Molded body and its manufacturing method
Patent Information
- Application Number
- JP2020145636
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Existing adhesive methods for reinforcing fibers in rubber products, such as those using RFL, resorcinol-formaldehyde resin, and isocyanate compounds, suffer from inferior adhesive properties, require high-temperature treatments that can degrade fibers, and may lead to decreased adhesion due to oil agents, posing health and environmental risks.
A molded article containing rubber and rubber reinforcing fibers with an adhesive component comprising a polymer with reactive carbon-carbon double or triple bonds and a plasticizer, having a specific swelling degree, which enhances adhesion without formaldehyde and resorcinol, allowing for improved bonding at lower temperatures.
The solution provides excellent adhesiveness between rubber reinforcing fibers and rubber, improving durability and manufacturing efficiency by preventing fiber deterioration and maintaining adhesive strength, while eliminating health hazards associated with formaldehyde and resorcinol.
Smart Images

Figure 0007554608000002 
Figure 0007554608000003 
Figure 0007554608000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a molded article containing rubber reinforcing fibers and rubber, and a method for producing the same. [Background technology]
[0002] In general, industrial rubber products such as tires, conveyor belts, and hoses (e.g., automotive oil brake hoses) are reinforced with synthetic fibers such as vinylon and rayon, or natural fibers such as cotton. In these products, in order to fully utilize the excellent physical properties of rubber (e.g., high strength and high elastic modulus), it is necessary to firmly bond the fiber and rubber. Conventionally, a method using an adhesive called RFL, whose main components are resorcinol-formaldehyde resin and rubber latex, has been widely known as such a method (Patent Documents 1 and 2).
[0003] However, since formaldehyde is suspected of being carcinogenic and resorcinol is suspected of being an environmental hormone, the development of alternative materials is desired. Specifically, Patent Document 3 proposes a technique using an adhesive containing an adhesive compound having an unsaturated carbon bond and an epoxy group that reacts with a vulcanizing agent used in vulcanization of rubber. Patent Document 4 proposes an adhesion method using an adhesive composition for organic fiber cords that contains a (blocked) isocyanate compound and / or an amine-based curing agent (A), an epoxy compound (B), and a rubber latex (C) and does not contain resorcinol or formaldehyde. Furthermore, Patent Document 5 proposes an adhesion technique using an adhesive component that contains a modified conjugated diene rubber that has a hydrogen-bonding functional group in a part of the conjugated diene rubber. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 54-4976 [Patent Document 2] Japanese Patent Application Publication No. 58-2370 [Patent Document 3] JP 2011-111563 A [Patent Document 4] International Publication No. 2010 / 125992 [Patent Document 5] International Publication No. 2019 / 230700 Summary of the Invention [Problem to be solved by the invention]
[0005] The method using an adhesive described in Patent Document 3 had significantly inferior adhesion compared to the conventional method using RFL. Also, the addition of blocked isocyanate to improve adhesion is described, but in this case, a high-temperature and / or long-term heat treatment is required to polymerize the blocked isocyanate on the coated fiber, which may cause deterioration of the coated fiber. Furthermore, the method using the adhesive described in Patent Document 4 has adhesive strength equal to or greater than that of the conventional method using RFL, but after forming an adhesive layer on the surface of the organic fiber cord, it is necessary to heat treat the cord at substantially high temperatures (180°C and 240°C).When carrying out such treatment, if organic fibers such as PVA-based fibers or PET-based fibers are used as reinforcing fibers, there is a risk that the performance of the reinforcing fibers will decrease due to degradation. Furthermore, Patent Document 5 describes a method of improving handleability by mixing an oil agent into a high-viscosity adhesive component. However, in reality, depending on the type, mixing ratio, and applied amount of the oil agent, there is a risk that the adhesive strength of the reinforcing fiber to the rubber will decrease. Therefore, there was a need for a bonding method that would not cause degradation of general-purpose fibers while providing adhesive strength equivalent to that of conventional RFL methods.
[0006] The present invention has been made in consideration of the above-mentioned problems in the prior art, and an object of the present invention is to provide a molded article having excellent adhesion between rubber reinforcing fibers and rubber, and a method for producing the same. [Means for solving the problem]
[0007] As a result of investigating the above-mentioned problems, the inventors found that by using a rubber reinforcing fiber having, on at least a part of the fiber surface, an adhesive component containing a specific polymer and a plasticizer whose swelling degree in rubber is equal to or greater than a specific value, a molded article having excellent adhesion between the rubber reinforcing fiber and rubber can be obtained. Based on this finding, the inventors conducted further investigations and have now completed the present invention.
[0008] That is, the present invention provides the following [1] to
[14] . [1] A molded article comprising rubber and rubber reinforcing fibers having an adhesive component on at least a portion of the fiber surface, wherein the adhesive component comprises a polymer having at least one type of multiple bond selected from a reactive carbon-carbon double bond and a reactive carbon-carbon triple bond in the molecule, and a plasticizer having a swelling degree of 5.0% or more with respect to the rubber, as calculated by the following formula (1): (Swelling degree relative to the rubber) (%) = (MM") / M" x 100 (1) (Wherein, M is the volume of 1.1 cm 3 is the mass (g) of a rubber piece after it has been immersed in a plasticizer at 60°C for 42 hours, and M" is the volume (g) of the rubber piece before it was immersed in the plasticizer (1.1 cm 3 is the mass of the rubber piece (g). [2] The molded article according to the above [1], wherein the polymer has a hydrogen-bonding functional group. [3] The molded article according to the above [1] or [2], wherein the polymer has at least a part of the multiple bonds in the polymer in its main chain. [4] The molded article according to any one of the above [1] to [3], wherein the polymer has a number average molecular weight of more than 2,000 and not more than 200,000. [5] The molded article according to any one of the above [1] to [4], wherein the polymer contains, in the molecule, a monomer unit derived from one or more selected from butadiene, isoprene, and farnesene. [6] The molded article according to any one of the above [2] to [5], wherein the hydrogen-bonding functional group is at least one selected from a hydroxy group, an aldehyde group, an acetalized aldehyde group, a carboxy group, a salt of a carboxy group, an esterified carboxy group, an acid anhydride of a carboxy group, an amino group, an amide group, a silanol group, an esterified silanol group, an imidazole group, a boronyl group, an epoxy group, and an isocyanate group. [7] The molded article according to any one of the above [1] to [6], wherein the amount of the adhesive component attached is from 0.01% by mass to 10.0% by mass with respect to 100% by mass of the rubber reinforcing fiber. [8] The molded article according to any one of the above [1] to [7], wherein the content of the polymer in the adhesive component is from 1% by mass to 80% by mass. [9] The molded article according to any one of the above [1] to [8], wherein the content of the plasticizer in the adhesive component is from 20% by mass to 95% by mass.
[10] The molded article according to any one of the above [1] to [9], wherein the fibers are at least one type selected from polyvinyl alcohol-based fibers, regenerated cellulose-based fibers, and hydrophobic fibers whose surfaces have been subjected to a hydrophilization treatment.
[11] The molded article according to the above
[10] , wherein the hydrophobic fiber is a polyester fiber.
[12] The molded article according to any one of the above [1] to
[11] , wherein the rubber reinforcing fiber is a woven fabric or a knitted fabric.
[13] The molded article according to any one of the above [1] to
[12] , which is a tire, a belt or a hose.
[14] A method for producing a molded article according to any one of the above [1] to
[13] , comprising the steps of: adhering a mixture of a polymer having one or more types of multiple bonds selected from reactive carbon-carbon double bonds and reactive carbon-carbon triple bonds in the molecule and a plasticizer to a fiber to obtain a rubber reinforcing fiber; and overlapping the obtained rubber reinforcing fiber and rubber to perform vulcanization. Effect of the Invention
[0009] According to the present invention, it is possible to provide a molded article having excellent adhesion between rubber reinforcing fibers and rubber, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Molded body] The molded article of the present invention is a molded article comprising rubber and rubber reinforcing fibers having an adhesive component on at least a portion of the fiber surface, wherein the adhesive component comprises a polymer having at least one type of multiple bond selected from a reactive carbon-carbon double bond and a reactive carbon-carbon triple bond in the molecule, and a plasticizer having a swelling degree with respect to the rubber of 5.0% or more, as calculated by the following formula (1): (Swelling degree relative to the rubber) (%) = (MM") / M" x 100 (1) (Wherein, M is the volume of 1.1 cm 3 is the mass (g) of a rubber piece after it has been immersed in a plasticizer at 60°C for 42 hours, and M" is the volume (g) of the rubber piece before it was immersed in the plasticizer (1.1 cm 3 is the mass of the rubber piece (g). According to the present invention, a rubber reinforcing fiber has an adhesive component containing a specific polymer on at least a part of the fiber surface and a plasticizer whose swelling degree with respect to the rubber to be reinforced is equal to or greater than a specific value, so that a molded article having excellent adhesion between the rubber reinforcing fiber and the rubber can be obtained. In addition, the increased adhesive strength between the rubber reinforcing fiber and the rubber suppresses friction between the rubber reinforcing fibers, improving the durability of the molded article.
[0011] [Rubber reinforcing fiber] The rubber reinforcing fiber used in the present invention has, on at least a portion of the fiber surface, an adhesive component that includes a polymer having at least one type of multiple bond selected from a reactive carbon-carbon double bond and a reactive carbon-carbon triple bond in at least one molecule, and a plasticizer having a swelling degree with respect to the rubber, calculated by the above formula (1), of 5.0% or more. The rubber reinforcing fiber has excellent adhesion to rubber because it contains a polymer (hereinafter also referred to as a reactive multiple bond-containing polymer) having at least one type of multiple bond selected from reactive carbon-carbon double bonds and reactive carbon-carbon triple bonds in the molecule as an adhesive component on at least a part of the fiber surface. In addition, the adhesive component contains a plasticizer having a swelling degree with respect to rubber of a specific value or more, thereby improving the affinity between the adhesive component and rubber and making the adhesiveness to rubber even more excellent. Furthermore, the adhesive component contains the plasticizer, which improves the bundling property of the fiber and also functions as a lubricant, so that the fiber does not peel off or fall off even if it is rubbed against various guides in the rubber reinforcing fiber manufacturing process, making it possible to suppress facility contamination and improve the manufacturing efficiency of the rubber reinforcing fiber.
[0012] In the present invention, "having an adhesive component on at least a portion of the surface of the fiber" may mean that the adhesive component is present on at least a portion of the surface of the fiber, for example, as a film or layer, or that the adhesive component is contained in the raw material of the fiber and the adhesive component is present on part of the surface of the fiber itself. In addition, the adhesive component used in the present invention can obtain a rubber reinforcing fiber having excellent adhesion to rubber even if it does not contain formaldehyde or a resin made from formaldehyde, which is harmful to the human body. In the present invention, if the adhesive component contains a resin made from formaldehyde, examples of the resin include resorcinol / formaldehyde resin, phenol / formaldehyde resin, melamine / formaldehyde resin, and derivatives thereof. If the adhesive component contains the formaldehyde component, the content is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably substantially free of the formaldehyde component, relative to 100 parts by mass of the liquid conjugated diene rubber. The formaldehyde content can be measured by extracting the adhesive component from the rubber reinforcing fiber with a solvent such as toluene, and then using HPLC or the like.
[0013] [Reactive multiple bond-containing polymer] The reactive multiple bond-containing polymer contained in the adhesive component (i.e., a polymer having at least one type of multiple bond selected from reactive carbon-carbon double bonds and reactive carbon-carbon triple bonds in the molecule) is not particularly limited, and examples thereof include polymers having reactive carbon-carbon double bonds such as conjugated diene rubber, ethylene-propylene-non-conjugated diene copolymer rubber (EPDM), polyacetylene, polynorbornene, polyparaphenylenevinylene, polydicyclopentadiene, polyoctenamer, polycyclooctene, polyethylene glycol diacrylate, and peptides containing dehydroalanine residues; and polymers having reactive carbon-carbon triple bonds such as polyphenylene butadiynylene, polyphenylene ethynylene, polyphenylene octatetraynylene, and polyyne compounds. In this specification, the term "reactive carbon-carbon double bond" refers to a carbon-carbon double bond that can react with other components by external energy such as heat or light, and generally does not include carbon-carbon double bonds contained in aromatic rings, but refers to aliphatic carbon-carbon double bonds. The term "reactive carbon-carbon triple bond" has the same meaning.
