A method for producing papermaking felt and a papermaking felt produced by said method.

The method for producing papermaking felts using core-sheath fibers with controlled compression addresses bending rigidity and hair loss issues, ensuring flexible installation and improved print quality.

JP7554123B2Active Publication Date: 2024-09-19NIPPON FELT CO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021009797
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-25
Publication Date
2024-09-19
Estimated Expiration
2041-01-25

AI Technical Summary

Technical Problem

Existing papermaking felts face issues with increased bending rigidity in the weft direction and hair loss due to the use of low-melting point fibers, which complicates installation and affects print quality.

Method used

A manufacturing method involving a laminate of a base fabric and a batt fiber layer using core-sheath fibers with specific melting points and fineness, compressed at a controlled temperature to suppress bending rigidity and prevent hair loss.

Benefits of technology

The method produces papermaking felts with reduced weft direction bending rigidity and improved hair loss prevention, maintaining flexibility and water squeezing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554123000006
    Figure 0007554123000006
  • Figure 0007554123000005
    Figure 0007554123000005
  • Figure 0007554123000007
    Figure 0007554123000007
Patent Text Reader

Abstract

To provide a manufacturing method of a felt for papermaking, which suppresses increase of bending rigidity in a weft direction and is excellent in resistance to hair removal, and a felt for papermaking manufactured by the manufacturing method.SOLUTION: A felt for papermaking that has a base cloth and a surface batt fiber layer that is laminated on a papermaking surface side of the base cloth, contains a core-sheath fiber having a fusion point of a sheath component of 165 to 185°C and higher a fusion point of a core component than that of the sheath component, and has fineness of 15 to 20 dtex. A manufacturing method of the felt for papermaking has a laminating step to obtain a laminate by entangling a base cloth material with a surface batt fiber layer material, and a compression treatment step to apply compression treatment to the laminate at a temperature higher than the fusion point of the sheath component of the core-sheath fiber by 0 to 10°C. When entire mass of the surface batt fiber layer is 100%, preferably 30 to 50% by mass of the core-sheath fiber is contained. The felt for papermaking is manufactured by the manufacturing method of the felt for papermaking.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a papermaking felt (hereinafter also referred to as "felt") used in the press part of a papermaking machine, and a papermaking felt produced by this method. More specifically, the present invention relates to a method for producing a papermaking felt that suppresses an increase in bending rigidity in the weft direction and is excellent in preventing hair loss, and a papermaking felt produced by this method. [Background technology]

[0002] Papermaking felt is used in the press part of a papermaking machine, where the wet paper formed in the wire part of the previous process is passed through a pair of press rolls together with the felt to mechanically compress it and squeeze out the water. The papermaking felt comprises a base fabric and a batt fiber layer formed by needling staple fibers into the base fabric. Generally, the base fabric is made of woven fabrics in which warp and weft threads are woven together, or nonwoven fabrics made by arranging threads in one direction and fixing them together. Needling refers to the process of mechanically bonding short fibers to each other and to the base fabric by using needles with hook-like structures called "barbs" to hook and transport short fibers. In the finishing process after the needling process, the felt is generally compressed with a high-temperature heated roll to compress the batt fiber layer to a high density and to smooth the surface of the batt fiber layer. When used in a papermaking machine, papermaking felt is repeatedly subjected to physical actions such as compression by the press rolls, impact from the high-pressure shower used to clean the felt, and friction with the felt suction box (suction device). These physical actions can cause some short fibers to detach from the felt's batt fiber layer and adhere to the wet paper. When printing is performed on paper with such fibers attached, the ink does not adhere to the areas where the fibers are attached, significantly impairing the quality of the print. The phenomenon of short fibers detaching from felt is called "hair loss" in the papermaking industry, and has long been pointed out as an issue with papermaking felt. A common method for preventing hair loss in papermaking felt is to use low-melting fibers. That is, low-melting fibers are blended into the batt fiber layer of the felt, and the felt is compressed in the finishing process with a roll heated to a temperature higher than the melting point of the low-melting fibers, thereby melting the low-melting fibers and fusing them together. As a result, the bonding strength between the fibers is improved, and the detachment of the fibers, i.e., hair loss, during the use of the papermaking felt is suppressed.

