Adhesive Sheet

The adhesive sheet with a thermosetting resin composition ensures high ultraviolet transmittance and adhesion, addressing sensitivity issues in ultraviolet sensors by maintaining sensor performance under varying conditions.

JP7554585B2Active Publication Date: 2024-09-20NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020103206
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-15
Publication Date
2024-09-20
Estimated Expiration
2040-06-15

AI Technical Summary

Technical Problem

Adhesive sheets used to bond glass members can affect the sensitivity of ultraviolet sensors due to their impact on ultraviolet transmittance.

Method used

An adhesive sheet comprising a resin composition with a thermosetting resin, preferably an acrylic resin with an epoxy group, and optionally including an inorganic filler, silane coupling agent, and antioxidant, which achieves a parallel light transmittance of 80% or more at 350 nm wavelength after thermosetting.

Benefits of technology

The adhesive sheet maintains excellent ultraviolet transmittance and adhesion strength while preventing peeling under high temperature and humidity conditions, ensuring the sensitivity of ultraviolet sensors is not compromised.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554585000001
    Figure 0007554585000001
Patent Text Reader

Abstract

To provide an adhesive sheet which is excellent in transmissivity of ultraviolet light after being thermally cured.SOLUTION: An adhesive sheet is provided which comprises resin composition, and in which the resin composition has a thermosetting resin, and parallel line transmissivity of a sheet with a thickness of 20 μm of the resin composition after being thermally cured is 80% or more in light having a wavelength of 350 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive sheet. [Background technology]

[0002] Adhesive sheets containing epoxy resin and acrylic resin are used for bonding glass members together (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-140408 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, when adhering the glass member of the ultraviolet sensor to another member, an adhesive sheet may be used, but depending on the location where the adhesive sheet is used, the adhesive sheet may affect the sensitivity of the ultraviolet sensor. Therefore, there is a demand for an adhesive sheet that has excellent ultraviolet light transmittance.

[0005] Therefore, an object of the present invention is to provide an adhesive sheet that has excellent ultraviolet light transmittance after thermal curing. [Means for solving the problem]

[0006] The adhesive sheet according to the present invention is an adhesive sheet comprising a resin composition, The resin composition comprises a thermosetting resin, After thermal curing, a sheet of the resin composition having a thickness of 20 μm has a parallel ray transmittance of 80% or more for light having a wavelength of 350 nm. Effect of the Invention

[0007] According to the present invention, it is possible to provide an adhesive sheet that has excellent ultraviolet light transmittance after thermal curing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, one embodiment of the adhesive sheet according to the present invention will be described.

[0009] The adhesive sheet according to this embodiment is made of a resin composition. The resin composition comprises an organic component that includes a thermosetting resin. The adhesive sheet according to this embodiment may also include an inorganic component including an inorganic filler. The adhesive sheet according to this embodiment has a single-layer structure made of a resin composition.

[0010] The organic component comprises a thermosetting resin. The organic component may also contain an antioxidant. Furthermore, the organic component may contain a silane coupling agent.

[0011] It is important that the adhesive sheet according to this embodiment has a parallel ray transmittance of 80% or more for light having a wavelength of 350 nm through a 20 μm thick sheet of the resin composition after thermal curing, and it is preferable that the parallel ray transmittance is 91% or more, and more preferably 92% or more. The parallel ray transmittance can be calculated by measuring the total light transmittance and the diffuse transmittance according to the following formula. Parallel light transmittance (%) = Total light transmittance (%) - Diffuse transmittance (%) The total light transmittance and the diffuse transmittance are values ​​measured on a 20 μm-thick sheet sample of the cured resin composition based on JIS K7105 (old; now abolished) (ISO 13468-2:1999), and can be measured as follows. That is, an apparatus is prepared in which an integrating sphere is provided with an entrance opening and an exit opening through which light passes, a sample is placed at the entrance opening, and a reflector is attached to the exit opening, making it possible to direct light into the sample in the thickness direction of the sample and detect all of the light emitted from the sample with the integrating sphere. Next, the reflector at the exit opening is removed, light is incident on the sample in the thickness direction of the sample, and the light emitted from the sample in a direction other than the light traveling direction is detected. Then, the ratio of this detected light intensity to the intensity of the light incident on the sample (incident light intensity) is calculated (detected light intensity / incident light intensity). This ratio (detected light intensity / incident light intensity) is defined as the diffuse transmittance. Also, without removing the reflector at the exit opening, light is incident on the sample in the thickness direction of the sample, and the total light emitted from the sample is detected. Then, the ratio of this detected light intensity to the intensity of the light incident on the sample (incident light intensity) (detected light intensity / incident light intensity) is calculated. This ratio (detected light intensity / incident light intensity) is defined as the total light transmittance. For example, the total light transmittance and the diffuse transmittance can be measured using a V-670DS (manufactured by JASCO Corporation).

