Polyester Film
The polyester film with controlled surface roughness and non-spherical inorganic particles addresses particle drop-off and scratches, enhancing moldability and efficiency in can manufacturing.
Patent Information
- Application Number
- JP2021027826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-24
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2041-02-24
AI Technical Summary
Existing polyester films for laminating metal plates in can manufacturing suffer from particle drop-off, scratches, and processing wrinkles during transport and processing, leading to reduced production efficiency and moldability issues.
A polyester film composition with 95 mol% ethylene terephthalate units, controlled surface roughness (0.1 to 0.16 μm arithmetic mean height and 2.5 to 4.0 μm maximum peak height), and inclusion of non-spherical inorganic particles like porous silica and calcium carbonate, with specific friction and porosity ranges, enhances slipperiness and scratch resistance.
The film significantly reduces particle shedding, scratches, and wrinkles, improving moldability and production efficiency in can manufacturing processes.
Smart Images

Figure 0007554389000001 
Figure 0007554389000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester film used for the purpose of preventing corrosion of metal containers for soft drinks, beer, canned goods, etc., and particularly relates to a polyester film suitable for use in three-piece cans. More specifically, the present invention relates to a polyester film that has excellent transportability and can-forming properties (for example, bending, joining, repairing joints, flanging, attaching a top lid, filling contents, attaching a bottom lid, and retort sterilization) for metal plates, a film-laminated metal plate obtained by laminating the film onto a metal plate, and a metal container obtained by forming the film-laminated metal plate. [Background technology]
[0002] Patent Document 1 discloses a polyester film for laminating metal sheets, which is made by adding polyether ester elastomer and spherical PMMA particles to polyethylene terephthalate resin. However, there is a problem that the particles fall off during the can-making process, reducing production efficiency.
[0003] Patent Document 2 proposes a polyester film for laminating metal sheets, which contains 95 mol % to 98 mol % of ethylene terephthalate units and 0.5 to 2.0 mass % of amorphous inorganic fine particles. Patent Document 2 reports that it is possible to prevent the falling off of fine particles during the can manufacturing process and the peeling of the film at welded parts. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-251140 A [Patent Document 2] International Publication No. 2016 / 143818 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a polyester film which has little particle shedding during the can-making process, is free from scratches and processing wrinkles during transportation and processing of the film-laminated metal sheet, and has excellent formability in can-making. [Means for solving the problem]
[0006] The present invention comprises the following configurations. [1] A polyester film containing a polyester resin containing 95 mol% or more of ethylene terephthalate units, (1) The porosity of the film is 0 to 5.0% by volume; (2) The arithmetic mean height Sa of the film surface is 0.1 to 0.16 μm; (3) The maximum peak height (Sp) of the film surface is 2.5 to 4.0 μm; (4) The haze of the film is 25-70%; A polyester film characterized by: [2] The polyester film according to [1], which contains at least two types of non-spherical inorganic particles. [3] The polyester film according to [2], wherein at least one of the non-spherical inorganic particles is a porous silica particle. [4] The polyester film according to [2] or [3], wherein at least one of the non-spherical inorganic particles is calcium carbonate particle. [5] The polyester film according to any one of [1] to [4], wherein the polyester film contains 1 to 5 mol % of ethylene isophthalate units. [6] A film-laminated metal sheet comprising a metal sheet and the polyester film according to any one of [1] to [5] laminated on at least one surface of the metal sheet. [7] A metal container formed from the film-laminated metal sheet described in [6]. Effect of the Invention
[0007] The polyester film of the present invention is excellent in formability in the can-making process since it can suppress particle drop-off during the can-making process and also suppresses scratches and wrinkles during transportation of the film-laminated metal sheet and during can-making processing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will be described in detail below. [Polyester resin composition] The polyester film of the present invention is made of a polyester resin composition containing 95 mol% or more of ethylene terephthalate units, preferably 96 to 99 mol%, more preferably 97 to 98 mol% of ethylene terephthalate units. By making the ethylene terephthalate units in the polyester resin composition 95 mol% or more, sufficient heat resistance can be obtained, and problems such as shrinkage and peeling can be suppressed even if the film is heated to a high temperature during can forming.
