Manufacturing method of electrolytic capacitor

The method of ultrasonic removal and resistance welding of partial etching layers on electrode foils in electrolytic capacitors addresses bonding and reliability issues, ensuring strong connections and reduced short circuits.

JP7554163B2Active Publication Date: 2024-09-19NICHICON CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021105341
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-25
Publication Date
2024-09-19
Estimated Expiration
2041-06-25

AI Technical Summary

Technical Problem

Conventional methods for connecting electrode foils and lead terminals in electrolytic capacitors face issues such as insufficient bonding strength, increased manufacturing costs, risk of short circuits, and damage to the electrode foil, leading to reliability concerns.

Method used

A manufacturing method involving ultrasonic removal of partial etching layers on both sides of the electrode foil, followed by resistance welding, to ensure a strong bond between the electrode foil and the lead terminal, while maintaining the integrity of the oxide film.

Benefits of technology

This method enhances the connection reliability between the electrode foil and lead terminal, reducing the risk of short circuits and leakage current, and maintaining the electrical characteristics of the electrolytic capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554163000009
    Figure 0007554163000009
  • Figure 0007554163000010
    Figure 0007554163000010
  • Figure 0007554163000006
    Figure 0007554163000006
Patent Text Reader

Abstract

To provide an electrolytic capacitor 1 capable of improving connection reliability between an electrode foil 3 and a lead terminal 5, and a method of manufacturing the same.SOLUTION: A method for manufacturing an electrolytic capacitor includes a step of bringing ultrasonic heads 31 and 32 into contact with a connection site AR1 of a lead terminal 5 on the front surface side of an electrode foil 3 and a site AR2 corresponding to the connection site of the lead terminal on the back surface side of the electrode foil 3 and causing ultrasonic oscillation, thereby removing an etching layer 18 on the front surface side of the electrode foil 3 so that 20 to 70% of the thickness thereof remains, and removing an etching layer 18 on the back surface side of the electrode foil 3 so that 70 to 90% of the thickness thereof remains, and a step of bringing electrodes into contact with the lead terminal 5 and the site at which the etching layer 18 on the back surface side of the electrode foil 3 is removed and energizing the electrodes in a state where the lead terminal 5 is brought into contact with the connection site of the lead terminal 5, thereby resistance-welding the electrode foil 3 and the lead terminal 5.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic capacitor and a method for manufacturing the same, and to bonding of an electrode foil and a lead terminal. [Background technology]

[0002] Conventionally, for example, when manufacturing a wound electrolytic capacitor, a lead terminal is connected to an electrode foil having an etching layer with an oxide film on its surface, and a capacitor element is formed by winding the electrode foil with a separator interposed between them. An electrolyte is retained in the separator of this capacitor element, and the capacitor element is housed in an exterior case to manufacture an electrolytic capacitor.

[0003] In such conventional methods of manufacturing electrolytic capacitors, known methods for connecting the electrode foil and the lead terminal include a method in which the etched layer of the electrode foil is completely removed before connection (see Patent Document 1), a method in which a laser is used to make the connection (see Patent Document 2), a method in which a part of the etched layer of only the surface of the electrode foil to which the lead terminal is connected is removed using a laser and then the lead terminal is connected (see Patent Document 3), and a method in which the electrode foil and the lead terminal are overlapped, a pinhole is drilled, and the whole is pressed to make the connection (see Patent Document 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Utility Model Application Publication No. 54-164451 [Patent Document 2] JP 2006-100559 A [Patent Document 3] JP 2007-103527 A [Patent Document 4] JP 2010-147336 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method described in Patent Document 1, resistance welding is performed after the etching layer is completely removed, and therefore, since there is no etching layer, sufficient Joule heat cannot be generated during welding, making it difficult to achieve a strong bond, which is a problem.

[0006] Furthermore, the method described in Patent Document 2 has the problem that the manufacturing cost is high because a laser is used. In addition, since the parts irradiated with the laser light are melted and joined, the molten metal may scatter and solidify in a convex shape, penetrating the separator and causing a short circuit.

[0007] Moreover, in the method described in Patent Document 3, the etching layer is removed from only one surface of the electrode foil, which causes a problem of poor welding when welding the lead-out terminal.

[0008] Furthermore, in the method of Patent Document 4, mechanically pressing the lead terminal against the electrode foil causes problems such as damage to the electrode foil, causing a short circuit in the capacitor element, an increase in leakage current (LC), and a decrease in bonding strength.

