Ultra-lightweight heat-insulating melt-blown nonwoven fabric and its manufacturing method

The propylene polymerization-based method addresses non-uniform airgel dispersion and detachment issues by uniformly integrating airgel within polypropylene nonwoven fabrics, resulting in lightweight, heat-insulating materials with enhanced durability and safety.

JP7554474B2Active Publication Date: 2024-09-20HONG WARM FIBERS TECH BEIJING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020560410
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-04-24
Filing Date
2019-04-11
Publication Date
2024-09-20
Estimated Expiration
2039-04-11

AI Technical Summary

Technical Problem

Existing methods for preparing airgel-modified nonwoven fabrics face issues with non-uniform dispersion of airgel particles, which are not adjustable in size and tend to easily detach during use, leading to reduced mechanical performance and environmental contamination.

Method used

A method involving propylene polymerization processes, such as gas, slurry, or liquid phase, to uniformly disperse airgel particles within polypropylene by adjusting particle size, porosity, and bulk density, ensuring airgel is uniformly integrated within the fabric without detachment.

Benefits of technology

The method achieves ultra-lightweight, heat-insulating nonwoven fabrics with uniform airgel dispersion and improved mechanical stability, enhancing service life and user safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides an aerogel-modified polypropylene, a method for preparing the same, and an ultra-lightweight, heat-insulating, and warm-retaining melt-blown nonwoven fabric containing the aerogel-modified polypropylene and a method for producing the same, which comprises adding aerogel to low-viscosity reactants before or during polymerization to achieve uniform dispersion of the aerogel, where the reactants include propylene monomer, a catalyst, and an auxiliary agent, and the aerogel has a particle size of 20 nm to 100 μm, a porosity of 40% to 99.9%, a bulk density of 3 to 500 g / L, and a volume fraction of 20% to 60% of the volume of the ultra-lightweight, heat-insulating, and warm-retaining melt-blown nonwoven fabric prepared from the aerogel-modified polypropylene. This method allows the preparation of aerogel-modified polypropylene particles with uniformly dispersed aerogel and good melt-blown properties, and also allows the preparation of melt-blown polypropylene nonwoven fabrics with ultra-lightweight thermal insulation and heat retention properties, and the aerogel does not easily fall off during use of the nonwoven fabric.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of nonwoven materials, in particular , super The present invention relates to a lightweight, heat-insulating, and heat-retaining melt-blown nonwoven fabric and a method for producing the same. [Background technology]

[0002] Nonwoven fabrics are fabrics formed without the need for spinning or weaving, but are made by simply arranging textile staple fibers or filaments in an oriented or random manner to form a web structure, which is then reinforced mechanically, thermally, chemically, or otherwise.

[0003] At present, there are various processes for preparing nonwoven fabrics. For example, in the paper "Study on the Preparation and Performance of Silica Aerogel / Polypropylene Melt-Blown Nonwoven Fabric Material", a method of preparing aerogel-modified polypropylene melt-blown nonwoven fabric by melt-mixing polypropylene and aerogel was proposed. In CN 104446333 A, PP (polypropylene) fiber was silanized with APTES (3-aminopropyltriethoxysilane) and then immersed in TEOS (tetraethoxysilane) solution to produce a nonwoven fabric with a thin layer of SiO2 aerogel through hydrolysis and co-crosslinking gel reaction. Then, immersion, co-hydrolysis, and co-crosslinking gel reaction were alternately repeated multiple times, and then dried to obtain PP fiber-reinforced SiO2 gel material. CN 106838547 A discloses a non-shedding nanovoid-containing thermal insulation felt (plate) and its manufacturing method, which involves using ordinary needle punching or carding technology to manufacture a fiber substrate for felt in a sheet or roll shape from fibers, then dipping or spraying a binder onto the fiber surface of the substrate, and finally spraying ground nanovoid insulation onto the fibers to obtain a thermal felt (plate) with nanovoid material bonded thereto.

