Anti-reflection film and its manufacturing method
The antireflection film with a urethane acrylate hard coat and hollow silica low refractive index layer addresses issues of antireflection, flexibility, and chemical resistance, ensuring effective moldability and durability.
Patent Information
- Application Number
- JP2021023832
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-18
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-02-18
AI Technical Summary
Existing antireflection films face challenges in achieving good antireflection properties, high elongation at break, moldability, and chemical resistance, particularly in applications requiring three-dimensional shaping and frequent hand contact, where issues like microcracking, peeling, and chemical corrosion occur.
An antireflection film comprising a hard coat layer made of a cured product of urethane acrylate derived from diisocyanate and pentaerythritol triacrylate, and a low refractive index layer containing hollow silica, with specific solid content ratios and molecular weights, to enhance flexibility and chemical resistance.
The film exhibits excellent antireflection, high elongation at break, and good moldability, making it suitable for in-mold and out-mold molding, while providing chemical resistance and preventing surface corrosion.
Smart Images

Figure 0007554134000001 
Figure 0007554134000002 
Figure 0007554134000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an antireflection film having a photocurable hard coat layer and a low refractive index layer, and a method for producing the same. [Background technology]
[0002] Acrylic photocurable resins are used in many fields to impart special properties to the surfaces of plastic films and plastic molded products. For example, hard coat films, which are applied to PET (polyethylene terephthalate) films to impart high hardness, are used in large quantities as films for touch panels and molding films. Among these, insert films are well known for use in molding, in which a pattern is printed on the film surface, and then the film is softened by heating and molded in three dimensions. However, if the hard coat resin layer applied to the film is hardened, microcracks are likely to occur on the curved surface when the film is processed into a three-dimensional shape, and there are limitations on the shape that can be processed. For this reason, the applicant has invented a hard coat agent containing a triazine ring-containing (meth)acrylate prepolymer and organic fine particles with an average primary particle size of 80 to 500 nm as a hard coat resin for insert molding that achieves both surface hardness and moldability (Patent Document 1). This hard coat agent has a film thickness of 1 to 10 μm and is excellent in that it can achieve both sufficient flexibility and surface physical properties. By selecting a hard coat agent suitable for such molding applications, restrictions on processing have been alleviated to some extent, but in recent years, there has been a demand for further anti-reflective properties, and extensibility has sometimes been insufficient. Also, in applications where the material is frequently touched by hands, such as the interior of automobiles, there is an issue that the hand cream on the surface of the hands corrodes the surface film of the hard coat, causing the surface film to peel off after long-term use, so there was room for improvement in order to achieve both processing properties (extensibility) and chemical resistance in addition to good anti-reflective properties. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4848200 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide an anti-reflection film having good anti-reflection properties, high breaking elongation, good formability, and excellent chemical resistance, and suitable for in-mold molding, out-mold molding, and a method for producing the same. [Means for solving the problem]
[0005] In order to solve the above problems, the invention of claim 1 provides an anti-reflection film having at least a hard coat layer and a low refractive index layer on a transparent support, the hard coat layer being a cured product of a hard coat resin composition containing a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate (hereinafter IPDI) to form a diisocyanate, and further reacting pentaerythritol triacrylate (hereinafter PETA) with the diisocyanate, and a photopolymerization initiator (B); The low refractive index layer Urethane Acrylate A cured product of a low refractive index resin composition comprising (A), a photopolymerization initiator (B), and hollow silica (C), Low Refraction rate The anti-reflection film is characterized in that the solid content ratio of (A):(C) in the resin composition is 45:55 to 5:95.
[0006] A second aspect of the present invention provides the antireflection film according to the first aspect, wherein the weight average molecular weight of (A) is 1,500 to 30,000.
[0007] The invention of claim 3 provides the anti-reflection film according to claim 1 or 2, characterized in that the dilution solvent for the low refractive index layer contains a ketone-based solvent and an alcohol-based solvent. The invention of claim 4 provides the antireflection film according to any one of claims 1 to 3, which is a film for molding.