[0009] The polyester resin composition of the present invention may contain ethylene isophthalate units as a copolymerization component. In this case, the ethylene isophthalate units are preferably contained in an amount of 1 to 5 mol%, more preferably 2 to 4 mol%. When the ethylene isophthalate units are contained in an amount of 1 mol% or more, the can forming property and slipperiness of the film are improved. In addition, the falling off of particles can be suppressed. When the content of the ethylene isophthalate units is 5 mol% or less, sufficient heat resistance can be obtained, and problems such as shrinkage and peeling can be suppressed even if the film is heated to a high temperature during can forming.
[0010] The polyester resin composition of the present invention may contain polyethylene terephthalate or copolymerized polyethylene terephthalate and other polyester resins. Examples of other polyester resins include polyester resins such as polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, and polypropylene terephthalate, and copolymerized polyesters obtained by copolymerizing these polyesters.
[0011] The intrinsic viscosity (IV) of the polyester resin composition in the present invention is preferably 0.57 to 1.2. If the intrinsic viscosity is less than 0.57, the mechanical properties of the resulting film may be degraded. If the intrinsic viscosity exceeds 1.2, no further improvement in the mechanical properties is obtained, and instead the productivity during the production of the polyester resin and polyester film decreases, which is uneconomical.
[0012] The polyester resin composition of the present invention may contain various additives, such as antioxidants, heat stabilizers, UV absorbers, plasticizers, pigments, antistatic agents, lubricants, crystal nucleating agents, etc. The amount of each of the above-mentioned additives is preferably 5% by mass or less based on 100% by mass of the polyester resin composition.
[0013] In order to impart electrostatic adhesion when forming a melt extrusion film, the polyester resin composition of the present invention may contain Mg salts such as magnesium acetate and magnesium chloride, Ca salts such as calcium acetate and calcium chloride, Mn salts such as manganese acetate and manganese chloride, Zn salts such as zinc chloride and zinc acetate, and Co salts such as cobalt chloride and cobalt acetate, in a total amount of 300 ppm or less of each metal ion. In this case, phosphoric acid or a phosphoric acid ester derivative such as trimethyl phosphate or triethyl phosphate may be added as a heat stabilizer in a range of 200 ppm or less as phosphorus atoms. If the total amount of metal ions other than the polymerization catalyst is 300 ppm or the phosphorus amount exceeds 200 ppm, the coloring of the obtained polyester resin becomes significant. In addition, the heat resistance and hydrolysis resistance of the polyester resin may also decrease, which is not preferable.
[0014] [Polyester film] The polyester film of the present invention is characterized in that the arithmetic mean height Sa of the surface roughness is 0.10 μm or more and 0.16 μm or less, and the maximum peak height Sp of the surface roughness is 2.5 μm or more and 4.0 μm or less. By having the arithmetic mean height and the maximum peak height of the surface roughness within the above ranges, the polyester film can be imparted with slipperiness and scratch resistance. As an example, slipperiness is a property required for film-laminated metal sheets to be easily peeled off one by one when a plurality of film-laminated metal sheets are transferred. In addition, slipperiness and scratch resistance are properties required for preventing scratches during transfer of cans and wrinkles during processing of the neck of the can in the can-making process (for example, bending, joining, repairing joints, flanging, attaching the top lid, filling the contents, attaching the bottom lid, and retort sterilization). These properties contribute to improving the forming processability of metal containers, particularly cans.
[0015] If the arithmetic mean height Sa is less than 0.10 μm, the transportability of the film-laminated metal sheet, and the effect of improving the scratching and wrinkle prevention in the can-making process and the molding processability may be insufficient. If it exceeds 0.16 μm, the particle dropout may be deteriorated. If the maximum peak height Sp is less than 2.5 μm, the transportability of the film-laminated metal sheet, and the effect of improving the scratching and wrinkle prevention in the can-making process and the molding processability may be insufficient. If it exceeds 4.0 μm, the particle dropout may be deteriorated.
[0016] As a method for keeping the arithmetic mean height Sa and the maximum peak height Sp within the range, there is a method in which at least two types of non-spherical inorganic fine particles are added to the polyester resin composition in an amount of 0.9 to 1.9 mass %, as described below.
