Crystalline europium compound and method for producing the same

By producing crystalline europium compounds through a mechanochemical reaction, the limitations of amorphous europium compounds are overcome, enabling lower cytotoxicity and luminescent properties for bioimaging and other applications.

JP7554424B2Active Publication Date: 2024-09-20OHARA INC +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020046604
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-17
Publication Date
2024-09-20
Estimated Expiration
2040-03-17

AI Technical Summary

Technical Problem

Europium compounds, such as europium chloride, europium hydroxide, and europium chloride hydroxide, are typically amorphous and lack crystalline forms, limiting their potential applications and effects.

Method used

A method involving a solid-phase mechanochemical reaction between a silicate base material and europium (III) chloride hexahydrate under specific conditions, including a molar ratio and load range, to produce crystalline forms of europium compounds with defined diffraction peaks.

Benefits of technology

The crystalline forms exhibit lower ion elution, reduced cytotoxicity, and luminescent properties, making them suitable for bioimaging and other applications like light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554424000009
    Figure 0007554424000009
  • Figure 0007554424000010
    Figure 0007554424000010
  • Figure 0007554424000008
    Figure 0007554424000008
Patent Text Reader

Abstract

To provide crystals of europium compound which contain europium.SOLUTION: Provided are crystals of an europium compound which, in a powder X-ray diffraction pattern, has a first diffraction peak in a diffraction angle (2θ) in a range of 34.3 to 36.1° with a half-value width being 1.8° or less, and / or has a second diffraction peak in a diffraction angle (2θ) in a range of 28.6 to 29.6°and a third diffraction peak in a diffraction angle (2θ) in a range of 36.8 to 38.4° with a half-value width of the second diffraction peak being 1.0° or less and a half-value width of the third diffraction peak being 1.6° or less, where the europium compound is at least one compound selected from compounds represented by the following chemical formulas (1) to (4): EuClx (1); Eu(OH)2 (2); Eu(OH)2Cl (3); and EuOCl (4) (in Formula (1), x is 0.05 to 5).SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crystalline europium compound and a method for producing a crystalline europium compound. [Background technology]

[0002] Europium compounds containing europium are used, for example, as luminescent substances. Such luminescent substances can be used, for example, in bioimaging technology, in which the luminescent substance is incorporated into cells or molecules in a living body, and the cells or molecules are visualized (imaged) to analyze their dynamics and functions (see Patent Document 1).

[0003] Here, europium compounds such as europium chloride, europium hydroxide, and europium chloride hydroxide are amorphous, and no crystals have been known so far. If crystals of these europium chloride, europium hydroxide, and europium chloride hydroxide can be provided, effects and applications that are difficult to obtain with amorphous substances can be expected. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 170531 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a crystal of a europium compound containing europium and a method for producing the same. [Means for solving the problem]

[0006] The present inventors have discovered a solid 29 Si(OSi) in Si-NMR spectrum 4The peak area derived from Q 4 Then, HO-Si(OSi) 3 The peak area derived from Q 3 When 4 / Q 3 The inventors have found that a crystalline body of a europium compound can be produced by mixing a silicate-based base material having a molecular weight of 2.0 to 3.9 with europium (III) chloride hexahydrate such that the ratio of the number of moles of europium to the total number of moles of silicon and europium in the silicate-based base material is 1.0 mol % or more, and subjecting the mixture to a solid-phase mechanochemical reaction under a load of 4 N to 24 N, thereby completing the present invention. That is, the present invention has the following configuration.

[0007] [1] A crystalline europium compound containing europium, In a powder X-ray diffraction pattern, a first diffraction peak is present in a diffraction angle (2θ) range of 34.3 to 36.1°, and the half width of the first diffraction peak is 1.8° or less, and / or a second diffraction peak is present in a diffraction angle (2θ) range of 28.6 to 29.6°, and a third diffraction peak is present in a diffraction angle (2θ) range of 36.8 to 38.4°, and the half width of the second diffraction peak is 1.0° or less, and the half width of the third diffraction peak is 1.6° or less, A crystalline europium compound, which is at least one compound selected from the compounds represented by the following formulas (1) to (4): EuCl x (1) Eu(OH) 2 (2) Eu(OH) 2 Cl···(3) EuOCl (4) (In formula (1), x is 0.05 or more and 5 or less.)

[0008] [2] A method for producing a crystalline form of the europium compound according to [1] above, comprising the steps of: The method includes a step of mixing a silicate-based substrate with europium(III) chloride hexahydrate and subjecting the mixture to a solid-phase mechanochemical reaction, The silicate-based substrate contains silicon (Si) and oxygen (O) and is a solid 29 Si(OSi) in Si-NMR spectrum 4 The peak area derived from Q 4 Then, HO-Si(OSi) 3 The peak area derived from Q 3 When 4 / Q 3 is 2.0 to 3.9, The solid-phase mechanochemical reaction is carried out by adding europium(III) chloride hexahydrate so that the ratio of the number of moles of europium element to the total number of moles of silicon element and europium element in the silicate-based substrate is 1.0 mol % or more, and the reaction is carried out under a load of 4 N or more and 24 N or less. Effect of the Invention

