Wear-resistant flooring and manufacturing method thereof

The flooring material with a base and protective layer structure, featuring a lower layer with protruding hard particles and a smoothing upper layer, addresses wear resistance and smoothness issues, enhancing durability and appearance.

JP7554652B2Active Publication Date: 2024-09-20TOLI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020198888
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-09-20
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

Conventional synthetic resin flooring materials face issues with wear resistance and surface smoothness, leading to increased frequency of replacement due to friction and pressure from objects with small contact areas, resulting in roughness and decreased appearance and stain resistance.

Method used

A flooring material with a specific layer structure comprising a base layer and a protective layer, where the protective layer includes a lower layer with ultraviolet curable resin and hard particles protruding from its surface, and an upper layer made of ultraviolet curable resin that levels out these protrusions, ensuring firm bonding and smoothness.

Benefits of technology

The flooring material achieves high durability and wear resistance while maintaining surface smoothness, effectively resisting shearing forces from objects with small contact areas, thus extending the material's lifespan and maintaining aesthetic appeal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554652000004
    Figure 0007554652000004
  • Figure 0007554652000005
    Figure 0007554652000005
  • Figure 0007554652000006
    Figure 0007554652000006
Patent Text Reader

Abstract

To provide a floor material capable of exhibiting higher durability while maintaining smoothness thereon.SOLUTION: A floor material includes a base material layer containing a resin component and a protective layer above the base material layer, in which (1) the protective layer includes a lower layer containing an ultraviolet curable resin and hard particles and an upper layer containing an ultraviolet curable resin, (2) the upper layer is laminated above the lower layer, (3) the protective layer has a projection part formed by partially projecting at least a part of the hard particles from the upper surface of the lower layer, and (4) the upper layer is formed so as to make the projection part uniform.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wear-resistant flooring material and a method for producing the same. [Background technology]

[0002] Flooring made of synthetic resin is often used as flooring in commercial facilities, hospitals, hotels, etc. In this case, the surface of the flooring is stepped on by shoes or subjected to friction from baby strollers, carrier bags with casters, carts, wheelchairs, etc., so the softer the surface of the flooring, the more severe the wear and the more frequently the flooring needs to be replaced. In particular, when the contact area is small, such as with high heels or canes, the pressure increases and the wear becomes more severe, and strong shear forces are applied between the layers of the flooring, so flooring with high wear resistance and strong interlayer bonding is required.

[0003] For this reason, various efforts have been made to increase the durability of the flooring surface, and flooring materials with excellent abrasion resistance have been proposed.

[0004] For example, a synthetic resin flooring material has been proposed that has a coating made of an energy ray-curable resin composition for synthetic resin flooring materials, which is characterized by containing an energy ray-curable monomer or oligomer, a photopolymerization initiator, and an inorganic filler with a Mohs hardness of 8 or more (Patent Document 1).

[0005] Also, for example, an interior material is known which is formed from a surface layer made of energy ray-curable resin and a lower layer made of one or more layers, the surface layer being formed by applying an energy ray-curable resin to the surface of the lower layer, uniformly scattering an inorganic filler on the surface of the applied energy ray-curable resin, and then irradiating the energy ray-curable resin to cure the energy curable resin (Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-213296 A [Patent Document 2] JP 2007-277439 A Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, these conventional techniques aim to increase durability by incorporating an inorganic filler in the surface layer of flooring materials and the like.

[0008] However, in these conventional techniques, not only are inorganic fillers intentionally protruded from the surface layer, but there are also cases where the inorganic fillers unintentionally protrude from the surface layer. In such cases, the floor surface becomes rough and the smoothness of the flooring surface decreases, resulting in a decrease in appearance, antifouling properties, etc.

[0009] Thus, there is a strong demand for the development of a resin flooring material that can exhibit greater durability while maintaining a smooth surface.

[0010] Therefore, a main object of the present invention is to provide a flooring material that can exhibit higher durability while maintaining surface smoothness. [Means for solving the problem]

[0011] The present inventors have conducted extensive research in light of these problems in the prior art and have discovered that the above-mentioned object can be achieved by employing a flooring material having a specific layer structure, thereby completing the present invention.

[0012] That is, the present invention relates to the following wear-resistant floor material and a method for producing the same. 1. A flooring material comprising a base layer containing a resin component and a protective layer thereon, (1) The protective layer includes a lower layer including an ultraviolet curable resin and hard particles, and an upper layer including an ultraviolet curable resin, (2) the upper layer is directly laminated on the lower layer; (3) At least some of the hard particles have protrusions formed by partially protruding from the upper surface of the lower layer, (4) The upper layer is formed so as to smooth out the protruding portion. A wear-resistant flooring material characterized by the above. 2. The wear-resistant flooring material according to item 1, wherein 1) the lower layer is 20 to 60 μm thick and contains hard particles having a particle size of 20 to 150 μm, and 2) the upper layer is 50 to 120 μm thick. 3. The wear-resistant flooring material according to item 1 or 2, wherein the content of the hard particles in the lower layer is 10 to 35% by weight. 4. The wear-resistant flooring material according to any one of items 1 to 3, wherein the lower ends of the hard particles forming the protrusions are located in the vicinity of the base layer. 5. A method for producing a wear-resistant floor covering, comprising: (1) A step of forming a coating film for an underlayer by applying a coating liquid containing an ultraviolet-curable resin and hard particles to a base layer containing a resin component or a layer laminated thereon; (2) forming an upper layer coating film by applying a coating liquid containing an ultraviolet curable resin to the lower layer coating film; (3) A step of curing the lower layer coating film and the upper layer coating film by irradiating the lower layer coating film and the upper layer coating film with ultraviolet light. A method for producing an abrasion-resistant flooring material, comprising: Effect of the Invention

