【0020】 本発明によれば、タンニンを主剤として含有し、ホルムアルデヒド及びグリオキザール樹脂を含有してなるので、タンニンとホルムアルデヒドとの反応を抑制して、硬化反応を安定させると共に、耐水性を向上させることができる。
Smart Images

Figure 0007554140000010 
Figure 0007554140000007 
Figure 0007554140000008
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive and a method for producing the same. [Background technology]
[0002] Tannin-containing adhesives have been researched and developed for use as adhesives for wood boards and plywood, for example.
[0003] For example, Patent Document 1 discloses a wood-based composite material obtained by heating and pressurizing a wood mat made of a mixture of elongated wood pieces and a tannin-based adhesive containing acacia-derived tannin, the wood mat being formed by stacking the elongated wood pieces oriented in one direction. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-179042 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in a tannin-based adhesive containing formaldehyde as a crosslinking agent, the reactivity of tannin with formaldehyde is high, and the condensation reaction proceeds very quickly, so that the curing reaction proceeds too quickly, making it difficult to effectively exert the adhesive strength. If the condensation reaction proceeds too quickly, the adhesive thickens and the adhesive's applicability decreases. If the amount of formaldehyde is not sufficient to slow down the condensation reaction, the adhesive will not have enough crosslinking points between the tannin molecules to exhibit high water resistance, resulting in an adhesive with low water resistance. Therefore, in order to slow down the condensation reaction, a tannin-based adhesive that reacts under alkaline conditions has been proposed. In this tannin-based adhesive, the condensation reaction can be slowed down by using hexamethylenetetramine, and sufficient crosslinking points can be formed, so that the properties can be stabilized. However, since wood is usually weakly acidic, it is difficult to maintain the adhesive at an alkaline condition, and there is also a problem that the wood itself is softened by maintaining the adhesive at an alkaline condition, resulting in a decrease in the strength of the wood.
[0006] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to inhibit the reaction between tannin and formaldehyde, thereby stabilizing the curing reaction and improving water resistance. [Means for solving the problem]
[0007] In order to achieve the above object, the adhesive of the present invention contains tannin as a main component and does not contain formaldehyde. and having a basic structure represented by the following formula (2): Glyoxal Resin and Does not contain The glyoxal resin is contained in an amount of 10 parts by mass or more per 100 parts by mass of the tannin. It is characterized by the above.
[0008] [ka]
[0009] (In formula (2), R represents a methylol group.) It is characterized by containing tannin as the main ingredient, formaldehyde and glyoxal resin.
[0010] According to the above configuration, since the adhesive contains glyoxal resin in addition to tannin and formaldehyde, the probability of reaction between tannin and formaldehyde is low, and the reaction between tannin and formaldehyde, which proceeds even at a relatively low temperature such as room temperature, is significantly delayed, and the curing reaction can be stabilized. Here, since the glyoxal resin has a relatively low viscosity, the viscosity of the adhesive can be reduced by mixing it with a relatively high-viscosity tannin aqueous solution, and the application suitability of the adhesive can be improved. In addition, when the adhesive is cured by a hot press or the like, not only do tannin and formaldehyde react with each other to form a crosslinked structure between tannin and formaldehyde, but also hydroxyl groups of tannin react with methylol hydroxyl groups of the glyoxal resin to form a crosslinked structure between tannin and glyoxal resin. Furthermore, the methylol groups of the glyoxal resin bond with the hydroxyl groups of cellulose constituting the wood fibers, wood chips, and wood strands. This increases the number of cross-linking points with the tannin and bonds the glyoxal resin with the cellulose, greatly improving water resistance. Therefore, the reaction between the tannin and formaldehyde is suppressed, stabilizing the hardening reaction and improving water resistance.
[0011] Furthermore, the adhesive according to the present invention may contain a curing accelerator.
[0012] According to the above configuration, by adding a curing accelerator to the adhesive, the reaction speed after the start of hot pressing can be increased, and the pressing time can be shortened and the amount of formaldehyde emitted can be reduced accordingly. Here, the curing accelerator is configured to react with formaldehyde after hot pressing to generate a strong acid and promote curing by changing the pH of the adhesive to 1 to 3, for example, so the curing speed at room temperature is not significantly improved.