[0017] The polyester film of the present invention is characterized in that the internal porosity is 0% by volume or more and 5.0% by volume or less. By making the internal porosity of the film 5.0% by volume or less, it is possible to suppress particle falling off during the can-making process. In order to set the arithmetic mean surface height Sa and maximum peak height Sp of the polyester film of the present invention within the above ranges and to make the internal porosity of the film 5.0% by volume or less, it is preferable to use non-spherical inorganic fine particles and to increase the stretching temperature and lower the stretching ratio in the longitudinal and transverse directions of the film.
[0018] The polyester film of the present invention preferably has a haze of 25 to 70%, more preferably 35 to 60%. The haze in the above range can impart the polyester film with concealing properties. As an example, the concealing properties can adequately conceal the steel sheet surface in the film-laminated metal sheet, thereby preventing malfunction of a defect detector for the metal sheet. If the haze is lower than 25%, there is a high possibility that a defect detector will malfunction in the process of detecting processing defects in the steel sheet in the film-laminated metal sheet. On the other hand, if the haze is higher than 70%, it becomes difficult to detect defects such as scratches and stains on the steel sheet of the film-laminated metal sheet.
[0019] The polyester film of the present invention preferably has a sum of the static friction coefficient and the kinetic friction coefficient between the films of 0.50 to 0.65. If it exceeds 0.65, the slipperiness is insufficient and the film may be easily scratched. On the other hand, if it is less than 0.50, the effects of slipperiness and scratch prevention are saturated, and particles are likely to fall off.
[0020] The polyester film of the present invention preferably has a tensile breaking strength in the longitudinal direction and the width direction of 100 to 300 MPa, and by keeping it in this range, the occurrence of film cracks when a laminated metal can is dropped can be suppressed. The polyester film of the present invention preferably has a tensile breaking elongation in the longitudinal direction and the width direction of 60 to 140%, and by keeping it in this range, the occurrence of film cracks when a laminated metal can is dropped can be suppressed.
[0021] The heat shrinkage rate of the polyester film of the present invention in the longitudinal direction of the film after heat treatment for 15 minutes at 150° C. is preferably 1% or more and 3% or less. If the heat shrinkage rate at 150° C. is less than 1%, operational troubles such as wrinkles and static electricity are likely to occur during thermal lamination, while if it exceeds 3%, the adhesive strength during thermal lamination is low and a high lamination temperature close to or higher than the melting point is required, which is not preferable from a practical standpoint.
[0022] The thickness of the polyester film of the present invention is not particularly limited, but is preferably 8 μm or more and 50 μm or less, more preferably 10 μm or more and 30 μm or less, from the viewpoints of the covering effect (rust prevention), formability, and furthermore, economy. If the film thickness is less than 8 μm, the covering effect cannot be obtained, and if it exceeds 50 μm, the quality is excessive and is not economically preferable.
[0023] [Inorganic fine particles] The polyester film of the present invention preferably contains inorganic fine particles, more preferably contains at least two kinds of non-spherical or amorphous inorganic fine particles. The inorganic fine particles are preferably selected from one or more kinds of inorganic fine particles that can impart the polyester film with concealment, slippage, and scratch resistance. The content of the inorganic fine particles is preferably 0.9% by mass or more, more preferably 1.0% by mass or more, and even more preferably 1.2% by mass or more. The upper limit is preferably 1.9% by mass or less, more preferably 1.8% by mass or less. If the non-spherical inorganic fine particles are contained in an amount of more than 3.0% by mass, the effects of concealment, slippage, and scratch resistance may be saturated, and particles may fall off or the film strength may decrease.
[0024] Here, the non-spherical inorganic fine particles are non-spherical inorganic fine particles such as spherical silica fine particles, spherical crosslinked PMMA fine particles, spherical crosslinked polystyrene fine particles, and spherical silicone fine particles. If only spherical or nearly spherical fine particles are contained, it becomes difficult to achieve both slipperiness and scratch resistance and the prevention of particle shedding. Examples of the non-spherical inorganic particles in the present invention include inorganic fine particles produced by pulverization and classification, such as porous silica fine particles and heavy calcium carbonate fine particles, as well as inorganic fine particles such as cubic fine particles and rectangular parallelepiped fine particles.
