Optimized tin source distributed Nb3Sn wire and preparation method thereof

By controlling the Ti element content in the CuNb composite rod and adding alloy elements to Sn, the problems of wire interruption of the distributed tin-source Nb3Sn wire during the stretching process and low critical current density after heat treatment were solved, achieving improvement in wire performance and Reduction in processing difficulty.

CN118800516AActive Publication Date: 2024-10-18XIAN SUPERCONDUCTING WIRE TECHNOLOGIES CO LTD

Patent Information

Application Number
CN202411280433.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-10-18
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing tin source distributed Nb3Sn wire is prone to breakage during the stretching process, and the critical current density is low after heat treatment, which affects the performance of the wire.

Method used

Using an optimized preparation method, the Ti element is introduced into the CuNb composite rod. The Ti element accounts for 1.0~3.0at.% of Nb, and Cu, Zn or Ni elements are added to Sn to improve the tensile properties and heat treatment process of the wire. Avoid the formation of Ti6Sn5 hard compounds and promote the formation of Nb3Sn phase.

Benefits of technology

It effectively improves the tensile properties of the wire, reduces the processing difficulty, significantly increases the critical current density of the wire, and enhances the current carrying capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800516A_ABST
    Figure CN118800516A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of superconducting wires, and discloses an optimized tin source distributed Nb3Sn wire and a preparation method thereof. According to the method, the Ti element is introduced into the CuNb composite rod, and the Ti element accounts for 1.0-3.0 at.% of the Nb element, so that the problem of wire breakage caused by a Ti6Sn5 hard compound in the wire stretching process is avoided, and the maximum wire outlet length of the wire is remarkably increased. Besides, Zn, Ni and other metal elements are added into Sn, Sn-Cu mutual diffusion can be accelerated during heat treatment, generation of an Nb3Sn phase with the uniform stoichiometric ratio is promoted, and the critical current density of the Nb3Sn wire can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting wires and relates to an optimized tin source distributed Nb3Sn wire and a preparation method thereof. Background Art

[0002] High-field superconducting magnets play a very important role in many large-scale physical experiments, especially in particle colliders and fusion confinement devices such as the Large Hadron Collider (LHC) and the International Thermonuclear Experimental Reactor (ITER). Nb3Sn is the most commonly used high-field superconductor in these applications. At present, the production methods of Nb3Sn mainly include the bronze method, the internal tin method and the powder tube method. As a new process route, the tin source distributed Nb3Sn wire can effectively increase the Nb content and the critical current density of the wire, while reducing the size of the Nb module, shortening the tin source diffusion distance, and reducing the wire loss. In addition, compared with other internal tin method Nb3Sn wire preparation methods, the tin source distributed Nb3Sn wire also eliminates the drilling step in the wire processing process, effectively shortening the wire processing cycle and reducing the wire processing cost.

[0003] During the preparation of Nb3Sn wire by the internal tin method, the Ti element is usually introduced. The addition of the Ti element can increase the rate of Sn-Cu interdiffusion and promote the formation of the Nb3Sn phase. During the preparation process, the Ti element is usually added to Sn. However, the Ti6Sn5 carbide block in the SnTi alloy has poor plastic deformation ability during the wire drawing process, which leads to wire breakage under smaller stretching conditions. During the medium-temperature stage of the final heat treatment of the wire, the Ti element in the SnTi alloy will be enriched around the Nb module, hindering the diffusion of Sn to the Nb core wire, thereby affecting the critical current density of the final wire. This requires further improvement of the existing tin source distributed Nb3Sn wire to solve the above-mentioned problems. Summary of the invention

[0004] In order to improve the tensile performance and critical current density of tin source distributed Nb3Sn wire and solve the problems of wire breakage during the tensile process and low critical current density after heat treatment of the existing tin source distributed Nb3Sn wire, the present invention provides an optimized tin source distributed Nb3Sn wire and a preparation method thereof.

[0005] In one aspect, the present invention provides a method for preparing an optimized tin source distributed Nb3Sn wire, the preparation method comprising: S1. Assemble the NbTi / Cu single core rod 100 and the Nb / Cu single core rod 200 in the oxygen-free copper sheath 300 to obtain a CuNb composite ingot containing the NbTi / Cu single core rod, and obtain a CuNb composite rod 600 containing a NbTi alloy after processing; in the CuNb composite ingot containing the NbTi / Cu single core rod, the Ti element accounts for 1.0~3.0at.% of the Nb element content.

