Lightning protection
A lightweight protective layer for composite structures using curable coatings and conductive materials addresses weight and environmental issues, enhancing lightning protection and durability while reducing manufacturing costs.
Patent Information
- Application Number
- JP2020088799
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-30
- Filing Date
- 2020-05-21
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-05-21
AI Technical Summary
Lightning protection systems for composite structures, such as aircraft components, face challenges due to increased weight, labor costs, and sensitivity to environmental conditions, including moisture and temperature changes, which can lead to cracking and corrosion.
A lightweight outer protective layer comprising curable coatings and electrically conductive materials, such as polyurethane, polyimide, or epoxy, with a conductive polymer weave, that provides electrical conductivity while resisting environmental conditions, reducing weight and manufacturing steps.
The protective layer effectively dissipates lightning energy, reduces weight by 50-80% compared to metal screens, and withstands environmental factors without additional coatings, thereby minimizing damage and labor costs.
Smart Images

Figure 0007554579000003 
Figure 0007554579000001 
Figure 0007554579000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to lightning strike protection for composite parts. Lightning strike protection may also be used to protect composite parts from environmental conditions or exposure to elements including solar radiation, moisture, and / or chemicals such as fuel. The lightning strike protection of the present disclosure is particularly effective for protecting aircraft parts. [Background technology]
[0002] Many components, e.g., aircraft components, are constructed of strong yet lightweight composite materials to help minimize the overall weight of the aircraft or the like. Such composite materials often include carbon reinforced fibers dispersed within a polymer matrix. However, such composite structures are usually substantially less conductive than metallic structures, and as a result, are less able to distribute and dissipate the electrical energy generated by a lightning strike. Thus, the exterior surfaces of such composite components often include lightning strike protection that provides a highly conductive electrical path along the exterior surface. Such conductive paths allow the electrical energy associated with a lightning strike to be rapidly dissipated across the protected surface, helping to minimize damage to the surface of the aircraft or the like at the point of strike. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] U.S. Pat. No. 4,980,234 [Patent Document 2] U.S. Pat. No. 4,980,234 [Patent Document 3] US Patent Application Publication No. 2008 / 0188609 [Patent Document 4] International Publication No. 2008 / 087467 [Patent Document 5] U.S. Pat. No. 4,980,234 [Patent Document 6] US Patent Application Publication No. 2008 / 0188609 [Patent Document 7] U.S. Patent No. 6,228,492 [Patent Document 8] U.S. Patent No. 6,228,492 Summary of the Invention [Problem to be solved by the invention]
[0004] Lightning protection for composite structures is commonly incorporated into a surface coating that is attached to the composite surface to dissipate the energy received by a lightning strike using expanded metal screens (meshes). While metal screens have proven effective in providing lightning protection, such materials can add undesirable weight to aircraft and the like. Furthermore, incorporating such surface coatings into composite structures can significantly increase labor costs. Also, such screens can be susceptible to environmental conditions, including moisture, chemicals, or frequent ambient temperature changes, which can initiate cracking and corrosion of the composite parts. Thus, a need remains for lightning protection that is lightweight, can be easily incorporated into composite structures, and exhibits resistance to environmental conditions. [Means for solving the problem]
[0005] In one aspect, the present disclosure relates to an exterior protective layer for protecting a composite structure from environmental conditions, the exterior protective layer comprising at least one curable coating and a conductive material, the at least one curable coating comprising at least one of polyurethane, polyimide, polyester, or epoxy when cured, the conductive material comprising a wireless conductive material and / or a conductive polymer weave, and a weight of the exterior protective layer ranging from about 0.02 pounds per square foot to about 0.1 pounds per square foot.
[0006] In some embodiments, the at least one curable coating comprises at least a first curable coating and a second curable coating, and the conductive material comprises a conductive polymer weave disposed between the first curable coating and the second curable coating, and the first curable coating and the second curable coating, separately, comprise at least one of polyurethane, polyimide, polyester, or epoxy when cured, and typically comprise polyurethane.
[0007] In another aspect, the present disclosure relates to an exterior protected composite structure comprising: a composite structure, the composite structure including a surface that may be exposed to environmental conditions; and an exterior protective layer, the exterior protective layer adhered to the composite structure surface that is exposed to environmental conditions, the exterior protective layer comprising at least one curable coating and a conductive material, the at least one curable coating comprising at least one of polyurethane, polyimide, polyester, or epoxy when cured, the conductive material comprising a wireless conductive material and / or a conductive polymer weave, and a weight of the exterior protective layer ranging from about 0.02 pounds per square foot to about 0.1 pounds per square foot.
[0008] In yet another aspect, the present disclosure relates to a method of forming an exterior protected composite structure, comprising disposing an exterior protective layer on a surface of a composite material, the exterior protective layer comprising at least one curable coating and a conductive material; and co-curing the exterior protective layer and the composite material to form a cured exterior protected structure, the at least one curable coating comprising at least one of polyurethane, polyimide, polyester, or epoxy upon curing, the conductive material comprising a wireless conductive material and / or a conductive polymer weave, the exterior protective layer having a weight ranging from about 0.02 pounds per square foot to about 0.1 pounds per square foot, and the exterior protective layer may be exposed to environmental conditions. [Brief description of the drawings]
[0009] [Figure 1] 1 illustrates an embodiment of an exterior protective layer as described in the detailed description. [Diagram 2] 1 illustrates an embodiment of an exterior protective composite structure as described in the detailed description. [Diagram 3] 1 illustrates an embodiment of an aircraft including a skin protection composite structure, as described in the detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] As used throughout, ranges are used as shorthand to describe each value included within the range. Any value within the range can be selected as the terminus of the range. In the event of a conflict between the definitions in this disclosure and a cited document, this disclosure controls. Unless otherwise specified, all percentages and amounts expressed in the detailed description and elsewhere herein should be understood to refer to weight percent. The amounts given are based on the active weight of the material.
[0011] Weights and ranges were measured using an analytical balance. Weights are by weight of total solids unless otherwise specified. Particle size was tested using a Coulter Counter unless otherwise specified.