[0004] However, all of the above methods have some technical problems. For example, in the paper "Study on the Preparation and Performance of Silica Aerogel / Polypropylene Melt-Blown Nonwoven Fabric Materials," aerogel-modified PP melt-blown nonwoven fabrics were prepared by melt mixing. However, due to the large difference in bulk density between PP and aerogel, the aerogel could not be uniformly dispersed in the melt-blown equipment with a limited melting section. particle size It is difficult to obtain adjustable nonwoven fabric. In CN104446333 A, the surface of the PP fiber must be silanized, then immersed in TEOS solution, co-hydrolyzed, and co-crosslinked gelled. This not only makes the process complicated and time-consuming, but also requires chemical modification of the PP fiber, which reduces the mechanical performance of the PP fiber and the mechanical performance of the final product. In addition, the SiO2 xerogel, which is not in direct contact with the surface of the PP fiber, is very easy to fall off during use, shortening the service life of the material, causing deterioration of the usage environment, and harming the health of the user. In CN 106838547 A, a non-shedding thermal insulation felt (plate) is prepared by combining three layers, namely a fiber layer, an adhesive layer, and a nanovoid insulation layer. The process is complicated, and the content of the nanovoid insulation in the thermal insulation felt (plate) and the depth of its penetration into the fiber substrate are greatly affected by the size of the voids between the fibers in the fiber substrate. In addition, the technology adds the nanovoid insulation by a spraying method, and the fiber substrate corresponds to a filtering material, so it is difficult to achieve the effect of blocking the nanovoid insulation only on the outer surface of the substrate and dispersing the nanovoid insulation evenly. During use, foreign matter such as dust easily adheres to the adhesive layer on the thermal insulation felt (plate), affecting the appearance and performance such as breathability. Summary of the Invention

[0005] The present invention aims to overcome the low uniformity of aerogel dispersion that exists in the existing technology of preparing aerogel-modified nonwoven fabrics by the melt-blown method, particle size To solve the problem that the aerogel is easily dropped off during use. Super We provide lightweight, heat-insulating, and thermally-retaining melt-blown nonwoven fabrics and their manufacturing methods.

[0006] In order to achieve the above object, according to one aspect of the present invention, there is provided a method for preparing an aerogel modified polypropylene, which comprises preparing the aerogel modified polypropylene by a propylene polymerization process, in which aerogel is added and mixed with a low viscosity reactant before or during the polymerization reaction to achieve uniform dispersion of the aerogel, where the reactant includes a propylene monomer, a catalyst, and an auxiliary, and the aerogel is formed. particle size The particle size is between 20 nm and 100 μm, the porosity is between 40% and 99.9%, the bulk density is between 3 and 500 g / L, and the volume fraction is between 20% and 60% of the volume of the ultra-lightweight, thermally insulating, and heat-retaining melt-blown nonwoven fabric prepared from aerogel-modified polypropylene.

[0007] Further, the propylene polymerization process is a gas phase propylene polymerization process, a slurry propylene polymerization process or a liquid phase propylene polymerization process.

[0008] Additionally, in the gas phase propylene polymerization process, adding aerogel to mix with the low viscosity reactants includes mixing the aerogel with the propylene monomer, or mixing with the catalyst, or adding it separately to the polymerization reactor and mixing with the reactants, or any combination of the above mixing methods.

[0009] Furthermore, in the slurry propylene polymerization process, adding aerogel and mixing it with the low viscosity reactants includes mixing the aerogel with a slurry liquid consisting of catalyst and hydrocarbon solvent, or mixing it with propylene monomer, or adding it separately to the polymerization reactor and mixing it with the reactants, or any combination of the above mixing methods.

[0010] Furthermore, in the slurry method propylene polymerization process, the obtained polypropylene raw material is deashed, precipitated, and dissolved in a solvent. Random and further comprising separating and kneading the mixture.

[0011] Furthermore, in the liquid phase propylene polymerization process, the aerogel can be added and mixed with the low viscosity reactants, mixed with the propylene monomer, mixed with the catalyst, or added separately to the polymerization reactor and mixed with the reactants, or any combination of the above mixing methods.

[0012] Furthermore, in the liquid phase propylene polymerization process, flash distillation separation is performed. Random Co Removing the polymer.

[0013] According to another aspect of the present invention, there is provided a method for preparing an ultra-lightweight, heat-insulating, and thermally-insulating melt-blown nonwoven fabric, comprising: preparing an aerogel-modified polypropylene by any of the methods described above; and feeding the aerogel-modified polypropylene into a melt-blown device to prepare an ultra-lightweight, heat-insulating, and thermally-insulating melt-blown nonwoven fabric.

[0014] According to yet another aspect of the present invention, there is provided an aerogel-modified polypropylene prepared by any one of the above-mentioned methods for preparing an aerogel-modified polypropylene, wherein the aerogel size in the aerogel-modified polypropylene is 15 nm to 100 μm.