[0014] The reactive multiple bond-containing polymer preferably has a hydrogen-bonding functional group from the viewpoint of allowing it to interact more strongly with the rubber reinforcing fibers and obtaining a molded article having excellent adhesion between the rubber reinforcing fibers and the rubber. In this specification, the term "hydrogen bond" refers to a bonding interaction formed between a hydrogen atom (donor) that is bonded to an atom with high electronegativity (O, N, S, etc.) and is electrically positively polarized, and an electronegative atom (acceptor) that has a lone pair of electrons.
[0015] In the present invention, the "hydrogen-bonding functional group" refers to a functional group that can function as a donor and an acceptor in the hydrogen bond. Specific examples of the functional group include a hydroxyl group, an ether group, a mercapto group, a carboxyl group, a carbonyl group, an aldehyde group, an amino group, an imino group, an imidazole group, a urethane group, an amide group, a urea group, an isocyanate group, a nitrile group, a boronyl group, an epoxy group, a silanol group, and derivatives thereof. An example of the derivative of the aldehyde group is an acetalized product thereof. An example of the derivative of the carboxyl group is a salt thereof, an esterified product thereof, an amidated product thereof, or an acid anhydride thereof. An example of the derivative of the boronyl group is a salt thereof, or an esterified product thereof. An example of the derivative of the silanol group is an esterified product thereof. An example of the carboxyl group is a group derived from a monocarboxylic acid or a group derived from a dicarboxylic acid. Among these, from the viewpoint of improving adhesion to rubber, preferred are one or more selected from a hydroxy group, an aldehyde group, an acetalized product of an aldehyde group, a carboxy group, a salt of a carboxy group, an esterified product of a carboxy group, an acid anhydride of a carboxy group, an amino group, an amide group, a silanol group, an esterified product of a silanol group, an imidazole group, a boronyl group, an epoxy group, and an isocyanate group, more preferred are one or more selected from a hydroxy group, a carboxy group, a salt of a carboxy group, an acid anhydride of a carboxy group, and a boronyl group, even more preferred are one or more selected from a carboxy group, an esterified product of a carboxy group, and a boronyl group, and even more preferred are groups derived from a dicarboxylic acid and a boronyl group.
[0016] The reactive multiple bond-containing polymer preferably has at least a part of the multiple bonds in the main chain, and is preferably a conjugated diene rubber. When the polymer has at least a part of the multiple bonds in the main chain, it can form a radical resonance structure when laminated with rubber and vulcanized, and the vulcanization reaction proceeds effectively.
[0017] The conjugated diene rubber contains at least a monomer unit derived from a conjugated diene (hereinafter also referred to as a "conjugated diene unit") in the molecule, and for example, it is preferable that the conjugated diene rubber contains 50 mol % or more of the monomer units derived from a conjugated diene out of all the monomer units in the conjugated diene rubber. Examples of the conjugated diene monomer include butadiene, 2-methyl-1,3-butadiene (hereinafter also referred to as "isoprene"), 2,3-dimethylbutadiene, 2-phenylbutadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, β-farnesene (hereinafter also referred to as "farnesene"), myrcene, and chloroprene. These conjugated dienes may be used alone or in combination of two or more. From the viewpoint of reactivity during vulcanization, the conjugated diene rubber more preferably has monomer units derived from one or more selected from butadiene, isoprene and farnesene. That is, the polymer is preferably a conjugated diene rubber, and more preferably a polymer containing, in the molecule, a monomer unit derived from one or more selected from butadiene, isoprene, and farnesene.
[0018] The conjugated diene rubber may contain units derived from other monomers than the conjugated diene monomers, as long as the units do not impair adhesion. Examples of the other monomers include copolymerizable ethylenically unsaturated monomers and aromatic vinyl compounds. Examples of the ethylenically unsaturated monomer include olefins such as ethylene, 1-butene, acrylonitrile, and isobutylene. Examples of the aromatic vinyl compound include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, and divinylbenzene. These may be used alone or in combination of two or more. When the conjugated diene rubber contains monomer units derived from monomers other than the conjugated diene monomer, the content thereof is preferably 30 mol % or less, more preferably 10 mol % or less, and further preferably 5 mol % or less.
[0019] The conjugated diene rubber is preferably a modified conjugated diene rubber having a hydrogen-bonding functional group in a part of the conjugated diene rubber, and more preferably a modified conjugated diene rubber containing a conjugated diene unit in at least a part of the polymer chain and having a hydrogen-bonding functional group in a side chain or at an end of the polymer chain. Specific examples of the hydrogen-bonding functional group are as described above. When the modified conjugated diene rubber is used as the conjugated diene rubber, the modified conjugated diene rubber interacts with the adherend rubber and fiber, respectively, and thereby they can be bonded together. When the modified conjugated diene rubber and the adherend rubber are vulcanized to form a covalent bond, a strong cohesive force is generated, and the adhesion is further improved. Furthermore, when hydrophilic fibers are used as the fibers, it is believed that the hydrogen-bonding functional groups contained in the modified conjugated diene rubber form hydrogen bonds with the hydrophilic fibers, thereby improving adhesion.
[0020] From the viewpoint of obtaining a rubber reinforcing fiber having excellent rubber adhesion, the number of hydrogen-bonding functional groups in the modified conjugated diene rubber is, on average, preferably 2 or more, more preferably 3 or more, and even more preferably 4 or more per molecule. Moreover, from the viewpoint of controlling the viscosity of the modified conjugated diene rubber within an appropriate range and improving handleability, the number of hydrogen-bonding functional groups is, on average, preferably 80 or less, more preferably 40 or less, even more preferably 30 or less, and even more preferably 20 or less per molecule.
[0021] The average number of hydrogen-bonding functional groups per molecule of the modified conjugated diene rubber is calculated from the equivalent weight (g / eq) of the hydrogen-bonding functional groups of the modified conjugated diene rubber and the number-average molecular weight Mn in terms of styrene, based on the following formula: The equivalent weight of the hydrogen-bonding functional groups of the modified conjugated diene rubber means the mass of the conjugated diene bonded to each hydrogen-bonding functional group and the mass of other monomers other than the conjugated diene that are included as necessary. Average number of hydrogen-bonding functional groups per molecule = [(number average molecular weight (Mn)) / (molecular weight of styrene unit) x (average molecular weight of conjugated diene and other monomer units other than conjugated diene contained as necessary)] / (equivalent weight of hydrogen-bonding functional group) The method for calculating the equivalent weight of the hydrogen-bonding functional group can be appropriately selected depending on the type of the hydrogen-bonding functional group.
[0022] Examples of methods for obtaining a modified conjugated diene rubber include a method of adding a modifying compound to a polymer of a conjugated diene monomer (hereinafter also referred to as "production method (1)"), a method of oxidizing a conjugated diene polymer (hereinafter also referred to as "production method (2)"), a method of copolymerizing a conjugated diene monomer with a radically polymerizable compound having a hydrogen-bonding functional group (hereinafter also referred to as "production method (3)"), and a method of adding a modifying compound capable of reacting with a polymerization active terminal to a polymer of an unmodified conjugated diene monomer having a polymerization active terminal before adding a polymerization terminator (hereinafter also referred to as "production method (4)").
[0023] [Production method of modified conjugated diene rubber (1)] The production method (1) is a method in which a modifying compound is added to a polymer of a conjugated diene monomer, that is, an unmodified conjugated diene rubber (hereinafter also referred to as "unmodified conjugated diene rubber"). The unmodified conjugated diene rubber can be obtained by polymerizing a conjugated diene and, if necessary, a monomer other than the conjugated diene, for example, by emulsion polymerization or solution polymerization.
[0024] As the solution polymerization method, a known method or a method similar to a known method can be applied. For example, a predetermined amount of a monomer containing a conjugated diene is polymerized in a solvent using a Ziegler catalyst, a metallocene catalyst, or an anionically polymerizable active metal or active metal compound, if necessary in the presence of a polar compound. Examples of the solvent include aliphatic hydrocarbons such as n-butane, n-pentane, isopentane, n-hexane, n-heptane, and isooctane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene.
[0025] Examples of the anionically polymerizable active metal include alkali metals such as lithium, sodium, potassium, etc., alkaline earth metals such as beryllium, magnesium, calcium, strontium, barium, etc., lanthanoid rare earth metals such as lanthanum, neodymium, etc. Among these anionically polymerizable active metals, alkali metals and alkaline earth metals are preferred, and alkali metals are more preferred. As the anionically polymerizable active metal compound, organic alkali metal compounds are preferred.As organic alkali metal compounds, for example, organic monolithium compounds such as methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, t-butyl lithium, hexyl lithium, phenyl lithium, stilbene lithium, etc.; polyfunctional organic lithium compounds such as dilithiomethane, dilithionaphthalene, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, 1,3,5-trilithiobenzene, etc.; sodium naphthalene, potassium naphthalene, etc. are included.Among these organic alkali metal compounds, organic lithium compounds are preferred, and organic monolithium compounds are more preferred.
[0026] The amount of the organic alkali metal compound used can be appropriately set depending on the melt viscosity, molecular weight, etc. of the target unmodified conjugated diene rubber and modified conjugated diene rubber, but it is usually used in an amount of 0.01 to 3 parts by mass per 100 parts by mass of all monomers including conjugated diene. The above organic alkali metal compounds can also be reacted with secondary amines such as dibutylamine, dihexylamine, dibenzylamine, etc. to form organic alkali metal amides.
[0027] In anionic polymerization, polar compounds are usually used to adjust the microstructure of the conjugated diene moiety without deactivating the reaction. Examples of polar compounds include ether compounds such as dibutyl ether, tetrahydrofuran, ethylene glycol diethyl ether, and 2,2-di(2-tetrahydrofuryl)propane; tertiary amines such as tetramethylethylenediamine and trimethylamine; alkali metal alkoxides, and phosphine compounds. The polar compounds are usually used in an amount of 0.01 to 1000 mol relative to the organic alkali metal compound. The temperature for the solution polymerization is usually in the range of −80 to 150° C., preferably in the range of 0 to 100° C., and more preferably in the range of 10 to 90° C. The polymerization mode may be either a batch system or a continuous system. The polymerization reaction can be terminated by adding a polymerization terminator. Examples of the polymerization terminator include alcohols such as methanol and isopropanol. The resulting polymerization reaction liquid is poured into a poor solvent such as methanol to precipitate the polymerized product, or the polymerization reaction liquid is washed with water, separated, and then dried to isolate the unmodified conjugated diene rubber. Of the above methods, the solution polymerization method is preferred as the method for producing the unmodified conjugated diene rubber.
[0028] The emulsion polymerization method may be a known method or a method similar to a known method, for example, a monomer containing a predetermined amount of conjugated diene is emulsified and dispersed in the presence of an emulsifier, and emulsion-polymerized by a radical polymerization initiator. Examples of the emulsifier include salts of long-chain fatty acids having 10 or more carbon atoms, rosin acid salts, etc. Examples of the long-chain fatty acid salts include potassium salts or sodium salts of fatty acids such as capric acid, lauric acid, myristic acid, palmitic acid, oleic acid, and stearic acid. As the dispersion solvent, water is usually used, and it may contain a water-soluble organic solvent such as methanol or ethanol within a range that does not impair the stability during polymerization. Examples of the radical polymerization initiator include persulfates such as ammonium persulfate and potassium persulfate, organic peroxides, and hydrogen peroxide. A chain transfer agent may be used to adjust the molecular weight of the resulting unmodified conjugated diene rubber. Examples of the chain transfer agent include mercaptans such as t-dodecyl mercaptan and n-dodecyl mercaptan; carbon tetrachloride, thioglycolic acid, diterpene, terpinolene, γ-terpinene, and α-methylstyrene dimer.
[0029] The temperature of the emulsion polymerization can be appropriately set depending on the type of radical polymerization initiator used, etc., but is usually in the range of 0 to 100° C., preferably in the range of 0 to 60° C. The polymerization mode may be either continuous polymerization or batch polymerization.
[0030] The polymerization reaction can be terminated by adding a polymerization terminator, such as an amine compound such as isopropylhydroxylamine, diethylhydroxylamine, or hydroxylamine, a quinone compound such as hydroquinone or benzoquinone, or sodium nitrite.
[0031] After the polymerization reaction is stopped, an antioxidant may be added as necessary. After the polymerization reaction is stopped, unreacted monomers are removed from the obtained latex as necessary, and then the polymerized product is coagulated using salts such as sodium chloride, calcium chloride, and potassium chloride as a coagulant, and an acid such as nitric acid or sulfuric acid is added as necessary to adjust the pH of the coagulation system to a predetermined value, and then the dispersion solvent is separated to recover the polymerized product. Next, the polymerized product is washed with water, dehydrated, and dried to obtain an unmodified conjugated diene rubber. During the coagulation, the latex and an extender oil that has been previously made into an emulsified dispersion may be mixed as necessary, and the product may be recovered as an oil-extended unmodified conjugated diene rubber.