[0012] The present inventors have developed a lightweight exterior protective layer for lightning strike protection of composite structures, such as those used in aircraft parts. In embodiments, the exterior protective layer does not require metal screens and / or interwoven wire fabric (IWWF), which can cause cracks in the composite structure due to thermal expansion. Additionally, the present exterior protective layer is resistant to environmental conditions and requires fewer manufacturing steps, reducing labor costs. These and other significant advantages of the present exterior protective layer are described in further detail herein.
[0013] item outer protective layer hardenable coating The present disclosure relates to an exterior protective layer for protecting a composite structure from exposure to environmental conditions, the exterior protective layer including at least two curable coatings and at least one electrically conductive material, etc. As described herein, the electrically conductive material may be incorporated into the curable coatings of the present disclosure or may form a layer and be disposed between a first curable coating and a second curable coating.
[0014] As used herein, the phrase "environmental conditions" encompasses natural environmental conditions or elements such as electromagnetic energy events, such as lightning strikes, electrostatic discharges, and electromagnetic interference, solar radiation, including ultraviolet radiation, ozone, humidity, and rain, and / or non-natural conditions and / or elements found in the environment, such as extreme heat generated by aircraft engines, conditions and / or chemicals, including those within the aircraft environment, such as antifreeze, fuel, hydraulic fluid, battery acid, cleaning agents, etc., that are passed by conduction and radiation to nearby equipment.
[0015] In some embodiments, at least one curable coating of the present disclosure is formed from a curable coating composition that includes a thermosetting resin. Thermosetting resins generally include prepolymers that are in the form of a soft solid or viscous liquid at room temperature (about 20° C. to about 25° C.) and typically cure to harden.
[0016] "Curing" refers to inducing a chemical reaction in a curable material, such as the curable coating compositions of the present application, that results in extensive cross-linking between polymer chains to produce an insoluble polymer network. Curing may be accomplished, for example, by processes including heating and / or exposure to ultraviolet light. In some embodiments, curing is accelerated by high pressure or by mixing with a curing agent or catalyst. As used herein, the phrase "at least partially cured" refers to subjecting a polymerizable composition to curing conditions that result in reaction of at least a portion of the reactive groups of the composition to form a solid polymer.
[0017] Examples of suitable thermosetting resins for use with the curable coating compositions of the present disclosure include polyester resins, epoxy resins, and polyimide resins, such as bismaleimide (BMI) and / or polyetherimide. In a more typical embodiment, the thermosetting resins for use with the curable coating compositions of the present disclosure include at least one polyisocyanate that forms a polyurethane upon curing, and at least one polyol. As used herein, the term "polyurethane" refers to a polymer that includes urethane (also known as carbamate) linkages, urea linkages, or combinations thereof, such as polyurethaneureas. Thus, the polyurethanes of the present disclosure may include at least urethane linkages, and optionally urea linkages.
[0018] In some embodiments, the curable coating composition of the present disclosure comprises a thermosetting resin in an amount ranging from about 5 to 100 weight percent (wt.%), such as about 15 to 75 weight percent (wt.%), about 25 to 60 weight percent (wt.%), based on the total weight of the curable coating composition.
[0019] In some embodiments, the curable coating compositions of the present disclosure further comprise non-conductive additives, such as fillers, flow control agents, toughening agents, pigments, stabilizers (e.g., antioxidants, thermal stabilizers, and ultraviolet (UV) stabilizers), curing agents, and / or catalysts.
[0020] Examples of non-conductive fillers suitable for use with the curable coating compositions of the present disclosure include chalk or precipitated lime carbonate, ground quartz, alumina, dolomite, carbon fiber, glass fiber, polymeric fiber, titanium dioxide, fused silica, carbon black, calcium oxide, calcium magnesium carbonate, barite, and especially silicate-like fillers of the aluminum magnesium calcium silicate type. Other suitable non-conductive fillers include ceramics, and fumed silica. The fillers may be in the form of flakes, powders, fibers, microspheres, or glass balloons, and may be solid or hollow structures. Further discussion of fillers can be found in U.S. Pat. No. 4,980,234.
[0021] In some embodiments, the filler may be present in the curable coating compositions of the present disclosure in an amount ranging from about 0 to 40 wt.%, based on the total weight of the curable coating composition, hi other embodiments, the filler may be present in a concentration ranging from about 5 to 30 wt.%.
[0022] Flow control agents may be used to modify the rheological properties of the curable coating compositions of the present disclosure. Examples of suitable flow control agents include fumed silica and metal powders. The flow control agent may be present in an amount ranging from about 0 to 40 wt.%, more typically about 0.1 to 10 wt.%, based on the total weight of the composition.
[0023] In some embodiments, toughening agents are added to the curable coating compositions of the present disclosure to adjust the stiffness of the coating after curing and the surface hardness of the coating. In some embodiments, the toughening agent may be a polymer or oligomer and may have a glass transition temperature below 20° C. (more typically below 0° C., or below −30° C., or below −50° C.) and / or may have functional groups such as carboxylic acid groups, amino groups, and / or hydroxyl groups that can react with other components of the curable coating compositions of the present disclosure when the composition is cured by heat.
[0024] Examples of suitable toughening agents include elastomeric toughening agents such as carboxylated nitriles (e.g., Nipol 1472 from Zeon Chemical, Inc.), carboxy-terminated butadiene acrylonitrile (CTBN), carboxy-terminated polybutadiene (CTB), poly(ether ether ketone) (PEEK), and polyether ketone ketone (PEKK). Further examples of suitable toughening agents are described in U.S. Pat. No. 4,980,234, U.S. Patent Publication No. 2008 / 0188609, and WO 2008 / 087467. The concentration of the toughening agent may range from about 5 to 40 wt.%, based on the total weight of the composition. In other embodiments, the concentration of the toughening agent may range from about 1 to 30 wt.%.
[0025] Pigments may be added to the curable coating compositions of the present disclosure to adjust the color and appearance of the curable coating. Suitable pigments include titanium dioxide, carbon black, black pigments, and other colored dyes. The pigments may be in the form of flakes, powders, fibers, or color-concentrated liquids. The total amount of all pigments may range from about 0 to 20 wt.%, based on the total weight of the composition.