[0013] The composition may contain 3 to 6 parts by mass of the formaldehyde and 10 to 21 parts by mass of the glyoxal resin relative to 100 parts by mass of the tannin.
[0014] According to the above configuration, the adhesive contains 3 to 6 parts by mass of formaldehyde and 10 to 21 parts by mass of glyoxal resin per 100 parts by mass of tannin, so that the adhesive can be used to manufacture a wood fiberboard that satisfies a specified water resistance performance (a water absorption thickness swelling rate of 17% or less in the water absorption thickness swelling rate test specified in JIS A5905, and a bending strength of 15 MPa or more in the wet bending strength A test) and a specified formaldehyde emission grade (F☆☆☆☆ in the classification specified in JIS A5905). Here, if the adhesive contains less than 3 parts by mass of formaldehyde per 100 parts by mass of tannin, the curing reaction of the adhesive becomes significantly slow, making it difficult to ensure the strength of the wood fiberboard manufactured using the adhesive. Also, if the adhesive contains more than 6 parts by mass of formaldehyde per 100 parts by mass of tannin, it becomes difficult to ensure the formaldehyde emission grade of F☆☆☆☆ in the above classification. Furthermore, if the glyoxal resin is less than 10 parts by mass per 100 parts by mass of tannin, the cross-linking points will be insufficient, making it difficult to ensure the water resistance of the manufactured wood fiberboard.Also, if the glyoxal resin is more than 21 parts by mass per 100 parts by mass of tannin, it will be difficult to ensure the formaldehyde emission grade of F☆☆☆☆ in the above classification.
[0015] The method for producing an adhesive according to the present invention is also directed to a method for producing an adhesive comprising the steps of: and having a basic structure represented by the following formula (2): Glyoxal Resin and Does not contain The glyoxal resin is contained in an amount of 10 parts by mass or more per 100 parts by mass of the tannin. The method for producing an adhesive for use in a coating composition for coating a coating material for coating ...
[0016] [ka]
[0017] (In formula (2), R represents a methylol group.) According to the above-mentioned manufacturing method, in the crosslinking agent mixing step, the glyoxal resin is added to the tannin aqueous solution prepared in the aqueous solution preparation step and mixed, and then formaldehyde is added and mixed. This reduces the probability of reaction between tannin and formaldehyde, and the reaction between tannin and formaldehyde, which proceeds even at a relatively low temperature such as room temperature, is significantly delayed, and the curing reaction can be stabilized. Here, since the glyoxal resin has a relatively low viscosity, by mixing it with a tannin aqueous solution having a relatively high viscosity, the viscosity of the adhesive can be reduced, and the application suitability of the adhesive can be improved. In addition, when the adhesive is cured by a hot press or the like, not only does the tannin react with formaldehyde to form a crosslinked structure between the tannin and formaldehyde, but also the hydroxyl group of the tannin reacts with the methylol hydroxyl group of the glyoxal resin to form a crosslinked structure between the tannin and the glyoxal resin. Furthermore, the methylol groups of the glyoxal resin bond with the hydroxyl groups of the cellulose that constitutes the wood fibers, wood chips, and wood strands. This increases the number of cross-linking points with the tannin and also bonds the glyoxal resin with the cellulose, greatly improving water resistance. This inhibits the reaction between tannin and formaldehyde, stabilizing the hardening reaction and improving water resistance.
[0018] The method may include a curing accelerator mixing step, which is performed after the crosslinking agent mixing step, of adding and mixing a curing accelerator to the mixture obtained by mixing the glyoxal resin and the formaldehyde in the crosslinking agent mixing step.
