming method

    JP1990075902A

  • Production of tip for atomic force microscope

    JP1996285872A

  • Afm cantilever

    JP1997178763A

  • Probe for scanning probe microscope

    JP2003240700A