Superconducting joint structure of oxide superconductor and superconducting device using the same
The use of a gallium-indium-tin alloy for oxide superconductor connections addresses the limitations of heat treatment and toxic materials in existing methods, providing easy, versatile, and environmentally friendly superconducting connections with enhanced magnetic properties.
Patent Information
- Application Number
- JP2020025965
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-19
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-02-19
AI Technical Summary
Existing methods for connecting oxide superconductors require heat treatment, which can damage the superconductors and are not versatile, and often involve toxic materials like lead, making them unsuitable for certain applications and environments.
A superconducting connection structure using a liquid alloy of gallium, indium, and tin with a specific composition range that allows for room temperature bonding without heat treatment, eliminating the need for surface polishing and avoiding toxic materials.
The solution enables easy and versatile superconducting connections with improved critical magnetic fields, reducing environmental impact and enabling connections in various shapes and locations without specialized equipment.
Smart Images

Figure 0007553932000005 
Figure 0007553932000004 
Figure 0007553932000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a superconducting joint structure of an oxide superconductor, and more particularly to a superconducting joint structure of an oxide superconductor that utilizes a liquid alloy containing gallium, indium, and tin. [Background technology]
[0002] In order to connect devices that utilize superconductivity, such as superconducting wires, superconducting coils, superconducting cavities, and superconducting electronic elements while maintaining the superconducting state, the connecting parts must also exhibit superconductivity. Connecting such superconductors while maintaining the superconducting state is called a superconducting connection (or superconducting junction), and it can be realized mainly in the following two ways.
[0003] (A) A mode in which an alloy that has a low melting point like solder and exhibits superconductivity at low temperatures (such as an alloy containing lead and bismuth, tin, bismuth and indium, tin, lead and bismuth, tin and indium, or tin and bismuth) is sandwiched between two superconductors and the connection is made by raising the temperature above the melting point (see, for example, Patent Documents 1 and 2). (i) A method in which two superconductors are connected by growing crystals of the superconductor itself between them.
[0004] In the above (a), heat treatment is required to melt the alloy sandwiched between the two superconductors and bond the alloy and the superconductors. In the above (i), heat treatment is required to grow the crystals of the superconductor itself on top of the superconductor and bond them to another superconductor. An electric furnace is required for the heat treatment, and some devices using superconductivity may not be able to withstand the increased temperature, or a special electric furnace may need to be prepared. In particular, if the superconductor is an oxide superconductor, the oxygen content may change due to the heat treatment, and the oxide superconductor itself may be altered. Therefore, it would be ideal to achieve a superconducting connection without heat treatment, and it would be necessary to sandwich between two oxide superconductors a superconductor with a melting point lower than room temperature or a material that grows as a superconductor at a temperature lower than room temperature.
[0005] On the other hand, Patent Document 3 discloses that some compositions of alloys containing gallium, indium, and tin become liquid alloys. And Non-Patent Document 1 discloses that some compositions of alloys containing gallium, indium, and tin become superconductors. However, to the best of the inventor's knowledge, there have been no reports of superconducting connections using liquid alloys containing gallium, indium, and tin. In particular, oxide superconductors are brittle, and therefore have the problem that processing of superconducting connections is more difficult than coil connections using metal-based superconductors such as alloys containing niobium and titanium. Furthermore, when Galinstan disclosed in Patent Document 3 is used, according to Non-Patent Document 1, the following problems arise. (1) Because the goal is printed electronics, the process is very labor-intensive, as it involves using an alloy containing gallium, indium, and tin fabricated into nanodroplets. (2) The composition of Galinstan, expressed in atomic percent, is Ga 41.64 In 39.61 Sn 18.75 Whether in droplet form or bulk form, its melting point is about 63°C, and even if it is heated above room temperature to turn it into a liquid state, it needs to be heated to above 60°C. Therefore, it is less versatile than liquid alloys containing gallium, indium, and tin. (3) Superconductivity is believed to occur when gallium, indium, and tin (elementary metals) are precipitated at low temperatures. Elemental metals are type I superconductors, and compared to type II superconductors, their critical magnetic field is smaller, making them disadvantageous in practical use. