Stretchable Film

A stretch film with an elastomer layer and ethylene copolymer surface layer containing calcium carbonate addresses heat resistance and stretchability issues, providing low rigidity and excellent blocking resistance.

JP7554189B2Active Publication Date: 2024-09-19C I TAKIRON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021524896
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-06
Filing Date
2020-06-04
Publication Date
2024-09-19
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

Existing stretch films using polyethylene for the surface layer have insufficient heat resistance, leading to deformation and cracking, while those using homopolypropylene lack sufficient stretchability and exhibit high rigidity when thickness is increased.

Method used

A stretch film configuration with an elastomer layer and a surface layer made of a copolymer with ethylene and calcium carbonate, where the surface layer contains 10-75% calcium carbonate and 30-70% polypropylene resin, with specific thickness ranges for both layers to achieve low rigidity, excellent blocking resistance, and stretchability.

Benefits of technology

The film achieves low rigidity, improved heat resistance, and enhanced stretchability, while maintaining stability and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554189000003
    Figure 0007554189000003
  • Figure 0007554189000004
    Figure 0007554189000004
  • Figure 0007554189000002
    Figure 0007554189000002
Patent Text Reader

Abstract

This stretchable film (1, 2) has an elastomer layer (10) and surface layers (20, 22) provided on any one side or both sides of a first surface (10a) and a second surface (10b) of the elastomer layer (10), wherein: the surface layers (20, 22) each include calcium carbonate and at least one polypropylene-based resin selected from the group consisting of a block polypropylene that is a copolymer with ethylene and a random polypropylene that is a copolymer with ethylene; the content of the calcium carbonate in the surface layers (20, 22) is 10-75 mass% with respect to the total mass of the surface layers (20, 22); the thickness of the elastomer layer (10) is 20-55 μm; and the thickness of the surface layers (20, 22) is 0.4-5.0 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretch film. This application claims priority based on Japanese Patent Application No. 2019-106404, filed on June 6, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] Stretch films are used in a wide range of fields, including hygiene products, sporting goods, and medical products, to improve handling, wearing comfort (fit), etc. For example, they are used in garments such as underwear, waistbands of disposable diapers, side panels, leg gathers, incontinence products, sanitary napkins, bandages, surgical drapes, tightening bands, hats, swimming trunks, sports supports, medical supporters, etc.

[0003] For stretch films, elastomers such as styrene-isoprene-styrene block copolymers and ethylene copolymers are used. Stretch films using elastomers have a problem with blocking. In order to suppress blocking, stretch films have been proposed in which a surface layer such as an olefin layer is provided on the surface of an elastomer layer. Patent Document 1 discloses a stretch film in which an olefin layer containing high density polyethylene (HDPE) or homopolypropylene (H-PP) is provided on the surface of an elastomer layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 2016-112878 Summary of the Invention [Problem to be solved by the invention]

[0005] As in Patent Document 1, stretch films using polyethylene such as HDPE for the surface layer have insufficient heat resistance, and are prone to deformation or hole formation when bonded to a backing film or nonwoven fabric using a hot melt adhesive, for example. Also, stretch films using H-PP for the surface layer are difficult to achieve sufficient stretchability. Although stretchability can be improved by making the elastomer layer thicker, the rigidity becomes too high, and a strong force is required to stretch the film.

[0006] An object of the present invention is to provide a stretch film that has low stiffness and excellent blocking resistance, heat resistance and stretchability. [Means for solving the problem]

[0007] The present invention has the following configuration.

[0008] [1] A stretch film having an elastomer layer and a surface layer provided on either or both of a first surface and a second surface of the elastomer layer, the surface layer containing one or more polypropylene-based resins selected from the group consisting of block polypropylenes which are copolymers with ethylene and random polypropylenes which are copolymers with ethylene, and calcium carbonate, the content of the calcium carbonate in the surface layer being 10 to 75 mass% relative to the total mass of the surface layer, the thickness of the elastomer layer being 20 to 55 μm, and the thickness of the surface layer being 0.4 to 5.0 μm.

[0009] [2] The stretch film according to [1], wherein the surface layer contains 30 to 70 mass % of the polypropylene-based resin and 30 to 70 mass % of the calcium carbonate, based on the total mass of the surface layer.

[0010] [3] The stretch film according to [1] or [2], wherein the melting point of the polypropylene-based resin is less than 160°C. Effect of the Invention

[0011] According to the present invention, it is possible to provide a stretch film that has low rigidity and excellent blocking resistance, heat resistance and stretchability. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view showing an example of the stretch film of the present invention. [Diagram 2] 1 is a cross-sectional view showing an example of the stretch film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following definitions of terms apply throughout the specification and claims. The machine direction (MD) is the extrusion direction (longitudinal direction) of the strip-shaped resin film, and the transverse direction (TD) is the direction perpendicular to the machine direction (MD) along the surface of the resin film.

