A method for producing papermaking felt and a papermaking felt produced by said method.
By using core-sheath fibers with specific melting points and a controlled compression process, the method addresses high bending rigidity in papermaking felts, achieving enhanced surface smoothness and efficient water extraction.
Patent Information
- Application Number
- JP2021009798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-25
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-01-25
AI Technical Summary
Existing papermaking felts using core-sheath fibers with low-melting point sheath components face high bending rigidity issues, making them difficult to load into paper machines due to folding requirements, despite improving surface smoothness.
A method involving a batt fiber layer with core-sheath fibers having a sheath melting point of 165 to 185°C and a core melting point higher than the sheath, combined with a compression treatment at 10 to 20°C below the sheath melting point, to maintain low bending rigidity and enhance surface smoothness.
The method produces papermaking felt with suppressed bending rigidity in the weft direction and improved surface smoothness, ensuring effective water extraction and reduced energy consumption.
Smart Images

Figure 0007554124000002 
Figure 0007554124000004 
Figure 0007554124000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a papermaking felt (hereinafter also referred to as "felt") used in the press part of a papermaking machine, and a papermaking felt produced by this method. More specifically, the present invention relates to a method for producing a papermaking felt which suppresses an increase in bending rigidity in the weft direction and has excellent surface smoothness, and a papermaking felt produced by this method. [Background technology]
[0002] Papermaking felt is used in the press part of a papermaking machine, where the wet paper formed in the wire part of the previous process is passed through a pair of press rolls together with the felt to mechanically compress it and squeeze out the water. The papermaking felt comprises a base fabric and a batt fiber layer formed by needling staple fibers into the base fabric. Generally, the base fabric is made of woven fabrics in which warp and weft threads are woven together, or nonwoven fabrics made by arranging threads in one direction and fixing them together. Needling refers to the process of mechanically bonding short fibers to each other and to the base fabric by using needles with hook-like structures called "barbs" to hook and transport short fibers. In the finishing process after the needling process, the felt is generally compressed with a high-temperature heated roll to compress the batt fiber layer to a high density and to smooth the surface of the batt fiber layer. Papermaking felt is compressed with the wet paper by a press roll to squeeze the water out of the wet paper, and the smoother the surface of the felt that is in direct contact with the wet paper, the more evenly pressure can be applied to the wet paper, and the more water can be squeezed out of it. If as much water as possible can be squeezed out of the wet paper, the steam energy required to dry the wet paper in the drying part following the pressing part can be saved, leading to energy savings throughout the papermaking process. Therefore, it is important that the surface of the felt is as smooth as possible. One method for making the surface of papermaking felt smooth is to use low melting point fibers.
[0003] As the low melting point fiber used for the above purpose, sheath-core fibers in which the melting point of the sheath component is 140°C or less and the melting point of the core component is higher than that of the sheath component are often used (for example, see
[0027] in Patent Document 1). In this way, the energy cost required for thermal melting of the sheath component can be kept low, and the core component can maintain sufficient fiber strength, which are advantages of using such sheath-core fibers. However, felts in which the core-sheath fibers having a sheath component melting point of 140° C. or less are used in the batt fiber layer to soften the fibers and smooth the surface have the disadvantage of high bending rigidity. That is, the surface smoothness improves as the blend ratio of the core-sheath fibers in the batt fiber layer increases. However, in the case of felt made by melting a normal low melting point fiber at a temperature higher than its melting point or felt made by softening a low melting point fiber at a temperature lower than its melting point, the bending rigidity increases as the blend ratio increases. When felt is inserted into a papermaking machine, it must be folded as it is passed through the gaps in the machine, making the insertion process particularly difficult for felt with high bending stiffness in the weft direction. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-182644 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a method for producing a papermaking felt having excellent surface smoothness and suppressing an increase in bending rigidity in the weft direction in a felt produced by using core-sheath fibers in a batt fiber layer and softening the sheath component by heat treatment to deform the fibers, and to provide a papermaking felt produced by this method. [Means for solving the problem]