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] USP No. 3156539 [Patent Document 2] Japanese Patent Application Publication No. 9-82445 [Patent Document 3] Patent No. 2574658 [Non-patent literature]
[0007] [Non-Patent Document 1] L. Ren et al., Adv. Functional. Mater. 26 (2016) 8111. Summary of the Invention [Problem to be solved by the invention]
[0008] The conventional technologies disclosed in Patent Documents 1 and 2 require heat treatment to connect two oxide superconductors to create a superconducting connection through which current can flow with zero electrical resistance, and require heat treatment equipment and conditions that take into account the physical properties of the oxide superconductors that are the subject of the superconducting connection, making the technologies less versatile. In addition, when connecting two oxide superconductors, whether using a low melting point alloy or connecting by crystal growth, the surface of the oxide superconductor needs to be flattened, but polishing the surface of the oxide superconductor to the required flatness takes time. In particular, when using crystal growth, it is necessary to create a clean surface so that the crystals can grow, and careful polishing is required. Some of the elements that make up low melting point alloys contain toxic lead, but sales are restricted by the RoHS (Restriction of the use of certain Hazardous Substances in Electrical and Electronic Equipment) Directive, and lead-containing Manufacturing The sale of these products within the EU will be prohibited. The present invention has been made to solve the above-mentioned problems, and aims to provide a superconducting connection structure that does not require surface polishing or heat treatment when connecting oxide superconductors, and that does not contain lead, and a superconducting device using the same. [Means for solving the problem]
[0009] [1] The present invention relates to a superconducting joint structure of oxide superconductors, in which a liquid alloy containing gallium, indium and tin is sandwiched between two oxide superconductors.
[0010] [2] In the superconducting joint structure of the oxide superconductor of the present invention, preferably, the composition of the low-melting-point alloy containing gallium, indium and tin, the melting point of which is 60° C. or less in a thermal equilibrium state, is Ga x In y Sn z The superconducting connection structure according to claim 1, characterized in that, when x, y, and z are expressed in atomic percent, the structure satisfies the range surrounding the following points (x, y, z) on a ternary phase diagram of gallium, indium, and tin. (90, 5, 5), (70, 5, 25), (60, 10, 30), (50, 17, 33), (45, 23, 32), (40, 30, 30), (39, 35, 26), (43, 36, 21), (50, 35, 15), (54, 36, 10), (54, 41, 5) and (90, 5, 5). [3] In the superconducting joint structure of the oxide superconductor of the present invention, the liquid alloy containing gallium, indium and tin preferably has a composition of Ga x In y Sn z When x, y, and z are expressed in atomic percent, it is preferable that the following ranges are satisfied. 55≦x≦90, 5≦y≦25, 5≦z≦20 and x+y+z=100. [4] In the superconducting joint structure of the oxide superconductor of the present invention, the liquid alloy containing gallium, indium and tin preferably has a composition of Ga x In y Sn z When x, y, and z are expressed in atomic percent, it is preferable that the following ranges are satisfied. 55≦x≦88, 5≦y≦25, 7≦z≦20 and x+y+z=100. [5] In the superconducting joint structure of the oxide superconductor of the present invention, the oxide superconductor is preferably an yttrium-based copper oxide superconductor {YBa2Cu3O6+δ (δ indicates the amount of oxygen vacancy, same below)), bismuth-based copper oxide superconductor {Bi2Sr2Ca nー1 Cu n O 2n+4+δ (n=1, 2 or 3)}, rare earth copper oxide superconductors {REBa2Cu3O 6+δ (RE is a rare earth element)}. [6] In the superconducting joint structure of the oxide superconductor of the present invention, the oxide superconductor is preferably an iron-based superconductor {REFeAsO 1-X F X (RE is a rare earth element), AFe2As2 (A is an alkali metal or an alkaline earth metal), and AFeAs}.
