Semi-flexible paving composition

A semi-flexible pavement composition with ecocement, expanding agents, and controlled water content addresses bending strength issues, enhancing durability and environmental sustainability.

JP7554020B2Active Publication Date: 2024-09-19TAIHEIYO CEMENT CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020179509
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-09-19
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

Conventional semi-flexible pavements using ecocement suffer from insufficient bending strength, particularly in high-traffic areas, and existing compositions do not adequately leverage the environmental benefits of ecocement.

Method used

A semi-flexible pavement composition incorporating ecocement, expanding agents, shrinkage reducing agents, and controlled water content, optimized to enhance bending strength and filling properties.

Benefits of technology

The composition achieves high bending strength and expands the use of ecocement, contributing to reduced environmental loads by utilizing waste materials effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554020000001
    Figure 0007554020000001
  • Figure 0007554020000002
    Figure 0007554020000002
Patent Text Reader

Abstract

To provide a composition for semiflexible pavement having a high flexural strength.SOLUTION: The composition for semiflexible pavement at least comprises one or more kinds selected from a swelling agent and a shrinkage reducing agent, an injection material for semiflexible pavement including ecocement, and water. Preferably, the content of the injection material for semiflexible pavement is 1,500 to 1,900 kg relative to 1 m3 of the composition for semiflexible pavement, and the content of the swelling agent is 10 to 60 kg relative to 1 m3 of the composition for semiflexible pavement.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to semi-flexible paving compositions having high flexural strength. [Background technology]

[0002] Semi-flexible pavement is a pavement in which the voids in the open-graded asphalt mixture are filled with cement milk (slurry of cement injection material for semi-flexible pavement). Open-graded asphalt mixtures have high conformability and flexibility, and the hardened cement milk has high rigidity, so semi-flexible pavement made of these has superior plastic deformation resistance and durability compared to asphalt pavement. Furthermore, reducing the water-powder ratio of the cement milk increases the bending strength of the hardened cement milk, which tends to improve the plastic deformation resistance of the semi-flexible pavement.

[0003] Several semi-flexible paving materials and injection materials for semi-flexible paving have been proposed in the past. The mixed semi-flexible paving material described in Patent Document 1 is a paving material made by mixing asphalt-coated aggregate, in which 3 to 15 parts by weight of asphalt is coated per 100 parts by weight of aggregate, cement paste formulated so that the volume ratio of the asphalt-coated aggregate is 60 to 90 and the volume ratio of the cement paste is 40 to 10, and a cement polymer as an additive. In addition, the semi-flexible paving material described in Patent Document 2 is a semi-flexible paving material containing cement, a hardening agent, and a non-reemulsifiable fine powder elastic polymer, in which the hardening agent contains calcium aluminate and sulfate and is present in an amount of 10 to 25 parts by weight per 100 parts by weight of the cement and the hardening agent, and the non-reemulsifiable fine powder elastic polymer is present in an amount of 2 to 10 parts by weight per 100 parts by weight of the cement and the hardening agent. Moreover, the semi-flexible pavement injection material described in Patent Document 3 is an injection material containing cement, calcium carbonate powder, re-emulsifiable powdered resin, and a water-reducing agent.

[0004] However, conventional semi-flexible pavements are prone to deterioration in areas with heavy traffic loads such as parking and stopping of large vehicles. In addition, even if the water-powder ratio of cement milk is reduced, the bending strength of the hardened body is not necessarily high in the case of the type of cement milk that uses ecocement (P2 in Table 1) (comparative example in Table 2), so the bending strength of the semi-flexible pavement material that uses this cement milk cannot be said to be sufficient. Ecocement is a cement made from various waste materials such as municipal waste incineration ash and sludge, instead of natural raw materials such as limestone, clay, and silica, which are the raw materials for Portland cement, and has the advantage of reducing the environmental burden, such as the burden of waste disposal, by turning these waste materials into resources, which is beneficial from the perspective of environmental protection. Therefore, if we can increase the amount of cement milk, including ecocement, it is expected to greatly contribute to reducing the environmental burden. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-302516 A [Patent Document 2] Japanese Patent Application Publication No. 11-228205 [Patent Document 3] Japanese Patent Application Publication No. 11-278901 Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, an object of the present invention is to provide a semi-flexible paving composition that has high bending strength even when ecocement is used. [Means for solving the problem]