[0012] The thermosetting resin preferably contains an acrylic resin having an epoxy group. The organic component preferably contains the acrylic resin in an amount of 90 to 100% by mass, and more preferably 95 to 100% by mass. The adhesive sheet according to this embodiment has excellent ultraviolet transmittance after thermal curing because the organic component contains 90% by mass or more of the acrylic resin. Furthermore, in the adhesive sheet according to this embodiment, since the acrylic resin has an epoxy group, the acrylic resins can undergo a curing reaction at the epoxy groups when heated, and as a result, the adhesive sheet can function as an adhesive sheet.

[0013] Furthermore, since the adhesive sheet according to this embodiment has an epoxy group in the acrylic resin, it can function as an adhesive sheet even without substantially containing a curing agent having an aromatic ring (e.g., a phenolic resin, an epoxy resin having an aromatic ring, etc.). The aromatic ring reduces the transmittance of ultraviolet light, and for this reason too, the adhesive sheet according to this embodiment has excellent transmittance of ultraviolet light after thermal curing. The adhesive sheet according to this embodiment preferably does not substantially contain a curing agent having an aromatic ring.

[0014] The acrylic resin preferably contains, as a structural unit, a monomer having an epoxy group. Examples of the monomer having an epoxy group include (meth)acrylic esters having an epoxy group. An example of the (meth)acrylic acid ester having an epoxy group is glycidyl (meth)acrylate.

[0015] The epoxy equivalent of the acrylic resin is preferably 300-1,500, and more preferably 300-1,100. In the adhesive sheet according to this embodiment, the acrylic resin has an epoxy equivalent of 1500 or less, and therefore the adhesive strength can be increased. Furthermore, the adhesive sheet according to this embodiment has good storage stability before curing because the acrylic resin has an epoxy equivalent of at least 300. Specifically, the adhesive sheet according to this embodiment can suppress changes in properties due to reaction of epoxy groups before curing because the acrylic resin has an epoxy equivalent of at least 300. Here, if the resin composition becomes too hard upon curing, stress will be applied locally to the adhesive sheet under high temperature and high humidity conditions, and the adhesive sheet may peel off from the adherend. However, in the adhesive sheet according to this embodiment, the acrylic resin has an epoxy equivalent of 300 or more, which prevents the resin composition from becoming too hard upon curing, and as a result, can prevent the resin composition from peeling off from the adherend.

[0016] The epoxy equivalent in the acrylic resin means "the mass of the acrylic resin containing one equivalent of an epoxy group." The epoxy equivalent in the acrylic resin can be determined from the content ratio of each monomer having an epoxy group contained in the acrylic resin. For example, when the only monomer having an epoxy group among the monomers constituting the acrylic resin is glycidyl methacrylate (GMA) (molecular weight: 142, number of epoxy groups in one molecule: 1), and the content of glycidyl methacrylate (GMA) in the acrylic resin is 42 mass%, the epoxy equivalent in the acrylic resin can be calculated as follows. 142 / 1 / (42 mass% ÷ 100 mass%) = 338

[0017] The acrylic resin contains a monomer having an epoxy group in an amount of preferably 10 to 50% by mass, and more preferably 16 to 40% by mass. The adhesive sheet according to this embodiment can enhance adhesive strength by containing 10% by mass or more of a monomer having an epoxy group in the acrylic resin. In addition, the adhesive sheet according to the present embodiment has good pre-curing storage stability because the acrylic resin contains 50% by mass or less of a monomer having an epoxy group. Specifically, the adhesive sheet according to the present embodiment has an acrylic resin containing 50% by mass or less of a monomer having an epoxy group, which can suppress changes in properties due to reaction of the epoxy group before curing. Here, if the resin composition becomes too hard upon curing, stress will be applied locally to the adhesive sheet under high temperature and high humidity conditions, and the adhesive sheet may peel off from the adherend. However, in the adhesive sheet of this embodiment, the acrylic resin contains 50% by mass or less of a monomer having an epoxy group, which prevents the resin composition from becoming too hard upon curing, and as a result, can prevent the resin composition from peeling off from the adherend.