[0015] According to yet another aspect of the present invention, there is provided an ultra-lightweight, heat-insulating, and heat-retaining melt-blown nonwoven fabric prepared by the above-mentioned method for preparing an ultra-lightweight, heat-insulating, and heat-retaining melt-blown nonwoven fabric, in which the size of the aerogel is 15 nm to 10 μm.

[0016] According to the technical solution of the present invention, under the condition that no dispersion aid is added, different particle size By selecting and using aerogels with different porosities, changing the amount of aerogel added, and improving the mixing method, aerogel-modified polypropylene particles in which the aerogel is uniformly dispersed and has good melt-blown performance, and melt-blown polypropylene nonwoven fabric with ultra-lightweight insulation and heat retention functions are prepared. The aerogel in the nonwoven fabric does not easily fall off during use, and has a long service life. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In addition, the embodiments and features in the embodiments of the present application may be combined with each other unless otherwise inconsistent. The present invention will be described in detail below with reference to the following examples.

[0018] In the existing technology, the uniformity of aerogel dispersion is low when preparing aerogel-modified nonwoven fabrics by the melt-blown method, particle size In order to solve the problem that the aerogel is easily dropped off and the temperature is not adjustable, the present invention uses propylene monomer as raw material based on the in-situ polymerization method to adjust the characteristic parameters of a specific aerogel ( particle size The present invention provides a method for preparing modified polypropylene in which the statistical size of aerogel can be adjusted and uniformly dispersed by limiting the porosity, bulk density (3-500g / L) (bulk density: the mass per unit volume in a naturally deposited state, including the pores inside and outside the particles and the voids between the particles), the amount of aerogel added, and the mixing method, and which has good melt-blown performance, and which can obtain an aerogel-modified melt-blown PP (polypropylene) nonwoven fabric having good heat insulation and heat retention function through melt-blown. According to the present invention, problems such as easy aerogel falling off, short service life, deterioration of the usage environment, and harm to the health of users, which exist in the technology for preparing aerogel felt (plate) by the existing fiber filling method, can be effectively avoided.

[0019] According to an exemplary embodiment of the present invention, there is provided a method for preparing an aerogel modified polypropylene, comprising preparing the aerogel modified polypropylene by a propylene polymerization process, in which aerogel is added and mixed with low viscosity reactants prior to or during the polymerization reaction to achieve uniform dispersion of the aerogel, where the reactants include propylene monomer, a catalyst, and an auxiliary agent, and the aerogel is formed. particle sizeThe diameter is between 20 nm and 100 μm, the porosity is between 40% and 99.9%, the bulk density is between 3 and 500 g / L, and the volume fraction is between 100 and 200 μm. It accounts for 20% to 60% of the volume of the nonwoven fabric.

[0020] In the present invention, the catalyst can be Ziegler-Natta catalyst system, metallocene catalyst system, the amount used is 30-0.8 kg.pp / g.cat (0.1-5 ppm), the auxiliary agent can be hydrogen, the amount used is 50-1000 ppm.

[0021] According to the technology of the present invention, different dispersion aids can be obtained without adding any dispersion aids. particle size By selecting and using aerogels with different porosities, changing the amount of aerogel added, and improving the mixing method, it is possible to prepare aerogel-modified polypropylene particles with uniformly dispersed aerogel and good melt-blown performance, and melt-blown polypropylene nonwoven fabric with ultra-lightweight insulation and heat retention properties. In addition, aerogel-modified polypropylene is obtained by in-situ polymerization, and this preparation method allows the powder to be uniformly dispersed, particle size A polymer with adjustable aerogel was obtained, and the aerogel was covered within the polypropylene substrate during processing due to the surface tension and flow shear force of the polypropylene melt. This resulted in the aerogel in the nonwoven fabric not falling off during use and having a long service life.

[0022] According to an exemplary embodiment of the present invention, the propylene polymerization process is a gas phase propylene polymerization process, a slurry propylene polymerization process or a liquid phase propylene polymerization process.

[0023] According to an exemplary embodiment of the present invention, adding aerogel to and mixing with low viscosity reactants in a gas phase propylene polymerization process includes mixing the aerogel with propylene monomer, or mixing with a catalyst, or adding it separately to the polymerization reactor and mixing with the reactants, or any combination of the above mixing methods.