[0032] (Modifying compound used in production method (1)) The modified compound used in the manufacturing method (1) is not particularly limited, but from the viewpoint of improving the adhesion between the rubber reinforcing fiber and the rubber, it is preferable to use a compound having a hydrogen-bonding functional group. Examples of the hydrogen-bonding functional group include the same as those described above. Among them, from the viewpoint of the strength of the hydrogen bond force, a hydroxyl group, an aldehyde group, an acetalized product of an aldehyde group, a carboxyl group, a salt of a carboxyl group, an esterified product of a carboxyl group, an acid anhydride of a carboxyl group, an amino group, an amide group, a silanol group, an esterified product of a silanol group, an imidazole group, a boronyl group, an epoxy group, and an isocyanate group are preferable, and a carboxyl group, a salt of a carboxyl group, an esterified product of a carboxyl group, an acid anhydride of a carboxyl group, a silanol group, an esterified product of a silanol group, and a boronyl group are more preferable. These modified compounds having a hydrogen-bonding functional group may be used alone or in combination of two or more kinds.
[0033] Examples of the modifying compound include unsaturated carboxylic acids such as maleic acid, fumaric acid, citraconic acid, perpropionic acid, and itaconic acid; unsaturated carboxylic anhydrides such as maleic anhydride, citraconic anhydride, 2,3-dimethylmaleic anhydride, and itaconic anhydride; unsaturated carboxylic esters such as maleic acid esters, fumaric acid esters, citraconic acid esters, and itaconic acid esters; unsaturated carboxylic amides such as maleic acid amides, fumaric acid amides, citraconic acid amides, and itaconic acid amides; unsaturated carboxylic imides such as maleic acid imides, fumaric acid imides, citraconic acid imides, and itaconic acid imides; vinyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, mercaptomethylmethyldiethoxysilane, mercaptomethyltrieth ... Examples of the silane compounds include silane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, 2-mercaptoethylmethoxydimethylsilane, 2-mercaptoethylethoxydimethylsilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyldimethoxymethylsilane, 3-mercaptopropyldiethoxymethylsilane, 3-mercaptopropyldimethoxyethylsilane, 3-mercaptopropyldiethoxyethylsilane, 3-mercaptopropylmethoxydimethylsilane, and 3-mercaptopropylethoxydimethylsilane; and boronate esters such as triethyl borate, tripropyl borate, triisopropyl borate, and tributyl borate.
[0034] The amount of the modifying compound used is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 50 parts by mass, and further preferably 1 to 30 parts by mass, based on 100 parts by mass of the unmodified conjugated diene rubber. The reaction temperature is usually preferably in the range of 0 to 200°C, more preferably in the range of 50 to 200°C. Alternatively, the unmodified conjugated diene rubber may be grafted with the modifying compound to introduce a hydrogen-bonding functional group, and then a modifying compound capable of reacting with the functional group may be added to introduce another hydrogen-bonding functional group into the polymer.Specifically, for example, a method may be used in which maleic anhydride is grafted onto an unmodified conjugated diene rubber obtained by living anionic polymerization, and then a compound having a hydroxyl group, such as 2-hydroxyethyl methacrylate or methanol, or a compound such as water is reacted therewith.
[0035] The amount of the modified compound added to the modified conjugated diene rubber is preferably 0.5 to 40 parts by mass, more preferably 1 to 30 parts by mass, and even more preferably 1.5 to 20 parts by mass, based on 100 parts by mass of the unmodified conjugated diene rubber. The amount of the modified compound added to the modified conjugated diene rubber can be calculated based on the acid value of the modified compound, or can be determined using various analytical instruments such as infrared spectroscopy and nuclear magnetic resonance spectroscopy.
[0036] The method of adding the modifying compound to the unmodified conjugated diene rubber is not particularly limited, and examples thereof include a method of heating an unmodified conjugated diene rubber, one or more modifying compounds selected from unsaturated carboxylic acids, unsaturated carboxylic acid derivatives, boronic acid derivatives, silane compounds, etc., and further adding a radical generator as necessary, in the presence or absence of an organic solvent. There is no particular limit to the radical generator used, and commercially available organic peroxides, azo compounds, hydrogen peroxide, etc. can be used. The organic solvent used in the above method generally includes hydrocarbon solvents and halogenated hydrocarbon solvents. Among these organic solvents, hydrocarbon solvents such as n-butane, n-hexane, n-heptane, cyclohexane, benzene, toluene, and xylene are preferred.
[0037] Furthermore, when the reaction of adding the modified compound is carried out by the above method, an antioxidant may be added from the viewpoint of suppressing side reactions, etc. The antioxidant can be a commercially available one, such as butylated hydroxytoluene (BHT), N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (Nocrac 6C), etc. The amount of the antioxidant added is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the unmodified conjugated diene rubber. When the amount of the antioxidant added is within the above range, side reactions can be suppressed, and the modified conjugated diene rubber can be obtained in good yield.
[0038] [Production method of modified conjugated diene rubber (2)] The production method (2) includes a method of obtaining an oxidized conjugated diene rubber having a functional group or bond containing oxygen generated by an oxidation reaction in the molecule by oxidizing a raw material conjugated diene rubber, specifically, a hydroxy group, an aldehyde group, a carbonyl group, a carboxy group, an ether bond, etc. The method for oxidizing the raw material conjugated diene rubber includes a method of heat treating the raw material conjugated diene rubber at a temperature equal to or higher than the oxidation temperature (hereinafter also referred to as "production method (2-1)"), a method of irradiating the raw material conjugated diene rubber with light having an absorption wavelength to activate the raw material conjugated diene rubber and reacting it with oxygen (hereinafter also referred to as "production method (2-2)"), etc. Among them, the method of heat treating the raw material conjugated diene rubber at a temperature equal to or higher than the oxidation temperature (production method (2-1)) is preferred. The stage at which the oxidation reaction of the conjugated diene rubber is carried out is not particularly limited, and may be carried out before the conjugated diene rubber and the plasticizer are mixed, may be carried out after the conjugated diene rubber and the plasticizer are mixed, or may be carried out after the conjugated diene rubber and the plasticizer are mixed and attached to the fibers.
[0039] [Production method of oxidized conjugated diene rubber (2-1)] The production method (2-1) is a method in which a raw material conjugated diene rubber is heat-treated at a temperature equal to or higher than its oxidation temperature in an atmosphere containing oxygen, preferably in an air atmosphere. The heat treatment temperature is not particularly limited as long as it is a temperature at which the raw material conjugated diene rubber is oxidized, but from the viewpoint of increasing the reaction rate of the oxidation and improving productivity, it is preferably 150° C. or higher, more preferably 170° C. or higher, and even more preferably 190° C. or higher. When the raw material conjugated diene rubber is oxidized on the surface of the hydrophilic fiber as described below, the heat treatment temperature is preferably 240° C. or lower, and more preferably 220° C. or lower, from the viewpoint of preventing deterioration of the fiber. The heat treatment time is not particularly limited as long as the raw material conjugated diene rubber does not deteriorate, but is preferably 30 minutes or less, more preferably 20 minutes or less. Furthermore, the temperature required for the oxidation reaction can be lowered by adding a thermal radical generator to the raw material conjugated diene rubber.
[0040] Examples of the thermal radical generator include peroxides, azo compounds, redox initiators, etc. Among them, peroxides are preferred from the viewpoint that the thermal radical generator bonds with the conjugated diene rubber and a structure containing oxygen is added to the conjugated diene rubber. Examples of the peroxides include t-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl peroxyoctanoate, t-butyl peroxyneodecanoate, t-butyl peroxyisobutyrate, lauroyl peroxide, t-amyl peroxypivalate, t-butyl peroxypivalate, dicumyl peroxide, benzoyl peroxide, potassium persulfate, and ammonium persulfate.
[0041] Examples of the azo compound include azobisisobutyronitrile (AIBN), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-butanenitrile), 4,4'-azobis(4-pentanoic acid), 1,1'-azobis(cyclohexanecarbonitrile), 2-(t-butylazo)-2-cyanopropane, and 2,2'-azobis[2-methyl-N-(1,1)-bis(hydroxymethyl)-2-hydroxyethyl]propane. Examples of the thermal radical generator include pionamide, 2,2'-azobis(2-methyl-N-hydroxyethyl)propionamide, 2,2'-azobis(N,N'-dimethyleneisobutylamidine) dichloride, 2,2'-azobis(N,N-dimethyleneisobutylamide), 2,2'-azobis(2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide), 2,2'-azobis(isobutylamide) dihydrate, etc. The thermal radical generator may be used alone or in combination of two or more.
[0042] The thermal radical generator may also be a redox initiator, such as a combination of persulfate, acidic sodium sulfite, and ferrous sulfate, a combination of t-butyl hydroperoxide, acidic sodium sulfite, and ferrous sulfate, or a combination of p-menthane hydroperoxide, ferrous sulfate, sodium ethylenediaminetetraacetate, and sodium formaldehyde sulfoxylate.
[0043] [Production method of oxidized conjugated diene rubber (2-2)] The production method (2-2) is a method in which a raw material conjugated diene rubber is activated by being irradiated with light having an absorption wavelength of the raw material conjugated diene rubber, and reacted with oxygen. The production method (2-2) is carried out in an atmosphere containing oxygen, preferably in an air atmosphere. The wavelength of the light used is not particularly limited as long as it is absorbed by the raw material conjugated diene rubber and causes a radical reaction, but ultraviolet light, which is strongly absorbed by the raw material conjugated diene rubber, is preferred. Furthermore, by adding a photoradical generator to the raw material conjugated diene rubber, the amount of light irradiation required for the oxidation reaction can be reduced.
[0044] Examples of the photoradical generator include acetophenone, acetophenone benzyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, xanthone, fluorenone, benzaldehyde, fluorene, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4,4'-dimethoxybenzophenone, benzoin propyl ether, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2-hydroxyphenyl ... Examples of the photoradical generator include thio-2-methyl-1-phenylpropan-1-one, thioxanthone, diethylthioxanthone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, etc. The photoradical generator may be used alone or in combination of two or more.
[0045] [Production method of modified conjugated diene rubber (3)] The production method (3) includes a method in which a conjugated diene monomer and a radically polymerizable compound having a hydrogen-bonding functional group are randomly copolymerized, block copolymerized, or graft copolymerized by a known method.
[0046] (Radically polymerizable compound having a hydrogen-bonding functional group used in production method (3)) The radical polymerizable compound having a hydrogen-bonding functional group used in the production method (3) is not particularly limited as long as it is a compound having both a hydrogen-bonding functional group and a reactive multiple bond in the molecule.Specific examples thereof include an aldehyde having a reactive multiple bond, an acetalized product of the aldehyde; a monocarboxylic acid having a reactive multiple bond, a salt of the monocarboxylic acid, an esterified product of the monocarboxylic acid, an acid anhydride of the monocarboxylic acid; an epoxy having a reactive multiple bond; a dicarboxylic acid having a reactive multiple bond, a salt of the dicarboxylic acid, an esterified product of the dicarboxylic acid, an acid anhydride of the dicarboxylic acid; and an amine compound having a reactive multiple bond.
[0047] Among the aldehydes having a multiple bond, examples of aldehydes having a reactive carbon-carbon double bond include acrolein, methacrolein, crotonaldehyde, 3-butenal, 2-methyl-2-butenal, 2-methyl-3-butenal, 2,2-dimethyl-3-butenal, 3-methyl-2-butenal, 3-methyl-3-butenal, 2-pentenal, 2-methyl-2-pentenal, 3-pentenal, and 3-methyl -4-Pentenal, 4-Pentenal, 4-Methyl-4-pentenal, 2-Hexenal, 3-Hexenal, 4-Hexenal, 5-Hexenal, 7-Octenal, 10-Undecenal, 2-Ethylcrotonaldehyde, 3-(Dimethylamino)acrolein, Myristoleinaldehyde, Palmitoleinaldehyde, Oleinaldehyde, Elaidinaldehyde, Bucksenaldehyde, Gadoleinaldehyde, El Alkenals having 3 to 30 carbon atoms, preferably 3 to 25 carbon atoms, such as kaolin aldehyde, nervonaldehyde, linolealdehyde, citronellal, cinnamaldehyde, and vanillin; alkadienals having 5 to 30 carbon atoms, preferably 5 to 25 carbon atoms, such as 2,4-pentadienal, 2,4-hexadienal, 2,6-nonadienal, and citral; linolenic aldehyde, eleostearic aldehyde, Examples of the unsaturated aldehydes include alkatrienals having 7 to 30 carbon atoms, such as aldehyde, preferably alkatrienals having 7 to 25 carbon atoms; alkatetraenals having 9 to 30 carbon atoms, such as stearidone aldehyde and arachidone aldehyde, preferably alkatetraenals having 9 to 25 carbon atoms; alkapentaenals having 11 to 30 carbon atoms, such as eicosapentaene aldehyde, preferably alkapentaenals having 11 to 25 carbon atoms. In addition, the aldehydes having cis-trans isomers include both cis and trans isomers. These aldehydes may be used alone or in combination of two or more kinds.