[0006] S2. Obtain a Sn-X alloy rod through the processes of smelting, turning, machining, extrusion, drawing, forming and stretching, cutting to length, and straightening; load the Sn-X alloy rod into an oxygen-free copper tube, and obtain a Sn-X / Cu single core rod 500 through multiple cold drawing, forming, cutting to length, and straightening; in the Sn-X alloy rod, X is selected from Cu, Zn, and Ni, and the content of X is ≤5wt.%; the cross section of the Sn-X / Cu single core rod 500 is hexagonal or fan-shaped; the Sn-X / Cu single core rod 500 has the same specifications as the CuNb composite rod 600 containing NbTi alloy.

[0007] S3. Arrange and assemble the CuNb composite rod 600 containing NbTi alloy and the Sn-X / Cu single core rod 500 in the barrier layer material 400 in a hexagonal close-packed manner, so that except for the Sn-X / Cu single core rod 500 at the edge position, each Sn-X / Cu single core rod 500 is surrounded by 6 CuNb composite rods 600 containing NbTi alloy adjacent to it, and then pass through the outer layer of copper 700 to obtain an optimized tin source distributed Nb3Sn composite ingot.

[0008] S4. Processing the optimized tin source distributed Nb3Sn composite ingot to obtain an optimized tin source distributed Nb3Sn wire.

[0009] In S1 of the above preparation method, the preparation method of the NbTi / Cu single core rod 100 includes: placing a NbTi alloy ingot into an oxygen-free copper sheath to obtain a NbTi / Cu single core ingot, and performing degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain the NbTi / Cu single core rod 100; the Ti content of the NbTi alloy ingot is 30~60wt.%; the copper ratio of the prepared NbTi / Cu single core rod 100 is 0.20~0.50.

[0010] In S1 of the above preparation method, the preparation method of the Nb / Cu single core rod 200 includes: placing a Nb ingot into an oxygen-free copper sheath to obtain a Nb / Cu single core ingot, and performing degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain the Nb / Cu single core rod 200.

[0011] In S1 of the above preparation method, the NbTi / Cu single core rod 100 and the Nb / Cu single core rod 200 are assembled to satisfy the following conditions: the NbTi / Cu single core rod 100 is close to the edge and symmetrically distributed in the CuNb composite ingot containing the NbTi / Cu single core rod.

[0012] In S1 of the above preparation method, the processing of the CuNb composite ingot containing the NbTi / Cu single core rod includes: degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length, and straightening.

[0013] In S3 of the above preparation method, the barrier layer material 400 is a Nb or Ta alloy tube; and the outer layer copper 700 is an oxygen-free copper tube or an oxygen-free copper sheath.

[0014] In S3 of the above-mentioned preparation method, the edge position is filled with a Sn—X / Cu single core rod 500 having a fan-shaped cross section.

[0015] In S3 of the above preparation method, when the diameter of the optimized tin source distributed Nb3Sn composite ingot is ≤75mm, it is loaded into an oxygen-free copper tube, and subjected to multiple drawing, twisting, final stretching, chrome plating and heat treatment to obtain the optimized tin source distributed Nb3Sn wire; when the diameter of the optimized tin source distributed Nb3Sn composite ingot is greater than 75mm, it is loaded into an oxygen-free copper sheath, and covered with upper and lower covers, and then subjected to vacuum electron beam welding, hydrostatic extrusion, multiple drawing, twisting, final stretching, chrome plating and heat treatment in sequence to obtain the optimized tin source distributed Nb3Sn wire.

[0016] On the other hand, the present invention claims protection for an optimized tin source distributed Nb3Sn wire prepared by the above method.

[0017] Compared with the prior art, the present invention "an optimized tin source distributed Nb3Sn wire and its preparation method" has at least the following beneficial effects: In the preparation process of the tin source distributed Nb3Sn wire, the present invention avoids the use of SnTi alloy containing Ti6Sn5 hard compounds, introduces Ti elements into the CuNb composite rod, and makes the percentage of Ti elements to Nb elements between 1.0 and 3.0 at.%, thereby avoiding the wire breakage problem caused by the Ti6Sn5 hard compounds during the wire drawing process and reducing the difficulty of wire processing.