[0025] The types of inorganic fine particles in the present invention include metal oxides such as silica, alumina, zirconia, and titanium oxide, composite metal oxides such as kaolin, zeolite, sericite, and sepiolite, sulfates such as calcium sulfate and barium sulfate, phosphates such as calcium phosphate and zirconium phosphate, carbonates such as calcium carbonate, etc. These inorganic fine particles may be natural or synthetic, so long as they are non-spherical.
[0026] The average particle size of the non-spherical inorganic fine particles in the present invention is preferably 0.5 to 5.0 μm, more preferably 0.8 to 4.0 μm. If the average particle size is less than 0.5 μm, the effect of improving the sliding property between the film and the metal plate at high temperatures may be small, and the film may be easily scratched. On the other hand, if the average particle size exceeds 5.0 μm, the above effect may be saturated, the fine particles may be easily dropped off from the film, the film may be easily broken during film formation, or the impact strength may be reduced. The average particle size of the above particles is a value measured by a laser method as a 50% mass average.
[0027] In a preferred embodiment of the present invention, at least one of the two or more types of non-spherical inorganic fine particles has an average particle size of 3.0 to 4.0 μm and a specific surface area of 350 to 650 m. 2 The porous silica particles have a particle size of 0.1 to 1.0 mass %, preferably 0.3 to 0.6 mass %. The porous silica particles mainly contribute to slip properties and scratch resistance.
[0028] The average particle size of the porous silica particles can be determined from the cumulative volume frequency 50% diameter value using a laser diffraction / scattering method. The specific surface area of the porous silica particles can be measured by a simplified BET method in accordance with JIS Z8830:2013.
[0029] In a preferred embodiment of the present invention, at least one of the two or more types of non-spherical inorganic fine particles has an average particle size of 0.50 to 2.5 μm and a specific surface area of 1 to 5 m. 2 / g. Particularly, heavy calcium carbonate particles are preferred. More preferably, the average particle size is 0.8 to 1.5 μm and the specific surface area is 1 to 5 m. 2 / g. The content of calcium carbonate particles is preferably 0.1 to 2.0% by mass, and more preferably 0.5 to 1.5% by mass. The calcium carbonate particles mainly contribute to hiding properties.
[0030] The average particle size of calcium carbonate particles can be determined from the value of the cumulative volume frequency of 50% using the laser diffraction / scattering method. The specific surface area of calcium carbonate particles can be measured by the air permeability method. Specifically, it is measured under the following measurement conditions using a constant pressure powder specific surface area measuring device (Shimadzu Corporation: SS-100). Specific gravity of ground calcium carbonate: 2.7g / ml Sample: 2.7g Amount of water to be aerated: 5ml Sample layer thickness: specific surface area 10,000 cm 2 If the specific surface area is less than 10,000 cm2 / g, adjust it to 8 mm to 9 mm; if the specific surface area is more than 10,000 cm2 / g, adjust it to 20,000 cm2 2 / g or less, adjust to 9mm~12mm; specific surface area 20000cm 2 If it exceeds / g, adjust it to between 12mm and 13mm.
[0031] The non-spherical inorganic fine particles may be added to the polyester film during the production process of the polyester resin composition, or may be added by melt-kneading the polyester resin composition and the inorganic fine particles, or may be added as a master batch containing a high concentration of inorganic fine particles during the production of the polyester film.
[0032] [Manufacturing method of polyester film] The method for producing the polyester film of the present invention is not particularly limited, but it is preferable to form an unstretched film by extrusion and then uniaxially or biaxially stretch the film. By forming the film into a stretched film, crystal orientation occurs, and strength and excellent processability can be obtained.
[0033] However, as for the stretching conditions at this time, it is desirable to give an appropriate temperature and stretching ratio within a range in which the film does not melt during the preheating and stretching process in order to obtain a film with few voids, which is one of the requirements of the present invention. Here, insufficient heat is not preferred because the interfacial stress between the inorganic fine particles and the polyethylene terephthalate due to orientation becomes large, resulting in large voids and significant particle drop-off, and a high temperature is not preferred because it makes it difficult to form protrusions on the film surface and may result in a decrease in scratch resistance and can-forming ability.