[0048] Among the acetalized products of aldehydes having a multiple bond, examples of the acetalized products of aldehydes having a reactive carbon-carbon double bond include acetalized products of the aldehydes, specifically, 3-(1,3-dioxalan-2-yl)-3-methyl-1-propene which is an acetalized product of 2-methyl-3-butenal, and 3-(1,3-dioxalan-2-yl)-2-methyl-1-propene which is an acetalized product of 3-methyl-3-butenal.
[0049] Among the aldehydes having a multiple bond and acetalized products of the aldehydes, examples of the aldehydes having a reactive carbon-carbon triple bond and acetalized products thereof include aldehydes having a carbon-carbon triple bond such as propioaldehyde, 2-butyn-1-al, and 2-pentyn-1-al, and acetalized products of the aldehydes.
[0050] Among the aldehydes having a multiple bond and the acetalized products of the aldehydes, aldehydes having a reactive carbon-carbon double bond are preferred, such as acrolein, methacrolein, crotonaldehyde, 3-butenal, 2-methyl-2-butenal, 2-methyl-3-butenal, 2,2-dimethyl-3-butenal, 3-methyl-2-butenal, 3-methyl-3-butenal, 2-pentenal, At least one selected from 2-pentenal, 2-methyl-2-pentenal, 3-pentenal, 3-methyl-4-pentenal, 4-pentenal, 4-methyl-4-pentenal, 2-hexenal, 3-hexenal, 4-hexenal, 5-hexenal, 7-octenal, 2-ethylcrotonaldehyde, 3-(dimethylamino)acrolein, and 2,4-pentadienal is preferred. Among them, at least one selected from acrolein, methacrolein, crotonaldehyde, and 3-butenal is more preferred because of their good reactivity during copolymerization.
[0051] Examples of the epoxy having a multiple bond include allyl glycidyl ether, methallyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, butadiene monoxide, and 1,4-cyclopentadiene monoepoxide, with allyl glycidyl ether being particularly preferred.
[0052] Examples of the monocarboxylic acid having a multiple bond, the salt of the monocarboxylic acid, the ester of the monocarboxylic acid, and the acid anhydride of the monocarboxylic acid include (meth)acrylic acid, a sodium salt of (meth)acrylic acid, a potassium salt of (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2 ... butyl, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, vinyl (meth)acrylate, 2-(trifluoromethyl)acrylic acid, methyl 2-trifluoromethylacrylate, ethyl 2-trifluoromethylacrylate, propyl 2-trifluoromethylacrylate, 2-butyl 2-trifluoromethylacrylate, 2-hydroxyethyl 2-trifluoromethylacrylate, vinyl 2-trifluoromethylacrylate, methyl cinnamate, vinyl cinnamate, methyl crotonate, vinyl crotonate, 3 -Methyl-3-butenoate, vinyl 3-methyl-3-butenoate, methyl 4-pentenoate, vinyl 4-pentenoate, methyl 2-methyl-4-pentenoate, vinyl 2-methyl-4-pentenoate, methyl 5-hexenoate, vinyl 5-hexenoate, methyl 3,3-dimethyl-4-pentenoate, vinyl 3,3-dimethyl-4-pentenoate, methyl 7-octenoate, vinyl 7-octenoate, methyl trans-3-pentenoate, vinyl trans-3-pentenoate, methyl trans-4-decenoate, vinyl trans-4-decenoate, 3-methyl-3- Ethyl butenoate, Ethyl 4-pentenoate, Ethyl 2-methyl-4-pentenoate, Ethyl 5-hexenoate, Ethyl 3,3-dimethyl-4-pentenoate, Ethyl 7-octenoate, Ethyl trans-3-pentenoate, Ethyl trans-4-decenoate, Methyl 10-undecenoate, Vinyl 10-undecenoate, (meth)acrylic anhydride, 2-(trifluoromethyl)acrylic anhydride, Cinnamic anhydride, Crotonic anhydride, 3-methyl-3-butenoic anhydride, 4-pentenoic anhydride, 2-methyl-4-pentenoic anhydride, 5-hexenoic anhydride, 3,Examples of the carboxylic acids having a reactive carbon-carbon double bond include 3-dimethyl-4-pentenoic anhydride, 7-octenoic anhydride, trans-3-pentenoic anhydride, trans-4-decenoic anhydride, 3-methyl-3-butenoic anhydride, 4-pentenoic anhydride, 2-methyl-4-pentenoic anhydride, and 10-undecenoic anhydride; and carboxylic acids having a reactive carbon-carbon triple bond and esters of the carboxylic acids, such as propiolic acid, methyl propiolate, ethyl propiolate, vinyl propiolate, tetrol acid, methyl tetrolate, ethyl tetrolate, and vinyl tetrolate. In this specification, the term "(meth)acrylic acid" collectively refers to "acrylic acid" and "methacrylic acid".
[0053] Examples of the dicarboxylic acid having a multiple bond, the salt of the dicarboxylic acid, the ester of the dicarboxylic acid, and the acid anhydride of the dicarboxylic acid include dicarboxylic acids having a reactive carbon-carbon double bond, salts of the dicarboxylic acid, esters of the dicarboxylic acid, and acid anhydrides of the dicarboxylic acid, such as maleic acid, sodium maleate, potassium maleate, methyl maleate, dimethyl maleate, maleic anhydride, itaconic acid, methyl itaconate, dimethyl itaconate, itaconic anhydride, himic acid, methyl himic acid, dimethyl himic acid, and himic acid anhydride.
[0054] As the monocarboxylic acid having a multiple bond, the salt of the monocarboxylic acid, the ester of the monocarboxylic acid, the monocarboxylic anhydride, the dicarboxylic acid having a multiple bond, the salt of the dicarboxylic acid, the ester of the dicarboxylic acid, and the acid anhydride of the dicarboxylic acid, a compound having a reactive carbon-carbon double bond is preferred, and among them, one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, vinyl (meth)acrylate, (meth)acrylic anhydride, 2-(trifluoromethyl)acrylic anhydride, cinnamic anhydride, crotonic anhydride, methyl maleate, dimethyl maleate, maleic anhydride, methyl itaconate, dimethyl itaconate, and itaconic anhydride are more preferred because of their good reactivity during copolymerization.
[0055] Among the amine compounds having multiple bonds, examples of amine compounds having a reactive carbon-carbon double bond include allylamine, 3-butenylamine, 4-pentenylamine, 5-hexenylamine, 6-heptenylamine, 7-octenylamine, oleylamine, 2-methylallylamine, 4-aminostyrene, 4-vinylbenzylamine, 2-allylglycine, S-allylcysteine, α-allylalanine, 2-allylaniline, geranylamine, vigabatrin, 4-vinylaniline, and 4-vinyloxyaniline, etc. Among these, one or more selected from allylamine, 3-butenylamine, and 4-pentenylamine are preferred because of their good reactivity during copolymerization.
[0056] [Production method of modified conjugated diene rubber (4)] The production method (4) is a method in which a modifying compound capable of reacting with the polymerization active terminal is added to a polymerized product of an unmodified conjugated diene monomer having a polymerization active terminal (unmodified conjugated diene rubber) before adding a polymerization terminator. The unmodified conjugated diene rubber having a polymerization active terminal can be obtained by polymerizing a conjugated diene monomer and, if necessary, a monomer other than the conjugated diene, for example, by emulsion polymerization or solution polymerization, as in the production method (1). Examples of modifying compounds that can be used in the production method (4) include dimethyldiethoxysilane, tetramethoxysilane, tetraethoxysilane, 3-aminopropyltriethoxysilane, tetraglycidyl-1,3-bisaminomethylcyclohexane, 2,4-tolylene diisocyanate, carbon dioxide, ethylene oxide, succinic anhydride, boronic acid esters such as triethyl borate, tripropyl borate, triisopropyl borate, and tributyl borate, boronic acid anhydride groups, boronic acid anhydrides such as phenylboronic acid anhydride, 4,4'-bis(diethylamino)benzophenone, N-vinylpyrrolidone, N-methylpyrrolidone, 4-dimethylaminobenzylideneaniline, and dimethylimidazolidinone, as well as other modifying agents described in JP2011-132298A.
[0057] In the production method (4), the amount of the modifying compound used is preferably in the range of 0.01 to 100 molar equivalents relative to the organic alkali metal compound, for example, when the polymerization is carried out using an organic alkali metal compound. The reaction temperature is usually in the range of -80 to 150°C, preferably 0 to 100°C, more preferably 10 to 90°C. Alternatively, the modifying compound may be added before the addition of the polymerization terminator to introduce a hydrogen-bonding functional group into the unmodified conjugated diene rubber, and then a modifying compound capable of reacting with the functional group may be added to introduce another hydrogen-bonding functional group into the polymer.
[0058] The modified conjugated diene rubber may contain units derived from other monomers than the conjugated diene monomer and the radical polymerizable compound having a hydrogen-bonding functional group, so long as the units do not impair adhesion. Examples of the other monomers include copolymerizable ethylenically unsaturated monomers and aromatic vinyl compounds, and the specific compounds and contents are the same as those described above.
[0059] The method for producing the modified conjugated diene rubber is not particularly limited, but from the viewpoint of productivity, it is preferable to produce it by the production method (1), (2) or (3), more preferably by the production method (1) or (3), and even more preferably by the production method (1).
[0060] From the viewpoint of adhesion between the conjugated diene rubber and the fibers, the conjugated diene rubber is preferably in a liquid state. In this specification, the term "liquid" means that the melt viscosity of the conjugated diene rubber measured at 38° C. is 4,000 Pa·s or less. From the viewpoint of handleability, the melt viscosity is preferably 0.1 Pa·s or more, more preferably 1 Pa·s or more, even more preferably 10 Pa·s or more, even more preferably 30 Pa·s or more, even more preferably 50 Pa·s or more, and is preferably 2,000 Pa·s or less, more preferably 1,500 Pa·s or less, even more preferably 1,000 Pa·s or less, and even more preferably 500 Pa·s or less. The melt viscosity of the conjugated diene rubber means a viscosity measured at 38° C. using a Brookfield viscometer (B-type viscometer).
[0061] The glass transition temperature (Tg) of the conjugated diene rubber may vary depending on the vinyl content of the conjugated diene unit, the type of conjugated diene, the content of units derived from monomers other than the conjugated diene, etc., but is preferably −100 to 10° C., more preferably −100 to −10° C., and even more preferably −100 to −20° C. If the Tg is within the above range, the viscosity can be prevented from increasing, making the rubber easy to handle.
[0062] [Physical properties of polymers containing reactive multiple bonds] The weight average molecular weight (Mw) of the reactive multiple bond-containing polymer is not particularly limited, but from the viewpoint of improving adhesion to rubber, it is preferably 2,000 or more, more preferably 5,000 or more, even more preferably 10,000 or more, even more preferably 15,000 or more, even more preferably 20,000 or more, and particularly preferably 25,000 or more, and from the viewpoint of handleability, it is preferably 150,000 or less, more preferably 120,000 or less, even more preferably 100,000 or less, even more preferably 75,000 or less, and even more preferably 50,000 or less.
[0063] The number average molecular weight (Mn) of the reactive multiple bond-containing polymer is not particularly limited, but from the viewpoint of improving adhesion to rubber, it is preferably more than 2,000, more preferably 5,000 or more, even more preferably 10,000 or more, still more preferably 15,000 or more, still more preferably 20,000 or more, and particularly preferably 25,000 or more, and from the viewpoint of handleability, it is preferably 200,000 or less, more preferably 120,000 or less, still more preferably 75,000 or less, still more preferably 50,000 or less, and still more preferably 45,000 or less. The Mw and Mn of the reactive multiple bond-containing polymer are the weight average molecular weight and number average molecular weight in terms of polystyrene determined by gel permeation chromatography (GPC).