[0009] According to the present invention, it is possible to provide a crystal of europium chloride, europium hydroxide, or europium chloride hydroxide. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic cross-sectional view showing a structure in which the entire surface of a spherical silicate-based substrate is covered with crystals of a europium compound. [Diagram 2] 1 is a solid-state 29Si-NMR spectrum of silicate-based substrate 1. [Diagram 3] 1 is a powder X-ray diffraction pattern of a silicate-based substrate 1. [Figure 4] 1 shows the results of measuring the average particle size of silicate-based substrate 1 using a field emission scanning electron microscope (FE-SEM). [Diagram 5] FIG. 2 is a schematic side view illustrating a manufacturing apparatus used in the manufacturing method of Example 1. [Figure 6] 1 shows powder X-ray diffraction patterns of particles of Examples and Comparative Examples. [Figure 7] 4 shows the excitation spectrum and fluorescence spectrum of the particles of the example. [Figure 8]1 is a powder X-ray diffraction pattern of particles of an example. [Figure 9] FIG. 1 shows the results of measuring cell density in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. <Europium compound crystals> The crystalline form of the europium compound of the present invention has, in a powder X-ray diffraction pattern, a first diffraction peak in the diffraction angle (2θ) range of 34.3 to 36.1°, with the half-width of the first diffraction peak being 1.8° or less, and / or a second diffraction peak in the diffraction angle (2θ) range of 28.6 to 29.6° and a third diffraction peak in the diffraction angle (2θ) range of 36.8 to 38.4°, with the half-width of the second diffraction peak being 1.0° or less, and the half-width of the third diffraction peak being 1.6° or less.

[0012] The europium compound crystal of the present invention contains at least one compound selected from the compounds represented by the following chemical formulas (1) to (4). EuCl x (1) Eu(OH) 2 (2) Eu(OH) 2 Cl···(3) EuOCl (4) (In formula (1), x is 0.05 or more and 5 or less.)

[0013] The europium compound crystal of the present invention may have a first diffraction peak in a diffraction angle (2θ) range of 34.3 to 36.1°, and the half width of the first diffraction peak may be 1.8° or less, or may have a second diffraction peak in a diffraction angle (2θ) range of 28.6 to 29.6° and a third diffraction peak in a diffraction angle (2θ) range of 36.8 to 38.4°, and the half width of the second diffraction peak may be 1.0° or less and the half width of the third diffraction peak may be 1.6° or less. Alternatively, the optical fiber may have a first diffraction peak in a diffraction angle (2θ) range of 34.3 to 36.1°, the half width of the first diffraction peak being 1.8° or less, a second diffraction peak in a diffraction angle (2θ) range of 28.6 to 29.6°, and a third diffraction peak (2θ) in a diffraction angle (2θ) range of 36.8 to 38.4°, the half width of the second diffraction peak being 1.0° or less, and the half width of the third diffraction peak being 1.6° or less. The half width of the first diffraction peak is preferably 1.1° or less, the half width of the second diffraction peak is preferably 0.6° or less, and the half width of the third diffraction peak is preferably 1.0° or less. The first diffraction peak is derived from a crystalline form of a compound represented by chemical formula (1) or (2), while the second and third diffraction peaks are derived from a crystalline form of a compound represented by chemical formula (3) or (4). In the chemical formula (1), x is preferably 0.2 or more and 0.6 or less.

[0014] "Having a diffraction peak with a diffraction angle (2θ) in the range of a° to b°" means that the peak top position of the diffraction peak (diffraction peak top position) is within the range of a° to b°. Therefore, for example, in the case of a broad peak, the entirety of the peak from end to end does not necessarily need to be within the range of a° to b°.

[0015] Furthermore, the crystalline form of the europium compound of the present invention may have other peaks in addition to the specific diffraction peaks described above. For example, in the case of a compound represented by chemical formula (1) or (2), the compound may have diffraction peaks in the range of a diffraction angle (2θ) of 25.9 to 26.5° and in the range of a diffraction angle (2θ) of 31.6 to 32.2°. The diffraction peak in the range of a diffraction angle (2θ) of 25.9 to 26.5° and the diffraction peak in the range of a diffraction angle (2θ) of 31.6 to 32.2° each preferably have a half-width of 0.6° or less, more preferably 0.4° or less. In the case of a crystalline form of the compound represented by chemical formula (3) or (4), the diffraction peak may also have a diffraction angle (2θ) in the range of 39.0 to 40.2°. The half-width of the diffraction peak in the range of diffraction angle (2θ) of 39.0 to 40.2° is preferably 1.2° or less, and more preferably 0.8° or less.

[0016] Conventionally, crystals of the compounds represented by the above chemical formulas (1) to (4) have not been known. However, as will be described in detail later, by using a specific silicate-based base material and europium (III) chloride hexahydrate and carrying out a solid-phase mechanochemical reaction under specific conditions, crystals of the compounds represented by the above chemical formulas (1) to (4) having the above specific diffraction peaks were obtained. The term "crystalline material" refers to a material that is not amorphous and has a crystallinity represented by the following formula (5) of greater than 0. The crystallinity is preferably greater than 0.10. Crystallinity = {crystalline diffraction peak area / amorphous halo diffraction peak area} (5) (In formula (5), the "crystalline diffraction peak area" is the sum of the areas of the diffraction peaks derived from the crystals at 2θ=20 to 55°, and the "amorphous halo diffraction peak area" is the value obtained by subtracting the crystalline diffraction peak area from the sum of the areas of all the diffraction peaks observed at 2θ=20 to 55°.)