[0003] As the low melting point fiber used for the above purpose, sheath-core fibers in which the melting point of the sheath component is 140°C or less and the melting point of the core component is higher than that of the sheath component are often used (for example, see

[0027] in Patent Document 1). In this way, the energy cost required for thermal melting of the sheath component can be kept low, and the core component can maintain sufficient fiber strength, which are advantages of using such sheath-core fibers. However, although the anti-hair loss effect of the felt is improved by including a large amount of low-melting point fibers in the batt fiber layer, the felt in which the fibers are heat-fused together has a high bending rigidity, and there is a problem in that the more low-melting point fibers the batt fiber layer includes, the higher the bending rigidity value becomes. The work of inserting felt into a papermaking machine requires that the felt be folded as it is passed through the gaps in the machine, which makes the work of inserting felt difficult, especially when the felt has a high bending stiffness in the weft direction. Therefore, there was a limit to the amount of low-melting fiber contained in the felt to improve the anti-hair-fall effect. In addition, in the past, when low-melting fiber contained in the batt fiber layer was used in a papermaking machine for household paper, there was a problem that the sheath component would remelt or soften during use because the operating temperature of the papermaking machine for household paper is higher than that of other papermaking machines. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-182644 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a method for producing a papermaking felt which is excellent in preventing hair loss and which uses core-sheath fibers in a batt fiber layer and which is produced by melting the sheath components through heat treatment to fuse the fibers together, thereby suppressing an increase in bending rigidity in the weft direction, and a papermaking felt produced by this method. [Means for solving the problem]

[0006] As a result of intensively studying means for solving the above problems, the present invention has been completed by the following means: That is, it has been found that a papermaking felt that is excellent in preventing shedding and suppressing an increase in bending rigidity can be manufactured by compressing a laminate using a batt fiber layer material containing high melting point core-sheath fibers of a predetermined fineness at a predetermined temperature. The present invention is as follows. 1. A base fabric; a surface batt fiber layer laminated on the papermaking surface side of the base fabric, the surface batt fiber layer containing core-sheath fibers having a sheath component melting point of 165-185°C and a core component melting point higher than the sheath component melting point, and a fineness of 15-20 dtex, a lamination step of entangling a base fabric material and a surface batt fiber layer material to obtain a laminate; A method for producing a papermaking felt, comprising: a compression treatment step of compressing the laminate at a temperature 0 to 10° C. higher than the melting point of the sheath component of the core-sheath fibers. 2. The method for producing a papermaking felt according to 1 above, wherein the core-sheath fibers account for 30 to 50% by mass when the entire surface batt fiber layer is taken as 100% by mass. 3. A papermaking felt produced by the method described in 1 or 2 above. Effect of the Invention

[0007] According to the method for producing a papermaking felt of the present invention, it is possible to produce a papermaking felt which is excellent in preventing hair loss by suppressing an increase in bending rigidity in the weft direction. Furthermore, when the surface batt fiber layer as a whole is taken as 100% by mass, if the core-sheath fiber is contained in an amount of 30 to 50% by mass, a papermaking felt having better hair loss prevention and water squeezing properties can be produced. Furthermore, the papermaking felt produced by the production method of the present invention suppresses an increase in bending rigidity in the weft direction and is excellent in preventing hair loss. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view of a laminate in the method for producing the papermaking felt according to the embodiment. [Diagram 2] 1A to 1C are explanatory diagrams illustrating a compression processing step in the manufacturing method according to the embodiment. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a papermaking felt according to an embodiment. [Figure 4] FIG. 1A is a schematic cross-sectional view showing a state in which a back batt fiber layer material is laminated onto a base fabric material in a manufacturing method for a papermaking felt according to an embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view of a laminate in which a front batt fiber layer material is further laminated. [Diagram 5] FIG. 11 is an explanatory diagram illustrating a compression processing step in the manufacturing method according to the embodiment. [Figure 6] FIG. 2 is a schematic cross-sectional view of a papermaking felt according to an embodiment of the present invention. [Figure 7] FIG. 1A is a schematic front view of a measuring device for evaluating a test specimen, and FIG. [Figure 8] 1 is a graph showing bending stiffness values ​​in the weft direction of test specimens of papermaking felt. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the present invention will be described in detail with reference to the drawings regarding embodiments thereof. The present invention is not limited to the specific examples shown in the drawings, and may be modified according to purpose and application. In addition, the same components are designated by the same reference numerals and the description thereof will be omitted.

