Top plate for cooker and cooker

The top plate design with a flaky inorganic filler in the adhesive shielding layer addresses the issue of adhesive seepage, ensuring the cooker's appearance is not damaged by high temperatures.

JP7554553B2Active Publication Date: 2024-09-20NIPPON ELECTRIC GLASS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2019190148
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-10-17
Publication Date
2024-09-20
Estimated Expiration
2039-10-17

AI Technical Summary

Technical Problem

The silica-containing inorganic paint layer fails to prevent adhesive from seeping into the inorganic pigment layer, especially when heated to high temperatures, causing damage to the appearance of the cooker top plate.

Method used

A top plate design featuring a glass substrate with a colored layer and an adhesive shielding layer containing a flaky inorganic filler, such as aluminum filler, to prevent adhesive penetration.

Benefits of technology

The design effectively prevents adhesive penetration, maintaining the appearance of the cooker top plate by using a flaky inorganic filler to block adhesive seepage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554553000001
    Figure 0007554553000001
  • Figure 0007554553000002
    Figure 0007554553000002
  • Figure 0007554553000003
    Figure 0007554553000003
Patent Text Reader

Abstract

To provide a top plate for cookers that resists degradation in appearance.SOLUTION: A top plate for cookers 1 has a glass plate that has a cooking face 2a to be in contact with a cooking utensil and a rear face 2b opposite the cooking face. The top plate has a colored layer 3 that is on the rear face 2b and contains a coloring pigment, and an adhesive blocking layer 4 that is on the colored layer 3 and contains a flaky inorganic filler.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a top plate for a cooking appliance and a cooking appliance. [Background technology]

[0002] A glass plate made of crystallized glass having a low thermal expansion coefficient is used for the top plate of a cooking appliance. When a transparent glass plate is used as the glass plate, a porous inorganic pigment layer made of inorganic pigment and glass powder is generally provided as a decorative layer on the back surface opposite to the cooking surface on which the cooking utensil is placed, as in Patent Document 1, in order to conceal the internal structure of the cooking appliance.

[0003] The top plate for the cooker is generally bonded to the frame of the cooker with an adhesive. Also, a temperature sensor for acquiring temperature information for controlling each of the heat sources is often attached to the back surface of the top plate for the cooker via silicone grease. In this case, in order to prevent the adhesive or silicone grease from penetrating into the inorganic pigment layer, for example, a top plate for the cooker in which a silica-containing inorganic paint layer is printed on the inorganic pigment layer has been proposed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-9958 A [Patent Document 2] JP 2016-11761 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the silica-containing inorganic paint layer cannot sufficiently prevent the adhesive from penetrating into the inorganic pigment layer. In particular, if the adhesive is heated to a high temperature of 200°C or higher and turns brown, the appearance of the cookware top plate will be marred.

[0006] In view of the above circumstances, an object of the present invention is to provide a top plate for a cooker whose appearance is not easily impaired. [Means for solving the problem]

[0007] The top plate for a cooker of the present invention, which was invented to solve the above problems, is a top plate for a cooker comprising a glass plate having a cooking surface with which a cooking utensil comes into contact and a back surface opposite the cooking surface, and further comprising a colored layer on the back surface containing a color pigment, and an adhesive shielding layer on the colored layer containing a flake-shaped inorganic filler.

[0008] In this way, by including the adhesive shielding layer, it is possible to prevent the adhesive from seeping into the colored layer, and to prevent the appearance of the cooking appliance top plate from being impaired.

[0009] In the above configuration, the flaky inorganic filler preferably contains aluminum filler.

[0010] By using an aluminum filler, it is possible to effectively prevent the adhesive from penetrating into the colored layer.

[0011] In the above-mentioned configuration, the average particle size of the flaky inorganic filler is preferably 5 to 40 μm.

[0012] By setting the average particle size within a predetermined range, it is possible to effectively prevent the adhesive from penetrating into the colored layer.

[0013] In the above configuration, the adhesive shielding layer preferably contains 5 to 45% by mass of the flaky inorganic filler.

[0014] By setting the average particle size within a predetermined range, the adhesive shielding layer can effectively prevent the adhesive from seeping into the colored layer when the cooker is used for a long period of time.