[0017] The europium compound crystal of the present invention is less susceptible to ion elution, such as chloride ion, than the amorphous form, and therefore the adverse effects caused by ion elution are suppressed. The europium compound crystal of the present invention has the characteristic of having lower cytotoxicity than the amorphous form, for example. In addition, the crystal of the europium compound of the present invention contains europium (III) and therefore functions as a luminescent substance. The crystal of the europium compound of the present invention is excited and emits light in the visible light region, and has an excitation wavelength λ ex is, for example, 395 nm or 464 nm, and the fluorescence wavelength λ em is, for example, 615 nm. Thus, the crystal of the europium compound of the present invention has low cytotoxicity and functions as a luminescent substance, and therefore can be preferably used in, for example, bioimaging technology. In addition, the crystal of the europium compound of the present invention has an excitation wavelength and an emission wavelength in the visible light region, so that in bioimaging, the deterioration of biological tissue and labeling materials due to light irradiation can be reduced, and the light scattering on the sample surface can be reduced, improving the observation sensitivity. When used in bioimaging technology, it is preferable to use the crystal in a spherical shape with an average particle size of about 50 nm to 470 nm.

[0018] <Method of manufacturing europium compound crystals> The above-mentioned crystal of the europium compound of the present invention includes a step of mixing a silicate-based base material with europium chloride (III) hexahydrate and subjecting it to a solid-phase mechanochemical reaction, and the silicate-based base material contains silicon element (Si) and oxygen element (O), and the solid 29 Si(OSi) in Si-NMR spectrum 4 The peak area derived from Q 4 Then, HO-Si(OSi) 3 The peak area derived from Q 3 When 4 / Q 3 is 2.0 to 3.9, and the solid-phase mechanochemical reaction can be produced by the method for producing a crystalline body of a europium compound of the present invention, in which europium (III) chloride hexahydrate is added so that the ratio of the number of moles of europium element to the total number of moles of silicon element (Si) and europium element (Eu) in the silicate-based base material (number of moles of Eu / (number of moles of Si+number of moles of Eu)) is 1.0 mol % or more, and the reaction is carried out under a load of 4 N or more and 24 N or less.

[0019] The silicate-based substrate used in the production method of the present invention contains silicon element (Si) and oxygen element (O). The molar ratio O / Si of O to Si in the silicate-based substrate is preferably 2.0 to 2.2. Examples of the silicate-based substrate include substrates made of silicon oxide such as silica and silicates, which may be crystalline or amorphous.

[0020] In addition, silicate-based substrates are solid 29 Si(OSi) in Si-NMR spectrum 4 The peak area derived from Q 4 Then, HO-Si(OSi) 3 The peak area derived from Q 3 When 4 / Q 3 is 2.0 to 3.9. 4 / Q 3 is preferably 2.2 to 2.6.

[0021] Such silicon element (Si) and oxygen element (O) are contained, and Q 4 / Q 3 The silicate-based base material having a refractive index of 2.0 to 3.9 can be produced by the following method. This Q 4 / Q 3 The silicate-based base material having a β-dispersion constant of 2.0 to 3.9 can be obtained as a particulate matter (soot body or by-product) generated in a conventionally known method for producing silica glass by a soot method (for example, a method for producing silica glass by VAD (Vapor phase Axial Deposition)). For example, when silica glass is produced as porous synthetic quartz glass (soot body) by hydrolyzing silicon tetrachloride as a raw material in an oxygen-hydrogen flame, particles that do not become porous synthetic quartz glass after the hydrolysis reaction in the oxygen-hydrogen flame and are detached from the flame can become the silicate-based substrate. The silicate-based substrate can be obtained by adjusting the manufacturing conditions. For example, silicon tetrachloride, the raw material, is introduced into the center of an oxygen-hydrogen flame burner, and the flame temperature zone length and the gas balance of oxygen and hydrogen gas are adjusted. Specifically, for example, the flame temperature zone length of 1000°C or higher: 100 mm to 800 mm, the volume ratio of hydrogen to oxygen (H 2 / O 2 ): Adjust nucleation and grain growth within the range of 1.0 to 2.5. When the flame temperature zone length is increased, Q 4 / Q 3 tends to be large, and H 2 / O 2 When Q is increased, 4 / Q 3 tends to be smaller.

[0022] The shape of the silicate-based substrate is not particularly limited and may be, for example, spherical or plate-like, and the size of the silicate-based substrate is also not particularly limited.

[0023] When the produced composite of a crystalline europium compound and a silicate-based substrate is used for bioimaging, from the viewpoint of cytotoxicity, it is preferable that the silicate-based substrate is spherical, has an average particle diameter of 50 nm or more and 470 nm or less, and is amorphous.

[0024] Such a silicate-based base material and europium (III) chloride hexahydrate are mixed so that the europium element (Eu) is 1.0 mol % or more relative to the silicon element (Si) of the silicate-based base material, and are subjected to a solid-phase mechanochemical reaction under a load of 4 N or more and 24 N or less. As long as the silicate-based substrate can be subjected to a solid-phase mechanochemical reaction with europium(III) chloride hexahydrate under a load of 4N to 24N, the method is not particularly limited. For example, a powdered silicate-based substrate and europium(III) chloride are placed in a mortar, and the pestle is rotated while applying a load of 4N to 24N to the pestle to crush the substrate. By carrying out the above operation with the mortar placed on an electronic balance, the load value can be read on the weighing indicator of the electronic balance. Alternatively, europium(III) chloride may be placed on the surface of the plate-shaped silicate-based substrate, and the pestle may be moved while applying a load of 4N to 24N to crush the substrate. In this case, by carrying out the above operation with the plate-shaped silicate-based substrate placed on the electronic balance, the load value can be read on the weighing indicator of the electronic balance. The load may be within the range of 4N to 24N, but the crystallinity can be increased by increasing the load. If no load is applied or if the load is small, the crystal of the europium compound of the present invention cannot be obtained.