[0006] As a result of intensively studying means for solving the above problems, the present invention has been completed by the following means: It has been discovered that by using a batt fiber layer material containing core-sheath fibers with a high melting point, it is possible to produce a felt with excellent surface smoothness without increasing the bending stiffness even when softened at a low temperature. The present invention is as follows. 1. A base fabric; A method for producing a papermaking felt comprising: a surface batt fiber layer laminated on the papermaking surface side of the base fabric, the surface batt fiber layer including core-sheath fibers having a sheath component with a melting point of 165 to 185°C and a core component with a melting point higher than that of the sheath component, a lamination step of entangling a base fabric material and a surface batt fiber layer material to obtain a laminate; A method for producing a papermaking felt, comprising: a compression treatment step of compressing the laminate at a temperature 10 to 20° C. lower than the melting point of the sheath component of the core-sheath fibers. 2. The method for producing a papermaking felt according to 1 above, wherein the fineness of the core-sheath fibers is 15 to 20 dtex. 3. The method for producing a papermaking felt according to 1. or 2. above, wherein the core-sheath fiber content is 30 to 50 mass % when the entire surface batt fiber layer is taken as 100 mass %. 4. A papermaking felt produced by the method according to any one of 1. to 3. above. Effect of the Invention
[0007] According to the method for producing a papermaking felt of the present invention, it is possible to produce a papermaking felt which is excellent in surface smoothness while suppressing an increase in bending rigidity in the weft direction. Furthermore, when the fineness of the core-sheath fibers is 15 to 20 dtex, the abrasion of the core-sheath fibers can be better prevented, and the falling off of the batt fibers can be better prevented. Furthermore, when the surface batt fiber layer contains 30 to 50% by mass of core-sheath fibers, assuming the total mass of the surface batt fiber layer to be 100%, a papermaking felt having excellent surface smoothness and excellent water drainage properties can be produced. Furthermore, the papermaking felt produced by the production method of the present invention suppresses an increase in bending rigidity in the weft direction and has excellent surface smoothness. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view of a laminate in the method for producing the papermaking felt according to the embodiment. [Diagram 2] 1A to 1C are explanatory diagrams illustrating a compression processing step in the manufacturing method according to the embodiment. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a papermaking felt according to an embodiment. [Figure 4] FIG. 1A is a schematic cross-sectional view showing a state in which a back batt fiber layer material is laminated onto a base fabric material in a manufacturing method for a papermaking felt according to an embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view of a laminate in which a front batt fiber layer material is further laminated. [Diagram 5] FIG. 11 is an explanatory diagram illustrating a compression processing step in the manufacturing method according to the embodiment. [Figure 6] FIG. 2 is a schematic cross-sectional view of a papermaking felt according to an embodiment of the present invention. [Figure 7] FIG. 1A is a schematic front view of a measuring device for evaluating a test specimen, and FIG. [Figure 8] 1 is a graph showing bending stiffness values in the weft direction of test specimens of papermaking felt. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the present invention will be described in detail with reference to the drawings regarding embodiments thereof. The present invention is not limited to the specific examples shown in the drawings, and may be modified according to purpose and application. In addition, the same components are designated by the same reference numerals and the description thereof will be omitted.
[0010] [1] Manufacturing method for papermaking felt The method for producing a papermaking felt according to the present invention comprises a base fabric, and a surface batt fiber layer laminated on the papermaking surface side of the base fabric and containing core-sheath fibers in which the melting point of the sheath component is 165-185°C and the melting point of the core component is higher than the melting point of the sheath component. The method comprises a lamination step of entangling the base fabric material and the surface batt fiber layer material to obtain a laminate, and a compression step of compressing the laminate at a temperature 10-20°C lower than the melting point of the sheath component of the core-sheath fiber.