[0015] The cooking appliance of the present invention, which was invented to solve the above problems, comprises a cooking appliance top plate having a glass plate with a cooking surface in contact with a cooking utensil and a back surface opposite the cooking surface, a heating appliance, and a frame bonded to the cooking appliance top plate via an adhesive, wherein the adhesive comprises silicone, and the cooking appliance top plate comprises a colored layer on the back surface which contains a color pigment, and an adhesive shielding layer on the colored layer which contains a flake-shaped inorganic filler.

[0016] In this way, by including the adhesive shielding layer, it is possible to prevent the adhesive from seeping into the colored layer, and to prevent the appearance of the cooking appliance top plate from being impaired. Effect of the Invention

[0017] According to the present invention, it is possible to provide a top plate for a cooker whose appearance is not easily marred. [Brief description of the drawings]

[0018] [Figure 1] 1 is a partial cross-sectional view showing a top plate for a cooker according to an embodiment of the present invention. [Diagram 2] 1 is a plan view of a top plate for a cooker according to an embodiment of the present invention, viewed from the cooking surface side. [Diagram 3] 1 is a cross-sectional view showing a cooking device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The following describes the form for carrying out the present invention. However, the present invention is not limited to the following embodiment. It should be understood that the scope of the present invention also includes modifications and improvements to the following embodiment as appropriate based on the ordinary knowledge of a person skilled in the art, provided that the modifications and improvements do not deviate from the spirit of the present invention.

[0020] (Cooking equipment top plate) Fig. 1 is a schematic partial front cross-sectional view showing a top plate for a cooker according to one embodiment of the present invention. As shown in Fig. 1, a top plate for a cooker 1 (hereinafter, "top plate for a cooker 1" will be simply referred to as "top plate 1") includes a glass substrate 2. The glass substrate 2 has a cooking surface 2a, which is a main surface on one side, and a back surface 2b, which is a main surface on the other side. The cooking surface 2a is the surface on which a cooking utensil such as a pot or frying pan is placed. The back surface 2b is the surface facing a heating device inside the cooker. Therefore, the cooking surface 2a and the back surface 2b are in a front-back relationship.

[0021] The glass substrate 2 transmits at least a part of light in the wavelength range of 450 nm to 700 nm. The glass substrate 2 may be colored and transparent, but is preferably colorless and transparent from the viewpoint of further enhancing the aesthetic appearance of the top plate 1. In this specification, being colorless and transparent means that the light transmittance in the visible wavelength range of 450 nm to 700 nm is 70% or more.

[0022] The top plate 1 is repeatedly heated and cooled. For this reason, the glass substrate 2 preferably has high heat resistance and a low thermal expansion coefficient. Specifically, the softening temperature of the glass substrate 2 is preferably 700° C. or higher, and more preferably 750° C. or higher. The average linear thermal expansion coefficient of the glass substrate 2 at 30° C. to 750° C. is −10×10 -7 / ℃~+60×10 -7 / °C, and is preferably within the range of -10×10 -7 / ℃~+50×10 -7 / °C, and more preferably within the range of -10×10 -7 / ℃~+40×10-7 / °C. Therefore, it is preferable that the glass substrate 2 is made of glass with a high glass transition temperature and low expansion, or low-expansion crystallized glass. A specific example of low-expansion crystallized glass is "N-0" manufactured by Nippon Electric Glass Co., Ltd. Note that borosilicate glass or the like may also be used as the glass substrate 2.

[0023] There is no particular limitation on the thickness of the glass substrate 2. The thickness of the glass substrate 2 can be appropriately set depending on the light transmittance, etc. The thickness of the glass substrate 2 can be, for example, about 2 mm to 6 mm.

[0024] As shown in FIG. 2, when the top plate 1 is used in a gas cooker, the glass substrate 2 is provided with openings 2c, 2c, 2c for installing a heating device, which will be described later.

[0025] A colored layer 3 is provided on the rear surface 2b of the glass substrate 2. The colored layer 3 is provided on the rear surface 2b of the glass substrate 2 in direct contact therewith. The colored layer 3 contains, for example, glass, an inorganic color pigment, and an extender pigment.

[0026] The inorganic color pigment is not particularly limited as long as it is a colored inorganic substance. Examples of the inorganic color pigment include white pigment powders such as TiO2 powder, ZrO2 powder, or ZrSiO4 powder, blue inorganic pigment powders containing Co, green inorganic pigment powders containing Co, Ti-Sb-Cr-based or Ti-Ni-based yellow inorganic pigment powders, Co-Si-based red inorganic pigment powders, brown inorganic pigment powders containing Fe, or black inorganic pigment powders containing Cu.