[0034] Taking the longitudinal stretching temperature during sequential biaxial stretching as an example, a preferred temperature range is 70 to 130°C, more preferably 80 to 100°C, as the stretching temperature during longitudinal stretching. The stretching temperature during widthwise stretching is preferably 90 to 160°C, more preferably 100 to 130°C, and the heat fixation degree is preferably 180 to 240°C, more preferably 200 to 230°C. It is also preferable to set the stretching ratio within an appropriate range, and a low stretching ratio may not provide the desired strength or surface protrusions or may impair the flavor of the contents, while a high stretching ratio may make production difficult, which is not preferable. The preferred stretching ratios for the sequential biaxial stretching are 3 to 5 times in the longitudinal direction and 3 to 5 times in the transverse direction, and more preferably 3 to 4.5 times in the longitudinal direction and 3 to 4.5 times in the transverse direction.
[0035] The polyester film of the present invention may have an adhesive layer on one side. The polyester film having such an adhesive layer is also included in the scope of the present invention. The adhesive layer can be formed by a method of forming an adhesive resin layer by co-extrusion during film production, or by a coating method. When the co-extrusion method is used, copolymerized polyethylene terephthalate, polybutylene terephthalate, or a mixed resin thereof can be used.
[0036] When the coating method is used, an organic solvent-soluble resin composition or a water-dispersed resin composition can be used, and a dispersion type resin composition is preferable. A water-dispersed resin composition is a resin composition that is insoluble in water itself but can be dispersed or dissolved in an aqueous solvent, and a known resin composition can be used. When the adhesive layer is formed by the coating method, it may be applied to a stretched film during film formation (in-line) or to a film after film formation (off-line).
[0037] The polyester film of the present invention may be subjected to a surface treatment such as a corona treatment, a plasma treatment or a flame treatment in order to improve the adhesion between the adhesive layer and the metal plate.
[0038] [Film-laminated metal sheet] The film-laminated metal sheet of the present invention can be obtained by laminating the polyester film of the present invention on at least one surface of a metal sheet.
[0039] The polyester film of the present invention can be laminated on at least one side of a metal plate by any known method, but is not particularly limited thereto. A preferred method is a thermal lamination method, and a particularly preferred method is a method of electrically heating a metal plate to perform thermal lamination. The polyester film may be laminated on both sides of the metal plate. When the polyester film is laminated on both sides of a metal plate, the two films may be laminated simultaneously or sequentially.
[0040] Furthermore, when a polyester film provided with an adhesive layer is laminated to at least one side of a metal plate, the adhesive layer is used as a layer to be laminated to the metal plate side, and in order to improve the barrier properties and corrosion resistance of the adhesive layer and to further improve the laminate adhesion, a known adhesive containing a thermosetting resin as a main component can be applied in advance to the adhesive layer.
[0041] The metal plate used in the film-laminated metal plate of the present invention is not particularly limited, but examples thereof include tinplate, tin-free steel, aluminum, and aluminum alloys. The thickness is not particularly limited, but is preferably 100 to 500 μm from the viewpoints of securing strength and economic efficiency. More preferably, it is 150 to 400 μm. The metal plate is preferably subjected to a treatment such as chromate treatment or alumite treatment in order to ensure sufficient adhesive strength with the film.
[0042] [Metal container] The metal container of the present invention can be obtained by molding the film-laminated metal sheet. The shape of the metal container is not particularly limited, but examples thereof include a can, a bottle, and a barrel. The method for forming the metal container of the present invention is also not particularly limited, but known methods such as drawing, ironing, drawing and ironing, cylindrical forming, welding, soldering, and roll-seaming can be used. EXAMPLES
[0043] The contents and effects of the present invention will be specifically explained below by way of examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.
[0044] Various evaluation methods in the present invention are described below. (1) Intrinsic viscosity of polyester resin (IV) 0.2 g of polyester resin was dissolved in 50 ml of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (60 / 40 (mass ratio)), and the viscosity was measured using an Ostwald viscometer at 30° C. The unit is dl / g. (2) Melting point of polyester resin The polyester composition was heated and melted at 300°C for 5 minutes, and then quenched with liquid nitrogen to obtain a sample (10 mg). The exothermic-endothermic curve (DSC curve) was measured in a nitrogen stream at a heating rate of 10°C / min using a differential scanning calorimeter (DSC). The apex temperature of the endothermic peak associated with melting was recorded as the melting point Tm (°C).
[0045] (3) Film thickness The measurement was performed in accordance with JIS K7130-1999 Method A using a dial gauge (manufactured by Mitutoyo Corporation).