[0011] (1)Lamination process The lamination step is a step of laminating a surface batt fiber layer material 12 on the front surface side (paper-making surface side) of a base fabric material 11 in an entangled manner, as shown in FIG. The base fabric material 11 can be a woven fabric in which warp and weft threads are woven together, or a nonwoven fabric in which threads are arranged in one direction and fixed together. The threads used for the base fabric material can be one or more of monofilament single threads or twisted threads thereof, multifilament twisted threads, or spun threads. There are no particular limitations on the material used for the threads, and polyamide, polyester, etc. can be used, for example.
[0012] The front batt fiber layer material 12 is composed of staple fibers, and can be made by melt spinning thermoplastic resin such as polyamide, polyester, etc. The front batt fiber layer material 12 of the present invention uses, as part of the staple fibers, core-sheath fibers 12a in which the melting point of the sheath component 121a is 165 to 185°C and the melting point of the core component 122a is higher than the melting point of the sheath component 121a. The core-sheath fiber 12a is not particularly limited in terms of its material as long as it is one of the above-mentioned materials. For example, the "core" may be made of nylon 6 and the "sheath" may be made of nylon 12. Here, the melting point of the sheath component 121a is 165 to 185°C, and more preferably 170 to 180°C. If the melting point of the sheath component 121a is less than 165°C, when the sheath component 121a is used in a papermaking machine for household paper, the operating temperature is higher than that of other papermaking machines, so there is a risk that the sheath component 121a may melt or soften during use. Also, if the melting point of the sheath component 121a is more than 185°C, there is a risk that the bending rigidity of the felt may become high due to the high rigidity of the core-sheath fiber 12a.
[0013] The fineness of the sheath-core fibers 12a is preferably 15 to 20 dtex, and more preferably 16 to 18 dtex. If the fineness of the sheath-core fibers 12a is less than 15 dtex, the fiber strength is insufficient, and therefore the amount of wear of the sheath-core fibers 12a increases when the felt is subjected to shear force from a press roll or friction from a felt suction box (suction device) during use, which is undesirable. Furthermore, if the fineness of the sheath-core fibers 12a exceeds 20 dtex, the number of the sheath-core fibers 12a per unit weight is too small, and the effect of smoothing the felt surface due to softening of the sheath-core fibers 12a is not sufficiently obtained.
[0014] The front batt fiber layer material 12 can contain "other staple fibers 12b" in addition to the core-sheath fibers 12a. The material and fineness of the "other staple fibers 12b" are not particularly limited, and for example, fibers of 2 to 20 dtex such as nylon 66 staple fibers and nylon 6 staple fibers can be used.
[0015] When the entire mass of the surface batt fiber layer material 12 is taken as 100% by mass, the core-sheath fibers 12a are preferably contained at 15 to 70% by mass, and particularly preferably at 30 to 50% by mass. When the entire mass of the surface batt fiber layer material is taken as 100% by mass, if the core-sheath fibers 12a are less than 15% by mass, the number of core-sheath fibers 12a is insufficient to make the felt surface smooth. If the core-sheath fibers 12a are more than 70% by mass, the entire surface batt fiber layer 22 of the felt 20 produced by the compression process will be flattened, and many of the voids inside the felt 20 will be blocked, resulting in a decrease in water squeezing performance.
[0016] To obtain the laminate 10 by entangling the surface batt fiber layer material 12 on the surface side of the base fabric material 11, for example, the surface batt fiber layer material 12, which is a blend of core-sheath fibers 12a and other short fibers 12b, can be formed into a sheet by an existing web forming method such as carding, and this can be needled to form the laminate 10 in which the surface of the base fabric material 11 and the surface batt fiber layer material 12 are integrated. Here, "entanglement" refers to a state in which the fibers are sufficiently entangled with each other, and does not include a state in which fiber layers are simply overlapped.