[0025] The ratio of the silicate-based base material to europium chloride hexahydrate must be such that the ratio of the number of moles of europium (Eu) to the total number of moles of silicon (Si) and europium (Eu) in the silicate-based base material (number of moles of Eu / (number of moles of Si+number of moles of Eu)) is 1.0 mol % or more, and it is preferable that the ratio of the number of moles of europium (Eu) to the total number of moles of silicon (Si) and europium (Eu) is 1.0 mol % or more and 7.0 mol % or less.

[0026] Conventionally, it has been difficult to produce different europium compounds. However, according to the production method of the present invention, it is possible to produce different compounds represented by chemical formulas (1) to (4) by changing the amount of Eu in the solid-phase mechanochemical reaction. Specifically, when the concentration of europium during the solid-phase mechanochemical reaction is low (when there is little OH during the reaction), the compounds represented by chemical formulas (1) and (2) coexist, and when a multilayer structure begins to form with an increase in the concentration of europium during the reaction, the compound represented by chemical formula (1) and the compound represented by chemical formula (2) tend to interact with each other and change to compounds represented by chemical formulas (3) and (4). Therefore, depending on the amount of Eu in the solid-phase mechanochemical reaction, the compounds represented by chemical formulas (1) to (4) can be produced separately. The compound represented by chemical formula (3) tends to be produced via the compound represented by chemical formula (4).

[0027] After the solid-phase mechanochemical reaction, the product is calcined and, if necessary, washed with an organic solvent or water.

[0028] By such a manufacturing method, the crystal of the europium compound of the present invention is formed on the surface of the silicate-based substrate. For example, when a spherical silicate-based substrate is used, a composite is formed in which at least a part of the surface of the spherical silicate-based substrate is coated with a crystal of the europium compound. As an example, a schematic cross section of a composite in which the entire surface of a spherical silicate-based substrate 1 is coated with a crystal of the europium compound 2 is shown in FIG. In addition, when a plate-shaped silicate-based substrate is used, a composite is formed in which at least a part of the surface of the plate-shaped silicate-based substrate is coated with a crystal of the europium compound. It is presumed that the crystals of the europium compound are firmly bonded to the silicate-based substrate through some kind of chemical bond, such as a coordinate bond between oxygen atoms present on the surface of the silicate-based substrate and europium atoms contained in the europium compound.

[0029] <Uses of europium compound crystals> The europium compound crystal of the present invention has low cytotoxicity and functions as a luminescent substance, and therefore can be preferably used in bioimaging technology. For example, the europium compound crystal of the present invention can be used in bioimaging technology as a composite of the europium compound crystal and the spherical silicate-based substrate used in producing the europium compound crystal (hereinafter also referred to as "luminescent nanoparticles").

[0030] The luminescent nanoparticles used in bioimaging technology preferably have a hydroxyl group (OH group) on the surface. It is also preferable that the surface of the luminescent nanoparticles is modified with an amino group, and may be formed, for example, by using a silane coupling agent containing an amino group. When the silicate-based base material has pores, the OH group and the amino group may be on the inner surface of the pores, but are preferably on the outer surface of the pores. When the OH group or the amino group is fixed to the cell-binding molecule by a covalent bond through hydrogen bonding or condensation polymerization, and the surface of the luminescent nanoparticle is modified with the cell-binding molecule, the cell-binding molecule can specifically bind to cancer cells or normal cells. When the cell-binding molecule specifically binds to the cell, the luminescent nanoparticles are taken up into the cell. This makes it possible to cause the luminescent nanoparticles in the cell to emit light and detect cancer cells, etc.

[0031] Examples of cell-binding molecules include HER2 antibodies, antibodies that specifically bind to human epidermal growth factor receptors, cancer-specific antibodies, phosphorylated protein antibodies, folic acid, antibodies that specifically bind to folate receptor β, vascular endothelial cell-specific antibodies, tissue-specific antibodies, transferrin, transferrin-binding peptides, and proteins that have binding properties to sugar chains. Among these, it is preferable to use folic acid, which tends to be taken up by cancer cells, as the cell-binding molecule. This is because cancer cells tend to specifically bind and take up folic acid molecules due to the overexpression of folic acid receptors on the cell membrane.

[0032] The surface of the luminescent nanoparticles may be modified with anticancer drug molecules. When the anticancer drug molecules specifically bind to the cancer cells, the luminescent nanoparticles are taken into the cells. This allows the luminescent nanoparticles in the cells to emit light, making it possible to detect the cancer cells, and the anticancer drug molecules are also taken into the cancer cells, allowing the anticancer drug to act and suppress the proliferation of the cancer cells.

[0033] The cell-binding molecules and anticancer drug molecules are preferably modified and fixed to the surface of the luminescent nanoparticles by chemical bonds, such as peptide bonds (-CO-NH-) and hydrogen bonds.