[0008] The invention of claim 5 provides a method for producing an anti-reflection film according to any one of claims 1 to 4, characterized in that a hard coat resin composition is applied onto a transparent support, and a low refractive index resin composition is applied directly or via another layer. Effect of the Invention
[0009] The film of the present invention has good antireflection properties, high breaking elongation, good formability, and excellent chemical resistance, and is therefore useful as a molding antireflection film for use in in-mold molding, out-mold molding, and the like. BEST MODE FOR CARRYING OUT THEINVENTION
[0010] The anti-reflection film of the present invention is a urethane resin obtained by reacting PETA with a diisocyanate obtained by reacting ethylene glycol with IPDI. N-A The hard coat layer is formed by curing a hard coat (hereinafter referred to as HC) resin composition containing an acrylate (A) and a photopolymerization initiator (B), and a low refractive index layer is formed by curing a low refractive index resin composition containing the acrylate (A), the photopolymerization initiator (B), and hollow silica (C). In this specification, (meth)acrylate includes both acrylate and methacrylate.
[0011] The urethane used in the present invention N-A IPDI, an alicyclic diisocyanate used in the synthesis of acrylate (A), is non-yellowing, has excellent weather resistance, and is also highly rigid, allowing the hardness of the cured product to be increased. By reacting it with ethylene glycol, which has a very short carbon chain, it is possible to increase the concentration of urethane bonds within the molecule, forming a main skeleton with a highly rigid linear structure that has excellent chemical resistance. Using polyethylene glycol instead of ethylene glycol is inappropriate because it reduces the concentration of urethane bonds and reduces chemical resistance.
[0012] The synthesis method of (A) is not particularly limited, and a known method can be used. The reaction may be performed without a solvent, but since stirring may become difficult as the molecular weight of (A) increases, ketones such as butanone, aromatic inactive solvents such as xylene, etc. may be used. In addition, it is preferable to use a catalyst for the reaction between the hydroxyl groups of ethylene glycol and PETA and the isocyanate groups. Examples of such a catalyst include tin-based catalysts such as dibutyltin dilaurate, and metal alkoxide-based catalysts such as cobalt naphthenate. The reaction temperature can be appropriately set, but is preferably 40 to 120°C, more preferably 60 to 100°C.
[0013] The weight average molecular weight (hereinafter, Mw) of (A) is preferably 1500 to 30000, more preferably 2000 to 15000, and particularly preferably 3000 to 10000. By making it 1500 or more, sufficient elongation at break can be secured, and by making it 30000 or less, it is easy to adjust the viscosity to have good workability. The Mw of (A) can be adjusted by the molar ratio of ethylene glycol and IPDI to be reacted, and Mw tends to increase when the molar ratio of IPDI to ethylene glycol is made closer. Note that Mw was measured and calculated by gel permeation chromatography using a column using a styrene-divinylbenzene-based packing material and a tetrahydrofuran eluent as the molecular weight in terms of standard polystyrene.
[0014] The amount of (A) in the HC resin composition is preferably 50 to 99% by weight, more preferably 75 to 98% by weight, and particularly preferably 90 to 97% by weight, based on the total solid content. By making it 50% by weight or more, sufficient breaking strength can be ensured, and by making it 99% by weight or less, sufficient curability can be ensured.
[0015] The photopolymerization initiator (B) used in the present invention generates radicals when irradiated with ultraviolet light or an electron beam, and the radicals trigger the polymerization reaction, and general-purpose photopolymerization initiators such as benzyl ketal, acetophenone, and phosphine oxide photopolymerization initiators can be used. By arbitrarily selecting the light absorption wavelength of the polymerization initiator, it is possible to impart curability over a wide wavelength range from the ultraviolet region to the visible light region. Specifically, benzyl ketals include 2,2-dimethoxy-1,2-diphenylethan-1-one, α-hydroxyacetophenones include 1-hydroxy-cyclohexyl-phenyl-ketone and 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, α-aminoacetophenones include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, and acylphosphine oxides include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, which may be used alone or in combination of two or more.