[0018] Examples of the structural unit contained in the acrylic resin other than the monomer having an epoxy group include a hydrocarbon group-containing (meth)acrylic acid ester, a carboxy group-containing monomer, an acid anhydride monomer, a hydroxy group-containing monomer, a sulfonic acid group-containing monomer, a phosphoric acid group-containing monomer, etc. In addition, acrylamide, acrylonitrile, etc. are also included.

[0019] Examples of the hydrocarbon group-containing (meth)acrylic acid ester include (meth)acrylic acid alkyl esters, (meth)acrylic acid cycloalkyl esters, and (meth)acrylic acid aryl esters. Examples of the "alkyl" in the above (meth)acrylic acid alkyl ester include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, pentyl, isopentyl, hexyl, heptyl, octyl, 2-ethylhexyl, isooctyl, nonyl, decyl, isodecyl, undecyl, dodecyl (lauryl), tridecyl, tetradecyl, hexadecyl, octadecyl, and eicosyl. Examples of the "cycloalkyl" in the above (meth)acrylic acid cycloalkyl ester include cyclopentyl, cyclohexyl, and the like. Examples of the "aryl" in the above (meth)acrylic acid aryl ester include phenyl and benzyl.

[0020] Examples of the carboxy group-containing monomer include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid.

[0021] Examples of the acid anhydride monomer include maleic anhydride and itaconic anhydride.

[0022] Examples of the hydroxy group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0023] Examples of the sulfonic acid group-containing monomer include styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.

[0024] The above-mentioned phosphate group-containing monomer includes, for example, 2-hydroxyethyl acryloyl phosphate.

[0025] The structural unit other than the monomer having an epoxy group contained in the acrylic resin may be of only one type, or may be of two or more types.

[0026] As a structural unit other than the monomer having an epoxy group contained in the acrylic resin, ethyl (meth)acrylate and butyl (meth)acrylate are preferred from the viewpoint of making it easy to adjust the tackiness of the adhesive sheet and from the viewpoint of providing the adhesive sheet with excellent ultraviolet light transmittance after thermal curing.

[0027] The acrylic resin is preferably an aliphatic resin.

[0028] In this specification, the term "(meth)acrylic acid" is a concept including acrylic acid and methacrylic acid. Moreover, the term "(meth)acrylate" is a concept that includes acrylate and methacrylate.

[0029] The mass average molecular weight of the acrylic resin is preferably 2.0×10 3 ~2.9×10 5 , more preferably 1.0×10 4 ~2.0×10 5 It is. The adhesive sheet according to the present embodiment has a mass average molecular weight of 2.0×10 3 ~2.9×10 5 This provides the advantage of excellent wettability and adhesiveness. In addition, the adhesive sheet according to the present embodiment has a mass average molecular weight of 2.0×10 3 ~2.9×10 5 This has the advantage that when the adhesive is attached to the adherend by embedding it therein (for example, when the adhesive is attached to the adherend by embedding it in a recess of an adherend having a recess on its surface), the adhesive can be sufficiently embedded in the adherend (hereinafter, also referred to as having "excellent embeddability"). The mass average molecular weight is measured by gel permeation chromatography (GPC) and converted into polystyrene equivalent. For example, the mass average molecular weight was measured using a Tosoh Corporation GPC "HLC-8320GPC" as the apparatus and a Tosoh Corporation column "TSK guardcolumn H HR (S)" and the Tosoh column "TSK GMH HR -H(S)" and the Tosoh Corporation column "TSK GMH HR The polystyrene equivalent value can be calculated from the results of GPC measurement using a total of three columns connected in series, a "TSK gel SuperH-RC" as the reference column, tetrahydrofuran as the eluent, and a column temperature of 40°C and a flow rate of 0.5 ml / min.

[0030] From the viewpoint of storage stability and ultraviolet light transmittance after thermal curing, the thermosetting resin has a mass average molecular weight of 2×10 3 It is preferable that the material is substantially free of the following: The thermosetting resin has a mass average molecular weight of 2×10 3Whether or not the following substances are substantially not contained can be confirmed by the same measuring method as that for measuring the mass average molecular weight.

[0031] When the resin composition contains an inorganic filler, it preferably contains a silane coupling agent, from the viewpoint of increasing the wettability of the inorganic filler and, as a result, increasing the adhesiveness.