[0026] Optionally, UV stabilizers may be added to the curable coating compositions of the present disclosure. In some embodiments, UV stabilizers include UV absorbers, antioxidants, pigments, screening agents, and fillers. In some embodiments, UV stabilizers include butylated hydroxytoluene (BHT), 2-hydroxy-4-methoxy-benzophenone (UV-9), 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 3,5-di-tert-butyl-4-hydroxybenzoic acid, n hexadecyl ester, titanium dioxide, and carbon black. In some embodiments, the UV stabilizers may each be present in an amount ranging from about 0.1 to 5 wt.%, based on the total weight of the composition. In other embodiments, the UV stabilizers may each be present in an amount ranging from about 0.5 to 3 wt.%, based on the total weight of the composition.
[0027] Examples of suitable curing agents and / or catalysts that may be added to the curable coating compositions of the present disclosure include aliphatic and aromatic primary amines, and aliphatic and aromatic tertiary amines. More specifically, amine curing agents and / or catalysts may include dicyandiamide, bis-urea (e.g., 2,4-toluene bis-(dimethylurea), 4,4'-methylene bis-(phenyl dimethylurea)), and 4,4'-diaminodiphenyl sulfone (4,4-DDS). Other suitable curing agents and / or catalysts include boron trifluoride complexes, guanidine, and dicyandiamide. Further examples of curing agents and / or catalysts can be found in U.S. Pat. No. 4,980,234 and U.S. Patent Application Publication No. 2008 / 0188609.
[0028] The one or more curing agents and / or catalysts may be present in an amount ranging from about 0.1 to 40 wt.%, based on the total weight of the curable coating composition. In other embodiments, the one or more curing agents and / or catalysts may be present in an amount ranging from about 0.5 to 10 wt.%, based on the total weight of the curable coating composition.
[0029] Other suitable additives that may be included in the curable coating compositions of the present disclosure include crosslinkers (e.g., aluminum or melamine crosslinkers), binders, corrosion inhibitors, plasticizers, and / or other conventional additives known to those of skill in the art. In some embodiments, the curable coating compositions of the present disclosure further include an electrically conductive material as described herein.
[0030] At least one curable coating of the present disclosure may be formed by adding one or more resins capable of forming a thermosetting polymer to a mixing vessel, as described herein. In some embodiments, non-conductive additives, such as one or more non-conductive fillers, flow control agents, pigments, UV stabilizers, curing agents, and / or catalysts, are further added to the mixing vessel. In some embodiments, one or more conductive materials, such as silver nanoparticles, are further added to the mixing vessel, as described herein.
[0031] In some embodiments, one or more solvents are included in the mixture to facilitate mixing of the components. Examples of such solvents may include methyl ethyl ketone (MEK), acetone, dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP).
[0032] After adding the above-mentioned components, the curable coating composition may be mixed using a high shear mixer or the like. Mixing may be carried out at a speed of about 1000-5000 revolutions per minute for, for example, 30-80 minutes until the components are substantially uniformly mixed and one or more conductive materials, if present, are uniformly dispersed within the curable coating composition.
[0033] The mixed curable coating composition may then be subsequently formed into a curable coating by coating using, for example, a hot melt coating or a solvent-based coating process, as known in the art. In some embodiments, at least one curable coating of the present disclosure, such as at least two curable coatings, may be stored in a refrigerator to inhibit curing, thereby extending its useful shelf life.
[0034] In some embodiments, at least two curable coatings are formed from one or more curable coating compositions. In such embodiments, the curable coatings may each comprise the same or different thermosetting resins. In some embodiments, the first and second curable coatings separately each comprise at least one of polyurethane, polyimide, polyester, or epoxy when cured. Typically, the first and second curable coatings each comprise polyurethane when cured.
[0035] Conductive Materials In some embodiments, the outer protective layer of the present disclosure comprises an electrically conductive material. As used herein, "electrically conductive" refers to having a high electrical conductivity at least as high as that characteristic of a metal, typically in a metallic state such as titanium, platinum, copper, aluminum, nickel, silver, gold, etc., and / or in an ICP such as polypyrrole, polycarbazole, polyaniline, polyacetylene, and polythiophene.
[0036] In some embodiments, the conductive materials of the present disclosure are "wireless." As used herein, "wire" refers to a continuous metal or metal alloy structure that is stretched into the shape of a thin, flexible filament or rod. Conductive materials that include wire include metal mesh and interwoven wire fabrics (IWWF), in which wires including phosphor bronze, aluminum, copper, and other metals or alloys are woven into a fabric, such as activated carbon fabric. Metal-coated filaments are also intended to be included in the term "wire."
[0037] The term "wire-free" in reference to conductive materials of the present disclosure includes metals and alloys that are not in the form of a wire, such as metal coated particles, metal particles, metal flakes, and / or metal nanoparticles. As described herein, the term "wire-free" further includes conductive materials that are not composed of metals and / or alloys, having any morphology, such as filaments, including ICPs.
[0038] In some embodiments, the wireless conductive material of the present disclosure includes metallic conductive materials, such as metal-coated particles, metal particles, and / or metal flakes. In some embodiments, the maximum average dimension of the metal-coated particles, metal particles, and / or metal flakes is greater than 1 micrometer (μm), such as 1 μm to 250 μm, 10 μm to 100 μm, 50 μm to 200 μm, etc. In some embodiments, the metal particles and / or metal flakes of the conductive material of the present disclosure include silver, gold, nickel, copper, aluminum, alloys thereof, and mixtures thereof. Examples of metal-coated particles include metal-coated glass balloons and metal-coated graphite. Examples of metals that may be used as coatings include silver, gold, nickel, copper, aluminum, alloys thereof, and mixtures thereof.