[0010] [1] Manufacturing method for papermaking felt The method for producing a papermaking felt according to the present invention is a method for producing a papermaking felt comprising a base fabric and a surface batt fiber layer containing core-sheath fibers having a fineness of 15-20 dtex, the sheath fiber having a melting point of 165-185°C and a melting point of the core fiber higher than that of the sheath fiber, and the method comprises a lamination step of entangling the base fabric material and the surface batt fiber layer material to obtain a laminate, and a compression step of compressing the laminate at a temperature 0-10°C higher than the melting point of the sheath fiber of the core-sheath fiber.

[0011] (1)Lamination process The lamination step is a step of laminating a surface batt fiber layer material 12 on the front surface side (paper-making surface side) of a base fabric material 11 in an entangled manner, as shown in FIG. The base fabric material 11 can be a woven fabric in which warp and weft threads are woven together, or a nonwoven fabric in which threads are arranged in one direction and fixed together. The threads used for the base fabric material can be one or more of monofilament single threads or twisted threads thereof, multifilament twisted threads, or spun threads. There are no particular limitations on the material used for the threads, and polyamide, polyester, etc. can be used, for example.

[0012] The front batt fiber layer material 12 is composed of staple fibers, and can be made by melt spinning thermoplastic resin such as polyamide, polyester, etc. The front batt fiber layer material 12 of the present invention uses, as part of the staple fibers, core-sheath fibers 12a having a melting point of 165 to 185°C for the sheath component 121a and a melting point of the core component 122a higher than the melting point of the sheath component 121a, and a fineness of 15 to 20 dtex. The core-sheath fiber 12a is not particularly limited in terms of its material as long as it is one of the above-mentioned materials. For example, the "core" may be made of nylon 6 and the "sheath" may be made of nylon 12. Here, the melting point of the sheath component 121a is 165 to 185°C, and more preferably 170 to 180°C. If the melting point of the sheath component 121a is less than 165°C, when it is used in a papermaking machine for household paper, the operating temperature is higher than other papermaking machines, and the sheath component 121a may remelt or soften during use. Also, if the melting point of the sheath component 121a exceeds 185°C, the compression treatment temperature becomes too high, and the compression treatment may cause a decrease in the strength of the yarn that constitutes the base fabric of the felt.

[0013] The fineness of the sheath-core fibers 12a is 15 to 20 dtex, and preferably 16 to 18 dtex. If the fineness of the sheath-core fibers 12a is less than 15 dtex, increasing the amount of fibers in the face batt fiber layer material 12 increases the rigidity, and the bending rigidity of the felt also increases. In other words, if the number of sheath-core fibers 12a per unit weight of the face batt fiber layer material 12 increases, the fibers melt and bond to each other excessively, and the bending rigidity of the felt increases. Therefore, it is preferable that the fineness of the core-sheath fibers 12a is 15 to 20 dtex, since the bending stiffness in the weft direction does not increase even if the blending ratio of the core-sheath fibers 12a is increased. Furthermore, if the fineness of the core-sheath fibers 12a is less than 15 dtex, the fiber strength is insufficient, and therefore the amount of wear of the core-sheath fibers 12a increases when the felt is subjected to shear force from the press roll or friction from the felt suction box (suction device) during use, which is undesirable. Furthermore, when the fineness of the core-sheath fibers 12a exceeds 20 dtex, the number of core-sheath fibers 12a per unit weight is too small, and the number of contact points between the core-sheath fibers 12a themselves and between the core-sheath fibers 12a and the other short fibers 12b is small, which is insufficient to prevent the batt fibers from falling off due to melting and bonding between the fibers.

[0014] That is, in the core-sheath fiber 12a, the sheath component 121a has a melting point of 165 to 185° C. and a fineness of 15 to 20 dtex, and more preferably, the sheath component 121a has a melting point of 170 to 180° C. and a fineness of 16 to 18 dtex. It is preferable that the melting point of the sheath component 121a of the core-sheath fiber 12a is 165 to 185°C and the fineness is 15 to 20 dtex, since there is no risk of the sheath component 121a remelting or softening during use of the felt, and the bending rigidity value in the weft direction does not increase even if the blending ratio of the core-sheath fiber 12a is increased.

[0015] The front batt fiber layer material 12 can contain "other staple fibers 12b" in addition to the core-sheath fibers 12a. The material and fineness of the "other staple fibers 12b" are not particularly limited, and for example, fibers of 2 to 20 dtex such as nylon 66 staple fibers and nylon 6 staple fibers can be used.