[0027] Specific examples of blue inorganic pigment powders containing Co include Co-Al or Co-Al-Ti inorganic pigment powders. Specific examples of Co-Al inorganic pigment powders include CoAl2O4 powder. Specific examples of Co-Al-Ti inorganic pigment powders include CoAl2O4-TiO2-Li2O powder.

[0028] Specific examples of green inorganic pigment powders containing Co include Co-Al-Cr or Co-Ni-Ti-Zn inorganic pigment powders. Specific examples of Co-Al-Cr inorganic pigment powders include Co(Al,Cr)2O4 powder. Specific examples of Co-Ni-Ti-Zn inorganic pigment powders include (Co,Ni,Zn)2TiO4 powder.

[0029] A specific example of the brown inorganic pigment powder containing Fe is, for example, an Fe-Zn-based inorganic pigment powder. A specific example of the Fe-Zn-based inorganic pigment powder is, for example, a (Zn,Fe)Fe2O4 powder.

[0030] Specific examples of black inorganic pigment powders containing Cu include Cu-Cr-based inorganic pigment powders and Cu-Fe-based inorganic pigment powders. Specific examples of Cu-Cr-based inorganic pigment powders include Cu(Cr,Mn)2O4 powder and Cu-Cr-Mn powder. Specific examples of Cu-Fe-based inorganic pigment powders include Cu-Fe-Mn powder.

[0031] The content of the inorganic color pigment contained in the colored layer 3 is preferably 10% by mass or more, more preferably 15% by mass or more. The content of the inorganic color pigment is preferably 80% by mass or less, more preferably 75% by mass or less. If the content of the inorganic color pigment is too low, the coloring of the top plate 1 may be insufficient. If the content of the inorganic color pigment is too high, the heat resistance and impact resistance of the top plate 1 may decrease. The content of the color pigment contained in the colored layer 3 is the content when the entire material constituting the colored layer 3 is taken as 100% by mass.

[0032] Examples of the glass that can be used include borosilicate glass, silicate glass containing at least one of an alkali metal component and an alkaline earth metal component, and phosphate glass containing zinc and aluminum. Examples of the shape of the glass include flakes and powder.

[0033] From the viewpoint of impact resistance, the glass content in the colored layer 3 is preferably within the range of 20 to 50 mass %. The glass content is more preferably 25 mass % or more, and even more preferably 30 mass % or more. The glass content is more preferably 45 mass % or less, and even more preferably 40 mass % or less. The glass content in the colored layer 3 is the content when the entire material constituting the colored layer 3 is taken as 100 mass %.

[0034] The extender pigment is not particularly limited, but for example, talc, mica, etc. can be used. These extender pigments may be used alone or in combination. The extender pigment can further increase the heat resistance and impact resistance of the top plate 1.

[0035] The average particle diameter of the extender pigment is preferably 5 to 50 μm from the viewpoint of dispersibility in the colored layer 3. Here, the average particle diameter is a median diameter derived from a volume distribution measured by a laser diffraction scattering method. The average particle diameter of the extender pigment is more preferably 10 μm or more, and even more preferably 15 μm or more. The average particle diameter of the extender pigment is more preferably 45 μm or less, and even more preferably 40 μm or less.

[0036] The colored layer 3 may contain a heat-resistant resin instead of glass. The heat-resistant resin is preferably one having high heat resistance. An example of such a heat-resistant resin is a silicone resin. The silicone resin contained in the colored layer 3 is preferably a silicone resin in which the functional group directly bonded to the silicon atom is at least one of a methyl group and a phenyl group. In this case, discoloration of the colored layer 3 when the top plate 1 becomes hot can be more effectively suppressed.

[0037] From the viewpoint of heat resistance and impact resistance, the content of the silicone resin in the colored layer 3 is preferably within the range of 30 to 60 mass %. The content of the silicone resin is more preferably 35 mass % or more, and even more preferably 40 mass % or more. The content of the silicone resin is more preferably 55 mass % or less, and even more preferably 50 mass % or less. The content of the silicone resin contained in the colored layer 3 is the content when the entire material constituting the colored layer 3 is taken as 100 mass %.