[0017] (2) Compression process The compression treatment step is a step of compressing the laminate 10 at a temperature 10 to 20° C. lower than the melting point of the sheath component 121a of the core-sheath fibers 12a. If the treatment temperature is more than 20°C lower than the melting point of the sheath component 121a, the sheath component will not be softened sufficiently, and the effect of smoothing the felt surface will be small. On the other hand, if the treatment temperature is less than 10°C lower than the melting point of the sheath component 121a, the fibers may adhere to each other due to the melting of the sheath component, leading to an increase in bending rigidity. The method of compression is not particularly limited, but for example, as shown in Fig. 2, the laminate 10 can be compressed through a pair of heating rolls 61, 62 heated to a surface temperature 10 to 20°C lower than the melting point of the sheath component 121a of the core-sheath fibers 12a to soften and deform the core-sheath fibers 12a. In this case, both of the pair of rolls 61, 62 that compress the laminate 10 may be heating rolls, or only one of the rolls 61 may be a heating roll. When only one of the rolls 61 is a heating roll, the front batt fiber layer material 12 including the core-sheath fibers 12a is brought into contact with the roll 61. In this way, by compressing the laminate 10 by passing it through a roll 61 whose surface temperature is raised to 10°C to 20°C lower than the melting point of the sheath component 121a of the core-sheath fiber 12a, at least a portion of the core-sheath fiber 12a is deformed, resulting in a smoother felt surface than before the compression process. Through the above steps, as shown in Fig. 3, a papermaking felt 20 is manufactured, which includes a base fabric 21 and a surface batt fiber layer 22 laminated on the papermaking surface side of the base fabric 21. The felt surface 22s has high smoothness.
[0018] The core-sheath fibers 12a contained in the surface batt fiber layer material 12 used to manufacture papermaking felt have a sheath component 121a with a melting point of 165 to 185°C and a core component 122a with a melting point higher than that of the sheath component 121a. The laminate 10 obtained by entangling the base fabric material 11 and the surface batt fiber layer material 12 is compressed at a temperature 10 to 20°C lower than the melting point of the sheath component 121a. The felt manufactured under the above conditions can maintain a low bending stiffness in the weft direction over a wide range of the content of the core-sheath fibers 12a in the surface batt fiber layer material 12 from 15 to 70 mass %, and has excellent surface smoothness. Under the above conditions, if the melting point of the sheath component 121a is 170 to 180° C., the bending stiffness in the weft direction can be further reduced, and the surface smoothness can be further improved.
[0019] (3) Other processes Although the method for producing the papermaking felt of the present invention in which only the front batt fiber layer is laminated has been described above, the papermaking felt of the present invention can be provided with a back batt fiber layer on the running surface side of the papermaking felt as necessary. For example, as in the examples described later, after the back batt fiber layer material is entangled and laminated to the base fabric material, the front batt fiber layer can be laminated according to the above-mentioned production method, and compression treatment can be performed.
[0020] [2] Papermaking felt The papermaking felt 20 of the present invention is manufactured by the above-mentioned method for manufacturing papermaking felt. As shown in Fig. 3, the papermaking felt 20 includes a base fabric 21 and a surface batt fiber layer 22 laminated and intertwined on the papermaking surface side of the base fabric 21. The base fabric 21 is formed from the above-mentioned base fabric material 11, and the surface batt fiber layer 22 is formed from the surface batt fiber layer material 12, and the materials and manufacturing methods thereof are as described above. The surface batt fiber layer 22 uses, as part of the short fibers, core-sheath fibers in which the melting point of the sheath component is 165 to 185° C. and the melting point of the core component is higher than the melting point of the sheath component. Since the melting point of the sheath component is high at 165 to 185°C, there is no risk of the sheath component melting or softening during use, even if the operating temperature is higher than in other papermaking machines, such as when used in a papermaking machine for household paper.
[0021] The fineness of the core-sheath fibers is preferably 15 to 20 dtex, and a fineness in this range provides sufficient fiber strength, and the amount of wear of the core-sheath fibers can be suppressed even if the felt is subjected to shear force from a press roll or friction from a felt suction box (suction device) during use. Furthermore, a fineness in this range provides an appropriate number of core-sheath fibers per unit weight, and the softening of the core-sheath fibers provides a sufficient effect of smoothing the felt surface.