[0011] [7] A superconducting device of the present invention has the above-mentioned superconducting joint structure of the oxide superconductor. [8] In the superconducting device of the present invention, preferably, the superconducting device includes at least one of a superconducting wire, a superconducting coil, a superconducting cavity, and a superconducting electronic element. [9] In the superconducting device of the present invention, preferably, the superconducting device is any one of a nuclear magnetic resonance imaging device, a nuclear magnetic resonance spectroscope, a superconducting magnet, a superconducting power transmission line, a superconducting filter for high frequency communication, a SQUID, a magnetic field detector, a superconducting linear motor, or a superconducting electromagnetic propulsion device for a ship. Effect of the Invention
[0012] The present invention has the following advantages. (i) The precipitation of superconductors from a liquid alloy containing gallium, indium, and tin at or below room temperature is utilized, eliminating the need for heat treatment to create superconducting connections and avoiding deterioration of oxide superconductors due to heat treatment. (ii) Since a superconducting joint can be made by simply applying a liquid alloy containing gallium, indium and tin, a superconducting joint can be easily made even over a large area, regardless of the shape of the oxide superconductor. (iii) Liquid and solid alloys containing gallium, indium and tin can be synthesized by simply mixing gallium, indium and tin (each of which is an elemental metal) at room temperature through a eutectic reaction or by heat treatment at 60°C or less, so no special equipment is required for synthesis. (iv) Even when using an alloy containing solid gallium, indium, and tin, no special equipment is required since it can be made at a temperature of 60 degrees C or less. Therefore, if there is an apparatus for applying a liquid alloy containing gallium, indium, and tin or an apparatus for heating a solid alloy containing gallium, indium, and tin to 60 degrees C or less, it is possible to make a superconducting connection on the spot regardless of location. (v) By using a liquid alloy containing gallium, indium and tin to connect two oxide superconductors, it is not necessary to polish the surface of the oxide superconductors. In addition, the liquid alloy containing gallium, indium and tin does not contain toxic lead, so it has a low environmental impact. (vi) The present invention Oxide superconductors In the superconducting connection structure, an alloy containing indium and tin, which is a type II superconductor, is precipitated, and therefore the critical magnetic field is larger than that of the single metal, which is a type I superconductor, disclosed in Non-Patent Document 1, and this is advantageous in practical use. [Brief description of the drawings]
[0013] [Figure 1] The melting point isotherm of a ternary alloy of gallium, indium and tin is shown. [Diagram 2] 1 is a diagram showing the melting point isotherms of ternary alloys of gallium, indium and tin, with an expanded range being shown for the liquid and low melting alloys preferred for use in the present invention. [Diagram 3] The structure formed by cooling a liquid alloy containing gallium, indium and tin is shown, along with a gallium phase and an alloy containing indium and tin. [Figure 4] 1 is a phase diagram of a binary alloy of indium and tin. [Diagram 5]FIG. 1 is a diagram showing a cross-sectional structure of a superconducting joint of an oxide superconductor using a liquid alloy containing gallium, indium, and tin according to one embodiment of the present invention, in which the oxide superconductor is YBa2Cu3O7 and a butt joint type is shown. [Figure 6] FIG. 6 is a graph showing the temperature change in electrical resistance of a superconducting joint of the oxide superconductor shown in FIG. [Figure 7] FIG. 6 is a diagram showing current-voltage characteristics of a superconducting connection of the oxide superconductor shown in FIG. [Figure 8] This is a diagram showing the cross-sectional structure of a superconducting connection of an oxide superconductor using a liquid alloy containing gallium, indium, and tin according to a second embodiment of the present invention, in which the oxide superconductor is Bi2Sr2CaCu2O8+δ and shows a stack type. [Figure 9] FIG. 9 is a graph showing the temperature change in electrical resistance of a superconducting joint of the oxide superconductor shown in FIG. [Figure 10] FIG. 9 is a diagram showing current-voltage characteristics of a superconducting connection of the oxide superconductor shown in FIG. [Figure 11] FIG. 13 is a diagram showing a superconducting connection structure of an oxide superconductor according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Ternary alloys containing gallium, indium and tin, with a composition in which the melting point temperature in a thermal equilibrium state is preferably 60°C or less, more preferably 40°C or less, and particularly preferably 23°C or less, have a lower melting point than alloys used in conventional superconducting connections, so that even if the alloy containing gallium, indium and tin is in a composition range in which it does not become liquid at room temperature, it is possible to create a superconducting connection at a temperature low enough that the oxide superconductor does not change in quality. In particular, ternary alloys containing gallium, indium and tin within a specific composition range have a melting point (freezing point) below room temperature due to a eutectic reaction, so that they become liquid at room temperature. Furthermore, the ternary alloy containing gallium, indium and tin may contain 0.8 atomic percent or less of bismuth and 1.4 atomic percent or less of antimony.