[0038] An adhesive shielding layer 4 is provided on the colored layer 3. The adhesive shielding layer 4 is provided to shield the adhesive used for assembling the cooker when viewed from the cooking surface 2a side of the top plate 1. In particular, the temperature around the opening 2c is likely to rise to 200°C or more when gas is ignited. As a result, the adhesive turns brown and appears as a stain when viewed from the cooking surface 2a side, damaging the appearance. By providing the adhesive shielding layer 4, it is possible to prevent the appearance of the top plate 1 from being damaged.

[0039] The adhesive shielding layer 4 essentially contains a flake-shaped inorganic filler, and optionally contains an inorganic color pigment, an extender pigment, and a heat-resistant resin. The flake-shaped inorganic filler contained in the adhesive shielding layer 4 is arranged so as to be folded in multiple layers, thereby exerting the effect of absorbing mechanical external forces when the heat-resistant resin contained in the adhesive shielding layer 4 thermally softens and the adhesive tries to penetrate. Therefore, the adhesive is blocked by the adhesive shielding layer 4, and the adhesive can be prevented from penetrating into the colored layer 3 side.

[0040] Here, the flake-like inorganic filler includes shapes such as plate-like and scale-like, and refers to a shape obtained by crushing a three-dimensional shape such as a sphere or a lump in one direction. Examples of the flake-like inorganic filler include flake-like copper powder (MA-C02K, etc.) manufactured by Mitsui Mining & Smelting Co., Ltd., zinc flake powder (Zn-S-D8) manufactured by Fukuda Metal Foil & Powder Co., Ltd., stainless steel flakes and Leafing Alpaste (registered trademark) manufactured by Toyo Aluminum Co., Ltd., and Xirallic (registered trademark) and Meoxal (registered trademark) manufactured by Merck Performance Materials Co., Ltd.

[0041] The flake-like inorganic filler is preferably, for example, an aluminum filler, which is a hard filler and has excellent mechanical durability.

[0042] The average particle diameter of the flaky inorganic filler is preferably 5 to 40 μm from the viewpoint of dispersibility in the adhesive shielding layer 4 and blocking during adhesion. If the average particle diameter of the flaky inorganic filler is too small, the flaky inorganic filler may be easily aggregated, and dispersibility may decrease. On the other hand, if the average particle diameter of the flaky inorganic filler is too large, gaps may be easily formed between the flaky inorganic filler, and the adhesive may pass through the gaps. The average particle diameter of the flaky inorganic filler is more preferably 7 μm or more, and more preferably 10 μm or more. In addition, the average particle diameter of the flaky inorganic filler is more preferably 35 μm or less, and more preferably 30 μm or less. Here, the average particle diameter is a median diameter derived from a volume distribution measured by a laser diffraction scattering method.

[0043] In addition, the particle size of the flaky inorganic filler in the direction perpendicular to the thickness direction is preferably within the range of 5 to 50 μm from the viewpoint of dispersibility in the adhesive shielding layer 4 and blocking during adhesion. Here, the particle size in the direction perpendicular to the thickness direction is a value calculated by determining the surface area of ​​the surface in the thickness direction of 20 flaky inorganic fillers in a photograph taken by a scanning electron microscope and determining the circle equivalent diameter of this surface area. The particle size of the flaky inorganic filler in the direction perpendicular to the thickness direction is more preferably 7 μm or more, and even more preferably 10 μm or more. In addition, the particle size of the flaky inorganic filler in the direction perpendicular to the thickness direction is more preferably 40 μm or less, and even more preferably 35 μm or less.

[0044] The content of the flaky inorganic filler in the adhesive shielding layer 4 is preferably within the range of 5 to 45 mass % in terms of suppressing deterioration of the appearance and dispersibility of the flaky inorganic filler. The content of the flaky inorganic filler is more preferably 10 mass % or more, and even more preferably 15 mass % or more. The content of the flaky inorganic filler is more preferably 35 mass % or less, and even more preferably 30 mass % or less. The content of the flaky inorganic filler contained in the adhesive shielding layer 4 is the content when the entire material constituting the adhesive shielding layer 4 is taken as 100 mass %.