[0016] In the case of the HC resin composition, the (B) preferably contains an α-hydroxyacetophenone type which is less prone to yellowing, and examples of commercially available products include Omnirad127D, Omnirad184, and Omnirad2959 (trade name: manufactured by IGM Resins). Among these, Omnirad2959, which is particularly less prone to yellowing and has excellent scratch resistance, is preferred. The blending amount of the (B) in the HC resin composition is preferably 1 to 10 parts by weight, more preferably 3 to 8 parts by weight, per 100 parts by weight of the radical polymerizable component. In the case of the low refractive index resin composition, it is preferable that (B) contains an α-hydroxyacetophenone system as in the case of the HC resin composition, and Omnirad 127D is particularly preferable in terms of curability in a thin film. The amount of (B) added to 100 parts by weight of the radical polymerizable component in the low refractive index resin composition is preferably 1 to 10 parts by weight, more preferably 3 to 8 parts by weight. The hollow nanosilica (C) used in the present invention has the function of lowering the refractive index of the low refractive index layer while maintaining the coating strength of the layer, and is a silica particle having cavities therein containing air with a refractive index of 1. While the refractive index of solid silica particles is about 1.45, the refractive index of (C) decreases as the occupancy rate of the internal cavities increases, and is about 1.20 to 1.40.
[0017] The primary particle size of (C) is preferably 5 to 150 nm, more preferably 10 to 100 nm, and particularly preferably 40 to 80 nm. By setting it in this range, good dispersibility can be obtained without impairing the transparency of the low refractive index layer. In particular, if it is 40 to 80 nm, the occupancy rate of the cavity can be increased to lower the refractive index while ensuring a thickness of the outer shell that does not cause a lack of strength. An example of a commercially available product is Sururia 4320 (trade name: manufactured by JGC Catalysts and Chemicals, primary average particle size 60 nm).
[0018] The amount of (C) blended is such that the solid content ratio of (A):(C) is 45:55 to 5:95, preferably 40:60 to 10:90, and more preferably 35:65 to 15:85. By making the solid content ratio of (A):(C) 45:55 or more, it is possible to sufficiently lower the refractive index, and by making it 5:95 or less, sufficient moldability and chemical resistance can be ensured.
[0019] To the composition of the present invention, reactive diluents, ultraviolet absorbers, adhesion promoters, antioxidants, bluing agents, pigments, leveling agents, defoamers, thickeners, precipitation inhibitors, antistatic agents, antifogging agents, antibacterial agents, waxes, matting agents, hydrophilic agents, water repellents, inorganic fillers, organic fine particles, and the like may be added as necessary within the range not impairing the performance.
[0020] The reactive diluent is preferably a (meth)acrylate monomer having less than 6 functionalities. For example, butyl (meth)acrylate, isobornyl (meth)acrylate, hydroxyethyl (meth)acrylate, (poly)ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, diglycerin tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. can be used alone or in combination of two or more. The blending ratio of the reactive diluent is preferably 20% by weight or less based on the total solid content.
[0021] When the HC resin composition and the low refractive index resin composition are applied to a transparent support, they may be diluted with a solvent to improve the coating properties. Examples of dilution solvents include alcohol-based solvents such as ethanol, n-propyl alcohol, isopropyl alcohol (hereinafter IPA), n-butyl alcohol, isobutyl alcohol, and diacetone alcohol, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone (hereinafter MIBK), and cyclohexanone, ester-based solvents such as ethyl acetate and butyl acetate, and ether-based solvents such as PGM, diethyl ether, and diisopropyl ether, which may be used alone or in combination of two or more. The solid content when diluted is not particularly specified, and can be appropriately set so as to have a viscosity that is easy to apply. In the case of HC resin, the solid content is exemplified as 10 to 50% by weight, and a mixed solvent of butyl acetate and PGM is preferred in that it has a good balance between volatility and compatibility and can form a film with good appearance. In the case of low refractive index resin, the solid content is exemplified as 0.5 to 10% by weight, and a mixed solvent of MIBK and IPA is preferred in that it has a good balance between volatility and compatibility and can form a film with good appearance.