[0015] Figure 1 shows the melting point isotherms of a ternary alloy of gallium, indium and tin. Figure 2 shows an enlarged phase diagram of a ternary alloy of gallium, indium and tin, which shows the preferred range of the liquid alloy used in the present invention. The melting point distribution curves in Figures 1 and 2 are taken from the "ASM Alloy Phase Diagram Database" and the original source is as follows: Kononenko VI, and Yatsenko SP, Equilibrium diagrams characterization of binary and ternary gallium systems with I-VI elements on deviation of liquid alloys structural-susceptible properties, Diagrammy Sostoyaniya Met. Sist., Mater. Vses. Soveshch., 4th, Vol. , 1971, p 254-257
[0016] The melting point distribution curves in Figures 1 and 2 were measured for a mixture of the raw materials gallium, indium, and tin (all solids). In contrast, Galinstan and the inventor's experiments measured the raw materials gallium, indium, and tin that were mixed and melted to become liquid metal. Therefore, the liquid metal becomes supercooled below the melting point (freezing point). In the present invention, the region in which the melting point temperature in a thermal equilibrium state is 60° C. or less is Ga x In y Sn z When x, y, and z are expressed in atomic percent, the range should be the range surrounding the following points (x, y, z) on the ternary phase diagram of gallium, indium, and tin (the range surrounded by the thick line in Figure 1): (90, 5, 5), (70, 5, 25), (60, 10, 30), (50, 17, 33), (45, 23, 32), (40, 30, 30), (39, 35, 26), (43, 36, 21), (50, 35, 15), (54, 36, 10), (54, 41, 5), and (90, 5, 5).
[0017] Next, the elements used in the liquid alloy of the present invention will be described. Gallium: 39 atomic percent ≦ x ≦ 90 atomic percent (when melting point temperature is 60°C or less) At room temperature and pressure, orthorhombic alpha gallium (specific gravity 5.9) is stable and is a bluish metallic luster metal. Its melting point is low at 29.8°C. It has three valence electrons (4s, 4p), but the 3d orbital is relatively shallow. Liquid metals have a strong tendency to become supercooled below their melting (freezing) point, and when Ga is made into nanoparticles, it can remain liquid even at 90 Kelvin. When crystals are seeded, it begins to freeze. By sealing gallium in a glass tube, it can be used as a high-temperature thermometer, similar to a mercury thermometer. Liquid gallium metal wets glass and skin. Below the critical temperature of 1.10 Kelvin, gallium becomes a superconductor. Since gallium is expensive, the composition ratio is preferably in a range close to the lower limit of 39 atomic percent, for example, in the range of 56 atomic percent to 78 atomic percent, and more preferably in the range of 60 atomic percent to 70 atomic percent. When based on a ternary phase diagram of gallium, indium and tin, gallium may be, for example, in the range of 55 atomic percent to 90 atomic percent, more preferably in the range of 55 atomic percent to 88 atomic percent.
[0018] Indium: 5 atomic percent ≦ y ≦ 41 atomic percent (when melting point temperature is 60°C or less) It has a tetragonal crystal structure (specific gravity 7.3) and is a soft silver-white metal. Its melting point is low at 156.4°C and it is stable in air. At a critical temperature of 3.37K or less, indium becomes a superconductor. Indium has excellent malleability and ductility. Since indium is expensive, the composition ratio is preferably close to the lower limit of 5 atomic percent, for example, it may be in the range of 6 atomic percent to 18 atomic percent, and more preferably in the range of 6 atomic percent to 10 atomic percent. On the other hand, if the composition ratio of indium is increased, the ratio of In3Sn, which has a high critical temperature, increases in the two types of eutectic structures of In3Sn and InSn4, which is preferable in terms of superconducting connection performance. When based on a ternary phase diagram of gallium, indium and tin, indium may be in the range of 5 atomic percent to 25 atomic percent.