[0034] For example, cells can be detected by introducing luminescent nanoparticles into the cells, irradiating the luminescent nanoparticles with light, and observing the cells. The luminescent nanoparticles can also be administered to a non-human animal and irradiated with light to treat the non-human animal. The medical device may also be provided with an examination section for examining the cells in the body, a diagnosis section for diagnosing the cells in the body, and / or a treatment section for treating the cells in the body, and further includes a light irradiation section for injecting light-emitting nanoparticles into the cells in the body and irradiating the light-emitting nanoparticles with light when performing the examination, diagnosis, and / or treatment. An example of the examination section for examining the cells in the body is a fluorescent endoscope for performing precision image diagnosis. An example of the diagnosis section for diagnosing the cells in the body is a device for performing tissue biopsy. An example of the treatment section for treating the cells in the body is a tumor removal device using an endoscope. Examples of the cells in the body include cancer cells related to oral cancer, pharyngeal cancer, esophageal cancer, colon cancer, small intestine cancer, lung cancer, breast cancer, and bladder cancer.

[0035] Furthermore, the europium compound crystals of the present invention can be used for purposes other than bioimaging, and are expected to be used in light-emitting devices such as light-emitting diodes. EXAMPLES

[0036] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0037] (Production of silicate-based substrate 1) Silicon tetrachloride was used as a raw material and was fully hydrolyzed in an oxygen-hydrogen flame to produce silica glass as porous synthetic quartz glass (soot body). In this case, after the hydrolysis reaction in the oxygen-hydrogen flame, the particles that were detached from the flame and did not become porous synthetic quartz glass were used as silicate-based substrate 1. Silicon tetrachloride was introduced from the center of the oxygen-hydrogen flame burner, the flame temperature zone length of 1000°C or higher was 400 mm, and the volume ratio of hydrogen to oxygen (H 2 / O 2 ) ratio was set to 1.5.

[0038] (Silicate-based solid 29 Q in Si-NMR spectrum 4 / Q 3 ) The obtained silicate-based substrate 1 was subjected to solidification under the following conditions. 29 The Si-NMR spectrum was measured, and the results are shown in Figure 2. <Measurement conditions> Device name: Bruker Advance 300wbs spectrometer (manufactured by BRUKER) Measurement method: DD (Dipolar Decoupling) method Sample tube: 7mm Sample rotation speed: 5000 rpm Resonance frequency: 59.62MHz Pulse width: 4.5msec. Waiting time: 60sec Accumulation times: 1000 times Standard sample: Hexamethylcyclotrisiloxane (-9.55 ppm) <Peak separation method> (How to create a baseline) Procedure (1): Calculate the average value 1 of the intensity in the range of -70 to -79 ppm and the average value 2 of the intensity in the range of -131 to -140 ppm. Procedure (2): Define the line that passes through the two points (-70 ppm, average value 1) and (-140 ppm, average value 2) as the baseline. Step (3): Remove the baseline value from the spectrum (Peak separation method) Separation method: Solver function in Microsoft Office 2016 Excel (registered trademark) Function used: Gaussian function (wherein A is the peak height, B is the peak position, and C is the half width).

number

[0039] From FIG. 2, for the silicate-based substrate 1, the obtained spectrum was defined as raw data, which was then subjected to spectral separation as described above. 29 Si(OSi) in Si-NMR spectrum 4 The peak area derived from Q 4 Then, HO-Si(OSi) 3 The peak area derived from Q 3 When 4 / Q 3 The result was 2.4. 2 (HO) 2 -Si (OSi) 2 This peak originates from

[0040] <Measurement of powder X-ray diffraction patterns of silicate-based substrates> For the silicate-based base material 1, a powder X-ray diffraction (XRD) pattern was measured. Measurements were performed using a horizontal sample X-ray diffractometer (XRD, Rigaku Corporation, Smart Lab) under the following conditions: X-ray source: CuKα source (λ: 1.5418 Å), output: 40 kV / 30 mA, scan speed: 3.0° / min, sampling width: 0.01°, measurement mode: continuous. The results are shown in Figure 3. As a result, the silicate-based substrate 1 had a large half-width of 6.7° in the amorphous halo pattern observed near 2θ=20°, and no peak derived from crystals was observed, indicating that the substrate was amorphous.

[0041] (Measurement of the average particle size of silicate-based substrates) The silicate-based base material 1 (particle powder) was fixed to a sample stage for observation with carbon paste and then dried. Next, the particles were observed using a field emission scanning electron microscope (FE-SEM) (Hitachi High-Technologies Corporation, SU8230), and the particle diameters of 100 or more particles were measured to calculate the average particle diameter. Specifically, the major axis and minor axis of each of 300 particles were measured, and the particle diameter of each particle was determined as (major axis + minor axis) / 2. The average particle diameter of each particle (the total value of the particle diameters of each particle divided by the number (300)) was determined as the average particle diameter (Ave.), and the coefficient of variation (Cv.) was calculated. The results are shown in FIG. 4. As a result, the average particle size of the silicate-based substrate 1 was 151 nm, and the coefficient of variation was 45%.