[0039] In some embodiments, the metal wire-free conductive material of the present disclosure comprises metal nanoparticles. In some embodiments, the maximum average diameter of the nanoparticles may be less than 100 nanometers, such as from about 1 nanometer to about 80 nanometers, such as from 10 to 50 nanometers. Metal nanoparticles suitable for use as the wire-free conductive material of the present disclosure include silver, gold, nickel, aluminum, or copper nanoparticles, alloys thereof, and mixtures thereof. Typically, silver nanoparticles are used.
[0040] In some embodiments, the concentration of metal wire-free conductive material, such as metal coated particles, metal particles, metal flakes, and / or metal nanoparticles, in the curable coating composition is greater than about 30 wt.%, such as about 39 wt.% to 65 wt.%, based on the total weight of the curable coating composition. In some embodiments, metal wire-free conductive material, such as metal coated particles, metal particles, metal flakes, and / or metal nanoparticles, is uniformly dispersed throughout the curable coating composition of the present disclosure and then formed into a curable coating to provide the exterior protective layer of the present disclosure.
[0041] In other embodiments, the exterior protective layer of the present disclosure includes a first curable coating, a second curable coating, and a conductive material including a metallic wire-free conductive material, the metallic conductive material being disposed between the first curable coating and the second curable coating. In such embodiments, the metallic wire-free conductive material, such as metal coated particles, metallic particles, metallic flakes, and / or metallic nanoparticles, is not incorporated into the curable coating composition of the present disclosure, but instead is formed into a conductive layer on the surface of the first curable coating. In some embodiments, a second curable coating is then disposed on the conductive layer formed of the metallic wire-free conductive material.
[0042] In some embodiments, at least a third curable coating may be laminated adjacent to the at least one curable coating, while in other embodiments, at least a third curable coating may be laminated adjacent to the first curable coating.
[0043] In other embodiments, the wire-free conductive materials of the present disclosure are metal-free. Examples of suitable conductive non-metals include conductive carbon black, graphite, antimony oxide, the ICPs described herein, and combinations thereof.
[0044] The form of the non-metallic conductive material may be in the form of particles coated with a conductive non-metal, such as ICP or carbon black, which may be coated, for example, on a non-conductive polymer, a non-metal particle, and / or a non-metal flake. In some embodiments, such non-metallic conductive materials have a maximum average dimension greater than 1 micron, e.g., between 10 microns and 100 microns, between 50 microns and 200 microns, or between 1 micron and 250 microns.
[0045] In some embodiments, the non-metallic conductive material may be in the form of a nanomaterial, such as a nanotube or nanoparticle, the maximum average diameter of such nanomaterials may be less than about 100 nanometers, such as from about 1 to about 80 nanometers, such as from about 10 to about 50 nanometers.
[0046] In some embodiments, the non-metallic conductive material is a carbon nanotube. The carbon nanotube may include a single-walled carbon nanotube (SWNT), a double-walled carbon nanotube (DNT), and a multi-walled carbon nanotube (MWNT). The carbon nanotube may be optionally surface functionalized. Examples of functional groups that may be used for functionalization may include hydroxyl, epoxy, and amine functional groups.
[0047] In some embodiments, the concentration of the non-metallic wire-free conductive material, such as the ICP coated particles, non-metallic particles, non-metallic flakes, and / or non-metallic nanoparticles described herein, in the curable coating composition is greater than about 30 wt.%, such as about 39 wt.% to 65 wt.%, based on the total weight of the curable coating composition. In some embodiments, the non-metallic wire-free conductive material, such as the ICP coated particles, non-metallic particles, non-metallic flakes, and / or non-metallic nanoparticles described herein, is uniformly dispersed throughout the curable coating composition of the present disclosure and then formed into a curable coating to provide the exterior protective layer of the present disclosure.
[0048] In other embodiments, the exterior protective layer of the present disclosure includes a first curable coating, a second curable coating, and a non-metallic conductive material, including a non-metallic wire-free conductive material formed into a layer, and the conductive layer is disposed between the first curable coating and the second curable coating. In such embodiments, the non-metallic wire-free conductive material, such as ICP-coated particles, non-metallic particles, non-metallic flakes, and / or non-metallic nanoparticles, is not incorporated into the curable coating composition of the present disclosure, but instead is formed into a conductive layer on the surface of the first curable coating. In some embodiments, a second curable coating is then disposed on the conductive layer formed of the non-metallic wire-free conductive material.
[0049] In some embodiments, at least a third curable coating may be laminated adjacent to the at least one curable coating, while in other embodiments, at least a third curable coating may be laminated adjacent to the first curable coating.
[0050] In some embodiments, the conductive material of the present disclosure comprises a conductive polymer weave. The conductive polymer weave of the present disclosure may be wire-free or may include wires. In some embodiments, the conductive polymer weave of the present disclosure comprises conductive fibers and optionally non-conductive fibers. In some embodiments, the conductive fibers of the conductive polymer weave of the present disclosure comprise non-metallic conductive fibers or metallic fibers. As used herein, "fiber" encompasses a single filament or fibers derived from multiple filaments. As used herein, "filament" refers to a single strand of material. As used herein, "weave" refers to many fibers that are plaited, knitted, braided, or woven to create a textile.
[0051] The fibers may be in the form of tows, bundles, sheets, plies, and combinations thereof. The fibers may use nonwoven, woven, knitted, stitched, wound, and braided configurations. Woven fiber structures may include a plurality of woven tows having less than about 1000 filaments, less than about 3000 filaments, less than about 6000 filaments, less than about 12000 filaments, less than about 24000 filaments, less than about 48000 filaments, less than about 56000 filaments, and less than about 125000 filaments.
[0052] In some embodiments, the conductive fibers include non-metallic conductive fibers, including carbon black, or more typical ICPs. ICPs are also known as "synthetic metals" because they have electrical, magnetic, and optical properties characteristic of metals and semiconductors. In some embodiments, the ICPs of the conductive polymer weaves of the present disclosure are 10 6 Siemens / centimeter (S / cm) ~ 10 7 S / cm, etc., 10 5 S / cm~10 7 They have a high electrical conductivity of 10 ...