[0024] According to an exemplary embodiment of the present invention, adding aerogel to mix with low viscosity reactants in a slurry propylene polymerization process includes mixing the aerogel with a slurry liquid of catalyst and hydrocarbon solvent, or mixing with propylene monomer, or adding the aerogel separately to a polymerization reactor and mixing with the reactants, or any combination of the above mixing methods.

[0025] Preferably, the slurry method propylene polymerization step comprises deashing, precipitating, and dissolving the resulting polypropylene raw material in a solvent. Random and further comprising separating and kneading the mixture.

[0026] According to an exemplary embodiment of the present invention, adding aerogel to mix with low viscosity reactants in a liquid phase propylene polymerization process includes mixing the aerogel with propylene monomer, or mixing with a catalyst, or adding the aerogel separately to a polymerization reactor and mixing with the reactants, or any combination of the above mixing methods.

[0027] Preferably, in the liquid phase propylene polymerization process, the propylene is separated by flash distillation. Random Copolymer This includes removing

[0028] According to an exemplary embodiment of the present invention, there is provided a method for preparing an ultra-lightweight, heat-insulating, and thermally-insulating melt-blown nonwoven fabric, the method including: preparing an aerogel-modified polypropylene by any of the methods described above; and feeding the aerogel-modified polypropylene into a melt-blown device to prepare an ultra-lightweight, heat-insulating, and thermally-insulating melt-blown nonwoven fabric.

[0029] According to an exemplary embodiment of the present invention, there is provided an aerogel-modified polypropylene, the aerogel-modified polypropylene being prepared by any one of the above-mentioned preparation methods, and the aerogel size in the aerogel-modified polypropylene is 15 nm to 100 μm.

[0030] According to an exemplary embodiment of the present invention, there is provided an ultra-lightweight, heat-insulating, and thermally-insulating melt-blown nonwoven fabric, which is prepared by the above-mentioned preparation method, and the size of the aerogel in the ultra-lightweight, heat-insulating, and thermally-insulating melt-blown nonwoven fabric is 15 nm to 10 μm. The nonwoven fabric has the advantages of being lightweight and having a high heat-insulating effect.

[0031] The beneficial effects of the present invention will be further illustrated by the following examples, and steps or materials not specifically described in the following examples can be realized by technical means commonly used in the art or by conventional materials.

[0032] Example 1 Gas phase method: The aerogel was dehydrated and dried by heating or using a dehydrating agent. The dehydrated aerogel was deoxidized using an inert gas or a deoxidizing agent to obtain a dried and deoxidized aerogel.

[0033] The ultra-high activity catalyst TiCl3 / diisobutyl dimethoxy silane / MgCl2 / Et3Al (mass ratio is 25:55:21:53, TiCl3 is 8 ppm), purified propylene monomer, hydrogen (150 ppm), dehydrated and deoxidized aerogel (2 wt% of propylene) are sequentially charged into the first horizontal stirred-bed reactor, stirring is started, the temperature is raised to 71°C, and the pressure is 2.25 MPa. The obtained polypropylene powder is charged into the second horizontal stirred-bed reactor by the powder conveying fan, and at the same time, purified propylene monomer and hydrogen are added to the second horizontal stirred-bed reactor, stirring is started, the temperature is raised to 71°C, and the pressure is 2.25 MPa. The pressure is 2.25 MPa. After the polymerization reaction, the polypropylene powder is separated from the gas in a bag filter, dried and inactivated in a degassing chamber, and then enters the extrusion granulation system for kneading and granulation.

[0034] According to GB / T 30923-2014 Plastics Polypropylene (PP) Melt Blown Special Material, the above polypropylene test results show that the melt index is 715g / 10min.

[0035] The above polypropylene particles were melt-blown using conventional polypropylene melt-blown equipment with the following process parameters to obtain an aerogel-containing melt-blown polypropylene nonwoven fabric with a thermal conductivity of 0.029W / (m K), in which the aerogel accounts for 56% of the volume fraction of the final ultra-lightweight, heat-insulating, and thermally insulating melt-blown nonwoven fabric. The specific melt-blown parameters were die temperature 245°C, die to catcher distance 0.152m, hot air temperature 145°C, and hot air velocity 500m / s.

[0036] Example 2 Liquid phase method: The aerogel was subjected to a drying deoxidation pretreatment in the same manner as in Example 1.