[0007] The present inventors have investigated semi-flexible paving compositions that meet the above-mentioned objectives, and have found that a cured product of the semi-flexible paving composition having the following composition has high bending strength, thereby completing the present invention. [1] Semi-flexible paving composition 1m 3 30 to 50 kg of expansive material , semi-flexible pavement injection materials including ecocement, and A semi-flexible paving composition comprising at least water. [2] The content of the injection material for semi-flexible paving is 1 m 3 The semi-flexible paving composition according to [1] above, wherein the load is 1500 to 1900 kg per unit area. [3] The expanding material is one or more selected from lime-based expanding materials and calcium sulfoaluminate-based expanding materials, or [2] 2. A semi-flexible paving composition as described in claim 1. [4] The water content is 1 m 3 The weight of the above [1] to [ 3 ] A semi-flexible paving composition according to any one of the preceding claims. Effect of the Invention

[0008] The semi-flexible paving composition of the present invention has high bending strength. Furthermore, the semi-flexible paving composition of the present invention can expand the applications of ecocement, thereby contributing to reducing the environmental load.

[0009] The semi-flexible paving composition of the present invention will now be described in detail. As described above, the semi-flexible paving composition of the present invention is a cement composition that contains at least one selected from the group consisting of expansive agents and shrinkage reducing agents, a semi-flexible paving injection material containing ecocement, and water. The content of ecocement in the semi-flexible paving grout is preferably 10-50% by mass, with the semi-flexible paving grout being 100% by mass. If the content of ecocement is within the above range, the bending strength of the semi-flexible paving composition is high. The content of ecocement is more preferably 30-40% by mass.

[0010] The content of the injection material for semi-flexible paving in the semi-flexible paving composition is 1 / m 3When the content of the semi-flexible paving grout is within the above range, the semi-flexible paving composition has high filling ability and bending strength. 3 On the other hand, the weight is more preferably 1550 to 1850 kg, and further preferably 1650 to 1800 kg. The semi-flexible pavement injection material is mainly composed of cement and limestone, and commercially available products include Ultrapack H and High Strength Semi-Flexible Paving Cement Injection Material - Ecocement Type (both manufactured by Chichibu Concrete Industry Co., Ltd.).

[0011] The content of the expansive material is 1 m 3 The content of the expansive agent is preferably 10 to 60 kg per 1 m of the semi-flexible pavement composition. If the content of the expansive agent is less than 10 kg, the expansion of the cement milk is small, so that the restraining force of the open-graded asphalt mixture against the expansion of the cement milk is small, and if the content of the expansive agent is more than 60 kg, the expansion of the cement milk is too large, so that the restraining force of the open-graded asphalt mixture against the expansion of the cement milk becomes excessively large, and in either case, the bending strength of the semi-flexible pavement is small. The content of the expansive agent is preferably 10 to 60 kg per m of the semi-flexible pavement composition. 3 On the other hand, the weight is more preferably 20 to 50 kg, further preferably 20 to 40 kg, and particularly preferably 30 to 40 kg. It is preferable to add the expansive additive to the semi-flexible paving injection material as a percentage of the total powder content, which ensures good filling of the semi-flexible paving composition into the open-graded asphalt mixture. The expanding agent may be a lime-based expanding agent or a calcium sulfoaluminate-based expanding agent. Commercially available products of these include lime-based expanding agents such as Taiheiyo Expan (registered trademark, manufactured by Taiheiyo Materials Co., Ltd.) and calcium sulfoaluminate-based expanding agents such as Denka CSA (manufactured by Denka Co., Ltd.).

[0012] The content of the shrinkage reducing agent in the semi-flexible paving composition is 1 / m 3The shrinkage reducing agent content is preferably 3 to 15 kg per 1 m of semi-flexible paving composition. If the shrinkage reducing agent content is within the above range, the effect of suppressing cracks due to shrinkage reduction is high. 3 In contrast, the weight is more preferably 4 to 12 kg, and further preferably 6 to 9 kg. The shrinkage reducing agent contains polyoxyalkylene alkyl ether as an active ingredient and has the effect of reducing drying shrinkage of semi-flexible pavement. Specific examples of the compound include one or more selected from polyethylene glycol polypropylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polyethylene glycol polypropylene glycol monoethyl ether, polyethylene glycol monoethyl ether, polyethylene glycol polypropylene glycol monopropyl ether, polyethylene glycol monopropyl ether, polyethylene glycol polypropylene glycol monobutyl ether, polyethylene glycol monobutyl ether, etc.