[0053] In some embodiments, the conductive polymer fibers are made of ICPs including polyacetylene, polyaniline, polycarbazole, polyfuran, polyheteroarylenevinylene, where the heteroarylene group is thiophene, furan, or pyrrole, as well as polyisothionaphthene, polyparaphenylene, polyparaphenylene sulfide, polyparaphenylenevinylene, polyperinaphthalene, polyphthalocyanine, polypyrrole, polyquinoline, polythiophene, and combinations thereof. Useful ICPs further include blends, copolymers, and derivatives of the aforementioned polymers, for example, where the monomeric components are replaced by side chains or groups. Typically, ICPs used with the conductive polymer weaves of the present disclosure include polypyrrole, polycarbazole, polyaniline, polyacetylene, polythiophene, and combinations thereof.
[0054] In other embodiments, the conductive fibers include metal fibers. In some embodiments, the metal fibers have a density of about 1.0×10 7 S / cm ~ approx. 7.0×10 7 S / cm, 5.98×10 7 S / cm~6.30×10 7 S / cm, etc., 10 5 S / cm~10 7 S / cm, 10 6 S / cm~10 7 The metal fibers may be made of metals or metal alloys including phosphor bronze, aluminum, nickel-coated copper, stainless steel, copper, silver, and nickel. Typically, copper, silver, and / or nickel are used. In some embodiments, the metal fibers include thin metal filaments having diameters ranging from about 1 μm to about 80 μm, which may be made by methods known in the art, such as those described in Meoli et al., 2002, Journal of Textile and Apparel, Technology and Management, 2, p. 12.
[0055] In some embodiments, the non-metallic conductive fibers and / or metallic fibers are composites made by coating non-conductive filaments with carbon black, ICP, metals, alloys thereof, combinations thereof, etc. The coated filaments may then be combined with other extruded filaments to form filament bundles, which may be processed into fibers.
[0056] In some embodiments, the non-conductive filaments coated with non-metallic or metallic conductive materials are non-conductive fiber-forming polymers. Non-conductive fiber-forming polymers may include, for example, cellulose (including cellulose acetate, cellulose triacetate, and viscous cellulose), polyacrylonitrile, polyamides, polyesters, polyolefins, polyurethanes, polyvinyl alcohol, polyvinyl chloride, copolymers thereof, and mixtures containing such polymers. Typical fiber-forming polymers include polyamides and polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polypropylene.
[0057] The filament component of the fiber may be extruded by any spinning process suitable for producing fibers from a particular polymer, including melt spinning, reaction spinning, plasticized melt spinning, adhesion spinning, wet spinning, dispersion spinning, dry spinning, dry jet wet or air gap spinning, emulsion spinning, gel spinning, lattice spinning, reaction spinning, etc. Generally, such spinning processes involve passing a melt or solution of the polymer through multiple holes in a spinneret to produce a liquid polymer stream that solidifies into filaments and ultimately bonds together into a fiber.
[0058] Filaments produced by the spinning process described above may then be coated, for example, with an ICP. Methods of forming coated filaments, such as ICP-coated filaments, are known in the art. See, for example, U.S. Patent No. 6,228,492, which describes the creation of ICP-coated filaments.
[0059] Methods known in the art may be used to apply the metal coating, such as sputtering, vacuum deposition, electroless plating, carbonization, and fiber loading. Such methods can produce highly conductive (10 6 S / cm~10 7 S / cm) can be achieved.
[0060] In some embodiments, the non-metallic and / or metallic conductive fibers described herein are interwoven with non-conductive polymer fibers, for example to form a conductive polymer weave of the present disclosure. In some embodiments, the non-conductive fibers comprise a non-conductive polymer. For example, examples of non-conductive polymers that may be used to form the non-conductive fibers interwoven with the conductive fibers include polyester, polyethylene terephthalate, polyethylene, polyethylene naphthalate, polypropylene, and combinations thereof.
[0061] Conductive and non-conductive fibers can be used to make conductive polymer weaves by a plaiting, knitting, braiding, or interlacing process. When conductive fibers are woven with non-conductive fibers, for example, in a controlled pattern, the resulting fabric contains both conductive and non-conductive regions.
[0062] In some embodiments, the exterior protective layer of the present disclosure includes a first curable coating, a second curable coating, and a conductive material, the conductive material being a conductive layer including a conductive polymer weave. In some embodiments, the conductive layer is disposed between the first curable coating and the second curable coating. In some embodiments, at least a third curable coating may be laminated adjacent to the first curable coating.
[0063] In some embodiments, the exterior protective layer of the present disclosure has a thickness in the range of about 0.075 mm to about 0.5 mm, such as about 0.075 mm to about 0.15 mm, about 0.075 mm to about 0.1 mm.
[0064] In some embodiments, the first and second curable coatings are the same thickness, while in other embodiments, the first and second curable coatings have separate thicknesses ranging from about 0.05 mm to about 0.33 mm, such as from about 0.05 mm to about 0.1 mm, or from about 0.05 mm to about 0.66 mm.
[0065] The electrical conductivity of the exterior protective layer achieved by combining the curable coating composition of the present disclosure with the electrically conductive material described herein may, for example, unexpectedly alleviate the need to use a relatively heavy metal screen. Thus, the exterior protective layer of the present disclosure provides sufficient electrical conductivity for lightning strike protection while still reducing the weight of the exterior protective layer. For example, a weight reduction of about 50-80% may be achieved compared to an exterior protective layer embedded with a metal screen. Furthermore, in some embodiments, the exterior protective layer does not require a finishing layer such as a primer and / or topcoat, thus achieving further weight reduction.
[0066] More specifically, in some embodiments, the weight of the exterior protective layer may be in the range of about 0.02 lbs / sqft to about 0.1 lbs / sqft, such as about 0.02 lbs / sqft to about 0.8 lbs / sqft, about 0.02 lbs / sqft to about 0.04 lbs / sqft.
[0067] An embodiment of an exterior protective layer of the present disclosure is shown in Figure 1. Exterior protective layer 20 includes a first curable coating 22 and a second curable coating 26. As shown, a conductive layer 24 is sandwiched between the first and second curable coatings. The exterior protective layer may then be adhesively disposed on the composite material as described later herein.