[0037] 12m 3 3000kg of purified propylene monomer was added to the polymerization kettle, and the dehydrated and deoxidized aerogel was added to the polymerization kettle through the raw material addition port and stirring was started. Then, the catalyst TiCl3 / AlEt2Cl / Lewis base (TiCl3 is 50ppm, the molar ratio of aluminum / titanium is 11, and the molar ratio of Lewis base / titanium is 3) and hydrogen (150ppm) were added, the temperature was raised to 75℃, and the pressure was 3.5MPa to start polymerization. Polymerization was continued until the conversion rate reached 70%-80%, and the reaction was stopped. Unreacted propylene monomer was discharged, and polypropylene was taken into a flash distillation kettle for flash distillation, and then air was passed through it, and it was taken out to obtain polypropylene powder, which was extruded and granulated to obtain polypropylene particles.

[0038] According to GB / T 30923-2014 Plastics Polypropylene (PP) Melt Blown Special Material, the above polypropylene was tested and the melt index was 898g / 10min.

[0039] The above polypropylene particles were melt-blown using conventional polypropylene melt-blown equipment with the following process parameters to obtain an aerogel-containing melt-blown polypropylene nonwoven fabric with a thermal conductivity of 0.031 W / (m K), in which the aerogel accounts for 49% of the volume fraction of the final ultra-lightweight, heat-insulating, and thermally insulating melt-blown nonwoven fabric. The specific melt-blown parameters were die temperature 240°C, die-to-catcher distance 0.152 m, hot air temperature 140°C, and hot air velocity 400 m / s.

[0040] Example 3 Slurry method: The aerogel was subjected to a drying deoxidation pretreatment in the same manner as in Example 1.

[0041] The catalyst TiCl3 / AlEt2Cl / Lewis base (TiCl3 is 50 ppm, the molar ratio of aluminum / titanium is 11, and the molar ratio of Lewis base / titanium is 3) and hydrogen (150 ppm) were added to a prepolymerization reactor and mixed with an inert solvent, hexane, until a slurry liquid was formed. A fixed amount of gaseous purified propylene was added under nitrogen blanket conditions, and polymerization was carried out at a temperature of 10 to 25°C for 1 to 2 hours to obtain a prepolymerized catalyst.

[0042] The prepolymerized catalyst and dehydrated and deoxidized aerogel are added to the liquid purified propylene, and stirring is started. The temperature is raised to 70℃, and the pressure is 1.0MPa to start polymerization. Polymerization is continued until the conversion rate reaches 70%-80%, and the reaction is stopped. Unreacted propylene monomer is discharged, and the polypropylene is taken into a flash distillation pot for flash distillation, after which air is passed through, washed, centrifuged, dried, and taken out to obtain polypropylene powder, which is then extruded and granulated to obtain polypropylene particles.

[0043] Using the polypropylene (PP) meltblown materials specified in GB / T 30923-2014 Plastics, the above polypropylene was tested and found to have a melt index of 912g / 10min.

[0044] The above polypropylene particles were melt-blown using conventional polypropylene melt-blown equipment with the following process parameters to obtain an aerogel-containing melt-blown polypropylene nonwoven fabric with a thermal conductivity of 0.035W / (m K), in which the aerogel accounts for 40% of the volume fraction of the final ultra-lightweight, heat-insulating, and thermally insulating melt-blown nonwoven fabric. The specific melt-blown parameters were die temperature 240°C, die to catcher distance 0.152m, hot air temperature 140°C, and hot air velocity 400m / s.

[0045] Example 4 Slurry method: The aerogel was subjected to a drying deoxidation pretreatment in the same manner as in Example 1.

[0046] The dehydrated and deoxidized aerogel, the catalyst TiCl3 / AlEt2Cl / Lewis base (TiCl3 is 50 ppm, the molar ratio of aluminum / titanium is 11, and the molar ratio of Lewis base / titanium is 3), and hydrogen (150 ppm) were added to a prepolymerization reactor and mixed with an inert solvent, hexane, until a slurry liquid was formed. A fixed amount of gaseous purified propylene was added under nitrogen blanket conditions, and the mixture was polymerized at a temperature of 10 to 25°C for 1 to 2 hours to obtain a prepolymerized catalyst.