[0009] The present invention has been made in consideration of the above points, and has an object to provide an electrolytic capacitor that can improve the connection reliability between the electrode foil and the lead terminal, and a method for manufacturing the same. [Means for solving the problem]

[0010] The method for manufacturing an electrolytic capacitor of the present invention is a method for manufacturing an electrolytic capacitor in which an extractor terminal is connected to the front side of an electrode foil having an etching layer having an oxide film on both sides thereof, and the electrode foil is wound via a separator, and the method includes the steps of: abutting an ultrasonic head against the connection portion of the extractor terminal on the front side of the electrode foil and a portion corresponding to the connection portion of the extractor terminal on the back side of the electrode foil and oscillating ultrasonic waves to remove the front side etching layer so that 20 to 70% of the thickness remains, and removing the back side etching layer so that 70 to 90% of the thickness remains; and a step of resistance welding the electrode foil and the extractor terminal by abutting electrodes against the portion of the back side of the electrode foil from which the etching layer has been removed and against the extractor terminal, with the electrode foil having the extractor terminal abutted against the connection portion of the extractor terminal, and passing an electric current through the electrodes.

[0011] According to this manufacturing method, it is possible to manufacture an electrolytic capacitor in which deterioration of characteristics is suppressed and the connection reliability of the lead terminal to the electrode foil is improved.

[0012] In addition, the manufacturing method of the electrolytic capacitor of the present invention is characterized in that, in the above-mentioned manufacturing method, the area ratio of the welding mark generated in the portion where the etching layer on the back side of the electrode foil has been removed by the resistance welding to the welding mark generated in the pull-out terminal by the resistance welding is 20 to 30%.

[0013] According to this manufacturing method, the bond between the electrode foil and the lead terminal can be strengthened.

[0014] The electrolytic capacitor of the present invention is an electrolytic capacitor in which a lead terminal is connected to the front side of an electrode foil having an etching layer with an oxide film on both sides thereof, and the electrode foil is wound via a separator, and is characterized in that on the front side of the electrode foil, the thickness of the etching layer at the connection portion of the lead terminal is 20 to 70% of the thickness of other portions of the etching layer, and on the back side of the electrode foil, the thickness of the etching layer at the portion corresponding to the connection portion of the lead terminal is 70 to 90% of the thickness of the other portions of the etching layer.

[0015] According to this configuration, it is possible to improve the connection reliability of the lead terminal to the electrode foil while suppressing deterioration of the characteristics of the electrolytic capacitor.

[0016] In addition, the electrolytic capacitor of the present invention, in the above configuration, is characterized in that the area ratio of the welding marks occurring in the portion of the back surface of the electrode foil from which the etched layer has been removed to the welding marks of the pull-out terminal is 20 to 30%.

[0017] This configuration makes it possible to strengthen the bond between the electrode foil and the lead terminal. Effect of the Invention

[0018] According to the present invention, it is possible to realize an electrolytic capacitor capable of improving the connection reliability between an electrode foil and a lead terminal, and a method for manufacturing the same. [Brief description of the drawings]

[0019] [Figure 1] 1 is a cross-sectional view showing an electrolytic capacitor according to an embodiment of the present invention. [Diagram 2] 1 is a perspective view showing a capacitor element according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a configuration of an electrode foil according to an embodiment of the present invention. [Figure 4] 2 is a schematic cross-sectional view showing an outline of an etching layer according to an embodiment of the present invention. FIG. [Diagram 5] FIG. 2 is a cross-sectional view showing an electrode foil on which etching pits are formed according to an embodiment of the present invention. [Figure 6] 1A to 1C are cross-sectional views illustrating a method for removing an etching layer according to an embodiment of the present invention. [Figure 7] 1A to 1C are cross-sectional views illustrating a method for removing an etching layer according to an embodiment of the present invention. [Figure 8] 1A to 1C are cross-sectional views illustrating a method for removing an etching layer according to an embodiment of the present invention. [Figure 9]5A to 5C are cross-sectional views illustrating a joining step of a lead tab according to an embodiment of the present invention. [Figure 10] 5A to 5C are cross-sectional views illustrating a joining step of a lead tab according to an embodiment of the present invention. [Figure 11] 4 is a cross-sectional view showing a joined state of a lead tab according to an embodiment of the present invention. FIG. [Figure 12] 3A and 3B are a plan view and a bottom view showing a welding mark according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. As shown in FIG. 1, a wound-type electrolytic capacitor 1 manufactured by the method for manufacturing an electrolytic capacitor in this embodiment is mainly composed of a capacitor element 2, an outer case 12, and a sealing body 11.