[0068] composite material In some embodiments, an exterior protective layer is disposed on a surface of the composite. Typically, the exterior protective layer is disposed on a surface of the composite that is exposed to environmental conditions. Disposition may be accomplished manually or by an automated mechanism (e.g., automated tape layup (ATL), automated fiber placement (AFP)).
[0069] In some embodiments, the composite material is formed of an organic matrix and fibers, such as epoxy resin and carbon fiber reinforced plastic (CFRP). In some embodiments, the composite material is in the form of a prepreg. As used herein, the term "prepreg" refers to one or more sheets or laminae of fibers impregnated with a matrix. The matrix may be present in a partially cured state, for example to exhibit a selected tackiness or degree of adhesion.
[0070] In some embodiments, the prepreg layers are disposed adjacent to one another. In some embodiments, the prepreg layers within a layup may be disposed in a selected orientation relative to one another. For example, a prepreg layup may include prepreg layers having a unidirectional fiber structure with the fibers oriented at 0°, 90°, a selected angle θ, and combinations thereof, relative to the largest dimension of the layup, such as length. It will be further understood that in some embodiments, prepregs having any combination of fiber structures, such as unidirectional and multidirectional, may be combined to form a prepreg layup.
[0071] In some embodiments, the prepreg layup is in a mold and an exterior protective layer is placed on the surface of the composite and co-cured. Co-curing typically incorporates the exterior protective layer into the composite. In some embodiments, co-curing includes baking the exterior protective layer and the composite at a temperature of about 121°C to about 200°C, such as about 121°C to about 130°C.
[0072] In some embodiments, the in-body cure is accomplished by oven curing, such as autoclave, microwave curing, or out of the autoclave curing. As used herein, "out of the autoclave" refers to a process in which a layup of prepregs, including, for example, the exterior protective layers of the present disclosure, is in a closed mold. Vacuum, pressure, and heat are then applied using means known in the art other than an autoclave, such as a resin transfer molding press.
[0073] 2 is a close-up side cross-sectional view of an embodiment of an exterior protective composite structure 40 according to the present disclosure. In this embodiment, the exterior protective layer includes a first curable coating 42, a second curable coating 46, and a conductive layer 44, such as a conductive polymer weave, which is adhesively disposed between the first curable coating 42 and the second curable coating 46. The exterior protective layer is adhesively disposed above a composite layer 48.
[0074] The composite structure of the exterior protection composite structure may form the interior of an aircraft portion, as shown in Figure 3. More specifically, Figure 3 shows a perspective view of an aircraft 70 incorporating an exterior protection composite structure 72. The exterior protection composite structure 72 is incorporated into a portion(s) of the aircraft, such as a body 76, tail section 78, and / or wings 78 of the aircraft 70. The exterior protection composite structure 72 is oriented such that the composite structure of the exterior protection composite structure 72 forms the interior of the airframe 76, with the exterior protection layer 80 being the outermost layer exposed to environmental conditions.
[0075] In some embodiments, an exterior protective layer, such as embodiment 80 shown in FIG. 3, not only acts as a lightning strike protectant, but also mitigates the effects of environmental conditions, e.g., chemicals, or solar radiation, such as ultraviolet radiation (UV). For example, without an exterior protective layer, a surface of a composite structure exposed to environmental conditions may be exposed to chemicals in the environment, e.g., battery acid, which may cause corrosion of the composite structure. In some embodiments, an exterior protective layer of the present disclosure is resistant to such chemicals. For example, in some embodiments, corrosion of a composite structure having an exterior protective layer of the present disclosure is reduced compared to corrosion of a composite structure without an exterior protective layer of the present disclosure.
[0076] Additionally, the composite structure may be degraded by exposure to solar radiation, such as UV radiation. However, in some embodiments, a composite structure having an outer protective layer of the present disclosure has a UV resistance of about 200 nanometers to about 800 nanometers, such as about 200 nanometers to about 400 nanometers.
[0077] In other embodiments, the exterior layer exhibits resistance to chemicals, such as hydraulic jet fuel, that would cause conventional exterior protective layers to soften and subsequently degrade the composite structure, etc. In contrast, in some embodiments, the exterior protective layers of the present disclosure may resist softening after at least 30 days of exposure, at least 2 months of exposure, at least 6 months or more up to about 1 year of exposure, etc.
[0078] Furthermore, in some embodiments, reduced corrosion and deterioration may be achieved without the need for finishes such as undercoats and topcoats. As is known in the art, a base undercoat of finish may be applied to the surface to inhibit corrosion. As is also known in the art, a topcoat finish is further applied to the lightning strike material to further protect the exposed surface from corrosion and deterioration. However, such deterioration can be mitigated by using the exterior protective layer of the present disclosure, which not only allows such additional coatings to be avoided, reducing labor costs, but also reduces the weight of the lightning strike protection agent.
[0079] method In another aspect, the present disclosure relates to a method of forming an exterior protective composite structure. In some embodiments, an exterior protective layer as described herein is disposed on a surface of a composite material, also as described herein. As described herein, the exterior protective layer may be disposed on a composite material surface that is exposed to environmental conditions. The exterior protective layer and the composite material surface may be co-cured to form a cured exterior protective structure, as described.
[0080] In some embodiments, the curing-in-place comprises baking the exterior protection layer and the composite structure at a temperature ranging from about 121° C. to about 200° C., as described herein. Typically, the curing-in-place comprises autoclaving the exterior protection and the composite material. In other embodiments, the curing-in-place is accomplished using an oven, such as a microwave oven, or a process other than an autoclave, as described herein.
[0081] (Predictive) Example The thermosetting compositions used in the curable coatings of the present disclosure are made by reacting a mixture of polyisocyanates and polyols. Specifically, the ingredients are added to a mixing vessel and mixed for approximately 30 minutes at 1000 rpm using a high shear lab mixer. If necessary, a solvent such as MEK is added to the resin to adjust the rheology and solids content of the composition.