[0064] The molecular weight distribution (Mw / Mn) of the reactive multiple bond-containing polymer is preferably 1.0 to 5.0, more preferably 1.0 to 3.0, even more preferably 1.0 to 2.0, even more preferably 1.0 to 1.5, and particularly preferably 1.0 to 1.3. When Mw / Mn is within the above range, the viscosity of the reactive multiple bond-containing polymer varies little, making it easy to handle. The molecular weight distribution (Mw / Mn) means the ratio of weight average molecular weight (Mw) / number average molecular weight (Mn) calculated in terms of standard polystyrene, determined by GPC measurement.
[0065] [Plasticizer] The plasticizer contained in the adhesive component has a swelling degree with respect to rubber, calculated by the following formula (1), of 5.0% or more. (Swelling degree relative to the rubber) (%) = (MM") / M" x 100 (1) (Wherein, M is the volume of 1.1 cm 3 is the mass (g) of a rubber piece after it has been immersed in a plasticizer at 60°C for 42 hours, and M" is the volume (g) of the rubber piece before it was immersed in the plasticizer (1.1 cm 3 is the mass of the rubber piece (g).
[0066] If the swelling degree of the plasticizer relative to the rubber calculated by the formula (1) is less than 5.0%, the adhesive component is less likely to penetrate into the rubber to be reinforced, and the adhesion between the rubber reinforcing fiber and the rubber may decrease. From this viewpoint, the swelling degree is preferably 5.5% or more, and more preferably 6.0% or more. Moreover, since the higher the swelling degree, the better, the upper limit may be 100% or less, 80% or less, or 50% or less. The plasticizer can be appropriately selected depending on the type of rubber to be reinforced. The swelling degree can be specifically measured by the method described in the Examples.
[0067] The plasticizer is not particularly limited as long as the swelling degree with respect to the rubber calculated by the formula (1) is 5.0% or more, and examples thereof include oils such as natural oils and synthetic oils; low molecular weight organic solvents such as methanol and acetone; etc. Among them, oils are preferred from the viewpoint of handling taking into account vapor pressure, flash point, toxicity, etc.
[0068] The natural oils include, for example, mineral oils and vegetable oils. Examples of mineral oils include paraffinic mineral oils, aromatic mineral oils, and naphthenic mineral oils obtained by conventional refining methods such as solvent refining and hydrogenation refining, as well as wax produced by the Fischer-Tropsch process (gas-to-liquid wax) and mineral oils produced by isomerizing wax. Commercially available paraffinic mineral oils include the "Diana Process Oil" series manufactured by Idemitsu Kosan Co., Ltd. and the "Super Oil" series manufactured by JX Energy Corporation. Examples of vegetable oils include linseed oil, camellia oil, macadamia nut oil, corn oil, mink oil, olive oil, avocado oil, camellia oil, castor oil, safflower oil, jojoba oil, sunflower oil, almond oil, rapeseed oil, sesame oil, soybean oil, peanut oil, cottonseed oil, coconut oil, palm kernel oil, and rice bran oil.
[0069] Examples of the synthetic oil include hydrocarbon synthetic oil, ester synthetic oil, ether synthetic oil, etc. Examples of the hydrocarbon synthetic oil include α-olefin oligomers such as polybutene, polyisobutylene, 1-octene oligomer, 1-decene oligomer, and ethylene-propylene copolymer, or hydrogenated products thereof, alkylbenzene, and alkylnaphthalene. Examples of the ester synthetic oil include triglycerin fatty ester, diglycerin fatty acid ester, monoglycerin fatty acid ester, monoalcohol fatty acid ester, polyhydric alcohol fatty acid ester, etc. Examples of the ether synthetic oil include polyoxyalkylene glycol and polyphenyl ether. Commercially available synthetic oils include the "Linearene" series manufactured by Idemitsu Kosan Co., Ltd., "FGC32", "FGC46", and "FGC68" manufactured by ANDEROL Co., Ltd., and "Lubinol HFP-100" manufactured by Lion Corporation.
[0070] The oil may be one selected from the natural oils and synthetic oils, or a mixture of two or more natural oils, two or more synthetic oils, or one or more natural oils and one or more synthetic oils.
[0071] From the viewpoint of safety, the flash point of the oil is preferably 70° C. or higher. From this viewpoint, the flash point of the oil is more preferably 100° C. or higher, even more preferably 130° C. or higher, and even more preferably 140° C. or higher. There is no particular upper limit to the flash point of the oil, but it is preferably 320° C. or lower, more preferably 260° C. or lower, and even more preferably 200° C. or lower.
[0072] <Composition of adhesive components> From the viewpoint of improving adhesive strength with rubber, the content of the reactive multiple bond-containing polymer in the adhesive component is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less. When the content of the reactive multiple bond-containing polymer in the adhesive component is within the above range, it is possible to prevent the viscosity of the adhesive component from becoming extremely high while obtaining sufficient adhesive strength.
[0073] The content of the plasticizer in the adhesive component is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less. When the content of the plasticizer in the adhesive component is within the above range, it is possible to prevent the viscosity of the adhesive component from becoming extremely high while obtaining sufficient adhesive strength.
[0074] The mass ratio of the reactive multiple bond-containing polymer to the plasticizer in the adhesive component [reactive multiple bond-containing polymer (M):plasticizer (P)] is preferably 0.1:9.9 to 5:5, more preferably 0.5:9.5 to 4.5:5.5, and even more preferably 1:9 to 4:6. By mixing the reactive multiple bond-containing polymer and the plasticizer at the specific mass ratio, it becomes possible to lower the viscosity while maintaining the adhesiveness, improving the handleability of the adhesive component and the workability of attaching it to fibers.
[0075] The reactive multiple bond-containing polymer may be used alone or in combination of two or more kinds, and the plasticizer may be used alone or in combination of two or more kinds.
[0076] Furthermore, the adhesive component in the present invention may contain other components in addition to the reactive multiple bond-containing polymer and the plasticizer, within the range that does not impair the adhesive strength with the rubber. Examples of the other components include other polymers (for example, unmodified conjugated diene rubbers), acids, alkalis, surfactants, antioxidants, curing agents, dispersants, pigments, dyes, adhesion aids, and carbon black. When the adhesive component contains other components, the content thereof is preferably 10,000 parts by mass or less, more preferably 1,000 parts by mass or less, even more preferably 100 parts by mass or less, still more preferably 50 parts by mass or less, still more preferably 25 parts by mass or less, and still more preferably 10 parts by mass or less, relative to 100 parts by mass of the reactive multiple bond-containing polymer.
[0077] 〔fiber〕 Although there is no particular limitation on the fibers used for the rubber reinforcing fibers, hydrophilic fibers are preferred from the viewpoint of affinity with the adhesive component. In the present invention, the term "fiber" includes not only monofilaments and long fibers, but also nonwoven fabrics, woven fabrics, knitted fabrics, felts, sponges, and other forms.
[0078] Examples of hydrophilic synthetic fibers include synthetic fibers made of a thermoplastic resin having hydrophilic functional groups such as hydroxyl groups, carboxyl groups, sulfonic acid groups, and amino groups, and / or hydrophilic bonds such as amide bonds. Specific examples of such thermoplastic resins include polyvinyl alcohol-based resins, polyamide-based resins (aliphatic polyamides such as polyamide 6, polyamide 66, polyamide 11, polyamide 12, polyamide 610, polyamide 612, and polyamide 9C (a polyamide composed of nonanediamine and cyclohexanedicarboxylic acid); semi-aromatic polyamides synthesized from aromatic dicarboxylic acids and aliphatic diamines, such as polyamide 9T (a polyamide composed of nonanediamine and terephthalic acid); wholly aromatic polyamides synthesized from aromatic dicarboxylic acids and aromatic diamines, such as polyparaphenylene terephthalamide), and polyacrylamide-based resins). Among these, polyvinyl alcohol-based resins and polyamide-based resins are preferred. The hydrophilic synthetic fibers may be used alone or in combination of two or more. In addition, these hydrophilic synthetic fibers may be further subjected to a hydrophilization treatment described below in order to further enhance the hydrophilicity.
[0079] Examples of hydrophilic natural fibers include natural cellulose fibers such as wood pulp, e.g., kraft pulp, and non-wood pulp, e.g., cotton pulp and straw pulp. Hydrophilic regenerated fibers include regenerated cellulosic fibers such as rayon, lyocell, cupra, and polynosic. These natural fibers and regenerated fibers may be used alone or in combination of two or more. Furthermore, these hydrophilic natural fibers and regenerated fibers may be further subjected to a hydrophilization treatment described later in order to further enhance the hydrophilicity.
[0080] The hydrophilic fiber may have at least a hydrophilic surface, and may be, for example, a hydrophobic fiber whose surface has been hydrophilized, or a core-sheath type composite fiber in which a hydrophobic resin is used as the core and a hydrophilic resin is used as the sheath. For examples of hydrophilic resins constituting the sheath, the description of hydrophilic synthetic fibers is cited. Examples of hydrophobic fibers made of hydrophobic resins include polyolefin fibers such as polyethylene and polypropylene, polyester fibers such as polyethylene terephthalate, and wholly aromatic polyester fibers, and among these, polyester fibers are preferred.
[0081] The hydrophilization treatment is not particularly limited as long as it is a treatment that chemically or physically imparts hydrophilic functional groups to the fiber surface. For example, the hydrophilic treatment can be carried out by a method in which a hydrophobic fiber made of the hydrophobic resin is modified with a compound containing a hydrophilic functional group such as an isocyanate group, an epoxy group, a hydroxyl group, an amino group, an ether group, an aldehyde group, a carbonyl group, a carboxyl group, or a urethane group, or a derivative thereof, or by a method in which the surface is modified by electron beam irradiation.
[0082] As the hydrophilic fibers used in the present invention, from the viewpoint of being used as rubber reinforcing fibers, synthetic fibers and regenerated fibers are preferred, and among them, one or more types selected from polyvinyl alcohol-based fibers made from polyvinyl alcohol-based resins, regenerated cellulose fibers, and fibers whose surfaces have been hydrophilized with a hydrophobic fiber are preferred. In the present invention, by using hydrophilic fibers, a strong affinity effect is exerted between the reactive multiple bond-containing polymer contained in the adhesive component and the hydrophilic fibers, and the adhesive component and the hydrophilic fibers are firmly bound together, thereby making it possible to improve the adhesive strength to rubber. As the polyvinyl alcohol-based fiber, from the viewpoint of suitably using the rubber-reinforced fiber for fluid transport hoses for automobiles, particularly for automobile brake oil hoses, it is commercially available from Kuraray Co., Ltd. under the product name "Vinylon", and one having a single fiber fineness of about 0.1 to 30 dtex can be suitably used. In the present invention, one type of fiber may be used alone, or two or more types may be used in combination.
[0083] [Properties of rubber reinforcing fibers] The rubber reinforcing fiber is preferably a multifilament having a single yarn fineness of 0.1 dtex or more and 30 dtex or less. The single yarn fineness may be less than 0.1 dtex, but is preferably 0.1 dtex or more since industrial production is difficult. Furthermore, if the single yarn fineness is 30 dtex or less, the surface area of the fiber when used as a rubber reinforcing fiber is large, improving adhesion to rubber. From this viewpoint, the rubber reinforcing fiber is preferably a multifilament having a single yarn fineness of more preferably 0.3 dtex or more, even more preferably 0.5 dtex or more, still more preferably 1 dtex or more, and more preferably 20 dtex or less, even more preferably 15 dtex or less, and still more preferably 10 dtex or less.
[0084] The rubber adhesive strength of the rubber reinforcing fiber is preferably 15 N / 25.4 mm or more, more preferably 20 N / 25.4 mm or more, even more preferably 25 N / 25.4 mm or more, even more preferably 30 N / 25.4 mm or more, and usually 200 N / 25.4 mm or less. When the rubber adhesive strength of the rubber reinforcing fiber is the lower limit value or more, a molded product having excellent adhesive strength with rubber can be obtained. The rubber adhesive strength of the rubber reinforcing fiber can be measured by the method described in the Examples.
[0085] The rubber reinforcing fiber can be used in any shape, but is preferably used in the form of a fiber cord, woven fabric, knitted fabric, etc., which contains the rubber reinforcing fiber at least in part, and is more preferably used as a woven fabric or knitted fabric which contains the rubber reinforcing fiber at least in part. For example, it can be used as a knitted fabric to be bonded to rubber, as described later. It can also be used as a rubber reinforcing fiber to be embedded in resin, cement, etc.