[0021] As shown in FIG. 2, capacitor element 2 is formed by winding anode foil 3a and cathode foil 3b, which have been subjected to etching and oxide film formation treatments, with separator (electrolytic paper) 4 interposed between them, and fixing them with element fixing tape 9 (FIG. 1).

[0022] This capacitor element 2 is impregnated with a driving electrolyte and / or a solid electrolyte, and then housed in a cylindrical exterior case 12 (FIG. 1) with a bottom.

[0023] A sealing member 11 made of resin, rubber or the like is attached to the opening of the exterior case 12, and the opening is sealed by drawing.

[0024] A lead wire 6 is welded to a lead tab (lead terminal) 5 that is drawn out from the capacitor element 2, and is drawn out to the outside via a sealing body 11. The exterior case 12 is covered with a sleeve 13.

[0025] In the capacitor element 2, the anode foil 3a is made of a valve metal such as aluminum, tantalum, niobium, etc. The surface of the anode foil 3a is roughened by etching, and an anodized film is formed by anodization (chemical conversion).

[0026] The cathode foil 3b is also made of aluminum or the like, like the anode foil 3a, and its surface is roughened and has a natural oxide film formed thereon. The cathode foil 3b may be a foil on which an anodized film is formed by chemical conversion after roughening, or a plain foil that is not roughened. Furthermore, a coating foil may be used in which a metal thin film or a carbon thin film containing at least one metal selected from the group consisting of titanium, nickel, titanium carbide, nickel carbide, titanium nitride, nickel nitride, titanium carbonitride, and nickel carbonitride is formed on the surface of the roughened foil or plain foil.

[0027] The separator 4 is impregnated with an electrolyte solution containing a solvent mainly made of an organic solvent, a solute made of an organic acid salt and an inorganic acid salt, and an additive such as a phosphorus compound. This forms a liquid electrolyte layer between the anode foil 3a and the cathode foil 3b. As another electrolyte, a solid conductive polymer formed between the anode foil 3a and the cathode foil 3b can also be used. The separator 4 is made of insulating paper having electrical insulation properties.

[0028] A lead tab 5 is connected to each of the anode foil 3a and the cathode foil 3b. The lead tab 5 is composed of a round bar portion 5a protruding from an end face of the capacitor element 2 and a flat portion 5b connected to one end of the round bar portion 5a and to which the electrode foils 3 (anode foil 3a, cathode foil 3b) are connected.

[0029] Lead tab 5 is formed by pressing one end of a round bar-shaped aluminum member to a predetermined length to form flat portion 5b, and the remaining portion to form round bar portion 5a.

[0030] A method for manufacturing a wound electrolytic capacitor of the present invention will be described with reference to Figures 3 to 12. This embodiment includes an etching layer removing step in which an ultrasonic oscillator is used to remove the etching layers (etched valve metal layers) of anode foil 3a and cathode foil 3b while leaving a portion of the etching layers in the thickness direction, and a resistance welding step in which flat portion 5b of lead tab 5 is welded by resistance welding to the portion from which the etching layers have been partially removed.

[0031] First, an etching layer 18 having an oxide film is formed on a metal foil (core metal portion 19) made of a valve metal such as aluminum as the anode foil 3a. Specifically, as shown in FIG. 3, the surface of the anode foil 3a is etched to form a roughened etching layer 18, and an electrically insulating dielectric film (oxide film) is formed on the surface by anodizing in a chemical conversion solution. As a result, as shown in FIG. 4, the etching layer 18 having an oxide film 51 on the surface is formed on the anode foil 3a. Note that FIG. 4 is a schematic diagram of the etching layer 18. For example, when an electrode foil having cylindrical etching pits or cubic etching pits formed in a chain is used as the etching layer 18, a state in which a plurality of etching pits P are formed is obtained as shown in FIG. 5.

[0032] Next, a predetermined ratio of the etching layer 18 in the thickness direction is removed from a portion of the etching layer 18 using an ultrasonic oscillator. Specifically, as shown in FIG. 6, cylindrical ultrasonic heads 31 and 32 are brought into contact with the etching layer 18, and an ultrasonic oscillator (not shown) is oscillated to apply ultrasonic vibration, thereby polishing and removing the surface of the etching layer 18. In this embodiment, ceramic grindstones are used as the ultrasonic heads 31 and 32, but the present invention is not limited to this, and for example, diamond grindstones can be used. The ceramic grindstones can polish only the surface of low-strength materials such as electrode foils without breaking the target.