[0019] Tin: 5 atomic percent ≦ z ≦ 33 atomic percent (when melting point temperature is 60°C or less) At room temperature and pressure, tetragonal β-tin (specific gravity 7.4) is stable and is a ductile silvery-white metal. On the other hand, α-tin, which is stable below 13.2°C, is a brittle, gray nonmetallic substance with a diamond-type crystal structure. Since α-tin is formed by covalent bonds, it does not have free electrons and does not have metallic properties. Thermodynamically, β-tin transforms to α-tin at 13.2°C, but the reaction actually begins to progress at low temperatures of -10°C, and the reaction rate reaches its maximum at -45°C. Tin becomes a superconductor at a critical temperature of 3.73 K or less. Compared to gallium and indium, the current trading price is about one-tenth of theirs. The proportion of tin is preferably in a range close to the upper limit of 33 atomic percent, for example, in the range of 15 atomic percent to 18 atomic percent, inclusive, so that the proportions of expensive gallium and indium may be lowered. When based on a ternary phase diagram of gallium, indium and tin, tin may be in the range of 5 atomic percent to 20 atomic percent, more preferably in the range of 7 atomic percent to 20 atomic percent.
[0020] Bismuth: 0.8 atomic percent or less Bismuth has a beneficial effect on the fluidity of the alloy. A content of bismuth above 0.8 atomic percent causes a significant and undesirable increase in the melting point. Antimony: 1.4 atomic percent or less Antimony improves oxidation resistance. Contents above 1.4 atomic percent of antimony result in a significant and undesirable increase in the melting point. Antimony, like tin, is a readily available and inexpensive component, while gallium and indium are expensive. The eutectic according to the invention may possibly have only a small content of impurities, such as lead or zinc, of less than 0.001 weight percent, preferably less than 0.0001 weight percent.
[0021] FIG. 3 shows the structure formed by cooling a liquid alloy containing gallium, indium and tin to form a gallium phase and an alloy containing indium and tin. When a liquid ternary alloy containing gallium, indium and tin is applied to an oxide superconductor to bond two oxide superconductors and cooled to below room temperature, the liquid alloy containing gallium, indium and tin is separated into two phases, a gallium phase and an alloy phase containing indium and tin, and the alloy phase containing indium and tin is precipitated at intervals of, for example, 5 to 20 micrometers. This alloy containing indium and tin has an alloy structure containing at least one of the alloys In3Sn and InSn4 depending on the composition ratio of indium and tin, and becomes a superconductor at or below the liquid helium temperature. Therefore, a current can be passed between the two oxide superconductors through the alloy containing indium and tin with zero electrical resistance.
[0022] FIG. 4 is a phase diagram of a binary alloy of indium and tin. In alloys of tin and indium, two intermetallic compounds, In3Sn and InSn4, are produced. The critical temperature of In3Sn is 5.5-6.5 Kelvin, and that of InSn4 is 4.5-5.0 Kelvin. In3Sn and InSn4 have critical temperatures higher than the liquidus temperature of helium, 4.2 Kelvin, and therefore serve as electrical pathways that realize superconducting connections between oxide superconductors. EXAMPLES
[0023] <Example 1> FIG. 5 is a diagram showing a cross-sectional structure of a superconducting joint of an oxide superconductor using a liquid alloy containing gallium, indium, and tin according to one embodiment of the present invention. The oxide superconductor is YBa2Cu3O 6+δ where δ indicates the amount of oxygen vacancies, and is in the range of 0≦δ≦2, for example. In oxide superconductors, there is a correlation between an increase in the amount of oxygen and an increase in the hole concentration. Ideally, 6+δ is 7, but there are also cases where it is slightly greater than 7. From a crystallographic point of view, if all the missing oxygen positions were filled with oxygen, 6+δ would be 8, so 0≦δ≦2 is used. Note that YBa2Cu3O 6+δ For YBa2Cu3O 7-δ (However, it can also be expressed as -1≦δ≦1). In the figure, two oxide superconductors 10 and 12 are YBa2Cu3O 6+δ It is a sintered body of oxide superconductor. Liquid alloy 20 is Ga 78 In 15 The liquid alloy 20 is Sn7 and has dimensions of 0.5 mm in width, 4 mm in depth and 1 mm in height. The two oxide superconductors 10, 12 are butt-jointed by the liquid alloy 20. That is, the two oxide superconductors 10, 12 are electrically connected by the liquid alloy 20 at the opposing ends in the longitudinal direction.