[0042] Example 1 5 is a schematic side view illustrating a manufacturing apparatus used in the manufacturing method of Example 1. As shown in FIG. 5, in an agate mortar 11 having a hemispherical concave space (diameter 65 mm, depth 30 mm), the silicate-based base material and europium (III) chloride hexahydrate were pulverized with a pestle 12 having a length of 80 mm and a hemispherical convex portion (tip diameter 20 mm, height 5 mm) under a load of 4 N to cause a solid-phase mechanochemical reaction. Specifically, europium chloride hexahydrate (EuCl ) was added to 0.4 g (6.66 mmol) of the silicate-based base material 1 dried at 120° C. for 24 hours in the mortar 11. 3 6H 2 O (Wako Pure Chemical Industries, Ltd., special grade reagent, purity 99.9 wt%) was added so that the ratio of the number of moles of Eu to the total number of moles of Si and Eu (number of moles of Eu / (number of moles of Si+number of moles of Eu)) was 5.0 mol %. Then, the pestle 12 was made to revolve around a circumference of a radius of 25 mm in the concave space in the mortar 11 for 5 minutes without rotating the pestle 12. The revolution of the pestle 12 was set to 120 revolutions / min, and a load of 4 N was applied to the pestle 12. The above operation was performed with the mortar 11 placed on the electronic balance 13, and the load value was read on the weighing display 14 of the electronic balance 13. The obtained powder was dried at 120° C. for 2 hours and calcined at 550° C. for 6 hours. Thereafter, the powder was washed with 40 mL of ethanol and subjected to solid-liquid separation by centrifugation, and the solid phase was dried at 120° C. for 2 hours to obtain particles (spherical powder) of Example 1.

[0043] Example 2 Particles of Example 2 were obtained by carrying out the same operation as in Example 1, except that europium chloride hexahydrate was added so that the ratio of the number of moles of Eu to the total number of moles of Si and Eu was 2.5 mol %.

[0044] Example 3 Particles of Example 3 were obtained by carrying out the same operation as in Example 1, except that europium chloride hexahydrate was added so that the ratio of the number of moles of Eu to the total number of moles of Si and Eu was 1.25 mol %.

[0045] Comparative Example 1 Particles of Comparative Example 1 were obtained by carrying out the same operation as in Example 1, except that europium chloride hexahydrate was added so that the ratio of the number of moles of Eu to the total number of moles of Si and Eu was 0.625 mol %.

[0046] Comparative Example 2 Europium chloride hexahydrate was used as the particles in Comparative Example 2.

[0047] <Powder X-ray diffraction (XRD)> For the particles of Examples 1 to 3 and Comparative Examples 1 and 2, powder X-ray diffraction (XRD) patterns were measured under the following conditions. A horizontal sample X-ray diffractometer (XRD, Rigaku Corporation, Smart Lab) was used for the measurements under the following conditions: X-ray source: CuKα source (λ: 1.5418 Å), output: 40 kV / 30 mA, scan speed: 3.0° / min, sampling width: 0.01°, measurement mode: continuous. The diffraction peak positions, diffraction angles, and half-widths were obtained using the software (Rigaku Corporation, software name: PDXL) that came with the device. The diffraction peaks were subjected to automatic profile processing by PDXL, with background removal and Kα 2 The diffraction peaks were detected by removing lines, smoothing, and fitting with a B-spline function (divided pseudo-Voigt function). The threshold (standard deviation cutoff value) for detecting the diffraction peaks was set to 3.0. This threshold means that if the intensity of a diffraction peak is 3.0 times the error or less, the diffraction peak is not considered to be a diffraction peak. The three points with the highest diffraction peak intensity (height of the diffraction peak) were selected in order and used to identify the crystals. Moreover, the crystallinity was calculated according to the above formula (5). The results are shown in Table 1 and FIG. 6. In Table 1, "m±n" indicating the diffraction angle 2θ at which each diffraction peak is located in the upper row indicates that the peak top position (diffraction peak top position) of the diffraction peak is m (°), the start point of the diffraction peak is mn (°), and the end point of the diffraction peak is m+n (°). Specifically, the diffraction peak top was defined as the maximum intensity (maximum height) between the start point and the end point of each diffraction peak by drawing a baseline from the start point to the end point. The position of the diffraction peak top (diffraction angle) was taken as the diffraction peak top position. In addition, in Table 1, the parentheses in the lower row indicate the half width of each diffraction peak. The half width indicates the width between the diffraction peak positions at which the intensity (height) is 50% of the diffraction peak top within the range of "mn"° to "m+n"°.

[0048] As shown in Table 1 and Figure 6, in the powder X-ray diffraction patterns of Examples 2 and 3, the diffraction peak (first diffraction peak) was in the range of diffraction angles (2θ) of 34.3 to 36.1°, the half-width of the diffraction peak in the range of diffraction angles (2θ) of 34.3 to 36.1° was 1.8° or less, and the crystals of the compound represented by chemical formula (1) or (2) were contained. Note that x in chemical formula (1) was 0.2 or more and 0.6 or less. In addition, each of Examples 2 and 3 had diffraction peaks in the diffraction angle (2θ) range of 25.9 to 26.5° and in the diffraction angle (2θ) range of 31.6 to 32.2°, and the half-widths of the diffraction peaks in the diffraction angle (2θ) range of 25.9 to 26.5° and in the diffraction angle (2θ) range of 31.6 to 32.2° were both 0.6° or less.

[0049] Moreover, in the powder X-ray diffraction pattern, Example 1 had diffraction peaks (second diffraction peak, third diffraction peak) in the diffraction angle (2θ) range of 28.6 to 29.6° and in the diffraction angle (2θ) range of 36.8 to 38.4°, the half-width of the diffraction peak in the diffraction angle (2θ) range of 28.6 to 29.6° was 1.0° or less, and the half-width of the diffraction peak in the diffraction angle (2θ) range of 36.8 to 38.4° was 1.6° or less, and the compound contained a crystalline form represented by chemical formula (3) or (4). Moreover, Example 1 had a diffraction peak in the diffraction angle (2θ) range of 39.0 to 40.2°, and the half-width of the diffraction peak in the diffraction angle (2θ) range of 39.0 to 40.2° was 1.2° or less. Furthermore, as shown in Table 1 and FIG. 6, the particles obtained in Examples 1 to 3 had a crystallinity of more than 0, and crystals of the europium compound were formed on the surface, whereas the particles in Comparative Examples 1 and 2 were amorphous.