[0033] Specifically, the method of removing the etching layer 18 by ultrasonic oscillation involves sandwiching and pressing the anode foil 3a between a pair of cylindrical ultrasonic heads 31, 32. In this state, the ultrasonic heads are vibrated by an ultrasonic oscillator at a frequency of 17 to 31 kHz to polish and remove the surface of the etching layer 18. If the frequency is less than 17 kHz, the work time may be prolonged or polishing may become difficult, and if the frequency exceeds 31 kHz, the object to be polished (anode foil 3a having the etching layer 18) may heat up and break. The etching layer 18 may be removed one side at a time.

[0034] In the removal process of the etching layer 18, as shown in Fig. 4, a removal thickness D1 is removed from the surface of the etching layer 18, leaving a remaining thickness D2. In this embodiment, for an area AR1 (Figs. 4, 6 to 12) on the surface side of the etching layer 18 to which a lead tab 5 (flat portion 5b) described later is connected by resistance welding, the ratio of the removal thickness D1 to the thickness (D1+D2) of the etching layer 18 is set to 80 to 30%, and the ratio of the remaining thickness D2 to the thickness (D1+D2) of the etching layer 18 is set to 20 to 70%, for the purpose of passing electricity between the lead tab 5 and the core metal portion 19 in a resistance welding process described later. If the ratio of the remaining thickness D2 is less than 20%, the strength of the anode foil 3a may be insufficient, and if it exceeds 70%, it may be difficult to resistance-weld the lead tab 5 (flat portion 5b) described later to the anode foil 3a. The thickness of etching layer 18 can be obtained by observing the cross section of the electrode foil with a metallurgical microscope or the like and averaging the thicknesses from the surface of the electrode foil to the core metal at the thickest and thinnest points.

[0035] In addition, in a region AR2 (FIGS. 4, 6 to 12) on the back side of the etching layer 18 that contacts a welding terminal (electrode 42 (FIG. 10)) in a process of connecting a lead tab 5 (flat portion 5b) described later by resistance welding, the ratio of the removed thickness D1 to the thickness (D1+D2) of the etching layer 18 is set to 30 to 10%, and the ratio of the remaining thickness D2 to the thickness (D1+D2) of the etching layer 18 is set to 70 to 90%. This is because if the ratio of the remaining thickness D2 is less than 70%, the tensile strength of the anode foil 3a becomes insufficient, and the leakage current (LC) tends to increase. Also, if the ratio of the remaining thickness D2 exceeds 90%, it may be difficult to resistance-weld the lead tab 5 (flat portion 5b) described later to the anode foil 3a.

[0036] If the etching layer 18 is removed too much from both sides of the anode foil 3a (the side where the lead tab 5 is resistance-welded and the back side), the resistance of the anode foil 3a decreases, the heat generated when the lead tab 5 (flat portion 5b) is resistance-welded tends to decrease, the bonding strength tends to decrease, and the risk of a short circuit occurring in the anode foil 3a increases. Therefore, it is desirable to increase the remaining thickness D2 of the etching layer 18 as long as poor bonding of the lead tab 5 (flat portion 5b) does not occur.

[0037] Under these conditions, the ultrasonic heads 31 and 32 are vibrated by an ultrasonic oscillator to polish and remove the etching layer 18 by a removal thickness D1 (FIGS. 4 and 8). The removal thickness D1 can be adjusted to a desired thickness by adjusting the vibration frequency and polishing time. By vibrating the ultrasonic head 31 at a predetermined frequency and for a predetermined time, the area AR1 on the front side of the anode foil 3a can be polished and removed to a desired thickness, and by vibrating the ultrasonic head 32 at a predetermined frequency and for a predetermined time, the area AR2 on the back side of the anode foil 3a can be polished and removed to a desired thickness.

[0038] After removing the etching layer 18 by a predetermined thickness D1 from the areas AR1 and AR2 on both sides of the anode foil 3a, the lead tab 5 (flat portion 5b) is connected to the area AR1 by resistance welding.