[0024] FIG. 6 is a graph showing the temperature dependence of the electrical resistance of the superconducting joint shown in FIG. 6+δThe electrical resistance decreases near 90 Kelvin, which is the superconducting transition temperature of oxide superconductors, and becomes zero near the liquid helium temperature, and below this temperature the superconducting connection exhibits superconductivity.
[0025] Figure 7 shows the current-voltage characteristics at 3.4 Kelvin of the superconducting joint shown in Figure 5. At currents of 0.3 milliamperes or less, current flows with the voltage remaining at zero, indicating that a superconducting joint is realized below this current.
[0026] <Example 2> FIG. 8 is a diagram showing a cross-sectional structure of a superconducting joint of an oxide superconductor using a liquid alloy containing gallium, indium, and tin according to a second embodiment of the present invention. The oxide superconductor is Bi2Sr2CaCu2O 8+δ where δ indicates the amount of oxygen vacancies, and is in the range of 0≦δ≦2, for example. The crystal structure of bismuth-based materials is complex (it has a modulated structure), so the amount of oxygen vacancies itself is not well understood. From a crystallographic point of view, if all the missing oxygen positions were filled with oxygen, 8+δ would be 10, so 0≦δ≦2 is used. In the figure, two oxide superconductors 30 and 32 are Bi2Sr2CaCu2O 8+δ It is a sintered body of oxide superconductor. Liquid Alloy 40 is Ga 78 In 15 The liquid alloy 40 is Sn7 and has dimensions of 2 mm in width, 2 mm in depth, and 0.1 mm in height. The two oxide superconductors 30, 32 are joined in an overlapping manner by the liquid alloy 40. That is, the two oxide superconductors 30, 32 are electrically connected by the liquid alloy 40 such that the opposing ends in the longitudinal direction partially overlap.
[0027] FIG. 9 is a graph showing the temperature dependence of the electrical resistance of the superconducting joint shown in FIG. 8+δ The electrical resistance decreases near 80 Kelvin, which is the superconducting transition temperature of oxide superconductors, and becomes zero near the liquid helium temperature, and below this temperature the superconducting connection exhibits superconductivity.
[0028] Figure 10 shows the current-voltage characteristics at 3.4 Kelvin of the superconducting joint shown in Figure 8. At currents of 0.025 amperes or less, current flows with the voltage remaining at zero, indicating that a superconducting joint is realized below this current.
[0029] 11 is a diagram showing a superconducting joint structure of oxide superconductors according to another embodiment of the present invention. The superconducting joint structure of oxide superconductors can be (A) a butt joint type, (B) a lap type, or (C) an indirect joint. (A) and (B) are direct bonds, in which the bonding part is made of the same material as the superconductor. (C) Indirect bonds are bonds in which the bonding part is made of a material different from the superconductor.