[0019] According to the above manufacturing method, by adding a curing accelerator in the curing accelerator mixing step, the reaction speed after the start of hot pressing can be increased, and the pressing time can be shortened and the amount of formaldehyde emitted can be reduced accordingly. Here, the curing accelerator is configured to react with formaldehyde after hot pressing to generate a strong acid and promote curing by making the pH of the adhesive 1 to 3, for example, so the curing speed at room temperature is not significantly improved. Effect of the Invention
[0020] According to the present invention, since the composition contains tannin as a main component, formaldehyde and glyoxal resin, it is possible to inhibit the reaction between tannin and formaldehyde, stabilize the curing reaction and improve water resistance. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a schematic diagram showing a cross-linked structure of an adhesive according to a first embodiment of the present invention. [Diagram 2] 1 is a table showing the results (water resistance (thickness expansion rate)) of an experiment conducted on a wood fiberboard prototype made using the adhesive according to the first embodiment of the present invention. [Diagram 3] 1 is a table showing the results (water resistance (bending strength)) of an experiment conducted on a wood fiberboard prototype made using the adhesive according to the first embodiment of the present invention. [Figure 4] 1 is a table showing the results (formaldehyde emission amount) of an experiment conducted on a wood fiber board prototype made using the adhesive according to the first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to the following embodiments.
[0023] First Embodiment Figures 1 to 4 show a first embodiment of an adhesive and a manufacturing method thereof according to the present invention. Here, Figure 1 is a schematic diagram showing a cross-linked structure of the adhesive of this embodiment. Also, Figures 2, 3 and 4 are tables showing the results of experiments (water resistance (thickness expansion rate), water resistance (flexural strength) and formaldehyde emission amount) conducted on wood fiberboards prototyped using the adhesive of this embodiment.
[0024] The adhesive of this embodiment contains tannin as a main component, and also contains formaldehyde, glyoxal resin, and a hardening accelerator. As a specific composition, the adhesive of this embodiment contains about 3 to 6 parts by mass of formaldehyde, about 10 to 21 parts by mass of glyoxal resin, and about 1 to 3 parts by mass of hardening accelerator, relative to 100 parts by mass of tannin. Note that, although the adhesive containing tannin, formaldehyde, glyoxal resin, and a hardening accelerator has been exemplified in this embodiment, the hardening accelerator in the adhesive may be omitted.
[0025] Tannin has a structure as shown in the following formula (1), and may be a condensed tannin with a molecular weight of about 500 to 3000, such as mimosa tannin extracted from the outer bark of acacia, kepracho tannin extracted from the heartwood of kepracho, and radiata pine tannin, or a mixture thereof. In addition, when an alkaline aqueous solution is used as a solvent for extracting tannin, the yield of tannin is improved, but the reactivity with formaldehyde is lost and the adhesive strength is reduced, so it is not suitable as a raw material for adhesives. In addition, when warm water or hot water is used as a solvent for extracting tannin, the time required for extraction is long, making it difficult to efficiently extract tannin. Therefore, it is preferable to extract tannin using a lower alcohol or a mixed solvent of a lower alcohol and an aqueous solvent. Here, in formula (1), the part pointed by the arrow is a highly reactive part of the benzene ring (for example, where formaldehyde reacts) (the black circle part in FIG. 1). In addition, in formula (1), R is hydrogen (H) or a hydroxyl group (OH). The tree species from which tannins are extracted is not particularly limited.
[0026] [ka]
[0027] As the formaldehyde, for example, formalin (aqueous formaldehyde solution), paraformaldehyde, hexamethylenetetramine, etc. can be used, and a mixture thereof can also be used. Furthermore, urea resin, urea-melamine co-condensed resin, phenolic resin, etc., which contain formaldehyde, can also be used. That is, since urea resin, urea-melamine co-condensed resin, phenolic resin, etc. contain excess formaldehyde, the adhesive of this embodiment can also be made by adding urea resin, urea-melamine co-condensed resin, phenolic resin, etc. to a mixed aqueous solution obtained by mixing a tannin aqueous solution and a glyoxal resin, as described below.
[0028] Glyoxal resin is a cyclic molecular structure formed by reacting glyoxal with urea and formaldehyde, and has the basic structure shown in formula (2) below. In formula (2), R is , M It is a tyrol group (CH2OH).