[0086] [Rubber] The rubber used in the present invention is made of a rubber composition obtained by compounding a rubber component with compounding agents usually used in the rubber industry. The rubber component is not particularly limited, but examples thereof include NR (natural rubber), IR (polyisoprene rubber), BR (polybutadiene rubber), SBR (styrene-butadiene rubber), NBR (nitrile rubber), EPM (ethylene-propylene copolymer rubber), EPDM (ethylene-propylene-non-conjugated diene copolymer rubber), IIR (butyl rubber), halogenated butyl rubber, and CR (chloroprene rubber). Among these, it is preferable to use NR, IR, BR, SBR, NBR, EPDM, IIR, and CR, and it is more preferable to use NBR, CREPDM, and IIR. These rubber components may be used alone or in combination of two or more. For tire applications, rubbers generally used in the tire industry can be used. Of these, it is preferable to use natural rubber alone or a combination of natural rubber and SBR. When natural rubber and SBR are combined, the mass ratio of natural rubber to SBR (natural rubber / SBR) is preferably in the range of 50 / 50 to 90 / 10 from the viewpoint of suppressing deterioration of physical properties due to reversion of rubber.
[0087] Examples of the natural rubber include natural rubber commonly used in the tire industry, such as TSR (Technically Specified Rubber) including SMR (Malaysian TSR), SIR (Indonesian TSR), and STR (Thailand TSR), and RSS (Ribbed Smoked Sheet); highly purified natural rubber, modified natural rubber including epoxidized natural rubber, hydroxylated natural rubber, hydrogenated natural rubber, and grafted natural rubber.
[0088] The SBR may be any of those commonly used in tires, but more specifically, the styrene content is preferably 0.1 to 70% by mass, more preferably 5 to 50% by mass, and even more preferably 15 to 35% by mass, and the vinyl content is preferably 0.1 to 60% by mass, and more preferably 0.1 to 55% by mass. The weight average molecular weight (Mw) of the SBR is preferably 100,000 to 2,500,000, more preferably 150,000 to 2,000,000, and even more preferably 200,000 to 1,500,000. Within the above range, both processability and mechanical strength can be achieved. The weight average molecular weight of the SBR is the weight average molecular weight calculated in terms of polystyrene and determined by gel permeation chromatography (GPC). The SBR may be modified SBR in which a functional group has been introduced into SBR, as long as the effect of the present invention is not impaired. Examples of the functional group include an amino group, an alkoxysilyl group, a hydroxy group, an epoxy group, and a carboxy group.
[0089] The rubber composition may further contain a filler in addition to the rubber component. Examples of the filler include inorganic fillers such as carbon black, silica, clay, mica, calcium carbonate, magnesium hydroxide, aluminum hydroxide, barium sulfate, titanium oxide, glass fiber, fibrous filler, and glass balloons; and organic fillers such as resin particles, wood powder, and cork powder. By including such a filler in the rubber composition, it is possible to improve physical properties such as mechanical strength, heat resistance, and weather resistance, adjust hardness, and increase the amount of rubber. From the viewpoint of improving physical properties such as mechanical strength, carbon black and silica are preferred among the above fillers.
[0090] Examples of the carbon black include furnace black, channel black, thermal black, acetylene black, and ketjen black. Among these carbon blacks, furnace black is preferred from the viewpoint of improving the crosslinking rate and mechanical strength. The average particle size of the carbon black is preferably 5 to 100 nm, more preferably 5 to 80 nm, and even more preferably 5 to 70 nm. The average particle size of the carbon black can be determined by measuring the diameter of the particles using a transmission electron microscope and calculating the average value.
[0091] Examples of the silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, aluminum silicate, etc. Among these silicas, wet silica is preferred. The average particle size of the silica is preferably from 0.5 to 200 nm, more preferably from 5 to 150 nm, and even more preferably from 10 to 100 nm. The average particle size of the silica can be determined by measuring the diameter of the particles using a transmission electron microscope and calculating the average value.
[0092] In the rubber composition, the amount of the filler per 100 parts by mass of the rubber component is preferably 20 to 150 parts by mass, more preferably 25 to 130 parts by mass, and further preferably 25 to 110 parts by mass. When a filler other than silica and carbon black is used as the filler, the content thereof is preferably 20 to 120 parts by mass, more preferably 20 to 90 parts by mass, and further preferably 20 to 80 parts by mass, based on 100 parts by mass of the rubber component. These fillers may be used alone or in combination of two or more.
[0093] The rubber composition may further contain a crosslinking agent to crosslink the rubber component. Examples of the crosslinking agent include sulfur, sulfur compounds, oxygen, organic peroxides, phenolic resins, amino resins, quinone and quinone dioxime derivatives, halogen compounds, aldehyde compounds, alcohol compounds, epoxy compounds, metal halides and organometallic halides, and silane compounds. These crosslinking agents may be used alone or in combination of two or more. From the viewpoint of the mechanical properties of the crosslinked product, the crosslinking agent is contained in an amount of usually 0.1 to 10 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.8 to 5 parts by mass, per 100 parts by mass of the rubber component.
[0094] The rubber composition may further contain a vulcanization accelerator when sulfur, a sulfur compound, etc. are contained as a crosslinking agent for crosslinking (vulcanizing) the rubber component. Examples of the vulcanization accelerator include guanidine-based compounds, sulfenamide-based compounds, thiazole-based compounds, thiuram-based compounds, thiourea-based compounds, dithiocarbamic acid-based compounds, aldehyde-amine-based compounds, aldehyde-ammonia-based compounds, imidazoline-based compounds, and xanthate-based compounds. These vulcanization accelerators may be used alone or in combination of two or more. The vulcanization accelerator is usually contained in an amount of 0.1 to 15 parts by mass, preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the rubber component.
[0095] When the rubber composition contains sulfur or a sulfur compound as a crosslinking agent for crosslinking (vulcanizing) the rubber component, the rubber composition may further contain a vulcanization aid. Examples of the vulcanization aid include fatty acids such as stearic acid, metal oxides such as zinc oxide, and fatty acid metal salts such as zinc stearate. These vulcanization aids may be used alone or in combination of two or more. The vulcanization aid is usually contained in an amount of 0.1 to 15 parts by mass, preferably 1 to 10 parts by mass, based on 100 parts by mass of the rubber component.
[0096] When the rubber composition contains silica as a filler, it is preferable that the rubber composition further contains a silane coupling agent, such as a sulfide compound, a mercapto compound, a vinyl compound, an amino compound, a glycidoxy compound, a nitro compound, or a chloro compound. These silane coupling agents may be used alone or in combination of two or more. The silane coupling agent is preferably contained in an amount of 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, and even more preferably 1 to 15 parts by mass, based on 100 parts by mass of silica. When the content of the silane coupling agent is within the above range, dispersibility, coupling effect, and reinforcing property are improved.
[0097] The rubber composition may contain, as needed, a softener such as silicone oil, aromatic oil, TDAE (Treated Distilled Aromatic Extracts), MES (Mild Extracted Solvates), RAE (Residual Aromatic Extracts), process oil such as paraffin oil or naphthene oil, aliphatic hydrocarbon resin, alicyclic hydrocarbon resin, C9 resin, rosin resin, coumarone-indene resin, or phenol resin, for the purpose of improving processability, flowability, etc., within a range that does not impair the effects of the present invention. When the rubber composition contains the process oil as a softener, the content thereof is preferably less than 50 parts by mass per 100 parts by mass of the rubber component.
[0098] The rubber composition may contain additives such as antiaging agents, waxes, antioxidants, lubricants, light stabilizers, scorch inhibitors, processing aids, colorants such as pigments and dyes, flame retardants, antistatic agents, matting agents, antiblocking agents, UV absorbers, release agents, foaming agents, antibacterial agents, antifungal agents, and fragrances, as necessary, for the purpose of improving weather resistance, heat resistance, oxidation resistance, and the like, within a range that does not impair the effects of the present invention. Examples of the antioxidant include hindered phenol compounds, phosphorus compounds, lactone compounds, and hydroxyl compounds. Examples of the antiaging agents include amine-ketone compounds, imidazole compounds, amine compounds, phenol compounds, sulfur compounds, and phosphorus compounds. These additives may be used alone or in combination of two or more.
[0099] The molded article of the present invention is not particularly limited as long as it contains the rubber reinforcing fiber and rubber. From the viewpoint of maintaining the shape of the rubber, the rubber reinforcing fiber used in the molded article is preferably used as a woven or knitted fabric at least partially containing the rubber reinforcing fiber, and more preferably used as a laminate in which a reinforcing layer made of a woven or knitted fabric at least partially containing the rubber reinforcing fiber and a rubber layer are laminated.
[0100] The molded article can be used as a component of rubber products such as tires, e.g., automobile tires, belts, e.g., conveyor belts, timing belts, hoses, and vibration-proof rubber. Among these, it is more preferable to use the molded article as a tire, a belt, or a hose. In the automobile tires, the present invention can be used for various members, such as belts, carcass plies, breakers, bead tapes, etc., which are made of a composite material of rubber reinforcing fibers and a rubber component. The hose can be used for the purpose of transporting various fluids in various applications, and is suitable, for example, as a hose for transporting fluids in automobiles. In particular, it is preferable to use the hose as a hose for liquid fuels in automobiles, a brake oil hose, and a hose for refrigerants in automobiles, and it is more preferable to use the hose as a brake oil hose in automobiles.
[0101] [Method of manufacturing molded body] The method for producing a molded article of the present invention includes a step of adhering a mixture of a polymer having one or more types of multiple bonds selected from reactive carbon-carbon double bonds and reactive carbon-carbon triple bonds in the molecule and a plasticizer to a fiber to obtain a rubber reinforcing fiber; The method includes a step of overlapping the obtained rubber reinforcing fiber and rubber and vulcanizing them.
[0102] (Step for obtaining rubber reinforcing fibers) In this process, a polymer having one or more types of multiple bonds selected from reactive carbon-carbon double bonds and reactive carbon-carbon triple bonds in its molecule (reactive multiple bond-containing polymer) is mixed with a plasticizer and attached to the fibers. By adhering the reactive multiple bond-containing polymer and the plasticizer in a mixed state to the fibers, the reactive multiple bond-containing polymer can be efficiently adhered to the fibers and contamination of the production equipment can be suppressed.
[0103] When the reactive multiple bond-containing polymer and the plasticizer are mixed, a surfactant may be further added to form an oil-in-water emulsion. By forming an oil-in-water emulsion, the viscosity can be suppressed from increasing and the handling property can be improved. In addition, by attaching the oil-in-water emulsion to a fiber, the adhesive component containing the reactive multiple bond-containing polymer, the plasticizer, and the surfactant can be attached to the fiber more uniformly and efficiently. The surfactant may be mixed with the reactive multiple bond-containing polymer and the plasticizer simultaneously, or the reactive multiple bond-containing polymer and the plasticizer may be mixed together, and then the surfactant may be mixed into the resulting mixture.
[0104] The surfactant is not particularly limited, and examples thereof include cationic surfactants, anionic surfactants, nonionic surfactants, and amphoteric surfactants. Among these, nonionic surfactants are preferred from the viewpoint of compatibility between the adhesive component and the rubber. These surfactants may be used alone or in combination of two or more. Examples of nonionic surfactants include polyoxyalkylene-type nonionic surfactants such as higher alcohol alkylene oxide adducts, alkylphenol alkylene oxide adducts, styrenated phenol alkylene oxide adducts, fatty acid alkylene oxide adducts, polyhydric alcohol aliphatic ester alkylene oxide adducts, higher alkylamine alkylene oxide adducts, and fatty acid amide alkylene oxide adducts; and polyhydric alcohol-type nonionic surfactants such as alkylglycoxides and sucrose fatty acid esters.
[0105] As a more specific method for producing rubber reinforcing fibers, from the viewpoint of obtaining a molded article having excellent adhesion to rubber, method (I) of forming an adhesive layer made of the adhesive component on the surface of the fiber is preferred.
[0106] [Method (I)] There are no particular limitations on method (I) as long as it is a method for forming an adhesive layer made of the adhesive component on the surface of the fiber. From the viewpoint of obtaining a molded product having excellent adhesion to rubber, a method having the following step I-1 is preferred. Step I-1: A step of attaching the adhesive component to the surface of the fiber
[0107] In step I-1, the method for attaching the adhesive component to the fiber is not particularly limited, and examples thereof include a method in which the adhesive component is attached as is, a method in which a solvent is added to the adhesive component as necessary, and the like. The adhesive component is preferably applied by one or more methods selected from immersion, roll coater, oiling roller, oiling guide, nozzle (spray) application, brush application, and the like.