[0016] When the entire mass of the front batt fiber layer material 12 is taken as 100% by mass, the core-sheath fibers 12a preferably constitute 15 to 70% by mass, and particularly preferably 30 to 50% by mass. When the entire mass of the front batt fiber layer material is taken as 100% by mass, if the core-sheath fibers 12a constitute less than 15% by mass, the short fibers constituting the front batt fiber layer material 12 will not melt and bond sufficiently to each other, making it difficult to prevent the short fibers from falling off from the front batt fiber layer material 12. If the core-sheath fibers 12a constitute more than 70% by mass, the fibers will melt and bond excessively to each other, causing many of the openings in the felt 20 to become clogged, resulting in reduced water squeezing performance.

[0017] To obtain the laminate 10 by entangling the surface batt fiber layer material 12 on the surface side of the base fabric material 11, for example, the surface batt fiber layer material 12, which is a blend of core-sheath fibers 12a and other short fibers 12b, can be formed into a sheet by an existing web forming method such as carding, and this can be needled to form the laminate 10 in which the surface of the base fabric material 11 and the surface batt fiber layer material 12 are integrated. Here, "entanglement" refers to a state in which the fibers are sufficiently entangled with each other, and does not include a state in which fiber layers are simply overlapped.

[0018] (2) Compression process The compression treatment step is a step of compressing the laminate 10 at a temperature 0 to 10° C. higher than the melting point of the sheath component 121a of the core-sheath fibers 12a. If the processing temperature is below the melting point, the effect of preventing the batt fibers from falling off due to melting and bonding of the core-sheath fibers cannot be fully obtained. Also, if the compression processing temperature is 10°C higher than the melting point, the fluidity of the molten sheath components becomes too high, and the fluidized sheath components may clog the voids inside the felt, resulting in a decrease in water squeezing performance. The method of compression is not particularly limited, but for example, as shown in Fig. 2, the laminate 10 can be compressed by passing it through a pair of heating rolls 61, 62 heated to a surface temperature 0°C to 10°C higher than the melting point of the sheath component 121a of the core-sheath fibers 12a, thereby thermally melting the sheath component 121a of the core-sheath fibers 12a and fusing the short fibers together. In this case, both of the pair of rolls 61, 62 that compress the laminate 10 may be heating rolls, or only one of the rolls 61 may be a heating roll. When only one of the rolls 61 is a heating roll, the front batt fiber layer material 12 including the core-sheath fibers 12a is brought into contact with the roll 61. Through the above steps, a papermaking felt 20 is manufactured, which includes a base fabric 21 and a surface batt fiber layer 22 laminated on the papermaking surface side of the base fabric 21, as shown in FIG.

[0019] The core-sheath fibers 12a contained in the surface batt fiber layer material 12 used to manufacture papermaking felt have a melting point of 165-185°C for the sheath component 121a and a melting point of the core component 122a higher than that of the sheath component 121a, and a fineness of 15-20 dtex. The laminate 10 obtained by entangling the base fabric material 11 and the surface batt fiber layer material 12 is compressed at a temperature 0-10°C higher than the melting point of the sheath component 121a. The felt manufactured under the above conditions can maintain a low bending rigidity value in the weft direction over a wide range of the content of core-sheath fibers 12a in the surface batt fiber layer material 12 from 15 to 70 mass %, and can prevent hair loss of the surface batt fiber layer. Under the above conditions, if the melting point of the sheath component 121a is 170 to 180°C and the melting point of the core component 122a is higher than the melting point of the sheath component 121a, and the fineness is 16 to 18 dtex, the bending rigidity in the weft direction can be further reduced, and hair loss of the surface batt fiber layer can be further prevented.

[0020] (3) Other processes Although the method for producing the papermaking felt of the present invention in which only the front batt fiber layer is laminated has been described above, the papermaking felt of the present invention can be provided with a back batt fiber layer on the running surface side of the papermaking felt as necessary. For example, as in the examples described later, after the back batt fiber layer material is entangled and laminated to the base fabric material, the front batt fiber layer can be laminated according to the above-mentioned production method, and compression treatment can be performed.

[0021] [2] Papermaking felt The papermaking felt 20 of the present invention is manufactured by the above-mentioned method for manufacturing papermaking felt. As shown in Fig. 3, the papermaking felt 20 includes a base fabric 21 and a surface batt fiber layer 22 laminated and intertwined on the papermaking surface side of the base fabric 21. The base fabric 21 is formed from the above-mentioned base fabric material 11, and the surface batt fiber layer 22 is formed from the surface batt fiber layer material 12, and the materials and manufacturing methods thereof are as described above. The surface batt fiber layer 22 uses, as part of the short fibers, core-sheath fibers with a sheath component having a melting point of 165-185° C. and a core component having a melting point higher than that of the sheath component, and a fineness of 15-20 dtex. Since the melting point of the sheath component is high at 165 to 185°C, there is no risk of the sheath component remelting or softening during use, even when the operating temperature is higher than in other papermaking machines, such as when used in a papermaking machine for household paper.