[0029] [ka]
[0030] As the hardening accelerator, for example, ammonium salts such as ammonium chloride and ammonium sulfate are preferable, but any strong acid / weak base salt can be used.
[0031] As shown in FIG. 1, the adhesive of the above configuration forms a cross-linked structure F by formaldehyde and a cross-linked structure G by glyoxal resin between a plurality of tannin T molecules or molecular linkages to form a three-dimensional mesh structure, thereby bonding wood fibers together to form a wood board such as a wood fiber board. Here, the cross-linked structure F is formed by an addition reaction and a dehydration condensation reaction between the benzene ring in the tannin T and formaldehyde. The cross-linked structure G is formed by a dehydration condensation reaction between the hydroxyl group in the tannin T and the methylol group of the glyoxal resin. In addition, as the wood fiber, for example, wood chips, veneer chips, plywood chips, bark, and other wood-based fibers, hemp, hemp, palm, kenaf, sorghum, bamboo, wheat straw, rice straw, beet pulp, and other plant-based fibers can be used, and mixtures thereof may also be used. In addition, in this embodiment, a wood fiber board formed by bonding the above-mentioned wood fibers together is exemplified as the wood board, but the wood board may be formed by bonding wood chips together, by bonding wood strands together, or by bonding a mixture of at least two of wood fibers, wood chips, and wood strands.
[0032] Next, a method for producing the adhesive of the present embodiment will be described. The method for producing the adhesive of the present embodiment includes the following aqueous solution preparation step, crosslinking agent mixing step, and curing accelerator mixing step.
[0033] <Aqueous solution preparation process> For example, 60 g of water at about 60 to 70°C is placed in a container such as a beaker, and 60 g of dried tannin powder is added little by little while stirring to dissolve the tannin in the warm water, thereby preparing a 50% by mass tannin aqueous solution. Note that, although the present embodiment illustrates a production method in which tannin powder is dissolved in warm water to prepare a tannin aqueous solution, for example, a 50% by mass tannin aqueous solution may be prepared by concentrating an extract obtained from the bark of Acacia mollissima or Acacia mangium, the heartwood of Keplaco, or the like.
[0034] <Crosslinking agent mixing process> A predetermined amount of glyoxal resin, for example, as an aqueous solution with a solid content of 40% by mass (so that the solid content amount is 10 to 21 parts by mass per 100 parts by mass of tannin, calculated as the solid content amount) is added to the 50% by mass tannin aqueous solution prepared in the above aqueous solution preparation step and mixed, and then a predetermined amount of formaldehyde, for example, as an aqueous solution (formalin) with a solid content of 37% by mass (so that the solid content amount is 3 to 6 parts by mass per 100 parts by mass of tannin) is added and mixed.
[0035] <Curing accelerator mixing process> A predetermined amount of ammonium chloride is added as a curing accelerator, for example, as a 25% by mass aqueous solution (so that the amount is 1 to 3 parts by mass per 100 parts by mass of tannin in terms of solid content) to the mixed liquid in which the glyoxal resin and formaldehyde are mixed in the crosslinking agent mixing step, and then mixed.
[0036] The adhesive of the present embodiment can be manufactured in the manner described above. The manufactured adhesive is then sprayed onto defibrated wood fibers, which are then molded into a mat shape, and heated and pressurized to manufacture a wood fiberboard.
[0037] Next, specific experiments carried out on the adhesive of this embodiment will be described.
[0038] First, using mimosa tannin as the tannin, formalin as the formaldehyde, an aqueous solution of a glyoxal resin with a molecular weight of several hundred and a resin content of 35 to 45% by mass, and a 25% by mass aqueous solution of ammonium chloride as the hardening accelerator, adhesives containing 3, 4, 5, 6, and 7 parts by mass of formaldehyde, 7, 10, 14, 21, and 29 parts by mass of glyoxal resin adhesive, and 2 parts by mass (fixed amount) of ammonium chloride per 100 parts by mass of tannin, as shown in the tables in Figures 2, 3, and 4, were produced in a manner similar to the manufacturing method described above.