[0082] Optionally, an elastomer toughening agent such as Nipol 1472 (Zeon Chemical, Inc.) is then added to the resin along with any flow control agents such as amorphous fumed silica, UV stabilizers BHT and 2-hydroxy-4-methoxy-benzophenone. MEK solvent is added as needed to control viscosity. The composition is then mixed at about 1000-3000 rpm for about 50-70 minutes. The temperature of the composition is typically maintained below about 70°C. The mixture is then typically cooled to a temperature below about 50°C and the curing agent is added. The temperature of the mixture during the addition of the curing agent is maintained below about 55°C.
[0083] The composition is deposited as a film and dried to form a surface coating. A layer of silver nanoparticles is then deposited on the surface of one curable coating, and then a second curable coating is placed on the layer of silver nanoparticles to form an outer protective layer.
[0084] The exterior protective layer is then laid down on, for example, six plies of prepreg, each formed of epoxy resin and carbon fiber reinforced plastic, with the exterior protective layer being the outermost layer. The layup and exterior protective layer are then cured together in an autoclave to incorporate the exterior protective layer into the composition and form a composite test panel.
[0085] Lightning direct impact testing is used to evaluate the performance of composite test panels used in different areas of an aircraft. Lightning testing is performed in accordance with RTCA / DO-160F, "Environmental Conditions and Test Procedures for Airborne Equipment" from the Radio Technical Commission for Aeronautics. Briefly, a surface coating / laminate composite test panel is placed in electrical contact with a current return component. Electrodes are positioned around and adjacent to the center of the test panel. An initiating wire extends from the electrode to the initial lightning strike point on the sample surface.
[0086] Tests are conducted to simulate lightning strikes in aircraft area 1A, the radome, and aircraft area 2A, mostly in the fuselage section. The tests simulate lightning strikes by subjecting the test panel to a high current test waveform. In general, the exterior protection composite structure of the present disclosure exhibits lightning strike protection equivalent to the performance of a control panel having an interwoven wire fabric. Furthermore, the surface damage of the exterior protection composite structure of the present disclosure is very limited.
[0087] Further aspects will be described in the following sections.
[0088] Item 1. An exterior protective layer (20, 80) for protecting a composite structure from environmental conditions, the exterior protective layer (20, 80) comprising at least one curable coating; and an electrically conductive material, wherein the at least one curable coating when cured comprises at least one of polyurethane, polyimide, polyester, or epoxy, the electrically conductive material comprises a wireless conductive material and / or a conductive polymer weave, and the weight of the external protective layer (20, 80) is in the range of about 0.02 pounds per square foot to about 0.1 pounds per square foot.
[0089] Item 2. The outer protective layer (20, 80) according to item 1, wherein at least one curable coating comprises polyurethane when cured.
[0090] Item 3. The outer protective layer (20, 80) according to item 1 or 2, wherein the wire-free conductive material comprises at least one of a nanomaterial or an intrinsically conductive polymer.
[0091] Item 4. The outer protective layer (20, 80) according to any one of items 1 to 3, wherein the conductive polymer weave comprises at least one metal selected from the group consisting of copper, nickel, silver, and combinations thereof, or an intrinsically conductive polymer.
[0092] Item 5. The exterior protective layer (20, 80) according to any one of items 1 to 4, wherein the at least one curable coating comprises at least a first curable coating (42) and a second curable coating (46), the conductive material comprises a conductive polymer weave disposed between the first curable coating (42) and the second curable coating (46), and the first curable coating (42) and the second curable coating (46) separately comprise at least one of polyurethane, polyimide, polyester, or epoxy when cured.
[0093] Item 6. The outer protective layer (20, 80) according to item 5, wherein the first curable coating (42) and the second curable coating (46) comprise polyurethane.
[0094] Item 7. The outer protective layer (20, 80) according to any one of items 1 to 6, wherein the thickness of the outer protective layer (20, 80) is in the range of about 0.075 millimeters to about 0.1 millimeters.
[0095] Item 8. An exterior protective composite structure (40, 72) comprising: a composite structure, the composite structure including a surface that may be exposed to environmental conditions; and an exterior protective layer (20, 80), the exterior protective layer (20, 80) being adhered to the composite structure surface that is exposed to environmental conditions, the exterior protective layer (20, 80) comprising at least one curable coating and a conductive material, the at least one curable coating comprising at least one of polyurethane, polyimide, polyester, or epoxy when cured, the conductive material comprising a wireless conductive material and / or a conductive polymer weave, and a weight of the exterior protective layer (20, 80) ranging from about 0.02 pounds per square foot to about 0.1 pounds per square foot.
[0096] Item 9. The exterior protective composite structure (40, 72) of item 8, wherein the at least one curable coating comprises at least a first curable coating (42) and a second curable coating (46), the conductive material comprises a conductive polymer weave disposed between the first curable coating (42) and the second curable coating (46), and the first curable coating (42) and the second curable coating (46) separately comprise at least one of polyurethane, polyimide, polyester, or epoxy when cured.
[0097] Item 10. The exterior protective composite structure (40, 72) according to items 8 and 9, wherein the conductive polymer weave comprises at least one metal selected from the group consisting of copper, nickel, silver, and combinations thereof.
[0098] Item 11. The exterior protective composite structure (40, 72) according to item 9 or 10, wherein the first curable coating (42) and the second curable coating (46) comprise polyurethane.
[0099] Item 12. The exterior protective composite structure (40, 72) according to any one of items 8 to 11, wherein the exterior protective structure (40, 72) does not include at least one finishing layer selected from at least one of an undercoat and a topcoat.
[0100] Item 13. The exterior protective composite structure (40, 72) according to any one of items 8 to 12, wherein the thickness of the exterior protective layer (20, 80) is in the range of about 0.075 millimeters to about 0.15 millimeters, and the environmental conditions include lightning strikes.
[0101] Item 14. An exterior protective composite structure (40, 72) according to any one of items 8 to 13, wherein the exterior protective layer (20, 80) reduces corrosion of the composite structure compared to corrosion of a composite structure not having an exterior protective layer (20, 80) bonded thereto, the exterior protective layer (20, 80) resists softening by hydraulic jet fuel for at least 30 days, or the exterior protective layer (20, 80) has a UV resistance in the range of about 200 nanometers to about 800 nanometers.