[0022] In addition, it is preferable that the fineness of the core-sheath fibers is 15 to 20 dtex, because the bending stiffness in the weft direction does not increase even if the blending ratio of core-sheath fibers is increased. In addition, this fineness provides sufficient fiber strength, and the amount of wear of the core-sheath fibers can be suppressed even if they are subjected to shear force from the press roll or friction from the felt suction box (suction device) during use of the felt. In addition, with a fineness in this range, the number of core-sheath fibers per unit weight is appropriate, and it is possible to prevent the batt fibers from falling off due to melting and adhesion between the fibers.

[0023] When the total mass of the surface batt fiber layer 22 is taken as 100 mass%, the core-sheath fibers are preferably contained in an amount of 15 to 70 mass%, and particularly preferably 30 to 50 mass%. If the core-sheath fibers are 15 mass% or more, the short fibers constituting the surface batt fiber layer 22 are sufficiently melted and bonded to each other, and it is possible to prevent the short fibers from falling off from the surface batt fiber layer 22. If the core-sheath fibers are 70 mass% or less, the fibers are appropriately melted and bonded to each other, and many of the openings in the felt 20 are not blocked, providing sufficient water squeezing performance.

[0024] The papermaking felt 20 according to the embodiment may be a seamed felt, but is preferably an endless felt. As in the papermaking felt 40 shown in FIG. 6, a back batt fiber layer 23 can be further provided on the back surface side (running surface side) of the base fabric 21. EXAMPLES

[0025] The present invention will be described in more detail below with reference to examples. A test piece of papermaking felt was prepared and its bending rigidity was tested according to the following procedure.

[0026] (Creating test specimens) (1)Lamination process The base fabric material 11 is made of two types of yarn: a weft yarn made of four 0.20 mm diameter 6 nylon monofilaments twisted together, and a warp yarn made of four 0.20 mm diameter 6 nylon monofilaments twisted together and three 420 denier 66 nylon multifilaments twisted together. The weight is 540 g / m 2 The fabric used was a double warp weave. As shown in FIG. 4(a), a staple fiber sheet made of 17 dtex 66 nylon staple fiber 13b is applied to the back side of the base fabric material 11 at 100 g / m 2 The fibers were then laminated by needle punching to form a back batt fiber layer material 13. As an example, the outer batt fiber layer material 12 was prepared from 17 dtex core-sheath fibers 12a, in which the sheath component 121a had a melting point of 175°C and the core component 122a had a melting point of 215°C, and 17 dtex 66 nylon staple fibers 12b, with three types of staple fiber sheets having different blending ratios. In addition, as Comparative Example 1, three types of staple fiber sheets with different blending ratios were prepared, each consisting of 3.3 dtex core-sheath fibers 12a in which the sheath component 121a had a melting point of 175°C and the core component 122a had a melting point of 215°C, and 17 dtex 66 nylon staple fibers 12b. Furthermore, as Comparative Examples 2 and 3, a total of six types of staple fiber sheets were prepared, each having a melting point of 135°C for the sheath component 121a and 215°C for the core component 122a, and each consisting of 3.3 dtex and 17 dtex core-sheath fibers 12a and 17 dtex 66 nylon staple fiber 12b, with three different blending ratios. Next, as shown in FIG. 4(b), a short fiber sheet of 600 g / m of each of the three examples and nine comparative examples was applied to the base fabric material 11. 2 The outer batt fiber layer material 12 is formed by interlacing and laminating the fibers by needle punching, and the total basis weight is about 1250 g / m 2 Thus, twelve types of laminates 30 were obtained.

[0027] (2) Compression process Next, this laminate 30 was compressed by passing it twice between a pair of rolls 61, 62 at a linear pressure of 20 kg / cm and a roll speed of 0.8 m / min, as shown in Fig. 5. Here, only one roll 61 of the pair of rolls 61, 62 used was a heating roll, and the laminate 30 was passed so that the surface batt fiber layer material 12 was in contact with the heated roll 61. The thus obtained test specimen of felt 40 was composed of a front batt fiber layer 22, a base fabric 21, and a back batt fiber layer 23, as shown in FIG. For all the test specimens according to the example and comparative examples 1 to 3, the surface temperature of the roll 61 was raised to a temperature 5° C. higher than the melting point of the sheath component 121a.