[0018] The present invention adds Cu, Zn or Ni elements to Sn, which can increase the rate of Sn-Cu mutual diffusion during wire heat treatment, promote the formation of Nb3Sn, and also facilitate the formation of Nb3Sn phase with uniform stoichiometric ratio, thereby effectively improving the critical current density of Nb3Sn wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of the cross section of a CuNb composite ingot containing a NbTi / Cu single core rod.

[0020] Figure 2 Schematic diagram of the cross section of the optimized tin source distributed Nb3Sn composite ingot.

[0021] Figure 3 The critical current density of the optimized tin source distributed Nb3Sn wire changes under different Ti element contents.

[0022] Explanation of the reference numerals: 100 is a NbTi / Cu single core rod; 200 is a Nb / Cu single core rod, 300 is an oxygen-free copper sheath; 400 is a barrier layer material, 500 is a Sn-X / Cu single core rod, 600 is a CuNb composite rod containing a NbTi alloy, and 700 is an outer layer of copper. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The embodiment of the present invention provides a method for preparing an optimized tin source distributed Nb3Sn wire, the method comprising: S1. Assemble the NbTi / Cu single core rod 100 and the Nb / Cu single core rod 200 in the oxygen-free copper sheath 300 to obtain a CuNb composite ingot containing the NbTi / Cu single core rod, and obtain a CuNb composite rod 600 containing a NbTi alloy after processing; in the CuNb composite ingot containing the NbTi / Cu single core rod, the Ti element accounts for 1.0~3.0at.% of the Nb element content.

[0025] S2. Obtain a Sn-X alloy rod through the processes of smelting, turning, machining, extrusion, drawing, forming and stretching, cutting to length, and straightening; load the Sn-X alloy rod into an oxygen-free copper tube, and obtain a Sn-X / Cu single core rod 500 through multiple cold drawing, forming, cutting to length, and straightening; in the Sn-X alloy rod, X is selected from Cu, Zn, and Ni, and the content of X is ≤5wt.%; the cross section of the Sn-X / Cu single core rod 500 is hexagonal or fan-shaped; the Sn-X / Cu single core rod 500 has the same specifications as the CuNb composite rod 600 containing NbTi alloy.

[0026] S3. Arrange and assemble the CuNb composite rod 600 containing NbTi alloy and the Sn-X / Cu single core rod 500 in the barrier layer material 400 in a hexagonal close-packed manner, so that except for the Sn-X / Cu single core rod 500 at the edge position, each Sn-X / Cu single core rod 500 is surrounded by 6 CuNb composite rods 600 containing NbTi alloy adjacent to it, and then pass through the outer layer of copper 700 to obtain an optimized tin source distributed Nb3Sn composite ingot.

[0027] S4. Processing the optimized tin source distributed Nb3Sn composite ingot to obtain an optimized tin source distributed Nb3Sn wire.

[0028] Illustratively, in S1 of the above-mentioned preparation method, the preparation method of the NbTi / Cu single core rod 100 includes: placing a NbTi alloy ingot into an oxygen-free copper sheath to obtain a NbTi / Cu single core ingot, and performing degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain the NbTi / Cu single core rod 100; the Ti content of the NbTi alloy ingot is 30~60wt.%; the copper ratio of the prepared NbTi / Cu single core rod 100 is 0.20~0.50.

[0029] Illustratively, in S1 of the above-mentioned preparation method, the preparation method of the Nb / Cu single core rod 200 includes: placing a Nb ingot into an oxygen-free copper sheath to obtain a Nb / Cu single core ingot, and performing degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a Nb / Cu single core rod 200.

[0030] Illustratively, in S1 of the above preparation method, the NbTi / Cu single core rod 100 and the Nb / Cu single core rod 200 are assembled to satisfy: the NbTi / Cu single core rod 100 is close to the edge and symmetrically distributed in the CuNb composite ingot containing the NbTi / Cu single core rod.

[0031] Illustratively, in S1 of the above preparation method, the processing of the CuNb composite ingot containing the NbTi / Cu single core rod includes: degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length, and straightening.

[0032] Illustratively, in S3 of the above preparation method, the barrier layer material 400 is a Nb or Ta alloy tube; and the outer layer copper 700 is an oxygen-free copper tube or an oxygen-free copper sheath.

[0033] Exemplarily, in S3 of the above preparation method, the edge position is filled with a Sn—X / Cu single core rod 500 having a fan-shaped cross section.