[0050] [Table 1]

[0051] <Light Emitting Characteristics> For the particles of Examples 1 to 3, the excitation spectrum and fluorescence spectrum were measured under the following conditions. Excitation spectrum The excitation spectrum was obtained by fixing the detection wavelength (615 nm) with a spectrophotometer (PL, JASCO Co., Ltd., FP-8500). The measurement conditions were as follows: atmosphere: air, excitation / detection slit size: 2.5 nm / 2.5 nm, step width: 1.0 nm, sample weight: 20 mg, shape: pellet. Fluorescence spectrum Using a spectrophotometer (PL, JASCO, FP-8500), the sample was irradiated with excitation light from a Xe lamp (excitation wavelength: 395 nm) at room temperature to obtain a PL spectrum (fluorescence spectrum). The measurement conditions were as follows: atmosphere: air, excitation / detection slit size: 2.5 nm / 2.5 nm, step width: 1.0 nm, sample weight: 20 mg, shape: pellet.

[0052] As shown in FIG. 7, in all of Examples 1 to 3, the excitation peak ( 7 F 0 → 5 D 4 transition, 7 F 0 → 5 G 4 transition, 7 F 0 → 5 L 6 transition, 7 F0 → 5 D 2 transition, 7 F 0 → 5 D 1 transition) and emission peak ( 5 D 0 → 7 F 1 transition, 5 D 0 → 7 F 2 transition, 5 D 0 → 7 F 3 transition, 5 D 0 → 7 F 4 transition) was observed. In addition, for each of the particles of Examples 1 to 3, from FIG. ex = 395 nm, emission wavelength λ em The internal quantum yield at 615 nm was found to be 1.0 to 4.0%.

[0053] Example 4 The same procedure as in Example 1 was carried out except that the load was set to 8.0 N, to obtain particles of Example 4.

[0054] Example 5 The same procedure as in Example 1 was carried out except that the load was set to 12.0 N, to obtain particles of Example 5.

[0055] For the particles of Examples 4 and 5, the results of powder X-ray diffraction (XRD) similar to that described above are shown in Table 2 and FIG. . As shown in Table 2 and FIG. 8, each of Examples 4 and 5 had diffraction peaks (second diffraction peak, third diffraction peak) in the diffraction angle (2θ) range of 28.6 to 29.6° and the diffraction angle (2θ) range of 36.8 to 38.4°, the half-width of the diffraction peak in the diffraction angle (2θ) range of 28.6 to 29.6° was 1.0° or less, and the half-width of the diffraction peak in the diffraction angle (2θ) range of 36.8 to 38.4° was 1.6° or less, and contained a crystalline form of the compound represented by chemical formula (3) or (4). Moreover, each of Examples 4 and 5 had a diffraction peak in the diffraction angle (2θ) range of 39.0 to 40.2°, and the half-width of the diffraction peak in the diffraction angle (2θ) range of 39.0 to 40.2° was 1.2° or less. Furthermore, as shown in Table 2 and FIG. 8, the particles obtained in Examples 4 and 5 all had a degree of crystallinity of more than 0, and crystals of the europium compound were formed on the surface. Furthermore, as shown in Table 2 and FIG. 8, it is understood that the crystallinity can be improved by increasing the load.

[0056] [Table 2]

[0057] Using the particles of Examples 1 to 3 or Comparative Examples 1 and 2, toxicity evaluation was carried out by cancer cell imaging and fluorescence intensity measurement according to the following method. (Modification of particles with cancer cell-binding molecules (folic acid derivative FA-NHS)) 12 mL of an aqueous HCl solution (pH=2) was added to 250 mg of the particles of Examples 1 to 3 or Comparative Examples 1 to 2, and ultrasonic treatment was performed. Next, a solution containing 0.78 mL (3.3 mmol) of 3-aminopropyltriethoxysilane (APTES) in 5 mL of ethanol was prepared, and added to the ultrasonically treated solution to obtain a mixed solution. The mixed solution was stirred at 40° C. for 20 hours (pH<6.5). After stirring, the mixed solution was centrifuged and washed with ethanol. After washing, it was dried under reduced pressure to obtain 150 mg of particles whose surfaces were modified with APTES. 25 mL of a 50 mM phosphate buffer (pH=7.0) was added to 150 mg of the particles whose surfaces were modified with APTES, and ultrasonic treatment was performed. Next, a solution containing 430 mg (0.8 mmol) of FA-NHS (folic acid derivative) in 12 mL of dimethyl sulfoxide (DMSO) was prepared, and added to the ultrasonically treated solution to obtain a mixed solution. The mixed solution was stirred at room temperature for 3 hours. After stirring, the mixed solution was centrifuged and washed with water, and then dried under reduced pressure to obtain FA (folic acid)-modified particles of Examples 1 to 3 or Comparative Examples 1 to 2.