[0047] The catalyst is added to the liquid purified propylene, stirring is started, the temperature is raised to 70℃, the pressure is 1.0MPa, and polymerization is started. Polymerization is continued until the conversion rate reaches 70%-80%, and the reaction is stopped. Unreacted propylene monomer is discharged, and the polypropylene is taken into a flash distillation pot for flash distillation, followed by passing air through it, washing, centrifuging, drying, and taking out to obtain polypropylene powder, which is then extruded and granulated to obtain polypropylene particles.

[0048] Using the GB / T 30923-2014 special material for polypropylene (PP) melt-blown in plastics, the above polypropylene was tested and the melt index was 804g / 10min.

[0049] The above polypropylene particles were melt-blown using conventional polypropylene melt-blown equipment with the following process parameters: aerogel-containing melt-blown polypropylene nonwoven fabric with a thermal conductivity of 0.030W / (m K), and the aerogel accounted for 52% of the volume fraction of the final ultra-lightweight, heat-insulating, and thermally insulating melt-blown nonwoven fabric. The specific melt-blown parameters were die temperature 245°C, die-to-catcher distance 0.152m, hot air temperature 145°C, and hot air velocity 500m / s.

[0050] Example 5: Gas phase method: The aerogel was dehydrated and dried by heating or using a dehydrating agent. The dehydrated aerogel was deoxidized using an inert gas or a deoxidizing agent to obtain a dried and deoxidized aerogel.

[0051] The ultra-high activity catalyst TiCl3 / diisobutyl dimethoxy silane / MgCl2 / Et3Al (mass ratio is 25:55:21:53, TiCl3 is 8 ppm), purified propylene monomer and hydrogen (150 ppm) are sequentially charged into the first horizontal stirred-bed reactor, stirring is started, the temperature is increased to 71 °C, and the pressure is 2.25 MPa. The obtained polypropylene powder is charged into the second horizontal stirred-bed reactor by the powder conveying fan, and simultaneously the dehydrated and deoxidized aerogel (0.8 wt% of the propylene in the first horizontal stirred-bed reactor), purified propylene monomer and hydrogen are charged into the second horizontal stirred-bed reactor. Then, the temperature is increased to 71℃ and the pressure is 2.25MPa. After the polymerization reaction, the polypropylene powder is separated from the gas in a bag filter, dried and inactivated in a degassing chamber, and then mixed and granulated in an extrusion granulation system.

[0052] Using the GB / T 30923-2014 Plastics Polypropylene (PP) Melt Blown Special Material, the above polypropylene was tested and the melt index was 1206g / 10min.

[0053] The above polypropylene particles were melt-blown using conventional polypropylene melt-blown equipment with the following process parameters to obtain an aerogel-containing melt-blown polypropylene nonwoven fabric with a thermal conductivity of 0.058W / (m K), in which the aerogel accounts for 23% of the volume fraction of the final ultra-lightweight, heat-insulating, and thermally insulating melt-blown nonwoven fabric. The specific melt-blown parameters were die temperature 245°C, die-to-catcher distance 0.152m, hot air temperature 145°C, and hot air velocity 500m / s.

[0054] Comparative Example 1: Slurry method: The aerogel was subjected to a drying deoxidation pretreatment in the same manner as in Example 1.

[0055] The catalyst TiCl3 / AlEt2Cl / Lewis base (TiCl3 is 50 ppm, the molar ratio of aluminum / titanium is 11, and the molar ratio of Lewis base / titanium is 3) and hydrogen (150 ppm) were added to a prepolymerization reactor and mixed with an inert solvent, hexane, until a slurry liquid was formed. A fixed amount of gaseous purified propylene was added under nitrogen blanket conditions, and polymerization was carried out at a temperature of 10 to 25°C for 1 to 2 hours to obtain a prepolymerized catalyst.

[0056] The prepolymerized catalyst and dehydrated and deoxidized aerogel are added to the liquid purified propylene, and stirring is started. The temperature is raised to 70℃, and the pressure is 1.0MPa, and polymerization is started. Polymerization is continued until the conversion rate reaches 70%-80%, and the reaction is stopped. Unreacted propylene monomer is discharged, and the polypropylene is taken into a flash distillation pot for flash distillation, after which air is passed through, washed, centrifuged, dried, and taken out to obtain polypropylene powder, which is then extruded and granulated to obtain polypropylene particles.

[0057] Using the GB / T 30923-2014 Plastics Polypropylene (PP) Melt Blown Special Material, the above polypropylene was tested and the melt index was 1327g / 10min.