[0014] The stretch film of the present invention has an elastomer layer and a surface layer provided on either or both of a first surface and a second surface of the elastomer layer.

[0015] Examples of embodiments of the stretch film of the present invention include stretch films 1 and 2 shown in Figures 1 and 2. As shown in Figure 1, stretch film 1 comprises an elastomer layer 10 and a first surface layer 20 provided on a first surface 10a of elastomer layer 10. As shown in Figure 2, stretch film 2 comprises an elastomer layer 10, a first surface layer 20 provided on the first surface 10a of elastomer layer 10, and a second surface layer 22 provided on the second surface 10b of elastomer layer 10. It should be noted that the dimensions in Figures 1 and 2 are merely examples, and the present invention is not necessarily limited to them, but can be modified as appropriate within the scope of the present invention defined in the claims.

[0016] The elastomer layer is a layer that includes an elastomer. An elastomer refers to a polymer that has rubber elasticity at or above its glass transition temperature. Therefore, elastomers generally have a glass transition temperature of room temperature (23°C) or lower. Specific examples of elastomers include styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, and polyester-based elastomers. Among these, olefin-based elastomers are preferred from the standpoint of strength and recovery. Furthermore, styrene-based elastomers are preferred from the standpoint of high dimensional stability during film transport. The elastomer layer may contain one type of elastomer or two or more types of elastomers.

[0017] Examples of styrene-based elastomers include styrene-isoprene-styrene copolymers (SIS elastomers), styrene-isoprene block copolymers, styrene-butadiene-styrene block copolymers, styrene-butadiene block copolymers, hydrogenated styrene-isoprene-styrene block copolymers (styrene-ethylene-propylene-styrene block copolymers), hydrogenated styrene-butadiene-styrene block copolymers (styrene-ethylene-butylene-styrene block copolymers), etc. Among these, SIS elastomers are preferred because of their higher strength and restorability.

[0018] The styrene unit content of the SIS elastomer is preferably 14 to 48% by mass. If the styrene unit content of the SIS elastomer is equal to or higher than the lower limit, moldability is improved. If the styrene unit content of the SIS elastomer is equal to or lower than the upper limit, sufficiently high stretchability can be obtained.

[0019] As the SIS elastomer, a commercially available product can be used. Commercially available SIS elastomers include, for example, Quintac3390 (SIS block copolymer, glass transition temperature: -53°C, styrene unit content: 48% by mass, manufactured by Zeon Corporation), Quintac3620 (SIS block copolymer, glass transition temperature: -50°C, styrene unit content: 14% by mass, manufactured by Zeon Corporation), and the like.

[0020] Examples of the olefin-based elastomer include copolymers or homopolymers mainly composed of an olefin having 3 or more carbon atoms, and copolymers mainly composed of ethylene and an olefin having 3 or more carbon atoms. Specific examples include α-olefin homopolymers such as propylene homopolymers and 1-butene homopolymers having low stereoregularity; α-olefin copolymers such as propylene-ethylene copolymers, propylene-ethylene-1-butene copolymers, 1-butene-ethylene copolymers, 1-butene-propylene copolymers, 4-methylpentene-1-propylene copolymers, 4-methylpentene-1-1-butene copolymers, 4-methylpentene-1-propylene-1-butene copolymers, propylene-1-butene copolymers, ethylene-propylene copolymers, ethylene-hexene copolymers, and ethylene-1-octene copolymers; and ethylene-α-olefin-diene terpolymers such as ethylene-propylene-ethylidenenorbornene copolymers, ethylene-propylene-butadiene copolymers, and ethylene-propylene-isoprene copolymers. Alternatively, the elastomer may be dispersed in a matrix of crystalline polyolefin. The olefin-based elastomer may be used alone or in combination of two or more kinds.

[0021] As the olefin-based elastomer, from the viewpoints of strength and resilience, a propylene-based elastomer which is a copolymer or homopolymer mainly composed of propylene (such as a propylene-ethylene copolymer, hereinafter also referred to as a "PP-based elastomer"), and an ethylene-octene elastomer which is a copolymer or homopolymer mainly composed of ethylene (such as an ethylene-octene copolymer) are preferred.