[0039] Next, each of the above experimental adhesives was sprayed onto 100 parts by mass of defibrated radiata pine wood fibers at a solid content ratio of 16 parts by mass, resulting in a target density of 800 kg / m 3The board was heated and pressed at a hot plate temperature of 180°C, a press time of 3 to 6 minutes, a maximum pressure of 4 MPa, and a target thickness of 3 mm. After this, both sides were sanded at 0.15 mm each with a No. 150 sandpaper to produce a prototype wood fiberboard with a thickness of 2.7 mm.
[0040] Furthermore, the prototype wood fiberboards were subjected to the following water resistance evaluation and formaldehyde emission measurement.
[0041] ~Water resistance evaluation~ Based on the water absorption thickness swelling rate test specified in JIS A5905, the thickness swelling rate was measured after immersion in water at 20℃±1℃ for 24 hours. As shown in the table in Figure 2, samples with a thickness swelling rate of 17% or less were evaluated as ◯, and samples with a thickness swelling rate of more than 17% were evaluated as ×.
[0042] Based on the wet bending strength A test specified in JIS A5905, the specimens were immersed in hot water at 70°C for 2 hours and then in water at 20°C for 1 hour, after which the bending strength was measured. As shown in the table in FIG. 3, specimens whose wet bending strength exceeded 15 MPa were evaluated as ◯, and specimens whose wet bending strength was below 15 MPa were evaluated as ×.
[0043] ~Formaldehyde emission measurement~ The test was conducted based on the desiccator method specified in JIS A1406, and evaluated according to the formaldehyde emission classification specified in JIS A5905, as shown in the table in Figure 4, with samples that met the F☆☆☆☆ grade (average formaldehyde emission of 0.3 mg / L or less, maximum 0.4 mg / L or less) being rated as ◯, and samples that were worse than that being rated as ×. The test was conducted with N=1, and the test specimens used were aged for approximately 2 days in a room conditioned at 20°C±1°C.
[0044] The experimental results, as shown in the tables in Figures 2, 3, and 4, confirmed that if an adhesive contains 3 to 6 parts by mass of formaldehyde and 10 to 21 parts by mass of glyoxal resin per 100 parts by mass of tannin, then wood fiberboard using that adhesive will meet the following water resistance requirements: a water absorption thickness swelling rate of 17% or less in the water absorption thickness swelling rate test specified in JIS A5905, a flexural strength of 15 MPa or more in the wet flexural strength A test, and a formaldehyde emission rating of F☆☆☆☆ in the classification specified in JIS A5905.
[0045] As described above, according to the adhesive and its manufacturing method of the present embodiment, in the crosslinking agent mixing step, the glyoxal resin is added to the tannin aqueous solution prepared in the aqueous solution preparation step and mixed, and then formaldehyde is added and mixed. This reduces the probability of reaction between tannin and formaldehyde, and the reaction between tannin and formaldehyde, which proceeds even at a relatively low temperature such as room temperature, is significantly delayed, and the curing reaction can be stabilized. Here, since the glyoxal resin has a relatively low viscosity, by mixing it with a tannin aqueous solution having a relatively high viscosity, the viscosity of the adhesive can be reduced, and the application suitability of the adhesive can be improved. In addition, when the adhesive is cured by a hot press or the like, not only does the tannin react with formaldehyde to form a crosslinked structure between the tannin and formaldehyde, but the hydroxyl group of the tannin reacts with the methylol hydroxyl group of the glyoxal resin to form a crosslinked structure between the tannin and the glyoxal resin. Furthermore, the methylol group of the glyoxal resin bonds with the hydroxyl group of the cellulose constituting the wood fiber, wood chips and wood strands. This increases the number of crosslinking points with the tannin, and the glyoxal resin bonds with the cellulose, so that the water resistance can be significantly improved. Therefore, the reaction between the tannin and formaldehyde can be suppressed, and the hardening reaction can be stabilized and the water resistance can be improved. Here, although some tannins have a high degree of polymerization and high viscosity when extracted, the viscosity of the adhesive of this embodiment is low, so that the adhesive's applicability can be improved. In addition, the adhesive of this embodiment exhibits appropriate performance as an adhesive for wood boards simply by mixing at room temperature, so that it is only necessary to store each raw material, and work such as autocondensation is unnecessary, and the manufacturing process of wood boards can be greatly simplified. Furthermore, since the adhesive of this embodiment can react with tannin under acidic conditions, it can be mixed with existing adhesives such as urea resin and urea-melamine co-condensation resin, or used in combination without mixing when manufacturing wood boards.