[0034] Exemplarily, in S3 of the above preparation method, when the diameter of the optimized tin source distributed Nb3Sn composite ingot is ≤75mm, it is loaded into an oxygen-free copper tube, and subjected to multiple drawing, twisting, final stretching, chrome plating and heat treatment to obtain the optimized tin source distributed Nb3Sn wire; when the diameter of the optimized tin source distributed Nb3Sn composite ingot is greater than 75mm, it is loaded into an oxygen-free copper sheath, and covered with upper and lower covers, and then successively subjected to vacuum electron beam welding, hydrostatic extrusion, multiple drawing, twisting, final stretching, chrome plating and heat treatment to obtain the optimized tin source distributed Nb3Sn wire.

[0035] Example 1 This embodiment provides a method for preparing an optimized tin source distributed Nb3Sn wire.

[0036] Step 1: Put a Nb30Ti alloy ingot (Ti content is 30wt.%) into an oxygen-free copper sheath, cover the upper and lower covers to obtain a NbTi / Cu single-core ingot, and obtain a hexagonal NbTi / Cu single-core rod 100 through degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening; the copper ratio of the NbTi / Cu single-core rod 100 is 0.40, and the size is H5.00mm.

[0037] Step 2: Place the Nb ingot into an oxygen-free copper sheath, cover the upper and lower covers to obtain a Nb / Cu single-core ingot, and undergo degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a Nb / Cu single-core rod 200 having the same specifications as the NbTi / Cu single-core rod 100 in step 1.

[0038] Step 3: After cleaning, the four NbTi / Cu single core rods 100 and the 195 Nb / Cu single core rods 200 are Figure 1 In the manner shown, the CuNb composite ingot containing a single core rod of NbTi / Cu is assembled in an oxygen-free copper sheath 300 to obtain a CuNb composite ingot containing a single core rod of NbTi / Cu. In the CuNb composite ingot containing a single core rod of NbTi / Cu, the Ti element accounts for 1.0 at.% of the Nb element content. The CuNb composite ingot containing a single core rod of NbTi / Cu is subjected to degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a hexagonal CuNb composite rod 600 containing a NbTi alloy. The total number of cores of the CuNb composite rod 600 containing a NbTi alloy is 199, and the size is H2.00×1000mm.

[0039] Step 4: Obtain a Sn-Zn alloy rod through the processes of smelting, turning, machining, extrusion, drawing, forming and stretching, cutting to length, and straightening; the Sn-Zn alloy rod has a Zn content of 5wt.%. The Sn-Zn alloy rod is loaded into a cleaned oxygen-free copper tube, and subjected to multiple cold drawing, forming, cutting to length, and straightening to obtain a Sn-Zn / Cu single core rod 500; the size of the Sn-Zn / Cu single core rod 500 is the same as that of the CuNb composite rod 600 containing the NbTi alloy.

[0040] Step 5: After cleaning, 138 CuNb composite rods 600 containing NbTi alloy and 61 hexagonal Sn-Zn / Cu single core rods 500 are arranged and assembled in a Ta alloy tube of size Φ34 / Φ32×1000mm in a hexagonal close-packed manner, and the edge is filled with 12 cleaned fan-shaped Sn-Zn / Cu single core rods 500, so that except for the Sn-Zn / Cu single core rods 500 at the edge position, each Sn-Zn / Cu single core rod 500 is surrounded by 6 CuNb composite rods 600 containing NbTi alloy adjacent to it, as shown in FIG. Figure 2 As shown. Then, it passes through an oxygen-free copper tube with a size of Φ50 / Φ35×1000mm to obtain an optimized tin source distributed Nb3Sn composite ingot. The diameter of the optimized tin source distributed Nb3Sn composite ingot is Φ50mm (i.e., the outer diameter of the oxygen-free copper tube).

[0041] Step 6: The optimized tin source distributed Nb3Sn composite ingot is subjected to multiple drawing, twisting, final stretching, chrome plating and heat treatment to obtain an optimized tin source distributed Nb3Sn wire. The critical current density of the optimized tin source distributed Nb3Sn wire is: 2310A / mm 2 .

[0042] Example 2 This embodiment provides a method for preparing an optimized tin source distributed Nb3Sn wire.

[0043] Step 1: Put a Nb47Ti alloy ingot (Ti content is 47wt.%) into an oxygen-free copper sheath, cover the upper and lower covers to obtain a NbTi / Cu single-core ingot, and obtain a hexagonal NbTi / Cu single-core rod 100 through degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening; the copper ratio of the NbTi / Cu single-core rod 100 is 0.30, and the size is H5.00mm.