[0032] The silane coupling agent may, for example, be a silane coupling agent having an epoxy group. As the silane coupling agent, a silane coupling agent having an epoxy group is preferable from the viewpoint of excellent affinity with an acrylic resin having an epoxy group. Examples of the silane coupling agent having an epoxy group include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (e.g., "KBM-303" manufactured by Shin-Etsu Silicones), 3-glycidoxypropylmethyldimethoxysilane (e.g., "KBM-402" manufactured by Shin-Etsu Silicones), 3-glycidoxypropyltrimethoxysilane (e.g., "KBM-403" manufactured by Shin-Etsu Silicones), 3-glycidoxypropylmethyldiethoxysilane (e.g., "KBE-402" manufactured by Shin-Etsu Silicones), and 3-glycidoxypropyltriethoxysilane (e.g., "KBE-403" manufactured by Shin-Etsu Silicones).

[0033] When the resin composition contains an inorganic filler, it contains a silane coupling agent in an amount of preferably 0.1 to 5.0% by mass, more preferably 0.2 to 4.0% by mass. When the resin composition contains 0.1% by mass or more of a silane coupling agent, the wettability of the inorganic filler is increased, and as a result, the adhesiveness is improved. Furthermore, by containing 5.0% by mass or less of a silane coupling agent, the resin composition can contain a large amount of acrylic resin, and as a result, the transmittance of ultraviolet light after thermal curing is further improved.

[0034] From the viewpoint of suppressing a decrease in the ultraviolet light transmittance of the adhesive sheet according to this embodiment after thermal curing due to oxidation of the acrylic resin, it is preferable that the adhesive sheet according to this embodiment contains an antioxidant.

[0035] Examples of the antioxidant include hindered phenol-based antioxidants and phosphorus-based antioxidants.

[0036] The resin composition contains an antioxidant in an amount of preferably 0.1 to 5% by mass, and more preferably 0.1 to 2% by mass. By containing 0.1% by mass or more of an antioxidant, the resin composition can suppress the generation of carbon-carbon double bonds in the acrylic resin due to oxidation of the acrylic resin, and as a result, can suppress a decrease in ultraviolet transmittance. Furthermore, by containing 5 mass % or less of an antioxidant, the resin composition can contain a large amount of acrylic resin, which results in even better ultraviolet transmittance after thermal curing and suppresses a decrease in ultraviolet transmittance caused by the antioxidant itself.

[0037] The adhesive sheet according to the present embodiment preferably contains an inorganic filler, from the viewpoint that the reactivity of the epoxy groups of the acrylic resin can be increased by the functional groups of the inorganic filler.

[0038] Examples of the inorganic filler include silica particles, boron nitride particles, and alumina particles.

[0039] From the viewpoints of workability, adhesion, and reliability, the resin composition contains an inorganic filler in an amount of preferably 15 to 60% by mass, and more preferably 20 to 50% by mass.

[0040] In the resin composition, from the viewpoints of workability, adhesion, and reliability, the inorganic filler preferably has a D50 of 5 to 30 nm, and more preferably 5 to 20 nm. The D50 of an inorganic filler means the particle diameter (D50) at which the cumulative value of the bubble volume is 50% in a cumulative frequency distribution curve of volumetric particle diameters plotted with the horizontal axis representing particle diameter and the vertical axis representing bubble volume. The D50 of the inorganic filler can be measured using a laser diffraction particle size distribution measuring device.

[0041] The adhesive sheet according to this embodiment has a thickness of preferably 5 to 200 μm, and more preferably 5 to 180 μm.

[0042] From the viewpoint of suppressing adhesion and facilitating contact with the adherend (from the viewpoint of workability), the adhesive sheet according to this embodiment has a tensile storage modulus at 25°C before thermal curing of preferably 10 MPa to 3,000 MPa, more preferably 20 MPa to 2,000 MPa, and even more preferably 30 MPa to 1,500 MPa.

[0043] From the viewpoint of improving adhesiveness after heat curing, the adhesive sheet according to this embodiment has a tensile loss modulus at 120° C. after heat curing of preferably 0.1 MPa to 5 MPa, more preferably 0.2 MPa to 4 MPa, and even more preferably 0.3 MPa to 3 MPa.

[0044] From the viewpoint of improving adhesiveness after heat curing, the adhesive sheet according to this embodiment has a tensile storage modulus at 250° C. after heat curing of preferably 0.5 MPa to 150 MPa, more preferably 1 MPa to 100 MPa, and even more preferably 10 MPa to 90 MPa.