[0058] The above polypropylene particles were melt-blown using conventional polypropylene melt-blown equipment with the following process parameters to obtain an aerogel-containing melt-blown polypropylene nonwoven fabric with a thermal conductivity of 0.084 W / (m K) and aerogel accounting for 10% of the volume fraction of the final ultra-lightweight, heat-insulating, and thermally insulating melt-blown nonwoven fabric. The specific melt-blown parameters were die temperature 240°C, die to catcher distance 0.152 m, hot air temperature 140°C, and hot air velocity 400 m / s.

[0059] As mentioned above, the above embodiments of the present invention can achieve the following technical effects.

[0060] 1) A simple and efficient aerogel mixing method was provided, and aerogel-modified PP with good melt-blown performance and ultra-lightweight, heat-insulating, and heat-retaining PP melt-blown nonwoven fabric were obtained.

[0061] 2) Aerogel in polypropylene and its melt-blown nonwoven fabric particle size Size and dispersion can now be adjusted.

[0062] The above is merely a preferred embodiment of the present invention, and is not intended to limit the present invention. Those skilled in the art can make various modifications and variations to the present invention. All modifications, equivalent replacements, improvements, etc. within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing an aerogel-modified polypropylene, comprising the steps of: adding an aerogel to and mixing with reactants before or during an in-situ polymerization reaction to achieve uniform dispersion of the aerogel; preparing the aerogel-modified polypropylene by a propylene polymerization process; wherein the reactants include a propylene monomer, a catalyst, and an auxiliary not including a dispersion auxiliary; the aerogel has a particle size of 20 nm to 100 μm, a porosity of 40% to 99.9%, a bulk density of 3 to 500 g / L, the aerogel occupies 20% to 60% of the volume of a thermal insulating and heat retaining melt-blown nonwoven fabric; and the auxiliary is hydrogen; and feeding the aerogel-modified polypropylene into a melt-blown device to prepare a thermally insulating, heat-retaining melt-blown nonwoven fabric.

2. 2. The method according to claim 1, wherein the propylene polymerization process is a gas phase propylene polymerization process, a slurry propylene polymerization process or a liquid phase propylene polymerization process.

3. 3. The method according to claim 2, wherein in the gas phase propylene polymerization process, adding and mixing the aerogel with the reactants includes mixing the aerogel with the propylene monomer, or mixing with the catalyst, or adding the aerogel separately to the polymerization reactor and mixing with the reactants, or any combination of the above mixing methods.

4. 3. The method according to claim 2, wherein in the slurry propylene polymerization process, adding aerogel to mix with reactants includes mixing the aerogel with a slurry liquid of catalyst and hydrocarbon solvent, or mixing with propylene monomer, or adding the aerogel separately to a polymerization reactor and mixing with reactants, or any combination of the above mixing methods.

5. The preparation method according to claim 4, characterized in that the slurry method propylene polymerization step further comprises deashing and precipitating the obtained polypropylene raw material to separate the solvent and the random mass, and kneading the mixture.

6. 3. The method according to claim 2, wherein in the liquid phase propylene polymerization process, adding and mixing the aerogel with the reactants includes mixing the aerogel with the propylene monomer, or mixing with the catalyst, or adding the aerogel separately to the polymerization reactor and mixing with the reactants, or any combination of the above mixing methods.

7. 7. The method according to claim 6, further comprising the step of removing random copolymers by flash distillation in the liquid phase propylene polymerization process.

8. The method of claim 1, wherein the size of the aerogel in the aerogel-modified polypropylene is 15 nm to 100 μm.

9. A thermal insulation and heat-retaining melt-blown nonwoven fabric prepared by the method according to any one of claims 1 to 8, characterized in that the size of the aerogel is 15 nm to 10 μm.

Citation Information

Patent Citations

  • Heat insulation and preservation fiber, and preparation method and application thereof

    CN106319662A

  • Ziegla-Natta catalyst, method for producing the same, and use in the polymerization of alkenes using the same.

    JP2008512506A

  • Dimensional stability melt blown nonwoven fabric fiber structure, its manufacturing method and manufacturing apparatus

    JP2016538439A

  • Synthetic fibers containing an aerogel and a polymer material, a method for producing the same, and an article including the same

    JP2018537599A

  • Manufacturing method of polypropylene with silica aerogel powder as filler and polypropylene product

    KR1020100116841A