[0022] The propylene unit content of the PP elastomer relative to the total units is preferably 70 to 95% by mass, more preferably 80 to 90% by mass. If the propylene content of the PP elastomer is equal to or higher than the lower limit, moldability is improved. If the propylene content of the PP elastomer is equal to or lower than the upper limit, high stretchability is easily obtained.

[0023] As the olefin-based elastomer, commercially available products can be used. Commercially available olefin-based elastomers include, for example, trade name "VISTAMAXX6102" (propylene-ethylene copolymer, ethylene unit content: 16% by mass, manufactured by ExxonMobil Corporation) and trade name "Infuse9007" (ethylene-octene copolymer, manufactured by Dow Chemical Corporation).

[0024] From the viewpoints of strength and recovery, the elastomer is preferably one selected from the group consisting of PP-based elastomers and ethylene-octene elastomers, although two or more elastomers may be used in combination. As the elastomer, a styrene-based elastomer is preferred because it has high dimensional stability during film transport, but two or more types of styrene-based elastomers may be mixed and used.

[0025] The elastomer layer may contain other components in addition to the thermoplastic elastomer, so long as the effects of the present invention are not impaired. Examples of the other components include additives such as weathering stabilizers, antistatic agents, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, UV absorbers, light stabilizers, antioxidants, discoloration inhibitors, pigments, dyes, and fillers.

[0026] The thickness of the elastomer layer is 20 to 55 μm, preferably 25 to 53 μm, and more preferably 30 to 50 μm. When the thickness of the elastomer layer is equal to or greater than the lower limit of the above range, the elastomer layer has excellent elasticity. When the thickness of the elastomer layer is equal to or less than the upper limit of the above range, the rigidity is low. The elastomer layer may be a single layer or multiple layers. When the elastomer layer is multiple layers, the total thickness of the elastomer layers is within the above range. In addition, when the elastomer layer is a multi-layer structure, the components of the different elastomer layers may be the same or different.

[0027] The surface layer is a layer containing one or more polypropylene-based resins (hereinafter also referred to as "polypropylene-based resin (B)") selected from the group consisting of block polypropylene (hereinafter also referred to as "B-PP"), which is a copolymer with ethylene, and random polypropylene (hereinafter also referred to as "R-PP"), which is a copolymer with ethylene, and calcium carbonate. By providing the surface layer on the surface of the elastomer layer, excellent blocking resistance is obtained. The polypropylene resin (B) contained in the surface layer may be one type or two or more types. When a first surface layer and a second surface layer are provided on both sides of the elastomer layer, the polypropylene-based resin (B) contained in the first surface layer and the polypropylene-based resin (B) contained in the second surface layer may be the same or different.

[0028] H-PP is a homopolymer of propylene, and has a high tacticity and therefore a high degree of crystallinity. As a result, films made from H-PP tend to be rigid and lack flexibility. In contrast, R-PP is a copolymer of propylene and ethylene, and has a lower tacticity and lower crystallinity than H-PP, making it flexible and heat-resistant. B-PP forms a sea-island structure consisting of a sea of ​​polypropylene and islands of ethylene, and while it has the same heat resistance as H-PP, it also has flexibility by forming an EPR phase at the boundary between the sea and islands.

[0029] The melting point of the polypropylene resin (B) is preferably less than 160°C, more preferably 135°C or more and less than 160°C. If the melting point of the polypropylene resin (B) is less than 160°C, the polypropylene resin (B) contains the necessary ethylene resin and has excellent flexibility, resulting in excellent stretchability of the stretch film. If the melting point of the polypropylene resin (B) is 135°C or more, the polypropylene resin (B) contains the necessary propylene resin and has excellent heat resistance. The melting point is a peak temperature measured by differential scanning calorimetry (DSC).

[0030] The content of the polypropylene resin (B) in the surface layer is preferably 25 to 90% by mass, more preferably 27 to 80% by mass, and even more preferably 30 to 70% by mass, based on the total mass of the surface layer. When the content of the polypropylene resin (B) is equal to or higher than the lower limit of the above range, the heat resistance is excellent. When the content of the polypropylene resin (B) is equal to or lower than the upper limit of the above range, the rigidity is low and the stretchability is excellent.

[0031] The content of calcium carbonate in the surface layer is 10 to 75 mass %, preferably 20 to 73 mass %, and more preferably 30 to 70 mass %, based on the total mass of the surface layer. If the content of calcium carbonate is equal to or greater than the lower limit of the above range, the rigidity is low and the stretchability is excellent. If the content of calcium carbonate is equal to or less than the upper limit of the above range, the production of the stretch film is stable.