[0013] The water content in the semi-flexible paving composition is 1 / m 3 When the water content is within the above range, the semi-flexible paving composition has high filling property and bending strength. 3 On the other hand, it is more preferably 340 to 410 kg, and further preferably 360 to 380 kg. EXAMPLES

[0014] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. 1. Preparation of cement milk and measurement of cement milk flow (fluidity) Using each component of the semi-flexible paving composition shown in Table 1, each material was mixed with a hand mixer according to the formulation shown in Table 2 to prepare cement milk. Next, the flow of the cement milk was measured according to JSCE-F521 "Test method for fluidity of injection mortar for prepacked concrete" (P funnel method). As shown in Table 2, the flow of the cement milk for all the blends met the target flow time of 20 to 30 seconds.

[0015] 2. Measurement of the expansion of cement milk A polyester film was placed inside a steel formwork measuring 10 cm in length, 10 cm in width, and 40 cm in length, and both ends of the film were sandwiched between a polystyrene board and a wooden board about 1 mm thick, and a Teflon (registered trademark) sheet was placed on the bottom of the formwork to reduce friction. Next, an embedded type strain gauge with temperature measurement function (KM-100BT, manufactured by Tokyo Measuring Instruments Laboratory) was fixed to the formwork using a cable tie, and the cement milk was poured in and sealed and cured at 20°C, and the expansion amount of the cement milk was measured. The results are shown in Table 2.

[0016] 3. Preparation of specimens and measurement of bending strength In a formwork measuring 30 cm in length, 30 cm in width, and 5 cm in height, an asphalt base material with a design void ratio of 25% was compacted using a tamper, and the cement milk was then infiltrated into the asphalt base material using a table vibrator. Next, the material was demolded after 1 day of age, and then subjected to moist air curing at 20°C for 7 days to obtain a hardened body. Furthermore, a test specimen measuring 150 mm in length, 100 mm in width, and 50 mm in thickness was cut out from the hardened body to prepare the test specimen. Next, the bending strength of the specimens was measured in accordance with the Tokyo Metropolitan Government's civil engineering material specifications. The results are shown in Table 2.

[0017] [Table 1]

[0018] [Table 2]

[0019] 5. Bending strength measurement results As shown in Table 2, the bending strength of the semi-flexible paving composition containing a semi-flexible paving injection material containing ecocement is up to about two times higher for the compositions containing an expansive agent and / or shrinkage-reducing agent (Examples 1 to 42) than for the composition not containing an expansive agent or shrinkage-reducing agent (Comparative Example), and is equal to or greater than the bending strength of the semi-flexible paving composition containing a semi-flexible paving injection material not containing ecocement (Reference Example).

Claims

1. A semi-flexible paving composition comprising at least 30 to 50 kg of an expansive agent per 1 m 3 of the semi-flexible paving composition, a semi-flexible paving injection material containing ecocement, and water.

2. The content of the injection material for semi-flexible paving is 1 m 3 2. The semi-flexible paving composition according to claim 1, wherein the load is 1500 to 1900 kg per unit area.

3. 3. The semi-flexible paving composition according to claim 1, wherein the expansive material is at least one selected from the group consisting of lime-based expansive materials and calcium sulfoaluminate-based expansive materials.

4. The water content is 1 m 3 The semi-flexible paving composition according to any one of claims 1 to 3, wherein the loading is 330 to 460 kg per unit area.

Citation Information

Patent Citations

  • Production of grout material

    JP1998230515A

  • Simple powder type polymer-cement composition for semiflexible paving

    JP1998265251A

  • Low shrinkage cement composition

    JP1999228195A

  • Half flexible paving material, half flexible paving body using the same and its construction

    JP1999228205A

  • Half-flexible grouting material and pavement construction using the same

    JP1999278901A