[0039] 9, a lead tab 5 (flat portion 5b) is placed on the anode foil 3a from which a predetermined thickness D1 of the etching layer 18 has been removed from the regions AR1 and AR2, and then, as shown in Figures 10(a) and 10(b), the lead tab 5 (flat portion 5b) placed on the region AR1 of the anode foil 3a and the region AR2 of the anode foil 3a are pressed between electrodes 41 and 42 while an electric current is passed, thereby resistance welding the lead tab 5 (flat portion 5b) and the anode foil 3a (region AR1). Note that the removed thickness D1 in the region AR1 where the lead tab 5 is joined and the region AR2 (region where the electrode 42 abuts) on the back side of the region AR1 may be the same thickness or different thicknesses as long as they satisfy the above-mentioned remaining thickness ratio.

[0040] By using the resistance welding method, it is possible to suppress the occurrence of foil breakage or cracks during connection. Therefore, the electrolytic capacitor 1 manufactured by the manufacturing method of this embodiment can suppress the occurrence of short circuits more effectively than electrolytic capacitors manufactured using other connection methods (e.g., cold welding, pinhole crimping, ultrasonic welding), and can reduce leakage current (LC) and equivalent series resistance (ESR), making it possible to provide an electrolytic capacitor 1 with excellent electrical connectivity and stable bonding strength between the lead tab and the electrode foil.

[0041] 10(c), 11, and 12(a), during welding in this resistance welding process, a depression 5c having a diameter X1 is formed as a weld mark in the lead tab 5 (flat portion 5b) in contact with the electrode 41. Also, as shown in FIG. 12(b), a weld mark M having a diameter X2 remains in an area AR2 on the back side of the anode foil 3a in contact with the electrode 42 during welding (when electricity is applied).

[0042] The area ratio of the weld mark M formed on the back side of the anode foil 3a to the depression 5c formed as a weld mark on the lead tab 5 is 20 to 30%, which shows that the weld is firmly welded. Incidentally, in the case of a removal method other than the method of polishing and removing the etching layer 18 using an ultrasonic oscillator (for example, removal by laser light), the area ratio is about 8%, and the bonding strength between the lead tab and the electrode foil is inferior.

[0043] Similarly to the anode foil 3a, the etching layer 18 is removed by ultrasonic oscillation and the lead tab 5 (flat portion 5b) is welded by resistance welding for the cathode foil 3b. EXAMPLES

[0044] After removing the etching layer 18 from the anode aluminum foil and cathode aluminum foil for high voltage withstand voltage 578V on which the etching layer 18 and oxide film 51 are formed, a resistance welding method is used to join the lead tab 5. Then, the anode aluminum foil (anode foil 3a) and the cathode aluminum foil (cathode foil 3b) are overlapped with the separator 4 interposed therebetween, and the wound aluminum electrolytic capacitor element 2 is impregnated with an electrolyte. Then, the round bar portions 5a of the anode side lead tab 5 and the cathode side lead tab 5 drawn out from the aluminum electrolytic capacitor element 2 are inserted through the insertion holes of the sealing body 11, and the aluminum electrolytic capacitor element together with the sealing body 11 is inserted into the exterior case 12. Next, the opening of the exterior case is curled and the outer peripheral surface is drawn to seal it. As a result, an aluminum electrolytic capacitor with a diameter of φ12.5 mm and a length of 13.5 mm was manufactured, and a reliability test was performed in an environment of 115°C, which exceeds the upper category temperature limit. The tensile strength of the lead tab 5, the capacitance (Cap), loss (tan δ), and leakage current (LC) of the aluminum electrolytic capacitor were measured. The results are shown in Table 1 for each remaining rate (90%, 70%, 50%, 30%, 0%) of the etching layer 18 on the side (area AR2) where the welding terminal (electrode 42) was abutted in the resistance welding process. In this aluminum electrolytic capacitor, the remaining rate of the etching layer 18 on the side where the lead tab 5 is connected in the area AR1 was set to 70%. Note that an attempt was made to join the lead tab 5 by resistance welding without removing the etching layer 18 with an ultrasonic oscillator, but the lead tab 5 could not be joined to the anode aluminum foil, and therefore an aluminum electrolytic capacitor could not be manufactured.