[0046] (4) Film haze The measurement was performed in accordance with JIS K7136-2000 using a haze meter (300A manufactured by Nippon Denshoku Industries Co., Ltd.) The measurement was performed three times, and the average value was calculated.
[0047] (5) Film porosity (%) The cross section of the obtained film in the longitudinal direction was cut and then fixed to the sample stage of a scanning electron microscope (Hitachi, TM3030plus). The cross section was gold sputtered for 1 minute using a sputtering device (Vacuum Device, MSP-mini) at a voltage of 0.3 KV and a current of 26 mA, and observed at a magnification of 2000 times using the scanning electron microscope. 2 ) and the total area (μm 2 ) was calculated and inserted into the following formula (1) to determine the porosity (%). By the above-mentioned procedure, five observation images were taken and the porosity was calculated. The average of the five images was taken as the porosity (%) of the polyester layer A. Porosity of polyester layer A (%) = Area of voids in polyester layer A (μm 2 ) / Total area of polyester layer A (μm 2 ) x 100.
[0048] (6) Film surface roughness (arithmetic mean height Sa and maximum peak height Sp) The obtained film was cut into an area of 10 cm in the longitudinal direction × 10 cm in the transverse direction, and a white laser interferometer (NEW VIEW8300) manufactured by Zygo was used to scan and measure the area using a 20x lens attached to the interferometer. Measurements were performed at 10 arbitrary points on the 10cm × 10cm sample, within a range of 0.82μm in the MD direction and 0.82μm in the transverse direction on one surface, and the arithmetic mean height Sa (μm) and maximum peak height Sp were measured.
[0049] (7) Sum of the friction coefficients of the films The obtained film was cut into a piece measuring 400 mm in the longitudinal direction and 100 mm in the width direction to prepare a sample film. This was aged for 12 hours in an atmosphere of 23°C and 65% RH. The sample was divided into a piece measuring 300 mm in the longitudinal direction and 100 mm in the width direction for the slide platform and a piece measuring 100 mm in the longitudinal direction and 100 mm in the width direction for the load. The sample for the slide platform was set on the slide platform, and the sample for the load was set with a metal load of 3.5 kg (the size of the base area was 39.7 mm 2 The static and dynamic friction coefficients of the metal load were measured using a Tensilon (RTG-1210) manufactured by AND Co., Ltd. under the conditions of a tensile speed of 200 mm / min, 23°C, and 65% RH, and the average of three measurements was calculated.
[0050] (8) Particle shedding property Using a Toyo Seiki Co., Ltd. color fastness friction tester, a 500g load friction element with 0.05mm thick aluminum foil set on it was rubbed on the film at 20-40°C for 30 seconds at 30 reciprocating strokes / min over a 100mm distance. After that, the particle shed marks on the film surface were observed at 500x magnification using a scanning electron microscope (Hitachi Co., Ltd., TM3030plus). The observed images were judged according to the following criteria. Judgment A: Almost no traces of particle shed were observed. Grade B: Traces of particle detachment are partially observed. Judgement: C: Traces of fallen particles are observed over the entire surface.
[0051] (9) Molding processability A degreased 190 μm thick metal plate (tin-free steel, L-type bright finish, surface roughness 0.3-0.5 μm, manufactured by Nippon Steel Corporation) was preheated to 140° C. The metal plate was aligned with the adhesive layer surface of a polyester film provided with an adhesive layer, and the laminated product was passed between rubber rolls at a pressure of 500 N / cm and a speed of 10 m / min. It was then rapidly cooled with water to obtain a film-laminated metal plate [thickness 202 μm (polyester film / metal plate=12 μm / 190 μm)]. Using a color fastness friction tester manufactured by Toyo Seiki Co., Ltd., a friction member with a load of 400 g on which a film sample was set was used to rub the obtained film-laminated metal plate for 1 minute under the condition of a reciprocating distance of 100 m at 30 reciprocating motions per minute. After that, scratches on the film surface of the film-laminated metal plate were visually observed and evaluated according to the following criteria. Note that a rating of B or higher indicates practical use. Judgment A: No scratches found. Judgment B: Thin scratches are visible. Judgement C: Scratches are visible.
[0052] [Production of polyester resin] Next, the types and contents of the polyesters used in the examples and comparative examples will be described.