[0108] From the viewpoint of improving adhesion between the rubber reinforcing fiber and the rubber, the amount of the adhesive component attached is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, relative to 100% by mass of the rubber reinforcing fiber, and is preferably 10.0% by mass or less, more preferably 8.0% by mass or less, and even more preferably 6.0% by mass or less.
[0109] In the present invention, since the reactive multiple bond-containing polymer and the plasticizer are used in combination, the adhesive component is attached to the fiber, and then the fiber is allowed to settle at room temperature of about 20°C for about 3 to 10 days to obtain the rubber reinforcing fiber. In some cases, however, the following step I-2 may be carried out. Step I-2: A step of heat treating the fiber to which the adhesive component is attached obtained in step I-1 The heat treatment in step I-2 is preferably carried out at a treatment temperature of 100 to 200° C. for a treatment time of 0.1 seconds to 2 minutes. Since the reactive multiple bond-containing polymer contained in the adhesive component has reactive multiple bonds, the heat treatment in the presence of oxygen is preferably carried out at 200° C. or less, and more preferably at 175° C. or less. When the heat treatment temperature is within the above range, the amount of reactive multiple bonds in the reactive multiple bond-containing polymer is not reduced, and the adhesive strength with the rubber can be improved, fiber deterioration is suppressed, and quality such as coloring is also improved.
[0110] The rubber reinforcing fiber may contain other components in addition to the hydrophilic fiber and the adhesive component, such as a crosslinking agent, an acid, a base, an inorganic salt, an organic salt, a pigment, a dye, an antioxidant, and a polymerization initiator. The total content of the hydrophilic fibers and the adhesive components in the rubber reinforcing fibers is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, from the viewpoint of improving adhesive strength with rubber and reinforcing strength.
[0111] (The process of layering rubber reinforcing fibers and rubber and vulcanizing them) In this process, the rubber reinforcing fiber obtained in the previous process and rubber are overlapped and vulcanized. Specifically, the rubber reinforcing fiber is embedded in an unvulcanized rubber composition, and the rubber composition is vulcanized to obtain a molded article in which the rubber reinforcing fiber and the rubber component are bonded via the adhesive component. As the rubber composition, those explained in the section [Rubber] can be used.
[0112] An example of a hose for transporting fluid is one which has an inner rubber layer and an outer rubber layer, and has one or two reinforcing layers made of the above-mentioned rubber reinforcing fibers between the inner rubber layer and the outer rubber layer. Examples of the rubber components constituting the inner rubber layer and the outer rubber layer include those mentioned above. Among them, examples of the rubber components constituting the inner rubber layer include NBR, IIR, EPDM, SBR, etc., and examples of the rubber components constituting the outer rubber layer include NBR, IIR, EPDM, CR, etc. The reinforcing layer can be formed by braiding rubber reinforcing fibers. In the method for producing the fluid transport hose, a reinforcing layer (first reinforcing layer) made by braiding the rubber reinforcing fibers is formed on the outer surface of the inner rubber layer. When forming two reinforcing layers, an intermediate rubber layer may be further formed on the outer surface of the first reinforcing layer, and a reinforcing layer (second reinforcing layer) made by braiding the rubber reinforcing fibers may be formed on the outer surface of the intermediate rubber layer. Then, the outer rubber layer is formed on the outer surface of the reinforcing layer (first reinforcing layer or second reinforcing layer), and the hose can be produced by vulcanizing the outer rubber layer. The vulcanization temperature can be appropriately selected depending on the types of materials constituting each layer of the hose, but from the viewpoint of suppressing deterioration of the rubber and the rubber reinforcing fibers and improving the adhesive strength between the rubber and the rubber reinforcing fibers, it is preferable that the vulcanization temperature be 200°C or lower. EXAMPLES
[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0114] [Production of reactive multiple bond-containing polymers] As reactive multiple bond-containing polymers, modified conjugated diene rubbers having monomer units represented by the following formulas (1a) to (1c), and modified conjugated diene rubbers having hydrogen-bonding functional groups at the molecular terminals represented by the following formula (1d) were produced.
[0115] Production of modified conjugated diene rubber having a monomer unit represented by the following formula (1a):
[0116] [ka]
[0117] Production Example 1: Production of modified conjugated diene rubber (A-1) A 5L autoclave that was thoroughly dried was purged with nitrogen, and 1260g of hexane and 36.3g of n-butyllithium (17% by mass hexane solution) were charged. The temperature was raised to 50°C, and then 1260g of butadiene was added successively while controlling the polymerization temperature to 50°C under stirring conditions, and polymerization was carried out for 1 hour. Methanol was then added to terminate the polymerization reaction, and a polymer solution was obtained. Water was added to the obtained polymer solution, and the mixture was stirred, and the polymer solution was washed with water. After stopping the stirring, it was confirmed that the polymer solution phase and the water phase were separated, and then the water was separated. The polymer solution after washing was vacuum dried at 70°C for 24 hours to obtain unmodified liquid polybutadiene. Next, 500 g of the unmodified liquid polybutadiene obtained was charged into a 1 L autoclave that had been purged with nitrogen, and 25 g of maleic anhydride and 0.5 g of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (trade name "Nocrac 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added and reacted at 170°C for 24 hours to obtain maleic anhydride-modified liquid polybutadiene. 8.1 g of methanol was added to 500 g of the maleic anhydride-modified liquid polybutadiene obtained, and the mixture was reacted at 80°C for 6 hours to obtain monomethyl maleate-modified liquid polybutadiene (A-1).
[0118] Production of modified conjugated diene rubber having a monomer unit represented by the following formula (1b):
[0119] [ka]
[0120] Production Example 2: Production of modified conjugated diene rubber (A-2) A 5L autoclave that was thoroughly dried was purged with nitrogen, and 1200g of hexane and 26.2g of n-butyllithium (17% by mass hexane solution) were charged. The temperature was raised to 50°C, and then 1200g of isoprene was added successively while controlling the polymerization temperature to 50°C under stirring conditions, and polymerization was carried out for 1 hour. Methanol was then added to terminate the polymerization reaction, and a polymer solution was obtained. Water was added to the obtained polymer solution, and the mixture was stirred, and the polymer solution was washed with water. After stopping the stirring, it was confirmed that the polymer solution phase and the water phase were separated, and then the water was separated. The polymer solution after washing was vacuum dried at 70°C for 24 hours to obtain unmodified liquid polyisoprene. Next, 500 g of the unmodified liquid polyisoprene obtained was charged into a 1 L autoclave that had been purged with nitrogen, and 25 g of maleic anhydride and 0.5 g of butylated hydroxytoluene (BHT) were added and reacted at 170° C. for 15 hours to obtain maleic anhydride-modified liquid polyisoprene. 8.1 g of methanol was added to 500 g of the maleic anhydride-modified liquid polyisoprene obtained, and the mixture was reacted at 80° C. for 6 hours to obtain monomethyl maleate-modified liquid polyisoprene (A-2).
[0121] Production of modified conjugated diene rubber (A-3) having a monomer unit represented by the following formula (1c):
[0122] [ka]
[0123] Production Example 3: Production of modified conjugated diene rubber (A-3) A 5L autoclave that was thoroughly dried was purged with nitrogen, and 1500g of cyclohexane and 12.6g of sec-butyllithium (10.5% by mass cyclohexane solution) were charged. The temperature was raised to 50°C, and then 1500g of butadiene was successively added and polymerized for 1 hour while controlling the polymerization temperature to 50°C under stirring conditions. Next, 75g of farnesene was added to this and polymerized for another 1 hour, and then methanol was added to stop the polymerization reaction, to obtain a polymer solution. Water was added to the obtained polymer solution and stirred, and the polymer solution was washed with water. After stopping the stirring and confirming that the polymer solution phase and the water phase were separated, the water was separated. The polymer solution after washing was vacuum dried at 70°C for 24 hours to obtain an unmodified liquid polyfarnesene polybutadiene copolymer. Next, 500 g of the unmodified liquid polyfarnesene polybutadiene copolymer obtained was charged into a 1 L autoclave that had been purged with nitrogen, and 25 g of maleic anhydride and 0.5 g of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (trade name "Nocrac 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added, and the mixture was reacted at 170 ° C. for 24 hours to obtain a maleic anhydride-modified liquid polyfarnesene polybutadiene copolymer. Further, 8.1 g of methanol was added to the maleic anhydride-modified liquid polyfarnesene polybutadiene copolymer obtained, and the mixture was reacted at 80 ° C. for 6 hours to obtain a monomethyl maleate-modified liquid polyfarnesene polybutadiene copolymer (A-3).
[0124] Production of modified conjugated diene rubber (A-4) having a hydrogen-bonding functional group at the molecular end represented by the following formula (1d):
[0125] [ka]
[0126] Production Example 4: Production of modified conjugated diene rubber (A-4) A 5L autoclave was thoroughly dried and substituted with nitrogen, and 1200g of cyclohexane, 54g of sec-butyllithium (10.5% by mass solution in cyclohexane), and 2.06g of TMEDA were charged. The temperature was raised to 50°C, and then 1300g of butadiene was added successively at 10ml / min under stirring conditions while controlling the polymerization temperature to 50°C. After the addition of butadiene, the mixture was heated for 1 hour to complete the polymerization. 16.6g of triisopropyl borate was added to the obtained polymerization solution to introduce boronic acid to the polymerization terminal (terminal introduction rate 95%). Ion-exchanged water was added to the obtained polymer solution and stirred to wash the polymer solution. After confirming that the polymer solution phase and the water phase were separated, the polymer solution phase was collected and dried under reduced pressure at 90°C for 12 hours to obtain boronic acid-modified liquid polybutadiene (A-4).
[0127] The methods for measuring and calculating the properties of the modified conjugated diene rubber are as follows. The results are shown in Table 1. <Methods for measuring weight average molecular weight, number average molecular weight and molecular weight distribution> The Mw, Mn and Mw / Mn of the modified conjugated diene rubber were determined as values converted into standard polystyrene by GPC (gel permeation chromatography) using the following measuring device and conditions: · Apparatus: Tosoh Corporation GPC device "GPC8020" Separation column: Tosoh Corporation's "TSKgelG4000HXL" Detector: Tosoh Corporation "RI-8020" Eluent: Tetrahydrofuran ·Eluent flow rate: 1.0ml / min Sample concentration: 5mg / 10ml Column temperature: 40℃
[0128] <Melt viscosity measurement method> The melt viscosity of the modified conjugated diene rubber at 38° C. was measured using a Brookfield viscometer (manufactured by BROOKFIELD ENGINEERING LABS. INC.).
[0129] <Method of measuring glass transition temperature> 10 mg of the modified conjugated diene rubber was placed in an aluminum pan, and a thermogram was measured by differential scanning calorimetry (DSC) at a heating rate of 10° C. / min. The DDSC peak top value was taken as the glass transition temperature.
[0130] <Average number of hydrogen-bonding functional groups per molecule> The average number of hydrogen-bonding functional groups per molecule of the modified conjugated diene rubber was calculated from the equivalent weight (g / eq) of the hydrogen-bonding functional groups of the modified conjugated diene rubber and the number average molecular weight Mn in terms of styrene by the following formula. Average number of hydrogen-bonding functional groups per molecule = [(number average molecular weight (Mn)) / (molecular weight of styrene unit) x (average molecular weight of conjugated diene and other monomer units other than conjugated diene contained as necessary)] / (equivalent weight of hydrogen-bonding functional group) The method for calculating the equivalent weight of the hydrogen-bonding functional group can be appropriately selected depending on the type of the hydrogen-bonding functional group.