[0022] When the total mass of the surface batt fiber layer 22 is taken as 100% by mass, the core-sheath fibers are preferably contained in an amount of 15 to 70% by mass, and particularly preferably 30 to 50% by mass. If the core-sheath fibers are 15% by mass or more, the number of core-sheath fibers is sufficient to make the felt surface smooth. If the core-sheath fibers are 70% by mass or less, most of the voids in the entire batt fiber layer 22 are not blocked, and water squeezing performance is sufficient.
[0023] The papermaking felt 20 according to the embodiment may be a seamed felt, but is preferably an endless felt. As shown in FIG. 6, a papermaking felt 40 may further include a back batt fiber layer 23 on the running surface side of the base fabric 21. EXAMPLES
[0024] The present invention will be described in more detail below with reference to examples. A test piece of papermaking felt was prepared and its bending rigidity was tested according to the following procedure.
[0025] (Creating test specimens) (1)Lamination process The base fabric material 11 is made of two types of yarn: a weft yarn made of four 0.20 mm diameter 6 nylon monofilaments twisted together, and a warp yarn made of four 0.20 mm diameter 6 nylon monofilaments twisted together and three 420 denier 66 nylon multifilaments twisted together. The weight is 540 g / m 2 The fabric used was a double warp weave. As shown in FIG. 4(a), a staple fiber sheet made of 17 dtex 66 nylon staple fiber 13b is applied to the back side of the base fabric material 11 at 100 g / m 2 The fibers were then laminated by needle punching to form a back batt fiber layer material 13. For the front batt fiber layer material 12, in Examples 1 and 2, the melting point of the sheath component 121a was 175°C, the melting point of the core component 122a was 215°C, and the staple fiber sheets were made of core-sheath fibers 12a of 3.3 dtex and 17 dtex, respectively, and 66 nylon staple fibers 12b of 17 dtex, with three different blending ratios, for a total of six types. As comparative examples 1 and 2, six types of staple fiber sheets were prepared in total, each having a melting point of 135°C for the sheath component 121a and a melting point of 215°C for the core component 122a, and each consisting of 3.3 dtex and 17 dtex core-sheath fibers 12a and 17 dtex 66 nylon staple fibers 12b, with three different blending ratios. Next, as shown in FIG. 4(b), the base fabric material 11 was coated with 600 g / m2 short fiber sheets of the six examples and six comparative examples. 2 The outer batt fiber layer material 12 is formed by interlacing and laminating the fibers by needle punching, and the total basis weight is about 1250 g / m 2 Thus, twelve types of laminates 30 were obtained.
[0026] (2) Compression process Next, this laminate 30 was compressed by passing it twice between a pair of rolls 61, 62 at a linear pressure of 20 kg / cm and a roll speed of 0.8 m / min, as shown in Fig. 5. Here, only one roll 61 of the pair of rolls 61, 62 used was a heating roll, and the laminate 30 was passed so that the surface batt fiber layer material 12 was in contact with the heated roll 61. The thus obtained test specimen of felt 40 was composed of a front batt fiber layer 22, a base fabric 21, and a back batt fiber layer 23, as shown in FIG. For the specimens according to Examples 1 and 2, the surface temperature of the roll 61 was raised to a temperature 15°C lower than the melting point of the sheath component 121a. Meanwhile, for Comparative Examples 1 and 2, the surface temperature of the roll 61 was raised to a temperature 5°C higher than the melting point of the sheath component 121a, and these specimens were designated Comparative Example 1-1 and Comparative Example 2-1. And, the surface temperature of the roll 61 was raised to a temperature 15°C lower than the melting point of the sheath component 121a, and these specimens were designated Comparative Example 1-2 and Comparative Example 2-2.