[0058] (Cell Culture) HeLa cancer cells were cultured in a PS flask (seeding concentration: 100 × 10 4 cells / 37cm 2 The thawing and seeding were carried out for 7 days. The cells were detached and separated. The concentration of Hela was (0.99±0.07)×10 5 cells / mL. The cell concentration was adjusted and cultured in DMEM (Dulbecco's modified medium) with 10 vol% FBS (fetal bovine serum). 4 It was cells. Polystyrene dish (TCPS) (culture area: 9.6 cm 2 ) at 2.25 mL / TCPS, with a seeding concentration of 1.8 × 10 4 cells / cm 2 (Microscopic observation). Then, the cells were cultured (temperature: 37°C, CO 2 Concentration: 5%, humidity 100%). After 12 hours, the FA (folic acid) modified particles of Examples 1 to 3 or Comparative Examples 1 to 2 were added to 10 vol % DMEM, dispersed, and adjusted to a concentration of 100 mg / mL.

[0059] (Measurement of cell density) After culturing the above cells, the polystyrene dish (TCPS) containing the cells was washed twice with 1 ml of phosphate-buffered saline (PBS) to remove FA (folic acid)-modified particles that had not been taken up by the cells. 0.1 ml of 0.05% Trypsin-EDTA was then added to the TCPS containing the cells, and the cells were incubated in CO 2The cells were allowed to stand in an incubator for 12 minutes to detach from the TCPS. After confirming detachment, the suspension containing the cells was placed in a 50 ml conical tube and centrifuged (2000 rpm, 2 min). After centrifugation, the supernatant was discarded, 7 ml of medium was added to the tube, and the tube was mixed by inversion about 10 times, followed by centrifugation (2000 rpm, 2 min). After that, the supernatant was discarded, 20 ml of medium was added to the tube, and 1 ml was dispensed into a 15 ml tube by pipetting about 20 times. Outside the clean bench, the cell suspension was placed in a disposable hemocytometer using a micropipette, the cell count was confirmed under a microscope, and the average value (cell / cm) was calculated. 2 ) was calculated. FIG. 9 shows the results of calculating the average cell density 3 hours, 12 hours, 24 hours, 36 hours, and 48 hours after spraying the FA (folic acid) modified particles onto the cell surface.

[0060] 9, in Examples 1 to 3 in which crystals of the europium compound were formed on the surface, normal cell proliferation behavior was observed, and it was confirmed that there was no cytotoxicity. In other words, it can be said that there is no cytotoxicity when the crystals are composited to a spherical silicate-based base material. In contrast, in Comparative Example 2, normal cell proliferation behavior was not observed, and the amorphous EuCl 3 6H 2 Since O alone is an unstable chloride, it is considered that it dissolved into the cell culture medium and became Eu ions or Eu chloride ions, which reacted directly with the cells. Similarly, when the amorphous particles of Comparative Example 1 were used, it is considered that it dissolved into the cell culture medium and became Eu ions or Eu chloride ions, which reacted directly with the cells. Therefore, it can be said that in the case of the amorphous body, there is cytotoxicity due to dissolution.

[0061] From the above, it is expected that when the crystalline europium compound of the present invention is complexed with a spherical silicate-based substrate, cells will grow well and the compound will be suitable for bioimaging in which the compound is taken up by cells and visualized. [Explanation of symbols]

[0062] 1. Silicate-based substrate (spherical) 2. Crystals of europium compounds

Claims

1. A crystal of a europium compound containing europium, In a powder X-ray diffraction pattern, there is a first diffraction peak in a diffraction angle (2θ) range of 34.3 to 36.1°, and the half width of the first diffraction peak is 1.8° or less, and / or there is a second diffraction peak in a diffraction angle (2θ) range of 28.6 to 29.6° and a third diffraction peak in a diffraction angle (2θ) range of 36.8 to 38.4°, and the half width of the second diffraction peak is 1.0° or less and the half width of the third diffraction peak is 1.6° or less, A crystalline europium compound, which is at least one compound selected from the compounds represented by the following chemical formulas (1) to (4). EuCl x ・・・(1) Eu(OH) 2 ・・・(2) Eu(OH) 2 Cl・・・(3) EuOCl...(4) (In formula (1), x is 0.05 or more and 5 or less.)

2. A method for producing a crystalline form of the europium compound according to claim 1, comprising the steps of: The method includes a step of mixing a silicate-based substrate with europium (III) chloride hexahydrate and subjecting the mixture to a solid-phase mechanochemical reaction, The silicate-based substrate contains silicon (Si) and oxygen (O) and is a solid 29 In the Si-NMR spectrum, Si(OSi) 4 The peak area derived from 4 and HO-Si(OSi) 3 The peak area derived from 3 When 4 / Q 3 is 2.0 to 3.9, The solid-phase mechanochemical reaction is carried out by adding europium(III) chloride hexahydrate so that the ratio of the number of moles of europium element to the total number of moles of silicon element and europium element in the silicate-based substrate is 1.0 mol % or more, and the reaction is carried out under a load of 4 N or more and 24 N or less.

Citation Information

Patent Citations

  • Process for producing granular rare earth chloride crystals by using rare earth chloride solution

    CN103172102A

  • EuCl2 nanocrystals with magnetic / fluorescent dual functions and EuCl2 nanocrystals with superlattice structure

    CN107311217A

  • Extraction of rare earth metallic compound

    JP1999071111A

  • Manufacturing of synthetic silica glass

    JP2013521208A

  • Light-emitting nanoparticles, cell detection method using the same, animal treatment method, medical device, cell visualization method, and method for reducing injury to cell

    JP2017179003A