[0044] Step 2: Place the Nb ingot into an oxygen-free copper sheath, cover the upper and lower covers to obtain a Nb / Cu single-core ingot, and undergo degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a Nb / Cu single-core rod 200 having the same specifications as the NbTi / Cu single-core rod 100 in step 1.

[0045] Step 3: After cleaning, 6 NbTi / Cu single core rods 100 and 307 Nb / Cu single core rods 200 are assembled in an oxygen-free copper sheath 300 to obtain a CuNb composite ingot containing NbTi / Cu single core rods. In the CuNb composite ingot containing NbTi / Cu single core rods, the Ti element accounts for 2.0 at.% of the Nb element content. The CuNb composite ingot containing NbTi / Cu single core rods is subjected to degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a hexagonal CuNb composite rod 600 containing NbTi alloy. The total number of cores of the CuNb composite rod 600 containing NbTi alloy is 313, and the size is H6.00×2000mm.

[0046] Step 4: Obtain a Sn-Ni alloy rod through the processes of smelting, turning, machining, extrusion, drawing, forming and stretching, cutting to length, and straightening; the content of Ni in the Sn-Ni alloy rod is 3wt.%. The Sn-Ni alloy rod is loaded into a cleaned oxygen-free copper tube, and subjected to multiple cold drawing, forming, cutting to length, and straightening to obtain a Sn-Ni / Cu single core rod 500; the size of the Sn-Ni / Cu single core rod 500 is the same as that of the CuNb composite rod 600 containing the NbTi alloy.

[0047] Step 5: After cleaning, 84 CuNb composite rods 600 containing NbTi alloy and 37 hexagonal Sn-Ni / Cu single core rods 500 are arranged and assembled in a Nb alloy tube with a size of Φ76 / Φ74×600mm in a hexagonal close-packed manner, and the edge is filled with 6 cleaned fan-shaped Sn-Ni / Cu single core rods 500, so that except for the Sn-Ni / Cu single core rods 500 at the edge position, each Sn-Ni / Cu single core rod 500 is surrounded by 6 CuNb composite rods 600 containing NbTi alloy adjacent to it. Then, pass through an oxygen-free copper sheath with a size of Φ110 / Φ77×660mm, cover with upper and lower covers, and obtain an optimized tin source distributed Nb3Sn composite ingot. The diameter of the optimized tin source distributed Nb3Sn composite ingot is Φ110mm.

[0048] Step 6: The optimized tin source distributed Nb3Sn composite ingot is subjected to vacuum electron beam welding, hydrostatic extrusion, multi-pass drawing, twisting, final stretching, chrome plating and heat treatment in sequence to obtain an optimized tin source distributed Nb3Sn wire. The critical current density of the optimized tin source distributed Nb3Sn wire is: 2470A / mm 2 .

[0049] Example 3 This embodiment provides a method for preparing an optimized tin source distributed Nb3Sn wire.

[0050] Step 1: Put a Nb60Ti alloy ingot (Ti content is 60wt.%) into an oxygen-free copper sheath, cover the upper and lower covers to obtain a NbTi / Cu single-core ingot, and obtain a hexagonal NbTi / Cu single-core rod 100 through degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening; the copper ratio of the NbTi / Cu single-core rod 100 is 0.50, and the size is H5.00mm.

[0051] Step 2: Place the Nb ingot into an oxygen-free copper sheath, cover the upper and lower covers to obtain a Nb / Cu single-core ingot, and undergo degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a Nb / Cu single-core rod 200 having the same specifications as the NbTi / Cu single-core rod 100 in step 1.

[0052] Step 3: After cleaning, 18 NbTi / Cu single core rods 100 and 937 Nb / Cu single core rods 200 are assembled in an oxygen-free copper sheath 300 to obtain a CuNb composite ingot containing NbTi / Cu single core rods. In the CuNb composite ingot containing NbTi / Cu single core rods, the Ti element accounts for 3.0 at.% of the Nb element content. The CuNb composite ingot containing NbTi / Cu single core rods is subjected to degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a hexagonal CuNb composite rod 600 containing NbTi alloy. The total number of cores of the CuNb composite rod 600 containing NbTi alloy is 955, and the size is H10.00×500mm.