[0045] The tensile storage modulus and the tensile loss modulus can be determined as follows. That is, the adhesive sheet is heat-cured, and a test piece (length: 40 mm, width: 10 mm) is cut out from the heat-cured adhesive sheet. Then, a dynamic viscoelasticity measuring device (product name "RSA-III, manufactured by TA Instruments) is used to perform a tensile test on the measurement object, and the tensile storage modulus and tensile loss modulus are measured. The conditions for this tensile test are as follows: Measurement mode: Tensile mode Initial chuck distance: 22.5mm Measurement temperature range: 0℃ to 150℃ Heating rate: 10℃ / min Dynamic strain: ±0.5μm Frequency: 10Hz In addition, in this embodiment, "after heat curing" means "after the adhesive sheet is heated until it is sufficiently cured." The heating temperature is, for example, 175°C.

[0046] The adhesive sheet according to this embodiment has a shear storage modulus at 100° C. before thermal curing of preferably 5 kPa to 800 kPa, more preferably 6 kPa to 600 kPa, and even more preferably 7 kPa to 400 kPa. The adhesive sheet according to this embodiment has the advantage of excellent wettability and embeddability because the shear storage modulus at 100° C. before thermal curing is within the above range.

[0047] The shear storage modulus can be determined as follows. That is, the adhesive sheet is punched out to prepare a cylindrical sample (Φ7.5 mm×1 mm). Then, a shear vibration having a frequency of 1 Hz is applied to one circular surface of the sample at a temperature of 120° C., and the shear vibration transmitted to the other circular surface is measured and analyzed to determine the shear storage modulus. For the measurement of shear vibration and the analysis of the measured values, for example, a viscoelasticity measuring device (manufactured by HAAKE, model: Mars series) can be used.

[0048] From the viewpoint of improving adhesiveness after thermal curing, the adhesive sheet according to this embodiment preferably has an adhesive strength to a Si wafer at 120° C. after thermal curing of 0.5 MPa or more, more preferably 0.8 MPa or more.

[0049] The adhesive strength can be determined as follows. First, a dicing tape having an adhesive layer and a base layer laminated thereon is placed with the adhesive layer facing up. Next, an adhesive sheet is laminated on the adhesive layer of the dicing tape, and then a Si wafer (for example, a bare wafer can be used as the Si wafer) (thickness: 500 μm) is placed on the adhesive sheet. The adhesive sheet and the Si wafer are laminated by heating at 60°C to obtain a Si wafer with an adhesive sheet. Then, a dicing device is used to obtain a 5 mm x 5 mm Si chip with an adhesive sheet from the Si wafer with the adhesive sheet. Next, the Si chip with the adhesive sheet is bonded to a Si wafer (for example, a bare wafer can be used as the Si wafer) (thickness: 500 μm) with the adhesive sheet side at a temperature of 150° C. for 2 seconds per 500 g of adhesive sheet (for example, 4 seconds if the adhesive sheet is 1000 g), and the adhesive sheet is sufficiently cured by heating (150° C., 1 hour) to obtain a measurement sample. Then, the adhesive strength is measured by a bond strength test using shear at 120° C. In the bond strength test, for example, Dega4000 can be used.

[0050] The resin composition has a ratio (AbC6H6 / AbCO) of the absorbance AbC6H6 attributable to aromatic rings to the absorbance AbCO attributable to carbonyl groups, as measured by Fourier transform infrared absorption spectroscopy (FT-IR), of preferably 0.05 or less, more preferably 0.04 or less, and even more preferably 0.03 or less. The aromatic ring reduces the transmittance of ultraviolet light. Since the resin composition of the adhesive sheet according to the present embodiment has an AbC6H6 / AbCO ratio of 0.05 or less, the adhesive sheet has excellent transmittance of ultraviolet light after thermal curing. Furthermore, AbC6H6 / AbCO is usually 0.01 or more.

[0051] The AbC6H6 / AbCO ratio can be calculated as follows. First, the infrared absorption spectrum of the resin composition is measured by Fourier transform infrared absorption spectrometry (FT-IR). The measurement conditions are as follows. Reflection method (ATR method) Wave number: 500~4000cm -1 Number of times: 32 As a measuring device, a "NICOLET380 FT-R" manufactured by Thermo Fisher Scientific can be used. From the infrared absorption spectrum obtained, 1506 cm -1 Measurement points at 1522 cm -1 1506-1522 cm when the line connecting the measurement points at is used as the baseline -1 The absorbance at the highest point of the peak in this wavenumber range is read and this absorbance is designated as AbC6H6. In addition, from the obtained infrared absorption spectrum, 1650 cm -1 Measurement points at 1800cm -1 The line connecting the measurement points at 1650 to 1800 cm is used as the baseline. -1 The absorbance at the highest point of the peak in the wavenumber range is read and this absorbance is designated as AbCO.