[0045] The inorganic color pigment and heat-resistant resin in the adhesive shielding layer 4 may be the same as those contained in the coloring layer 3. The total amount of the flaky inorganic filler and heat-resistant resin in the adhesive shielding layer 4 is preferably 85% by mass or more, and more preferably 90% by mass or more. The content of the inorganic color pigment is preferably 5% by mass or less, more preferably 1% by mass or less, and most preferably 0.3% by mass or less.

[0046] The adhesive shielding layer 4 preferably has a light transmittance of 30% or less in the visible wavelength region at wavelengths of 450 nm to 700 nm. The adhesive shielding layer 4 prevents the adhesive from penetrating to the colored layer 3 side, but the adhesive may discolor the adhesive shielding layer 4 itself. If the adhesive shielding layer 4 has a high visible light transmittance, the inside of the cookware may be visible and the discolored adhesive shielding layer 4 may also be visible. For this reason, it is preferable that the light transmittance in the visible wavelength region at wavelengths of 450 nm to 700 nm is low.

[0047] In order to reduce light transmittance in the visible wavelength range and efficiently block the adhesive, the thickness of the adhesive shielding layer 4 is preferably within the range of 3 to 30 μm. The thickness of the adhesive shielding layer 4 is more preferably 5 μm or more, and even more preferably 7 μm or more. The thickness of the flaky inorganic filler is more preferably 25 μm or less, and even more preferably 20 μm or less.

[0048] The adhesive shielding layer 4 does not need to be provided so as to cover the entire colored layer 3, but may be provided only in the portion that comes into contact with the adhesive and in the vicinity thereof.

[0049] (Manufacturing method of top plate 1) The top plate 1 can be manufactured, for example, by the following method. First, a color paste containing a heat-resistant resin, an inorganic color pigment powder, and an extender pigment powder, and an adhesive shielding paste containing a heat-resistant resin, an inorganic color pigment powder, an extender pigment powder, and a flake-like filler powder are prepared. Next, the prepared color paste is directly applied onto the rear surface 2b of the glass substrate 2 and dried. After drying, the adhesive shielding paste is applied onto the rear surface 2b of the glass substrate 2 and dried. In this way, a top plate 1 having a color layer 3 and an adhesive shielding layer 4 can be manufactured. Depending on the composition of the color layer 3 and the adhesive shielding layer 4, the top plate 1 may be obtained by firing after drying.

[0050] The application speed and viscosity of the paste can be appropriately set according to the contents of the flaky inorganic filler powder, inorganic color pigment powder, and extender pigment powder contained in the colored layer 3 and the adhesive shielding layer 4. For example, when the contents of the flaky inorganic filler powder, inorganic color pigment powder, and extender pigment powder in the adhesive shielding layer 4 are high, it is preferable to lower the viscosity of the paste and slow down the application speed of the heat-resistant resin. Methods for lowering the viscosity of the paste include changing the type of heat-resistant resin and adding a solvent to the paste.

[0051] The drying temperature for the applied paste can be, for example, about 50° C. to 100° C. The drying time can be, for example, about 5 minutes to 1 hour. In this way, in the manufacturing method of this embodiment, the colored paste and the adhesive shielding paste are applied to the rear surface 2b of the glass substrate 2 and dried to manufacture the top plate 1, so there is no process of baking the glass frit onto the rear surface 2b of the glass substrate 2. Therefore, tensile stress is unlikely to occur on the rear side of the glass substrate 2, and the top plate 1 is unlikely to break when a load or impact is applied to the cooking surface 2a of the glass substrate 2. In addition, since there is no need to bake the glass frit in an undercooked state, the design is unlikely to deteriorate. Therefore, the top plate 1 obtained by the manufacturing method of this embodiment can improve heat resistance and impact resistance without impairing the design.

[0052] (cooker) FIG. 3 is a schematic front cross-sectional view of a part of a cooking device according to an embodiment of the present invention. As shown in FIG. 3, the cooking device 10 includes a top plate 1. A heating device 6 is attached to a frame 5 that is shaped like a lidless box. The heating device 6 in this embodiment is a heating device that is heated by gas and has an outlet 6a from which a flame produced by burning gas is ejected. The top plate 1 is bonded by an adhesive 7 via an adhesive shielding layer 4. The heating device 6 is disposed at a position corresponding to the opening 2c of the top plate 1. Therefore, the top plate 1 and the heating device 6 can be positioned at the same height. A sensor 8 for detecting temperature is attached to the top plate 1, and a trivet 9 is attached to the top plate 1.