[0053] Step 4: Obtain a Sn-Cu alloy rod through the processes of smelting, turning, machining, extrusion, drawing, forming and stretching, cutting to length, and straightening; the content of Cu in the Sn-Cu alloy rod is 2wt.%. The Sn-Cu alloy rod is loaded into a cleaned oxygen-free copper tube, and subjected to multiple cold drawing, forming, cutting to length, and straightening to obtain a Sn-Cu / Cu single core rod 500; the size of the Sn-Cu / Cu single core rod 500 is the same as that of the CuNb composite rod 600 containing the NbTi alloy.

[0054] Step 5: After cleaning, 84 CuNb composite rods 600 containing NbTi alloy and 37 hexagonal Sn-Cu / Cu single core rods 500 are arranged and assembled in a Ta alloy tube with a size of Φ125 / Φ123×500mm in a hexagonal close-packed manner, and the edge is filled with 6 cleaned fan-shaped Sn-Cu / Cu single core rods 500, so that except for the Sn-Cu / Cu single core rods 500 at the edge position, each Sn-Cu / Cu single core rod 500 is surrounded by 6 CuNb composite rods 600 containing NbTi alloy adjacent to it. Then, pass through an oxygen-free copper sheath with a size of Φ180 / Φ126×560mm, cover with upper and lower covers, and obtain an optimized tin source distributed Nb3Sn composite ingot. The diameter of the optimized tin source distributed Nb3Sn composite ingot is Φ180mm.

[0055] Step 6: The optimized tin source distributed Nb3Sn composite ingot is subjected to vacuum electron beam welding, hydrostatic extrusion, multi-pass drawing, twisting, final stretching, chrome plating and heat treatment in sequence to obtain an optimized tin source distributed Nb3Sn wire. The critical current density of the optimized tin source distributed Nb3Sn wire is: 2630A / mm 2 .

[0056] Example 4 This example describes the performance comparison between the optimized tin source distributed Nb3Sn wire prepared in Examples 1 to 3 and the ordinary Nb3Sn wire produced by the prior art.

[0057] Table 1. Test results of Nb3Sn wire performance provided by the present invention

[0058] As shown in Table 1, compared with ordinary Nb3Sn wires, the maximum wire length of the Nb3Sn wires prepared in Examples 1 to 3 is significantly increased, indicating that the processing difficulty of the wires is reduced, and the wire breakage problem of Ti6Sn5 during the stretching process is avoided. In addition, the critical current density of the Nb3Sn wire is significantly increased, indicating that the wires have excellent current carrying capacity.

[0059] Example 5 This embodiment describes the change of the critical current density of the optimized tin source distributed Nb3Sn wire under different Ti element contents.

[0060] Figure 3 The critical current density of the optimized tin source distributed Nb3Sn wire corresponding to different Ti content (0.5~3.5at.%) in the CuNb composite ingot containing NbTi / Cu single core rod was statistically analyzed. Figure 3It can be seen that the critical current density increases first and then decreases, and reaches a peak value when the Ti content is about 1.5 at.%; when the Ti content is less than 1.0 at.% or greater than 3.0 at.%, the critical current density shows a significant attenuation. It can be seen that when the Ti content is between 1.0 and 3.0 at.%, it is more conducive to improving the critical current density of the optimized tin source distributed Nb3Sn wire.

[0061] The embodiments described above are only some embodiments of the present invention, not all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but only represents selected embodiments of the present invention. All other embodiments obtained without creative work and related deductions and substitutions made by ordinary technicians in the field under the conditions of the concept of the present invention belong to the scope of protection of the present invention.