[0052] The adhesive sheet according to this embodiment is particularly suitable for use when the material of the adherend is glass or Si.

[0053] The adhesive sheet of this embodiment can be used as a component of an ultraviolet sensor. An example of an ultraviolet sensor in which the adhesive sheet of the present embodiment can be used is as follows. The ultraviolet sensor of this embodiment includes a light receiving section having a light receiving surface that receives ultraviolet (UV) rays, and a cover sheet that directly or indirectly covers the light receiving section. The cover sheet has a laminated structure of at least two layers: a cover sheet body made of a glass plate or the like, and an adhesive layer made of the adhesive sheet of this embodiment. The ultraviolet sensor of this embodiment is configured to detect ultraviolet light by allowing the ultraviolet light to reach the light receiving portion through the adhesive layer. The adhesive layer may be used to adhere the cover sheet body to the light-receiving surface or to an area outside the light-receiving section so that the cover sheet directly covers the light-receiving section, or it may be used to adhere the cover sheet to a support member that supports the cover sheet at a distance from the light-receiving surface so that the cover sheet indirectly covers the light-receiving section by leaving a space between the cover sheet and a support member that supports the cover sheet at a distance from the light-receiving surface.

[0054] The matters disclosed in this specification include the following.

[0055] (1) An adhesive sheet comprising a resin composition, The resin composition comprises a thermosetting resin, an adhesive sheet, the parallel ray transmittance of a 20 μm-thick sheet of the resin composition after thermal curing is 80% or more for light with a wavelength of 350 nm.

[0056] (2) The adhesive sheet according to (1) above, which has a tensile storage modulus at 25° C. before thermal curing of 10 MPa to 3,000 MPa.

[0057] (3) The adhesive sheet according to (1) or (2) above, which has a shear storage modulus at 100° C. before thermal curing of 5 kPa to 800 kPa.

[0058] (4) The adhesive sheet according to any one of (1) to (3) above, wherein the resin composition after thermal curing has an adhesive strength to a Si wafer at 120° C. of 0.5 MPa or more.

[0059] (5) The adhesive sheet according to any one of (1) to (4) above, which has a tensile loss modulus at 120° C. after thermal curing of 0.1 MPa to 5 MPa.

[0060] (6) The adhesive sheet according to any one of (1) to (5) above, which has a tensile storage modulus at 250° C. after thermal curing of 0.5 MPa to 150 MPa.

[0061] The adhesive sheet according to the present invention is not limited to the above-mentioned embodiment. The adhesive sheet according to the present invention is also not limited by the above-mentioned action and effect. Furthermore, the adhesive sheet according to the present invention can be modified in various ways without departing from the gist of the present invention.

[0062] For example, the adhesive sheet according to this embodiment has a single-layer structure made of a resin composition, but the adhesive sheet according to the present invention may be a laminate of a layer made of the resin composition and another layer. EXAMPLES

[0063] Next, the present invention will be described more specifically with reference to examples and comparative examples. The following examples are intended to further illustrate the present invention and are not intended to limit the scope of the invention.

[0064] Example 1 An adhesive composition solution A (solid content: 20% by mass) was prepared by dissolving an acrylic resin, an inorganic filler, a silane coupling agent, and an antioxidant in a solvent in the blending ratio shown in Table 1 below. The acrylic resin, inorganic filler, silane coupling agent, and antioxidant used were as follows. Acrylic resin: An acrylic resin containing 42% by mass of glycidyl methacrylate (GMA), 50% by mass of ethyl acrylate (EA), and 8% by mass of butyl methacrylate (BMA) as structural units (mass average molecular weight: 240,000) Inorganic filler: Silica particles (MEK-ST-40, manufactured by Nissan Chemical Industries, Ltd.) Silane coupling agent: 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (KBM303, Shin-Etsu Silicone Co., Ltd.) Antioxidant: Hindered phenol-based antioxidant (Irganox 1010, manufactured by BASF Japan) Solvent: Methyl ethyl ketone In addition, a polyethylene terephthalate film (thickness: 50 μm) that had been treated with silicone for release properties was prepared as a separator. The adhesive composition solution A was then applied to the surface of the separator (the surface that had been subjected to the release treatment) and dried by heating at 130°C for 2 minutes, thereby producing an adhesive sheet (thickness: 20 µm) on the separator.