[0028] (Test Method) The bending rigidity in the weft direction of 12 types of felt specimens 40, including three types of examples and nine types of comparative examples, prepared by the above procedure, was evaluated. A homemade measuring device 80 shown in Figs. 7(a) and (b) was used to evaluate the bending rigidity. 7(a) and (b) are a schematic front view and a schematic right side view, respectively, of the measurement device 80. The upper part of the measurement device 80 is a load meter 81, and the load applied to the load meter 81 from below is displayed on a display unit 81a. There is a gap of 3 cm between the load meter 81 and the lower base 85. The load gauge 81 used was a handheld digital force gauge DFG-50R manufactured by Nidec-Shimpo Corporation. To use the measuring device 80, a felt specimen cut into a 10 cm square was folded in half in the weft direction (CMD direction) so that the surface 22s of the felt was on the inside, as shown in Figure 7(a), and was then sandwiched between the load meter 81 and the base 85, with a gap of 3 cm between them. Next, the load meter 81 was lowered to a position where the distance between the load meter 81 and the upper surface of the base 85 was 1 cm, and the maximum value of the load (g / cm) applied to the load meter 81 was read from the display unit 81a.

[0029] (Test Results) Table 1 shows the measurement results of the bending stiffness in the weft direction of each of the test specimens of the example and comparative examples 1 to 3.

[0030] [Table 1]

[0031] FIG. 8 is a graph created to compare the bending stiffness in the weft direction between the examples and the comparative examples for each blend ratio of core-sheath fibers. As a result, for the felt of the example having a core-sheath fiber fineness of 17 dtex, the bending stiffness was stably suppressed to a low value, regardless of the blend ratio (17 to 67% by mass). More specifically, when the melting point of the sheath component is 175°C and the surface temperature of roll 61 is set to 180°C, which is 5°C higher than the melting point of the sheath component, for a felt using 17 dtex core-sheath fibers, the bending rigidity in the weft direction is low and the bending rigidity is in the range of 302 to 342 g / cm. Therefore, it was shown that the felt of the examples has an excellent effect of maintaining good threadability even when the sheath component of the core-sheath fiber is melted and the fibers are fused together to prevent hair loss, regardless of the blending ratio of the core-sheath fiber. On the other hand, in the felts of Comparative Examples 1 to 3, the bending stiffness in the weft direction increases with an increase in the blending ratio of the core-sheath fibers, and it can be said that it is difficult to maintain good threading properties when the sheath component of the core-sheath fibers is melted and the fibers are fused together. [Explanation of symbols]

[0032] 10, 30; laminate, 11; base fabric material, 12; front batt fiber layer material, 12a; core-sheath fiber, 121a; sheath component, 122a; core component, 13; back batt fiber layer material, 20, 40; papermaking felt, 21; base fabric, 22; front batt fiber layer, 23; back batt fiber layer.

Claims

1. A base fabric; Laminated on the papermaking side of the base fabric, A method for producing a papermaking felt comprising: a surface batt fiber layer containing core-sheath fibers having a sheath component with a melting point of 165-185°C and a core component with a melting point higher than that of the sheath component, and a fineness of 15-20 dtex, The surface batt fiber layer also contains other short fibers having a fineness of 2 to 20 dtex, The surface batt fiber layer contains 30 to 70% by mass of the core-sheath fiber when the entire surface batt fiber layer is taken as 100% by mass, a lamination step of entangling a base fabric material and a surface batt fiber layer material to obtain a laminate; a compression treatment step of compressing the laminate at a temperature 0 to 10° C. higher than the melting point of the sheath component of the core-sheath fiber, The compression treatment step is a step of compressing the laminate by passing it through a pair of rolls, and at least one of the pair of rolls is heated to a surface temperature that is 0 to 10°C higher than the melting point of the sheath component of the core-sheath fibers, thereby thermally melting the sheath component of the core-sheath fibers and fusing the short fibers together.

2. The method for producing a papermaking felt according to claim 1, wherein the surface batt fiber layer contains 30 to 50% by mass of the core-sheath fibers when the entire surface batt fiber layer is taken as 100% by mass.

Citation Information

Patent Citations

  • Press felt for papermaking

    JP2007182644A

  • Press felt for papermaking

    JP2007217848A

  • Papermaking press felt

    JP2012154014A