[0027] (Test Method) The bending rigidity in the weft direction of 18 types of test specimens of felt 40, including 6 types of examples and 12 types of comparative examples, produced by the above procedure, was evaluated. A homemade measuring device 80 shown in Figs. 7(a) and (b) was used to evaluate the bending rigidity. 7(a) and (b) are a schematic front view and a schematic right side view, respectively, of the measurement device 80. The upper part of the measurement device 80 is a load meter 81, and the load applied to the load meter 81 from below is displayed on a display unit 81a. There is a gap of 3 cm between the load meter 81 and the lower base 85. The load gauge 81 used was a handheld digital force gauge DFG-50R manufactured by Nidec-Shimpo Corporation. To use the measuring device 80, a felt specimen cut into a 10 cm square was folded in half in the weft direction (CMD direction) so that the surface 22s of the felt was on the inside, as shown in Figure 7(a), and was then sandwiched between the load meter 81 and the base 85, with a gap of 3 cm between them. Next, the load meter 81 was lowered to a position where the distance between the load meter 81 and the upper surface of the base 85 was 1 cm, and the maximum value of the load (g / cm) applied to the load meter 81 was read from the display unit 81a.
[0028] (Test Results) Table 1 shows the measurement results of the bending stiffness in the weft direction of each test specimen of Examples 1 and 2 and Comparative Examples 1-1, 1-2, 2-1, and 2-2.
[0029] [Table 1]
[0030] FIG. 8 is a graph created to compare the bending stiffness in the weft direction between the examples and the comparative examples for each blend ratio of core-sheath fibers. As a result, for the core-sheath fiber felts according to Examples 1 and 2, the bending stiffness was stably suppressed to a low value, regardless of the blending ratio (17 to 67% by mass). That is, when the surface temperature of the roll 61 is set to 160°C, which is 15°C lower than the melting point of the sheath component, for a felt using sheath-core fibers with a melting point of 175°C, the bending rigidity in the weft direction is low, and in Example 2 (fineness 17 dtex), the bending rigidity hardly increases even when the blend ratio of sheath-core fibers increases. Furthermore, in Example 1 (fineness 3.3 dtex), the bending rigidity actually decreases as the blend ratio of sheath-core fibers increases. On the other hand, in Comparative Examples 1-1 to 2-2, the bending stiffness values were consistently higher than those of the Examples, and the bending stiffness value in the weft direction increased with an increase in the blend ratio of core-sheath fibers. In addition, in the case of conventional felts using sheath-core fibers with a melting point of the sheath component of 135°C, as in Comparative Examples 1-2 and 2-2, simply setting the surface temperature of the roll 61 to 120°C, which is 15°C lower than the melting point of the sheath component, did not reduce the bending rigidity in the weft direction very much, and furthermore, the bending rigidity increased as the blending ratio of the sheath-core fibers increased. [Explanation of symbols]
[0031] 10, 30; laminate, 11; base fabric material, 12; front batt fiber layer material, 12a; core-sheath fiber, 121a; sheath component, 122a; core component, 13; back batt fiber layer material, 20, 40; papermaking felt, 21; base fabric, 22; front batt fiber layer, 23; back batt fiber layer.
Claims
1. A base fabric; A method for producing a papermaking felt comprising: a surface batt fiber layer laminated on the papermaking surface side of the base fabric, the surface batt fiber layer including core-sheath fibers having a sheath component with a melting point of 165 to 185°C and a core component with a melting point higher than that of the sheath component, a lamination step of entangling a base fabric material and a surface batt fiber layer material to obtain a laminate; and a compression treatment step of compressing the laminate at a temperature 10 to 20° C. lower than the melting point of the sheath component of the core-sheath fibers.
2. 2. The method for producing papermaking felt according to claim 1, wherein the fineness of the core-sheath fibers is 15 to 20 dtex.
3. The method for producing a papermaking felt according to claim 1 or 2, wherein the surface batt fiber layer contains 30 to 50% by mass of the core-sheath fibers when the entire surface batt fiber layer is taken as 100% by mass.
Citation Information
Patent Citations
Smoothing press device
JP2007009389A
Press felt for papermaking
JP2007182644A
Felt for making paper
JP2008013878A
Felt for papermaking
JP2009127135A
Papermaking press felt
JP2012154014A