[0045] [Table 1]

[0046] The following can be seen from Table 1: When the remaining rate of the etching layer (ratio of remaining thickness D2 in the etching layer) on the side where the electrode 42 is abutted during resistance welding (region AR2) is 30%, 50%, 70%, or 90%, the tensile strength of the lead tab is higher, the loss (tan δ) is smaller, and the leakage current (LC) is smaller than when the remaining rate is 0%. That is, the deterioration of the characteristics of the electrolytic capacitor 1 is small. In particular, when the remaining rate of the etching layer is 70% or 90%, the tensile strength is high, the leakage current (LC) is small, and good results are obtained in both mechanical and electrical characteristics. That is, it was found that the higher the removal rate of the etching layer (ratio of removal thickness D1 in the etching layer) is (the lower the remaining rate of the etching layer is), the greater the deterioration of the characteristics of the electrolytic capacitor 1 tends to be. The same tendency is observed when the remaining rate of the etching layer 18 in the region AR1 on the side where the lead tab 5 is connected is 20% or more and less than 70%.

[0047] Furthermore, from the above results, in the manufacturing method of the electrolytic capacitor according to this embodiment, which includes the step of removing the etching layer 18 using the ultrasonic oscillator and the step of connecting the lead tab 5 by resistance welding, it is possible to increase the tensile strength of the lead tab 5 while suppressing deterioration of the characteristics of the electrolytic capacitor 1 by simply shallowly removing the etching layer 18. This makes it possible to reduce the risk of damage to the electrode foil and the occurrence of short circuits while suppressing deterioration of the characteristics.

[0048] It can be seen from the above results that the higher the remaining rate of the etching layer 18, the higher the tensile strength of the lead tab 5. This is because by not completely removing the etching layer 18, the oxide film 51 (FIG. 4) with high electrical resistance remains, which can generate high Joule heat when the lead tab 5 is resistance-welded, making it possible to perform stronger welding.

[0049] As described above, the manufacturing method of the electrolytic capacitor according to the present embodiment includes an etching layer removal step (a removal step that leaves a part of the etching layer) using an ultrasonic oscillator and a subsequent resistance welding step, so that the etching layer 18 can be removed while leaving a part of it without causing cracks or breaks in the electrode foil 3, and further, the remaining part of the etching layer 18 can generate high Joule heat in the subsequent resistance welding step, so that strong welding can be performed. That is, by making the removal thickness D1 of the etching layer 18 shallow and leaving the etching layer 18, it is possible to reduce the occurrence of damage to the electrode foil 3 (anode foil 3a, cathode foil 3b), and strong welding by high Joule heat during resistance welding is possible.

[0050] In the electrolytic capacitor 1 manufactured by this manufacturing method, the area ratio of the depression 5c formed in the lead tab 5 (flat portion 5b) to the welding mark M remaining in the region AR2 where the electrode 42 of the electrode foil 3 contacts is 20 to 30%, which indicates that the welding is strong.

[0051] Although the embodiments of the present invention have been described above based on examples, the scope of the present invention should not be considered to be limited to these embodiments. The scope of the present invention is not limited to the above description, but is indicated by the claims, and includes all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0052] 1. Electrolytic capacitor 2. Capacitor elements 3 Electrode foil 3a anode foil 3b Cathode foil 4. Separator 5 Leittab 5b Flat part 5c Hollow 18 Etching layer 31, 32 Ultrasonic head 41, 42 electrode 51 Oxide film M Welding mark

Claims

1. A method for manufacturing an electrolytic capacitor, comprising the steps of: connecting a lead terminal to a front side of an electrode foil having an etching layer having an oxide film on both sides thereof; and winding the electrode foil with a separator interposed therebetween, a step of contacting an ultrasonic head with a connection portion of the lead terminal on the front side of the electrode foil and a portion of the back side of the electrode foil corresponding to the connection portion of the lead terminal and oscillating ultrasonic waves to remove the front side etching layer so that 70% of the thickness remains, and remove the back side etching layer so that 70 to 90% of the thickness remains; a step of resistance-welding the electrode foil and the lead-out terminal by applying an electric current to the electrode foil having the lead-out terminal abutted against the connection portion of the lead-out terminal and a portion of the electrode foil from which the etched layer has been removed and the lead-out terminal, respectively; A method for manufacturing an electrolytic capacitor comprising:

2. The area ratio of the welding mark generated in the portion where the etching layer on the back surface side of the electrode foil has been removed by the resistance welding to the welding mark generated in the lead terminal by the resistance welding is 20 to 30%.

2. The method for producing an electrolytic capacitor according to claim 1.

Citation Information

Patent Citations

  • JP1971004504Y1

  • JP1979164451U

  • Manufacture of electrolytic capacitor

    JP1990222517A

  • Aluminum electrolytic capacitor and its manufacture

    JP2000082640A

  • Method for joining aluminium capacitor electrode

    JP2004079769A