[0046] Furthermore, according to the adhesive and manufacturing method of the present embodiment, the adhesive contains 3 to 6 parts by mass of formaldehyde and 10 to 21 parts by mass of glyoxal resin per 100 parts by mass of tannin, so that the adhesive can be used to manufacture wood boards that meet specified water resistance (water absorption thickness swelling rate of 17% or less in the water absorption thickness swelling rate test specified in JIS A5905, and bending strength of 15 MPa or more in the wet bending strength A test) and a specified formaldehyde emission grade (classification F☆☆☆☆ specified in JIS A5905).
[0047] Furthermore, according to the wood board using the adhesive of this embodiment, the reaction between tannin and formaldehyde in the adhesive can be suppressed, the hardening reaction can be stabilized, and the water resistance can be improved, so that the water resistance of the wood board can be improved. Also, since hardening before molding into a wood board can be suppressed, the strength of the wood board can be improved, the performance can be stabilized, and the water absorption rate can be reduced.
[0048] Other Embodiments In the above embodiment, formaldehyde is exemplified as one of the crosslinking agents, but the present invention can also be applied to adhesives that use, instead of formaldehyde, compounds that can react with tannins, such as isocyanate resins such as hexamethylenetetramine and MDI (diphenylmethane diisocyanate), urea resins, urea-melamine co-condensation resins, amino resins, and epoxy resins.
[0049] In addition, in the above embodiment, glyoxal resin is exemplified as one of the cross-linking agents (reaction stabilizers), but the present invention can also be applied to adhesives that use, instead of glyoxal resin, compounds such as epoxy resins and polyethylene glycol that have molecular chains of appropriate length and react with hydroxyl groups of tannin to increase the number of cross-linking points. [Industrial Applicability]
[0050] INDUSTRIAL APPLICABILITY As described above, the present invention is extremely useful since it can suppress the reaction between tannin and formaldehyde and stabilize the curing reaction.
Claims
1. The composition contains tannin as a main component, formaldehyde, and a glyoxal resin having a basic structure represented by the following formula (2): An adhesive comprising 10 parts by mass or more of the glyoxal resin per 100 parts by mass of the tannin. 【Chemistry 2】 (In formula (2), R represents a methylol group.)
2. 2. The adhesive according to claim 1, An adhesive comprising a curing accelerator.
3. The adhesive according to claim 1 or 2, The adhesive comprises 100 parts by mass of the tannin, 3 to 6 parts by mass of the formaldehyde, and 10 to 21 parts by mass of the glyoxal resin.
4. The composition contains tannin as a main component, formaldehyde, and a glyoxal resin having a basic structure represented by the following formula (2): A method for producing an adhesive containing 10 parts by mass or more of the glyoxal resin per 100 parts by mass of the tannin, A step of preparing an aqueous tannin solution by dissolving the tannin in water; a crosslinking agent mixing step of adding and mixing the glyoxal resin to the tannin aqueous solution prepared in the aqueous solution preparation step, and then adding and mixing the formaldehyde. 【Chemistry 2】 (In formula (2), R represents a methylol group.)
5. The method for producing an adhesive according to claim 4, A method for producing an adhesive, comprising, after the crosslinking agent mixing step, a curing accelerator mixing step of adding and mixing a curing accelerator to the mixed liquid obtained by mixing the glyoxal resin and the formaldehyde in the crosslinking agent mixing step.
Citation Information
Patent Citations
JP1975146629A
Adhesive composition for wood
JP1979080341A
Processing method for hardening surface and stabilizing dimension of wood by impregnating with resin
JP1991253303A
Water-based adhesive composition and method for producing the same
JP2005344084A
Woody composite material and method for manufacturing the same