[0053] (1) Polyester resin A Terephthalic acid and ethylene glycol were added to a stainless steel autoclave equipped with a stirrer, distillation column, and pressure regulator, and an esterification reaction and a polycondensation reaction using a catalyst were carried out to obtain a polyester resin with an IV of 0.61 dl / g. This polyester resin was used in a batch-type solid-phase polymerization apparatus to obtain a polyester resin A with an IV of 0.68 dl / g. The melting point (Tm) of this polyester resin A was 255.0°C.
[0054] (2) Polyester resin B Terephthalic acid, isophthalic acid, and ethylene glycol were added to a stainless steel autoclave equipped with a stirring stirrer, a distillation column, and a pressure regulator, and an esterification reaction and a polycondensation reaction using a catalyst were carried out. After that, this polyester resin was used in a batch-type solid-phase polymerization apparatus to obtain polyester resin B with an isophthalic acid copolymerization amount of 10.8 mol% and IV=0.63 dl / g among the acid components. The melting point (Tm) of this polyester resin B was 225.0°C.
[0055] (3) Polyester resin C Polyester resin C was obtained by melt-kneading 95 parts by mass of polyester resin A with 5 parts by mass of non-spherical calcium carbonate particles (manufactured by Maruo Calcium Co., Ltd., Caltex 5, irregular shape, average particle size 1 μm) in a twin-screw extruder.
[0056] (4) Polyester resin D Polyester resin A was mixed with 98 parts by mass of non-spherical porous silica particles (Fuji Silysia, Silica 550, amorphous, average particle size 3.9 μm, specific surface area 500 m 2 Polyester resin D was obtained by melt-kneading 2 parts by mass of each of the polyester resins (1 / g) in a twin-screw extruder.
[0057] (5) Polyester resin E Polyester resin A was mixed with 98 parts by mass of non-spherical porous silica particles (Fuji Silysia, Silica 310, amorphous, average particle size 2.7 μm, specific surface area 300 m 2 Polyester resin E was obtained by melt-kneading 2 parts by mass of each of the polyester resins (1 / g) in a twin-screw extruder.
[0058] (6) Polyester resin F Polyester resin A was mixed with 98 parts by mass of non-spherical porous silica particles (Fuji Silysia, Silica 350, amorphous, average particle size 3.9 μm, specific surface area 300 m 2 Polyester resin F was obtained by melt-kneading 2 parts by mass of each of the polyester resins (1 / g) in a twin-screw extruder.
[0059] (7) Polyester resin G Polyester resin A was mixed with 98 parts by mass of non-spherical porous silica particles (Fuji Silysia, Silica 710, amorphous, average particle size 2.8 μm, specific surface area 700 m 2 Polyester resin G was obtained by melt-kneading 2 parts by mass of each of the polyester resins (1 / g) in a twin-screw extruder.
[0060] (8) Polyester resin H Polyester resin A was mixed with 98 parts by mass of non-spherical porous silica particles (Fuji Silysia, Silica 730, amorphous, average particle size 4.0 μm, specific surface area 700 m 2 Polyester resin H was obtained by melt-kneading 2 parts by mass of each of the polyester resins (1 / g) in a twin-screw extruder.
[0061] (9) Polyester Resin I Polyester resin A was mixed with 95 parts by mass of spherical polymethyl methacrylate (PMMA) particles (manufactured by Nippon Shokubai Co., Ltd., Eposter MA1002, spherical, average particle size 2 μm, specific surface area 2 m 2 The mixture (5 parts by mass of ethylenediaminetetraacetate / g) was melt-kneaded in a twin-screw extruder to obtain a polyester resin I having an IV of 0.52 dl / g.
[0062] Example 1 As the film raw material, polyester resins A, B, C and D were mixed in a mass ratio of 37.2:27.8:20:15 so that the ethylene isophthalate unit was 3 mol% and the content of inorganic fine particles was as shown in the table, and fed to a hopper, and melt-extruded from a T-die of an extruder at a resin temperature of 280°C, cast onto a rotating cooling drum and cooled to solidify to obtain an unstretched sheet. The unstretched sheet was then stretched 3.7 times in the longitudinal direction at 110°C and 4.1 times in the transverse direction at 130°C, heat-set at 225°C, and then relaxed 5% in the transverse direction at the same temperature to produce a biaxially stretched polyester film with a thickness of 12 μm.