[0022] When the low refractive index resin composition of the present invention is applied onto the HC layer, the urethane acrylate resin in the HC resin layer is slightly dissolved due to the low solid content and high solvent content. Therefore, when the cross section of the low refractive index layer is observed from its outermost surface toward the HC layer, the uppermost part has the lowest refractive index because hollow silica is exposed to the air, and the lower part has a gradually lower hollow silica ratio due to the influence of the urethane acrylate dissolved from the HC layer, resulting in a configuration in which the refractive index increases gradually. Therefore, the reflection of light from the outside can be effectively reduced. When the solid content ratio of (A):(C) in the low refractive index resin composition is increased to a ratio of (A) higher than 45:55, the solubility of the urethane acrylate resin component from the HC resin layer decreases, affecting the refractive index, resulting in a high reflectance against light from the outside.
[0023] Examples of the transparent support on which the HC resin composition is applied include polyester film, triacetyl cellulose film, polycarbonate (hereinafter referred to as PC) film, polysulfone film, nylon film, cycloolefin film, acrylic (hereinafter referred to as PMMA) film, polyimide film, ABS film, polyolefin film, PVC film, PVA film, etc. Among them, biaxially stretched polyester film is preferably used from the viewpoints of weather resistance, processability, dimensional stability, etc. Furthermore, PMMA film, PC film, and laminated film thereof are preferably used for automobile interior decoration. The thickness of the film may be about 20 μm to 500 μm.
[0024] For the purpose of improving adhesion to the HC resin composition, the transparent support substrate may be subjected to a surface treatment such as a primer treatment, a sandblasting method, a solvent treatment, or the like to make the surface uneven, or a surface treatment such as a corona discharge treatment, a chromic acid treatment, or a surface oxidation treatment such as an ozone / ultraviolet light irradiation treatment.
[0025] The method for applying the resin composition is not particularly limited, and the resin composition can be applied by a known coating method such as spray coating, roll coating, die coating, air knife coating, blade coating, spin coating, reverse coating, gravure coating, or wire bar coating, or a printing method such as gravure printing, screen printing, offset printing, or inkjet printing. The thickness of the HC resin composition when dry can be, for example, 1 μm to 10 μm, but is not limited thereto. The thickness of the low refractive index resin composition applied onto the HC resin layer when dry is preferably 50 to 200 nm, more preferably 80 to 150 nm. If the thickness of the low refractive index layer is within this range, it is possible to sufficiently reduce the reflectance.
[0026] Examples of light sources for ultraviolet irradiation used when curing the resin composition include low pressure mercury lamps, high pressure mercury lamps, extra high pressure mercury lamps, carbon arc lamps, xenon lamps, metal halide lamps, LED lamps, and electrodeless ultraviolet lamps, and the atmosphere for irradiation may be air or an inert gas such as nitrogen or argon. In addition, the curability can be further improved by heating the coating film during ultraviolet irradiation using a back roll or an IR heater. Irradiation conditions include an irradiation intensity of 500 mW / cm. 2 ~3000mW / cm 2 , exposure dose 50-400mJ / cm 2 are given as examples, but are not limited to these.