[0053] The present invention will be described in more detail below with reference to examples. However, the following examples are merely illustrative and the present invention is not limited to the following examples in any way.

[0054] Example 1 First, two types of pastes for the colored layers (a first paste and a second paste) are prepared. The first paste was prepared by mixing 60 mass % silicone resin (resin solid content) and 40 mass % silver pigment of mica coated with TiO2, and adding 60 mass % of an organic solvent to 100 mass % of this mixture. The second paste was prepared by mixing 56% by mass (resin solids) silicone resin, 6% by mass of a Co-Al-Zn-based blue pigment, and 38% by mass of a Co-Si-Ni-based purple pigment, and then adding 56% by mass of an organic solvent to 100% by mass of this mixture.

[0055] Next, a paste for the adhesive barrier layer is prepared. The adhesive shielding paste was made by mixing 58% by mass of silicone resin (resin solid content), 12% by mass of talc, and 30% by mass of flaky aluminum filler powder, and then adding 58% by mass of organic solvent to the 100% by mass mixture.

[0056] Next, this paste was applied to a transparent crystallized glass plate (manufactured by Nippon Electric Glass Co., Ltd., product name "N-0", average linear thermal expansion coefficient at 30°C to 750°C: 0.5 × 10 -7 The first paste, the second paste, and the adhesive shielding paste were screen-printed in that order over the entire surface of a plate (100°C, thickness 4 mm) so that each paste had a thickness of 10 μm. The plate was then dried at 100°C for 10 minutes and then baked at 300°C for 15 minutes to form a colored layer and an adhesive shielding layer, producing a top plate for a cooking appliance (top plate).

[0057] Comparative Example 1 The adhesive shielding paste of Example 1 was prepared by mixing 55% by mass (resin solids) silicone resin, 15% by mass of Cu-Fe-Mn black pigment, and 30% by mass of talc, and adding 55% by mass of organic solvent to 100% by mass of this mixture. A top plate was prepared in the same manner as Example 1, except that the paste was used.

[0058] (Whether or not there are stains) The top plates of Example 1 and Comparative Example 1 were coated with adhesive and heated in a muffle furnace at 200°C for 8 hours. After that, the portion coated with adhesive was visually inspected from the cooking surface side of the top plate to see if it could be visually inspected. As a result, the adhesive could not be observed in Example 1. On the other hand, the adhesive could be observed in Comparative Example 1. [Explanation of symbols]

[0059] 1...Cooking equipment top plate 2. Glass substrate 2a…Cooking surface 2b…Back side 3...Heat-resistant resin layer 4...Adhesive shielding layer

Claims

1. a glass plate having a cooking surface that contacts a cooking utensil and a back surface opposite the cooking surface; A top plate for a cooker having a color layer containing a color pigment on the back surface; and an adhesive shielding layer on the colored layer, the adhesive shielding layer including a flake-like inorganic filler; The top plate for a cooker, wherein the colored layer does not include glass but includes a silicone resin.

2. The top plate for a cooker according to claim 1 , wherein the flaky inorganic filler comprises an aluminum filler.

3. 3. The top plate for a cooker according to claim 1, wherein the average particle size of the flaky inorganic filler is 5 to 40 μm.

4. The top plate for a cooker according to any one of claims 1 to 3, wherein the adhesive shielding layer contains 5 to 45 mass % of the flaky inorganic filler.

5. a glass plate having a cooking surface that contacts a cooking utensil and a back surface opposite the cooking surface; A top plate for a cooking appliance having the above structure; A heating device that heats with gas; A frame bonded to the cooking appliance top plate via an adhesive; A cooking device having the adhesive comprises silicone; The top plate for the cooker comprises: a color layer containing a color pigment on the back surface; and an adhesive shielding layer on the colored layer, the adhesive shielding layer including a flake-like inorganic filler; The cookware, wherein the colored layer does not include glass but includes a silicone resin.

Citation Information

Patent Citations

  • Top plate for cooking devices

    JP2005038622A

  • Top plate for cooker

    JP2005298266A

  • Glass or glass-ceramic products with decorative coatings

    JP2008536791A

  • Top plate for cooker

    JP2010009958A

  • Scratch resistant silicone coating for cooking face comprising glass or glass ceramic

    JP2010120846A