[0063] (Examples 2 and 3) As the film raw materials, the mixing ratio of polyester resins A, B, C and D was changed so as to obtain the composition shown in Table 1, and a biaxially stretched polyester film was obtained in the same manner as in Example 1.
[0064] (Comparative Examples 1 to 8) As film raw materials, polyester resins A to I were mixed to have the compositions shown in Table 1, and a biaxially stretched polyester film was obtained in the same manner as in Example 1.
[0065] [Table 1]
[0066] Table 2 shows the physical properties of the polyester films produced in Examples 1 to 3 and Comparative Examples 1 to 8, as well as the evaluation results of particle shedding, moldability, and visibility.
[0067] [Table 2]
[0068] As shown in the results of Table 2, the films of Examples 1 to 3 had a porosity and arithmetic mean height Sa within the specified range, so they were not scratched during transportation of the laminated metal sheet, had excellent can-making properties and little particle shedding during the can-making process, and had excellent molding processability in can making.
[0069] In Comparative Examples 1 and 2, in which spherical microparticles were used, the arithmetic mean height Sa of the obtained film was within the specified range, but the porosity was high, resulting in a lot of particle dropout and reducing production efficiency. In Comparative Examples 3 and 4, in which porous silica microparticles with a small specific surface area were used, the porosity of the resulting film was within the specified range, but the Sa and Sp were low, and the sum of the friction coefficients was also large, resulting in scratches during transportation of the film-laminated metal plate and poor molding processability during can manufacturing. In Comparative Examples 5 and 6, in which porous silica fine particles having a large specific surface area were used, the films obtained were unable to achieve both prevention of particle shedding and moldability, resulting in reduced production efficiency. In Comparative Example 7, in which the content of fine particles was less than the specified amount, the Sa and Sp of the obtained film were smaller than the specified ranges, and the moldability was poor. In Comparative Example 8, in which the content of fine particles was higher than the specified amount, the porosity of the obtained film was high, leading to a large amount of particle dropout and a decrease in production efficiency. [Industrial Applicability]
[0070] The polyester film of the present invention has excellent transportability of film-laminated metal sheets and can-forming properties (for example, bending, joining, joint repair, flanging, top lid attachment, filling with contents, bottom lid attachment, and retort sterilization) and causes little particle drop-off and little contamination during the can-forming process. Therefore, the polyester film of the present invention is useful in applications such as films for metal containers for coffee drinks, soft drinks, canned goods, etc., and is expected to make a great contribution to the industrial world.
Claims
1. A polyester film containing a polyester resin containing 95 mol % or more ethylene terephthalate units, comprising two or more types of non-spherical or irregular inorganic fine particles, at least one of the two or more types of inorganic fine particles having an average particle diameter of 3.0 to 4.0 μm, a specific surface area of 350 to 650 m 2 / g, and a content of 0.1 to 1.0 mass %, and at least one of the two or more types of inorganic fine particles having an average particle diameter of 0.50 to 2.5 μm, a specific surface area of 1 to 5 m 2 / g, and a content of 0.1 to 2.0 mass %, (1) The porosity of the film is 0 to 5.0 volume %; (2) The arithmetic mean height Sa of the film surface is 0.1 to 0.16 μm; (3) The maximum peak height (S) of the film surface is 2.5 to 4.0 μm; (4) The haze of the film is 25 to 70%; A polyester film characterized by:
2. 2. The polyester film according to claim 1, comprising at least two types of non-spherical inorganic particles.
3. 3. The polyester film according to claim 2, wherein at least one of the non-spherical inorganic particles is a porous silica particle.
4. 4. The polyester film according to claim 2, wherein at least one of the non-spherical inorganic particles is a calcium carbonate particle.
5. The polyester film according to any one of claims 1 to 4, wherein the polyester film contains 1 to 5 mol % of ethylene isophthalate units.
6. A film-laminated metal sheet, comprising a metal sheet and the polyester film according to any one of claims 1 to 5 laminated on at least one surface of the metal sheet.
7. A metal container produced by molding the film-laminated metal sheet according to claim 6.
Citation Information
Patent Citations
Polyester film for three-piece can lamination