[0032] The surface layer may contain other components than the polypropylene resin (B) and calcium carbonate, as long as the effects of the present invention are not impaired. Examples of other components include the additives listed for the elastomer layer. The surface layer may also contain inorganic fillers other than calcium carbonate, such as zeolite and silica. The surface layer may also contain resins other than the polypropylene resin (B), such as homopolypropylene (H-PP) and polyethylene (PE).

[0033] The thickness of the surface layer is 0.4 to 5.0 μm, preferably 0.5 to 4.5 μm, and more preferably 1 to 4.0 μm. If the thickness of the surface layer is equal to or greater than the lower limit of the above range, the production of the stretch film becomes more stable. If the thickness of the surface layer is equal to or less than the upper limit of the above range, the stretch film can be made thinner, and the surface layer formed of the polypropylene-based resin (B), which has higher rigidity than elastomers, in particular, becomes thinner, thereby reducing the effect of the rigidity of the surface layer on the stretch film. Therefore, the rigidity of the stretch film becomes lower, and the stretchability becomes excellent. When a first surface layer and a second surface layer are provided on both sides of the elastomer layer, the thicknesses of the first surface layer and the second surface layer are each within the above-mentioned ranges. The thickness of the first surface layer and the thickness of the second surface layer may be the same or different.

[0034] The total thickness of the stretch film is preferably 20 to 60 μm, more preferably 25 to 55 μm, and even more preferably 30 to 50 μm. When the total thickness of the stretch film is equal to or greater than the lower limit of the above range, the stretch film has excellent stretchability. When the total thickness of the stretch film is equal to or less than the upper limit of the above range, the stretch film can be made thinner, has lower rigidity, and has excellent stretchability.

[0035] The method for producing the stretch film is not particularly limited, and examples thereof include an inflation method, a cast film process, etc. Among these, the cast film process is preferred from the viewpoint of productivity.

[0036] The uses of the stretch film of the present invention are not particularly limited, and it can be used in sanitary products, sports goods, medical products, etc. For example, it can be used in clothing such as underwear, waistbands of paper diapers, side panels, leg gathers, incontinence products, sanitary napkins, bandages, surgical drapes, tightening bands, hats, swimming trunks, sports supports, medical product supports, etc.

[0037] As described above, the stretch film of the present invention has a surface layer containing a polypropylene resin (B) and a specific ratio of calcium carbonate on either or both of the first and second sides of the elastomer layer, and the thicknesses of the elastomer layer and the surface layer are controlled within specific ranges. By providing such a surface layer, excellent blocking resistance is obtained, and low rigidity, excellent heat resistance, and stretchability are also obtained. (Example)

[0038] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description.

[0039] [Measurement and evaluation methods] (Thickness of each layer) The thicknesses of the elastomer layer and the surface layer in the stretch film were determined by observing the cross section with a microscope.

[0040] (Heat resistance) A hot melt at 135° C. was applied to the stretch film and left for 1 minute, after which the shape of the film was visually observed and the heat resistance was evaluated according to the following criteria. ◯ (Good): No deformation or breakage of the film was observed, and the heat resistance was excellent. × (bad): Deformation or breakage of the film was observed, and the heat resistance was insufficient.

[0041] (Permanent deformation of stretch film) A rectangular test piece of 100 mm in the stretch direction of the film and 25 mm in the direction perpendicular to the stretch direction was cut from the stretch film. The test piece was fixed to the gripper of a precision universal testing machine (Shimadzu Corporation, Autograph, material test operation software: TRAPEZIUM2) so that the distance between the grippers was 25 mm. The test piece was stretched in the longitudinal direction at a speed of 254 mm / min so that the elongation calculated by the following formula (I) was 100%, and then the test piece was immediately contracted at the same speed. The permanent set was calculated from the following formula (II). The test was performed at 23°C ± 2°C. Elongation = (L1-L0) / L0 x 100 (I) Permanent set = (L2-L0) / L0 x 100 (II) Here, L0 is the distance between the grips (mm) before stretching, L1 is the distance between the grips (mm) after stretching, and L2 is the distance between the grips (mm) when the load (N / 25mm) of the test piece becomes 0 when contracting. The stretching direction of the film is MD when an olefin-based elastomer is used, and is TD when a styrene-based elastomer is used.

[0042] (rigidity) The stiffness of the stretch film was evaluated according to the following criteria from the stress-strain curve (SS curve) measured in a permanent set test. ○ (Good): The test force at 50% elongation is 4N or less. × (bad): The test force at 50% elongation during elongation was more than 4 N.