[0030] In the above embodiment, the oxide superconductor is YBa2Cu3O 6+δ Oxide superconductors and Bi2Sr2CaCu2O 8+δ Although oxide superconductors are shown, the oxide superconductor of the present invention is not limited to these, and may be Bi2Sr2Ca nー1 Cu n O 2n+4+δ (n=1 or 3) Oxide superconductor, rare earth barium copper oxide superconductor {REBa2Cu3O 6+δ or REBa2Cu3O 7-δ (RE is a rare earth element)}, iron-based superconductors {REFeAsO 1-X F X , AFe2As2 (A is an alkali metal or alkaline earth metal), AFeAs}. [Industrial Applicability]
[0031] According to the superconducting connection structure of the oxide superconductor of the present invention, a superconducting connection structure that does not require heat treatment can be obtained, and therefore the structure is suitable for use in nuclear magnetic resonance imaging devices, nuclear magnetic resonance spectroscopy devices, superconducting magnets, power transmission lines, superconducting filters for high-frequency communication, SQUIDs, magnetic field detectors, superconducting linear motors, or motors for ship propulsion. [Explanation of symbols]
[0032] 10, 12 Oxide superconductors {YBa2Cu3O 6+δ} 20 Liquid metal layer (Ga 78 In 15 Sn7) 30, 32 Oxide superconductors {Bi2Sr2CaCu2O 8+δ} 40 Liquid metal layer (Ga 78 In 15 Sn7)
Claims
1. In a superconducting connection structure of oxide superconductors, a liquid alloy made of gallium, indium, and tin or a low-melting-point alloy having a composition range in which the melting point temperature in a thermal equilibrium state is 60° C. or less is sandwiched between two oxide superconductors, The liquid alloy made of gallium, indium and tin or the low melting point alloy having a melting point of 60° C. or less in a thermal equilibrium state has a composition of Ga x In y Sn z A superconducting connection structure characterized in that, when x, y, and z are expressed in atomic percent, the following ranges are satisfied: 60≦x≦70, 5≦y≦25, 5≦z≦20 and x+y+z=100.
2. A superconducting connection structure of oxide superconductors, comprising a liquid alloy consisting of essential elements of gallium, indium, and tin, and optional elements of bismuth of 0.8 atomic percent or less and antimony of 1.4 atomic percent or less, or a low-melting-point alloy having a composition range such that the melting point temperature in a thermal equilibrium state is 60°C or less, sandwiched between two oxide superconductors; The liquid alloy or the low melting point alloy has a composition of Ga x In y Sn z A superconducting connection structure characterized in that, when x, y, and z are expressed in atomic percent, the following ranges are satisfied: 60≦x≦70, 5≦y≦25, 5≦z≦20, and x+y+z={100−[bismuth composition ratio]−[antimony composition ratio]}.
3. The oxide superconductor is a yttrium-based copper oxide high-temperature superconductor (YBa 2 Cu 3 O 6+δ , δ indicates the amount of oxygen vacancy), bismuth-based copper oxide superconductor {Bi 2 Sr 2 Ca nー1 Cu n O 2n+4+δ (n=1, 2 or 3)}, rare earth element-based copper oxide superconductor {REBa 2 CuO 6+δ 3. The superconducting joint structure according to claim 1, characterized in that the superconducting element is one selected from the group consisting of: (RE is a rare earth element).
4. The oxide superconductor is an iron-based superconductor {REFeAsO 1-X F X (RE is a rare earth element), AFe 2 A.S. 2 3. The superconducting joint structure according to claim 1, characterized in that A is one selected from the group consisting of AFeAs, where A is an alkali metal or an alkaline earth metal.
5. A superconducting device having a superconducting joint structure of the oxide superconductor according to any one of claims 1 to 4.
6. 6. The superconducting device according to claim 5, comprising at least one of a superconducting wire, a superconducting coil, a superconducting cavity, and a superconducting electronic element.
7. 7. The superconducting device according to claim 5 or 6, wherein the superconducting device is any one of a nuclear magnetic resonance imaging device, a nuclear magnetic resonance spectrometer, a superconducting magnet, a superconducting power transmission line, a superconducting filter for high frequency communication, a SQUID, a magnetic field detector, a superconducting linear motor, and a superconducting electromagnetic propulsion device for ships.
Citation Information
Patent Citations
Alloy for making electrical binding between superconducting materials and said binding between said superconducting material and conducting material or semiconductor material
JP1991150273A
Superconductive connecting method for oxide type superconductive wire
JP1997082445A
Liquid metal joining material and joining method therefor
JP2015174129A
Transition metal pnictide compound and manufacturing method therefor
JP2016150861A
Superconducting wire junction structure and device therewith
JP2018129294A