Claims

1. A method for preparing an optimized tin source distributed Nb3Sn wire, characterized in that: include: S1. Assembling a NbTi / Cu single core rod (100) and a Nb / Cu single core rod (200) in an oxygen-free copper sheath (300) to obtain a CuNb composite ingot containing the NbTi / Cu single core rod, and processing to obtain a CuNb composite rod (600) containing a NbTi alloy; In the CuNb composite ingot containing the NbTi / Cu single core rod, the Ti element accounts for 1.0-3.0 at.% of the Nb element content; S2. Obtaining a Sn-X alloy rod by smelting, turning, machining, extrusion, drawing, forming and stretching, cutting to length, and straightening; loading the Sn-X alloy rod into an oxygen-free copper tube, and subjecting the tube to multiple cold drawing, forming, cutting to length, and straightening to obtain a Sn-X / Cu single core rod (500); In the Sn-X alloy rod, X is selected from Cu, Zn, and Ni, and the content of X is ≤5wt.%; The cross section of the Sn-X / Cu single core rod (500) is hexagonal or fan-shaped; The Sn-X / Cu single core rod (500) and the CuNb composite rod (600) containing NbTi alloy have the same specifications; S3. Arranging and assembling the CuNb composite rod (600) containing NbTi alloy and the Sn-X / Cu single core rod (500) in a hexagonal close-packed manner in the barrier layer material (400), so that, except for the Sn-X / Cu single core rod (500) at the edge position, each Sn-X / Cu single core rod (500) is surrounded by 6 CuNb composite rods (600) containing NbTi alloy adjacent to it, and then passing through the outer layer of copper (700) to obtain an optimized tin source distributed Nb3Sn composite ingot; S4. Processing the optimized tin source distributed Nb3Sn composite ingot to obtain an optimized tin source distributed Nb3Sn wire.

2. The preparation method according to claim 1, characterized in that: In S1, the method for preparing the NbTi / Cu single core rod (100) comprises: placing a NbTi alloy ingot into an oxygen-free copper sheath to obtain a NbTi / Cu single core ingot, and performing degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length cutting, and straightening to obtain a NbTi / Cu single core rod (100); the Ti content of the NbTi alloy ingot is 30-60wt.%; and the copper ratio of the prepared NbTi / Cu single core rod (100) is 0.20-0.

50.

3. The preparation method according to claim 1, characterized in that: In S1, the method for preparing the Nb / Cu single core rod (200) comprises: placing a Nb ingot into an oxygen-free copper sheath to obtain a Nb / Cu single core ingot, and performing degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cutting to length, and straightening to obtain a Nb / Cu single core rod (200).

4. The preparation method according to claim 1, characterized in that: In S1, the NbTi / Cu single core rod (100) and the Nb / Cu single core rod (200) are assembled to satisfy the following conditions: the NbTi / Cu single core rod (100) is close to the edge and symmetrically distributed in the CuNb composite ingot containing the NbTi / Cu single core rod.

5. The preparation method according to claim 1, characterized in that: In S1, the processing of the CuNb composite ingot containing the NbTi / Cu single core rod includes: degassing, vacuum electron beam welding, hot isostatic pressing, extrusion, multi-pass drawing, hexagonal forming, cut-to-length, and straightening.

6. The preparation method according to claim 1, characterized in that: In S3, the barrier layer material (400) is a Nb or Ta alloy tube; and the outer layer copper (700) is an oxygen-free copper tube or an oxygen-free copper sheath.

7. The preparation method according to claim 1, characterized in that: In S3, the edge position is filled with a Sn-X / Cu single core rod (500) having a fan-shaped cross section.

8. The preparation method according to claim 1, characterized in that: In S3, when the diameter of the optimized tin source distributed Nb3Sn composite ingot is ≤75 mm, it is loaded into an oxygen-free copper tube, and subjected to multiple drawing, twisting, final stretching, chrome plating and heat treatment to obtain the optimized tin source distributed Nb3Sn wire; When the diameter of the optimized tin source distributed Nb3Sn composite ingot is greater than 75mm, it is placed in an oxygen-free copper sheath and covered with upper and lower covers, and then sequentially undergoes vacuum electron beam welding, hydrostatic extrusion, multi-pass drawing, twisting, final stretching, chrome plating and heat treatment to obtain the optimized tin source distributed Nb3Sn wire.

9. An optimized tin source distributed Nb3Sn wire, characterized in that: The method according to claim 1 is used to prepare the product.

Citation Information

Patent Citations

  • Preparation method for NbTi / Cu multi-core composite superconducting wire with rectangular section

    CN101728029A

  • Method for preparing high-field Nb3Sn superconducting strand with Nb47Ti bar to add Ti

    CN102339664A

  • High strength hot-dip galvanized steel sheet with superior workability and production method therefor

    CN102859022A

  • Method for improving deformation uniformity of core wires of NbTi / Cu superconducting wire

    CN108735388A

  • Preparation method of short-range diffusion type Nb3Sn superconducting wire

    CN114694894A

Cited By

  • Low-cost internal tin method Nb3Sn CuNb composite sheath assembling method

    CN119361233A

  • Double-distributed Nb3Sn wire and preparation method thereof

    CN121545843A