[0027] The antireflection film of the present invention preferably has a breaking elongation of 100% or more, more preferably 200% or more, in an atmosphere at 130° C. If the breaking elongation is less than 100%, cracks may occur during molding in applications involving deep drawing. The present invention will be described in detail below with reference to examples and comparative examples, but these are illustrative and are not intended to be limiting. Unless otherwise specified, measurements were performed at room temperature of 25°C and relative humidity of 65%. The units in the recipe table are parts by weight. EXAMPLES
[0028] Preparation of urethane (meth)acrylate (hereinafter referred to as ureac) 1 200 parts by weight of ethylene glycol (hereinafter referred to as EG) and 835 parts by weight of IPDI (manufactured by Sumika Bayer Urethane Co., Ltd., product name Desmodur I, NCO group 37.5%) were added together with a catalyst to MEK solvent (solid content 50%) and stirred and reacted for 30 minutes at 30°C. The reaction was terminated when the peak of the isocyanate group reached a specified amount by infrared absorption analysis. Next, 230 parts by weight of PETA (manufactured by Nippon Kayaku Co., Ltd., product name PET30, solid content 100%) was added and stirred and reacted for 30 minutes at 10°C, and then stirred and reacted for 30 minutes at 60°C. The disappearance of the isocyanate group was confirmed by infrared absorption analysis, and the solid content was adjusted to 50% with MEK to obtain 6-functional ureac 1 with Mw.6,600. Preparation of ureac 2 200 parts by weight of ethylene glycol (hereinafter referred to as EG) and 798 parts by weight of IPDI (manufactured by Sumika Bayer Urethane Co., Ltd., product name Desmodur I, NCO group 37.5%) were added together with a catalyst to MEK solvent (solid content 40%) and stirred and reacted for 30 minutes at 30°C. The reaction was terminated when the peak of the isocyanate group reached a specified amount by infrared absorption analysis. Next, 150 parts by weight of PETA (manufactured by Nippon Kayaku Co., Ltd., product name PET30, solid content 100%) was added and stirred and reacted for 30 minutes at 10°C, and then stirred and reacted for 30 minutes at 60°C. The disappearance of the isocyanate group was confirmed by infrared absorption analysis, and the solid content was adjusted to 50% with MEK to obtain 6-functional ureac 2 with Mw.8,000. Preparation of ureac 3 200 parts by weight of ethylene glycol (hereinafter referred to as EG) and 922 parts by weight of IPDI (manufactured by Sumika Bayer Urethane Co., Ltd., product name Desmodur I, NCO group 37.5%) were added together with a catalyst to MEK solvent (solid content 60%) and stirred and reacted for 30 minutes at 30°C. The reaction was terminated when the peak of the isocyanate group reached a specified amount by infrared absorption analysis. Next, 400 parts by weight of PETA (manufactured by Nippon Kayaku Co., Ltd., product name PET30, solid content 100%) was added and stirred and reacted for 30 minutes at 10°C, and then stirred and reacted for 30 minutes at 60°C. The disappearance of the isocyanate group was confirmed by infrared absorption analysis, and the solid content was adjusted to 50% with MEK to obtain 6-functional ureac 3 with Mw.4,200. According to the above method, urea 4 having the following structure was obtained. Urea 4: PETA-IPDI-polyethylene glycol-IPDI-PETA backbone; 6 functional groups, solid content 50%, Mw.5500 Preparation of HC resin composition The above-prepared (A) corresponding Ureacs 1 to 3, (A) not corresponding Ureacs 4 and dipentaerythritol hexaacrylate (hereinafter DPHA), and (B) Omnirad2959 (product name: manufactured by IGM Resins) were mixed as shown in Table 1 in terms of solid content, and further diluted with a mixed solvent of butyl acetate and PGM (mixing ratio 1:1) to make the solid content 30% by weight, and stirred until uniformly dissolved and dispersed to obtain HC resin compositions HC1 to 5. Examples 1 to 6 The HC1 to 3 prepared above were used as the HC resin composition, and UreaC1 to 2 were used as the low refractive index resin composition (A), Omnirad127D (product name: manufactured by IGM Resins) was used as the low refractive index resin composition (B), and Suluria 4320 (product name: manufactured by JGC Catalysts and Chemicals, primary average particle size 60 nm) was used as the low refractive index resin composition. These were mixed as shown in Table 2 in terms of solid content, and further diluted with a mixed solvent of MIBK and IPA (mixing ratio 1:1) so that the solid content became 1.5% by weight, and stirred until uniformly dissolved and dispersed to obtain the resin compositions of Examples 1 to 6. Comparative Examples 1 to 6 In addition to the materials used in the examples, HC4 to 5 prepared above as the HC resin composition and DPHA were used as the low refractive index resin composition, and were mixed as shown in Table 2 in terms of solid content. These were further diluted with a mixed solvent of MIBK and IPA (mixing ratio 1:1) to make the solid content 1.5% by weight (Comparative Examples 1 to 2, 4) and 2.7% by weight (Comparative Examples 5 to 6), and stirred until uniformly dissolved and dispersed, to obtain the resin compositions of Comparative Examples 1 to 6. Table 1 JPEG0007554134000001.jpg113139
[0029] Table 2 JPEG0007554134000002.jpg48135
[0030] The evaluation method was as follows. Creating HC Film Using HC resin compositions HC1 to 5, a photocurable resin was applied to a PMMA / PC film DF02UL (product name: manufactured by Mitsubishi Gas Chemical Company, thickness 125 μm) so that the dry film thickness was 3 μm. After drying at 80°C for 1 minute, the resin was cured with a high-pressure mercury lamp at 200 mJ to form an HC film.