[0102] Item 15. An aircraft (70) part comprising an exterior protective composite structure (40, 72) according to any one of items 8 to 15.
[0103] Item 16. The aircraft (70) portion according to item 15, wherein the aircraft (70) portion is selected from at least one of a body (76), a tail (78), or a wing of the aircraft (70).
[0104] Item 17. A step of disposing an exterior protective layer (20, 80) on a surface of the composite material, the exterior protective layer (20, 80) including at least one curable coating and a conductive material; and a step of co-curing the exterior protective layer (20, 80) and the composite material to form a cured exterior protective structure, the at least one curable coating including at least one of polyurethane, polyimide, polyester, or epoxy when cured, and the conductive material including a wireless conductive material and / or a conductive polymer weave; A method of forming an exterior protective composite structure (40, 72), wherein the exterior protective layer (20, 80) has a weight in the range of about 0.02 pounds per square foot to about 0.1 pounds per square foot, and wherein the exterior protective layer (20, 80) may be exposed to environmental conditions.
[0105] Item 18. The method of item 17, wherein the at least one curable coating comprises at least a first curable coating (42) and a second curable coating (46), and the conductive material comprises a conductive polymer weave disposed between the first curable coating (42) and the second curable coating (46), and the first curable coating (42) and the second curable coating (46) separately comprise at least one of a polyurethane, a polyimide, a polyester, or an epoxy when cured.
[0106] Item 19. The method according to item 17 or 18, wherein the co-curing step includes a step of baking the outer protective layer (20, 80) and the composite material at a temperature in the range of about 121°C to about 200°C.
[0107] Item 20. The method according to any one of items 17 to 19, wherein the co-curing step includes autoclaving the outer protective layer (20, 80) and the composite material. [Explanation of symbols]
[0108] 20 Outer protective layer 22 First hardening coating 24 Conductive layer 26 Second hardening coating 40 External protection composite structure 42 First hardening coating 44 Conductive Layer 46 Second hardening coating 48 Composite layer 70 aircraft 72 External protection composite structure 76 Aircraft 78 Tail and / or Wings 80 Outer protective layer
Claims
1. An exterior protective layer (20, 80) for protecting a composite structure from environmental conditions, said exterior protective layer (20, 80) comprising: At least a first curable coating (42) and a second curable coating (46); and a conductive material. the first curable coating (42) and the second curable coating (46) separately comprise, when cured, at least one of a polyurethane, a polyimide, a polyester, or an epoxy; the conductive material includes a wireless conductive material and / or a conductive polymer weave; the weight of said exterior protective layer (20, 80) is in the range of 0.02 pounds per square foot to 0.1 pounds per square foot; the conductive material includes a conductive polymer weave disposed between the first curable coating (42) and the second curable coating (46); the conductive polymer weave comprises at least one metal selected from the group consisting of copper, nickel, silver, and combinations thereof, or an intrinsically conductive polymer; Outer protective layer (20, 80).
2. The exterior protective layer (20, 80) of claim 1, wherein the at least one curable coating comprises a polyurethane when cured.
3. a composite structure, the composite structure including a surface that may be exposed to environmental conditions; and an exterior protective layer (20, 80) that is adhered to a surface of the composite structure that is exposed to the environmental conditions; The outer protective layer (20, 80) at least a first curable coating (42) and a second curable coating (46); and a conductive material. the first curable coating (42) and the second curable coating (46) separately comprise, when cured, at least one of a polyurethane, a polyimide, a polyester, or an epoxy; the conductive material comprises a wireless conductive material and / or a conductive polymer weave; the weight of said exterior protective layer (20, 80) is in the range of 0.02 pounds per square foot to 0.1 pounds per square foot; the conductive material includes a conductive polymer weave disposed between the first curable coating (42) and the second curable coating (46); the conductive polymer weave comprises at least one metal selected from the group consisting of copper, nickel, silver, and combinations thereof, or an intrinsically conductive polymer; External protection composite structure (40, 72).
4. The exterior protective composite structure (40, 72) of claim 3, wherein the thickness of said exterior protective layer (20, 80) is in the range of 0.075 millimeters to 0.15 millimeters, and said environmental conditions include a lightning strike.
5. the exterior protective layer (20, 80) reduces corrosion of the composite structure compared to corrosion of the composite structure without the exterior protective layer (20, 80) adhered thereto; or, The outer protective layer (20, 80) has a UV resistance in the range of 200 nanometers to 800 nanometers. An exterior protective composite structure (40, 72) according to claim 3 or 4.
6. An aircraft (70) portion comprising an exterior protective composite structure (40, 72) according to any one of claims 3 to 5.
7. Placing an outer protective layer (20, 80) on a surface of the composite material, The outer protective layer (20, 80) is at least a first curable coating (42) and a second curable coating (46); a conductive material; and co-curing said exterior protective layer (20, 80) and said composite material to form a cured exterior protective structure; the first curable coating (42) and the second curable coating (46) separately comprise, when pre-cured, at least one of a polyurethane, a polyimide, a polyester, or an epoxy; the conductive material includes a wireless conductive material and / or a conductive polymer weave; the weight of said exterior protective layer (20, 80) is in the range of 0.02 pounds per square foot to 0.1 pounds per square foot; the conductive material includes a conductive polymer weave disposed between the first curable coating (42) and the second curable coating (46); the conductive polymer weave comprises at least one metal selected from the group consisting of copper, nickel, silver, and combinations thereof, or an intrinsically conductive polymer; The outer protective layer (20, 80) may be exposed to environmental conditions. A method for forming an exterior protective composite structure (40, 72).
Citation Information
Patent Citations
Lightweight lightning protection surface layer, and preparation and application methods thereof
CN107825810A
Multilayer stack with enhanced conductivity and stability
JP2019116089A
Epoxy compositions having improved impact resistance
US20080188609A1
Epoxide resin compositions and method
US4980234A
Preparation of fibers containing intrinsically conductive polymers
US6228492B1