[0131] The average number of hydrogen-bonding functional groups per molecule of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber was calculated by determining the acid value of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber and calculating the equivalent weight (g / eq) of the hydrogen-bonding functional group from the acid value. After the modification reaction, the sample was washed four times with methanol (5 mL per 1 g of sample) to remove impurities such as antioxidants, and then dried under reduced pressure at 80° C. for 12 hours. 180 mL of toluene and 20 mL of ethanol were added to 3 g of the sample after the modification reaction to dissolve it, and then neutralized with a 0.1 N ethanol solution of potassium hydroxide, and the acid value was calculated using the following formula. Acid value (mgKOH / g)=(AB)×F×5.611 / S A: Amount of 0.1N potassium hydroxide ethanol solution added for neutralization (mL) B: Amount of 0.1N potassium hydroxide ethanol solution dropped into a blank containing no sample (mL) F: Potency of 0.1N potassium hydroxide in ethanol S: mass of weighed sample (g)
[0132] From the acid value, the mass of the hydrogen-bonding functional group contained in 1 g of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber was calculated using the following formula, and the mass other than the functional group (polymer main chain mass) contained in 1 g of the monomethyl maleate-modified conjugated diene rubber and the boronic acid-modified conjugated diene rubber was calculated. Then, the equivalent weight (g / eq) of the hydrogen-bonding functional group was calculated using the following formula. [Hydrogen-bonding functional group mass per 1 g] = [acid value] / [56.11] x [hydrogen-bonding functional group molecular weight] / 1000 [Mass of polymer main chain per 1g] = 1 - [Mass of hydrogen-bonding functional group per 1g] [Equivalent weight of hydrogen-bonding functional group] = [mass of polymer main chain per 1 g] / ([mass of hydrogen-bonding functional group per 1 g] / [molecular weight of hydrogen-bonding functional group])
[0133] [Table 1]
[0134] [Example 1] (1) Manufacturing of rubber reinforcing fibers having an adhesive component on at least a portion of the surface of the fibers The modified conjugated diene rubber (A-1) obtained in the above-mentioned Production Example 1 was mixed as a reactive multiple bond-containing polymer with a fatty acid ester (trade name "Rubinol HFP-100", manufactured by Lion Corporation) having a swelling degree of 5.0% or more with respect to NBR of the following compounding composition as a plasticizer in a mass ratio of 3:7 to obtain an adhesive component. This adhesive component was applied to vinylon fiber that had been subjected to a hydrophilization treatment described below using an oiling guide, and then the fiber was wound up. The vinylon fiber to which the adhesive component had been attached in this way was twisted at a twist rate of 45 T / m to produce a fiber cord.
[0135] [NBR compound composition] NBR rubber: 100 parts by mass Filler (carbon black): 30 parts by weight Vulcanizing agent (thiol type): 5 parts by mass Vulcanization aid (zinc oxide, stearic acid): 11 parts by mass Vulcanization accelerator (peroxide): 6 parts by mass
[0136] [Hydrophilic Treatment of Vinylon Fiber] A polyvinyl alcohol fiber, Vinylon fiber ("Kuraray Co., Ltd." "Kuralon 1239", total fineness 1330 dtex, single yarn fineness 6.65 dtex) was immersed in an aqueous solution prepared to the following composition, and then the liquid was squeezed out with a roller. The resulting fiber was then dried at 120°C for 5 seconds, and further heat-treated at 240°C for 5 seconds and wound up to produce a hydrophilized Vinylon fiber.
[0137] [Composition of hydrophilic treatment agent for vinylon fiber] Water: 86.8 parts by mass Meikanote DM-350Z: 4.8 parts by weight Denacol EX-512: 2 parts by weight The hydrophilic treatment agent was prepared using a blocked isocyanate and an epoxy resin. As the blocked isocyanate, "Meikanote DM-350Z" manufactured by Meisei Chemical Industry Co., Ltd. was used, and as the epoxy resin, "Denacol EX-512" manufactured by Nagase ChemteX Corporation was used.
[0138] (2) Production of molded articles containing rubber reinforcing fibers and rubber The fiber cords obtained in (1) were arranged on a masking tape in a curtain-like shape so that the fiber cords did not overlap each other, and then the unvulcanized NBR rubber (width 25.4 mm, length 240 mm) having the above-mentioned compounding composition was overlaid. Then, the fiber cords were heated at 150°C under a pressure of 20 kg / cm. 2 A molded product was produced by press-vulcanizing for 30 minutes under the above conditions.
[0139] [Comparative Example 1] A fiber cord and a molded body were produced in the same manner as in Example 1, except that a mineral oil (purity 99.9% or more, flash point 184°C) having a swelling degree of less than 5.0% with respect to the NBR of the above-mentioned blended composition was used as the plasticizer.
[0140] [Examples 2 to 6] Fiber cords and molded bodies were produced in the same manner as in Example 1, except that the modified conjugated diene rubber, the mass ratio of the modified conjugated diene rubber to the plasticizer, and the amount of adhesive component attached to the fiber were changed as shown in Table 2.
[0141] [Example 7] A fiber cord and a molded body were produced in the same manner as in Example 1, except that the rubber to be reinforced was changed to IIR with the following compounding composition, a mineral oil (purity 99.9% or more, flash point 184°C) with a swelling degree for IIR of 5.0% or more was used as the plasticizer, and the amount of adhesive component attached to the fiber was changed as shown in Table 2.
[0142] [IIR composition] IIR rubber: 100 parts by mass Softener (process oil): 5 parts by weight Anti-aging agent: 2 parts by mass Filler (carbon black): 60 parts by weight Vulcanizing agent (sulfur powder): 1.5 parts by weight Vulcanization aid (zinc oxide, stearic acid): 7 parts by mass Vulcanization accelerator (thiuram type, thiazole type): 2 parts by mass
[0143] [Comparative Example 2] A fiber cord and a molded body were produced in the same manner as in Example 7, except that a fatty acid ester having a swelling degree to IIR of less than 5.0% (product name: Luvinol HFP-100, manufactured by Lion Corporation) was used as the plasticizer.
[0144] [Example 8] A fiber cord and a molded article were produced in the same manner as in Example 1, except that PET fibers that had been subjected to a hydrophilization treatment described below were used as the fibers.
[0145] [Comparative Example 3] A fiber cord and a molded product were produced in the same manner as in Comparative Example 1, except that PET fibers that had been subjected to a hydrophilization treatment described below were used as the fibers.
[0146] [Hydrophilic treatment of PET fibers] PET fiber (Toray Industries, Inc. "702C", total fineness 1670 dtex, single yarn fineness 5.80 dtex), a polyester fiber that had been immersed in hexane to wash off the oil components on the fiber, was immersed in an aqueous solution prepared to the composition below, and then squeezed with a roller. The fiber obtained was then dried at 120°C for 5 seconds, and further heat-treated at 240°C for 5 seconds and wound up to produce a hydrophilized PET fiber.
[0147] [Composition of hydrophilic treatment agent for PET fiber] Water: 86.8 parts by mass Meikanote DM-350Z: 2 parts by weight Denacol EX-512: 4.8 parts by mass The hydrophilic treatment agent was prepared using a blocked isocyanate and an epoxy resin. As the blocked isocyanate, "Meikanote DM-350Z" manufactured by Meisei Chemical Industry Co., Ltd. was used, and as the epoxy resin, "Denacol EX-512" manufactured by Nagase ChemteX Corporation was used.
[0148] <Measurement of swelling degree of plasticizer in rubber to be reinforced> The swelling degree was measured with reference to JIS-K-6258:2016. A 0.7 mm thick unvulcanized rubber sample to be reinforced was heated at 150°C and a pressure of 20 kg / cm. 2 A rubber sheet was press-vulcanized for 30 minutes under the above conditions, and cut into a size of 4.0 cm length x 4.0 cm width to prepare a test specimen for evaluation. The mass M" of the obtained test specimen before immersion in the plasticizer was measured. Next, the test specimen was placed in a test container, and enough plasticizer was added to the test container so that the test specimen was completely immersed in the liquid, and the test specimen was left to stand at 60°C for 42 hours using a hot air dryer. After immersion, the test specimen was removed, and excess plasticizer adhering to the surface of the test specimen was wiped off with a rag. The mass M of the test specimen was immediately measured, and the swelling degree was calculated from the following formula (1). (Swelling degree relative to rubber)(%)=(MM”) / M”×100 (1) In the formula (1), M is the volume of 1.1 cm 3 is the mass (g) of a rubber piece after it has been immersed in a plasticizer at 60°C for 42 hours, and M" is the volume (g) of the rubber piece before it was immersed in the plasticizer (1.1 cm 3 is the mass of the rubber piece (g).
[0149] <Measurement of adhesion amount of adhesive component> The amount of the adhesive component attached was measured by the following method. Approximately 10 g of the obtained fiber cord was collected as a sample, and its mass X (g) was measured. The adhesive component was extracted from the sample, and the extracted mass Y (g) was measured. Toluene was used as the solvent for extraction, and extraction was performed for 3 hours using a Soxhlet extractor. The adhesion amount of the adhesive component was calculated using the following formula (2). Amount of adhesive component attached to rubber reinforcing fiber (mass%) = (Y / X) × 100 (2) The reactive multiple bond-containing polymer content (mass %) in the adhesive component was calculated from the mass ratio of the reactive multiple bond-containing polymer in the solid content of the adhesive component.
[0150] <Rubber adhesive strength measurement> The force (N / 25.4 mm) required to perform T-type peeling from the rubber of the fiber cords of the molded articles obtained in Examples 1 to 8 and Comparative Examples 1 to 3 was measured and evaluated as rubber adhesion. The results are shown in Table 2. In the evaluation results of rubber adhesion, a higher numerical value indicates a higher adhesive strength between the rubber reinforcing fiber and the rubber.
[0151] [Table 2] In Table 2, "adhesive component adhesion amount" indicates the amount (mass %) relative to 100 mass % of the rubber reinforcing fiber.
[0152] As is clear from the results of the Examples and Comparative Examples, the molded article of the present invention has excellent adhesion between the rubber reinforcing fibers and the rubber.
Claims
1. A molded article comprising a rubber-reinforced fiber having an adhesive component on at least a portion of the fiber surface, and a rubber, The rubber is obtained by vulcanizing a rubber composition containing one or more of NBR (nitrile rubber) and IIR (butyl rubber), and a vulcanizing agent, The adhesive component is characterized by including a polymer having at least one type of multiple bond selected from a reactive carbon-carbon double bond and a reactive carbon-carbon triple bond in the molecule, and a plasticizer having a swelling degree with respect to the rubber, calculated by the following formula (1), of 5.0% or more. (Swelling degree relative to the rubber) (%)=(M-M") / M×100 (1) (Wherein, M is the volume of 1.1 cm 3 is the mass (g) of a rubber piece (vulcanized rubber sheet with a thickness of 0.7 mm, length of 4.0 cm × width of 4.0 cm) after it has been immersed in a plasticizer at 60°C for 42 hours, and M" is the volume (1.1 cm) of the rubber piece before it was immersed in the plasticizer. 3 is the mass (g) of the rubber piece.
2. The molded article according to claim 1 , wherein the polymer has a hydrogen-bonding functional group.
3. The molded article according to claim 1 or 2, wherein the polymer has at least a part of the multiple bonds in the main chain.
4. The molded article according to any one of claims 1 to 3, wherein the polymer has a number average molecular weight of more than 2,000 and not more than 200,000.
5. 5. The molded article according to claim 1, wherein the polymer contains, in a molecule, a monomer unit derived from one or more selected from the group consisting of butadiene, isoprene, and farnesene.
6. The molded article according to any one of claims 2 to 5, wherein the hydrogen-bonding functional group is at least one selected from a hydroxy group, an aldehyde group, an acetalized product of an aldehyde group, a carboxy group, a salt of a carboxy group, an esterified product of a carboxy group, an acid anhydride of a carboxy group, an amino group, an amide group, a silanol group, an esterified product of a silanol group, an imidazole group, a boronyl group, an epoxy group, and an isocyanate group.
7. The molded article according to any one of claims 1 to 6, wherein the amount of the adhesive component attached is 0.01% by mass or more and 10.0% by mass or less with respect to 100% by mass of the rubber reinforcing fiber.
8. The molded article according to any one of claims 1 to 7, wherein the content of the polymer in the adhesive component is 1% by mass or more and 80% by mass or less.
9. The molded body according to any one of claims 1 to 8, wherein the content of the plasticizer in the adhesive component is 20% by mass or more and 95% by mass or less.
10. The molded article according to any one of claims 1 to 9, wherein the fibers are at least one selected from the group consisting of polyvinyl alcohol fibers, regenerated cellulose fibers, and hydrophobic fibers whose surfaces have been subjected to a hydrophilization treatment.
11. The molded article according to claim 10, wherein the hydrophobic fiber is a polyester fiber.
12. The molded article according to any one of claims 1 to 11, wherein the rubber reinforcing fiber is a woven fabric or a knitted fabric.
13. The molded article according to any one of claims 1 to 12, which is a tire, a belt or a hose.
14. A method for producing a molded body according to any one of claims 1 to 13, A step of adhering a mixture of a polymer having one or more types of multiple bonds selected from reactive carbon-carbon double bonds and reactive carbon-carbon triple bonds in the molecule and a plasticizer to a fiber to obtain a rubber reinforcing fiber; and The method for producing a molded article includes a step of overlapping the obtained rubber reinforcing fiber and rubber and vulcanizing the overlapped rubber reinforcing fiber and rubber.
Citation Information
Patent Citations
Adhesives between synthetic texitile and rubber and textiles treated with same
JP1977152484A
Bonding of fibers for reinforcing rubbers
JP1979004976A
Adhesive between rubber and fiber