[0065] Example 2 An adhesive composition solution B (solid content concentration: 20 mass %) was prepared by dissolving an acrylic resin, an inorganic filler, a silane coupling agent, and an antioxidant in a solvent in the blending ratio shown in Table 1 below. The materials used were the same as those used in Example 1 except for the materials described below. Acrylic resin: Acrylic resin containing 14% by mass of glycidyl methacrylate (GMA), 50% by mass of ethyl acrylate (EA), and 36% by mass of butyl methacrylate (BMA) as structural units (mass average molecular weight: 20,000) Inorganic filler: Silica particles (MEK-EC-2130Y, manufactured by Nissan Chemical Industries, Ltd.) Then, an adhesive sheet (thickness: 20 μm) was produced on a separator in the same manner as in Example 1, except that adhesive composition solution B was used instead of adhesive composition solution A.

[0066] Example 3 An adhesive composition solution C (solid content: 20% by mass) was prepared by dissolving an acrylic resin, an inorganic filler, a silane coupling agent, and an antioxidant in a solvent in the blending ratio shown in Table 1 below. The materials used were the same as those used in Example 1 except for the materials described below. Acrylic resin: Acrylic resin containing 30% by mass of glycidyl methacrylate (GMA), 42% by mass of ethyl acrylate (EA), and 28% by mass of butyl methacrylate (BMA) as structural units (mass average molecular weight: 100,000) Inorganic filler: Silica particles (CHO-ST-M, Nissan Chemical) Then, an adhesive sheet (thickness: 20 μm) was produced on a separator in the same manner as in Example 1, except that adhesive composition solution C was used instead of adhesive composition solution A.

[0067] Comparative Example 1 An adhesive composition solution D (solid content: 20% by mass) was prepared by dissolving an acrylic resin, a phenolic resin as a curing agent, an inorganic filler, a silane coupling agent, and an antioxidant in a solvent in the blending ratio shown in Table 1 below. The materials used were the same as those used in Example 1 except for the materials described below. Acrylic resin: An acrylic resin containing 12% by mass of glycidyl methacrylate (GMA), 52% by mass of ethyl acrylate (EA), and 36% by mass of butyl methacrylate (BMA) as structural units (mass average molecular weight: 300,000) Phenolic resin: MEHC-7800H, manufactured by Meiwa Kasei Co., Ltd. Inorganic filler: Silica particles (SC25R, manufactured by Admatechs Co., Ltd.) Then, an adhesive sheet (thickness: 20 μm) was produced on a separator in the same manner as in Example 1, except that adhesive composition solution D was used instead of adhesive composition solution A.

[0068] Comparative Example 2 An adhesive composition solution E (solid content: 20% by mass) was prepared by dissolving an acrylic resin, a phenolic resin as a curing agent, an epoxy resin as a curing agent, and an inorganic filler in a solvent in the blending ratio shown in Table 1 below. The materials used were the same as those used in Example 1 except for the materials described below. Acrylic resin: An acrylic resin containing 12% by mass of glycidyl methacrylate (GMA), 52% by mass of ethyl acrylate (EA), and 36% by mass of butyl methacrylate (BMA) as structural units (mass average molecular weight: 300,000) Phenolic resin: MEHC-7800H, manufactured by Meiwa Kasei Co., Ltd. Epoxy resin: HP-7200, manufactured by DIC Inorganic filler: Silica particles (MEK-ST-ZL, manufactured by Nissan Chemical Industries, Ltd.) Then, an adhesive sheet (thickness: 20 μm) was produced on a separator in the same manner as in Example 1, except that adhesive composition solution E was used instead of adhesive composition solution A.

[0069] The mass average molecular weight of the acrylic resin was determined by the method described above.

[0070] "Average particle size of inorganic filler," "Parallel beam transmittance (350 nm) after heat curing," "Tensile storage modulus at 25°C before heat curing," "Shear storage modulus at 100°C before heat curing," "Adhesion strength to Si wafer at 120°C after heat curing," "Tensile loss modulus at 120°C after heat curing," "Tensile storage modulus at 250°C after heat curing," "AbCO," "AbC6H6," and "AbC6H6 / AbCO" were determined by the method described above. These values ​​are shown in Table 1 below.