[0043] (stretchability) The stretchability of the stretch film was evaluated according to the following criteria from the stress-strain curve (SS curve) measured in a permanent set test. Good: Permanent distortion is 20% or less. × (bad): Permanent set is more than 20%.

[0044] [Raw materials] The raw materials used in this example are shown below. (Elastomer) Elastomer (A-1): Ethylene-octene elastomer (Infuse 9007, manufactured by The Dow Chemical Company) Elastomer (A-2): PP-based elastomer (Vistamaxx6102FL, Exxon) Elastomer (A-3): SIS elastomer (Quintac 3390, styrene content 48% by mass, manufactured by Zeon Corporation) Elastomer (A-4): SIS elastomer (Quintac 3620, styrene content 14% by mass, manufactured by Zeon Corporation)

[0045] (Polypropylene resin (B)) Resin (B-1): R-PP (F227, melting point 152°C, manufactured by Prime Polymer) Resin (B-2): B-PP (MFX3, melting point 157°C, manufactured by WAYMAX)

[0046] (Inorganic filler) Calcium carbonate (Ryton S, manufactured by Bihoku Powder Industry Co., Ltd.)

[0047] (Comparative resin) Resin (X-1): Homopolypropylene (H-PP, D101, melting point 163°C, manufactured by Noblen) Resin (X-2): Polyethylene (PE, CE3506, melting point 117°C, manufactured by Sumikasen)

[0048] [Examples 1 to 8, Comparative Examples 1 to 7] A resin mixture was obtained by mixing the components forming the surface layer in a tumbler mixer in the proportions shown in Tables 1 and 2. Then, a cast film process was used to produce a stretch film having an elastomer layer and a first surface layer and a second surface layer formed of the resin mixture on both sides of the elastomer layer.

[0049] [Table 1]

[0050] [Table 2]

[0051] As shown in Table 1, the stretch films of Examples 1 to 8, which contained a polypropylene-based resin (B) and had a surface layer containing calcium carbonate at a specific ratio, had low rigidity and excellent heat resistance and stretchability. On the other hand, the film of Comparative Example 1, in which H-PP was used instead of the polypropylene-based resin (B), had high rigidity. The film of Comparative Example 2, in which PE was used instead of the polypropylene-based resin (B) in the surface layer, had insufficient heat resistance. The films of Comparative Example 3, in which the surface layer did not contain calcium carbonate, and Comparative Example 4, in which the elastomer layer was too thin, had insufficient stretchability. The films of Comparative Example 5, in which the elastomer layer was too thick, and Comparative Example 6, in which the surface layer was too thick, had high rigidity and insufficient stretchability. In Comparative Example 7, in which the content of calcium carbonate in the resin mixture forming the surface layer was too high, a film could not be produced. [Industrial Applicability]

[0052] According to the present invention, it is possible to provide a stretch film that has low rigidity and excellent blocking resistance, heat resistance and stretchability. [Explanation of symbols]

[0053] 1, 2... stretch film, 10... elastomer layer, 10a... first surface, 10b... second surface, 20... first surface layer, 22... second surface layer

Claims

1. An elastomer layer and a surface layer provided on either or both of a first surface and a second surface of the elastomer layer, the surface layer comprises one or more polypropylene-based resins selected from the group consisting of block polypropylenes which are copolymers with ethylene and random polypropylenes which are copolymers with ethylene, and calcium carbonate; The content of the calcium carbonate in the surface layer is 10 to 75% by mass based on the total mass of the surface layer, The thickness of the elastomer layer is 20 to 55 μm, The thickness of the surface layer is 0.4 to 5.0 μm, The melting point of the polypropylene-based resin is 135°C or higher and lower than 160°C.

2. The stretch film according to claim 1, wherein the surface layer contains 30 to 70% by mass of the polypropylene resin and 30 to 70% by mass of the calcium carbonate, based on the total mass of the surface layer.

3. The stretch film described in claim 1 or claim 2, wherein the elastomer layer comprises an olefin-based elastomer.

4. The stretch film described in claim 3, wherein the olefin-based elastomer includes a propylene-based elastomer.

5. The stretch film described in claim 4, wherein the olefin-based elastomer includes a propylene-ethylene copolymer.

Citation Information

Patent Citations

  • Laminate and medical container

    JP2013014127A

  • Silane-grafted polyolefin, and silane-crosslinked polyolefin resin

    JP2013119583A

  • Elastic laminate and article including the same, and elastic laminate elongation and article including the same

    JP2016112878A

  • Stretchable film, stretchable laminate, and product including the same

    JP2018103439A

  • Mold release film and method for producing same

    WO2014103781A1