[0031] Creating anti-reflective film Using the low refractive index resin composition in Table 2, a low refractive index layer was applied onto the HC layer prepared above so that the film thickness after drying was 100 nm. After drying at 80°C for 1 minute, the layer was cured with a high pressure mercury lamp at 200 mJ in a nitrogen atmosphere to form an HC film. Formability: The anti-reflection film prepared above was cut to a size of 25 mm wide x 50 mm long, and a tensile test was performed using Minebia's TechnoGraph TGI-1KN at an atmospheric temperature of 130°C and a tensile speed of 300 mm / min. Cracks were visually confirmed, and an elongation rate of 100% or more was marked as ○, and an elongation rate of 200% or more was marked as ◎. Calculation formula: Calculate how many mm it has stretched based on 50 mm as the base. Stretched length (mm) / 50mm x 100 = stretch rate % Reflectance: The surface opposite the coated surface was scratched with sandpaper, covered with a black pigment marker, and then black PET was attached to set the reflectance of the opposite surface to 0%. The reflectance of the HC surface was then plotted in 1 nm increments in the range of 380 nm to 780 nm using a spectrophotometer, and the minimum reflectance was measured. Reflectance of less than 1.0% was marked with ◎, 1.0 to 2.0% was marked with ◯, and over 2.0% was marked with ×.
[0032] Chemical resistance: Hand cream, Neutrogena SPF45 (product name: Johnson & Johnson) was applied to the cured film and left at 80°C for 24 hours, then returned to room temperature and wiped off, after which the surface was observed. If the coating did not whiten, it was marked with an O, if it whitened, it was marked with an X. Evaluation results Table 3 JPEG0007554134000003.jpg37135
[0033] The examples were excellent with no problems in terms of moldability, reflectance and chemical resistance. On the other hand, Comparative Example 1, in which the blending amount of (C) was small, and Comparative Example 3, which did not have a low refractive index layer, had high reflectance, Comparative Examples 2 and 5, in which the low refractive index layer and HC layer used binders that did not correspond to (A), had poor moldability, and Comparative Example 4, in which the ureac raw material of the HC layer was PEG, and Comparative Example 6, which did not have an HC layer, had poor chemical resistance, and none of these were suitable for the present invention.
Claims
1. An antireflection film having at least a hard coat layer and a low refractive index layer on a transparent support, the hard coat layer being a cured product of a hard coat resin composition containing a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate to form a diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate, and a photopolymerization initiator (B); the low refractive index layer is a cured product of a low refractive index resin composition containing the urethane acrylate (A), a photopolymerization initiator (B), and hollow silica (C), An anti-reflection film, characterized in that the solid content ratio of (A):(C) in the low refractive index resin composition is 45:55 to 5:
95.
2. 2. The anti-reflection film according to claim 1, wherein the weight average molecular weight of the (A) is 1,500 to 30,000.
3. 3. The anti-reflection film according to claim 1, wherein the dilution solvent for the low refractive index layer includes a ketone-based solvent and an alcohol-based solvent.
4. 4. The anti-reflection film according to claim 1, which is a film for molding.
5. 5. The method for producing an anti-reflection film according to claim 1, wherein the hard coat resin composition is applied onto a transparent support, and the low refractive index resin composition is applied onto the hard coat resin composition directly or via another layer.
Citation Information
Patent Citations
JP1973048200A
Hard coat film
JP2009042647A
Anti-reflection film
JP2010014819A
Ultraviolet-curable resin composition and hard coat film
JP2018111793A
Antireflection hard coat film for molding
JP2020042199A