[0071] <Embeddability test before heat curing> The adhesive sheet was attached to one side of a glass plate. Next, a glass plate with an adhesive sheet was bonded to the substrate having concave and convex portions on its surface. Then, in order to confirm the embedding property of the adhesive sheet in the recesses of the substrate, the adhesive sheet was photographed with a microscope from the glass plate side (within a 10 mm square area) to obtain an image. Next, this image was binarized using analysis software to determine the ratio of the total area of ​​the parts where the adhesive sheet was embedded in the recesses to the total area of ​​the recesses ((total area of ​​the parts where the adhesive sheet was embedded in the recesses / total area of ​​the recesses) x 100) (%), and evaluated according to the following criteria. 〇: 80% or more ×: Less than 80% The results are shown in Table 1 below.

[0072] <Tear test using TCT after heat curing> The adhesive sheet was attached to a mirror chip (9.5 mm square) at 60°C. Next, the adhesive sheet with the mirror chip attached was bonded to a glass plate with the adhesive sheet side on the condition of a temperature of 120° C., a pressure of 0.1 MPa, and a time of 2 seconds to obtain a sample. The sample was then heat-treated in a pressure oven at 150°C and 0.7 MPa for 1 hour. Thereafter, the heat-treated sample was subjected to repeated heating and cooling between −40° C. and 125° C. 1000 times (1 cycle: 30 minutes) using a TCT device (temperature cycle test device). Next, it was visually confirmed whether the adhesive sheet had peeled off from the mirror chip. And the evaluation was carried out according to the following criteria. ○: No peeling ×: Peeling occurred The results are shown in Table 1 below.

[0073] <Peeling test during reflow after thermal curing> The adhesive sheet was attached to a mirror chip (9.5 mm square) at 60°C. Next, the adhesive sheet with the mirror chip attached was bonded to a glass plate with the adhesive sheet side on the condition of a temperature of 120° C., a pressure of 0.1 MPa, and a time of 2 seconds to obtain a sample. The sample was then heat-treated in a pressure oven at 150°C and 0.7 MPa for 1 hour. Thereafter, the heat-treated sample was placed under conditions of a temperature of 30° C. and a humidity of 60% RH for 72 hours to allow the sample to absorb moisture. The moisture-absorbed sample was then passed through an IR reflow furnace set to maintain a temperature of 260° C. or higher for 10 seconds. Thereafter, the above test was carried out on nine samples for each of the examples and comparative examples, and each sample was visually inspected to see whether the adhesive sheet had peeled off from the mirror chip, and the number of samples for which peeling had occurred was counted. The results are shown in Table 1 below.

[0074] [Table 1]

Claims

1. An adhesive sheet comprising a resin composition, The resin composition has a thermosetting resin and an inorganic filler, the thermosetting resin includes an acrylic resin having an epoxy group, The content of the inorganic filler is 15 to 50 mass %, The inorganic filler has a D50 of 5 to 30 nm; The parallel ray transmittance of a 20 μm-thick sheet of the resin composition after thermal curing is 80% or more for light having a wavelength of 350 nm; An adhesive sheet having a tensile storage modulus at 25°C before heat curing of 10 MPa to 3,000 MPa.

2. 2. The adhesive sheet according to claim 1, which has a shear storage modulus at 100° C. before thermal curing of 5 kPa to 800 kPa.

3. 3. The adhesive sheet according to claim 1, wherein the resin composition after thermal curing has an adhesive strength to a Si wafer of 0.5 MPa or more at 120°C.

4. 4. The adhesive sheet according to claim 1, which has a tensile loss modulus at 120° C. after heat curing of 0.1 MPa to 5 MPa.

5. 5. The adhesive sheet according to claim 1, having a tensile storage modulus at 250° C. after thermal curing of 0.5 MPa to 150 MPa.

Citation Information

Patent Citations

  • Adhesive composition for electronic device, adhesive sheet for electronic device, and electronic component and device using the same

    JP2008063551A

  • Adhesive resin composition and adhesive sheet

    JP2011127073A

  • Curable resin composition for forming adhesive layer and method for integrating substrate and substrate to be adhered

    JP2015134841A

  • Adhesive composition, electronic member using the adhesive composition and manufacturing method of semiconductor device

    JP2015140408A

  • Glue film

    JP2017137453A