[0013] According to the present invention, it is possible to provide a flooring material that can exhibit higher durability while maintaining surface smoothness.

[0014] In particular, the wear-resistant flooring material of the present invention is provided with a protective layer that includes a lower layer containing hard particles and having protrusions where some of the hard particles protrude partially, and an upper layer that smoothes the lower layer, so that it is possible to realize a smooth flooring surface as well as high wear resistance. In particular, when pressed by an object with a small contact area such as a high heel or a cane, the pressure applied to the floor surface is high, so that the wear of the floor surface becomes more severe and the shear force between the layers of the flooring material becomes stronger, but in the flooring material of the present invention, the lower layer and the upper layer are firmly bonded via the hard particles, so that it is possible to exhibit high durability against such shear force.

[0015] Flooring materials with these characteristics can be ideally used in a variety of areas where abrasion resistance and design are required, such as floor surfaces, corridors, passageways, bathrooms, dressing rooms, and toilets in hotels, commercial facilities, offices, hospitals, apartment buildings, etc. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a diagram showing an example of a layer structure of the wear-resistant flooring material of the present invention. [Diagram 2] FIG. 2 is an enlarged view showing the structure of the lower and upper layers of the wear-resistant flooring material. [Diagram 3] 1 shows the results of observing the cross-sectional structure of the flooring material obtained in Example 1 using a scanning electron microscope (SEM image). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] 1. Wear-resistant flooring The wear-resistant flooring material of the present invention (flooring material of the present invention) is a flooring material comprising a base layer containing a resin component and a protective layer thereon, (1) The protective layer includes a lower layer including an ultraviolet curable resin and hard particles, and an upper layer including an ultraviolet curable resin, (2) the upper layer is directly laminated on the lower layer; (3) At least some of the hard particles have protrusions formed by partially protruding from the upper surface of the lower layer, (4) The upper layer is formed so as to smooth out the protruding portion. It is characterized by:

[0018] 1) Basic structure of the flooring material of the present invention The basic structure of the flooring material of the present invention will be described. The flooring material of the present invention includes, for example, a floor sheet or a floor tile specified in JIS A 5705:2016. The floor sheet and the floor tile may have a single-layer structure or a multi-layer structure. According to the Japanese Industrial Standard JIS A 5705:2016, the single-layer structure floor sheet includes, for example, a single-layer vinyl floor sheet, and the multi-layer structure floor sheet includes, for example, a multi-layer vinyl floor sheet, a foamed multi-layer vinyl floor sheet, a cushion floor, and the like. In addition, the single-layer structure floor tile includes, for example, a single-layer vinyl floor tile, a composition vinyl floor tile, and the like, and the multi-layer structure floor tile includes, for example, a multi-layer vinyl floor tile.

[0019] The basic layer structure of the flooring material of the present invention is shown in Figure 1. The flooring material of the present invention 10 has a protective layer 12 formed on the top of a base material layer 11 containing a resin component.

[0020] The protective layer 12 includes a lower layer 13 formed on the surface of the base material layer 11, and an upper layer 14 formed on the surface of the lower layer 13. In Fig. 1, the lower layer 13 is composed of a region 13a containing an ultraviolet curable resin and hard particles 13b. The upper layer 14 is composed of a region 14a containing an ultraviolet curable resin.

[0021] In the lower layer 13, as shown in Fig. 1, at least some of the hard particles 13b partially protrude from the upper surface of the lower layer. More specifically, as shown in Fig. 2, the hard particles 13a protrude from the surface (upper surface) of the lower layer to form a protruding portion P. As a result, the protruding portion P is in a state of invading the upper layer 14 side across the boundary between the lower layer 13 and the upper layer 14. As a result, the hard particles act as a "clamp" connecting the lower layer and the upper layer, thereby obtaining an anchor effect, and as a result, the lower layer and the upper layer are firmly bonded together, which contributes to improving durability.

[0022] The upper layer 14 is composed of an area 14a containing an ultraviolet-curable resin, and is particularly formed to smooth out the protruding portion P. In other words, the upper layer 14 is formed on the surface of the lower layer 13 so as to smooth out the unevenness caused by the protruding portion P on the surface of the lower layer 13 and not to reflect the unevenness on the surface of the upper layer 14. This reduces noticeable unevenness on the floor surface, creating a flatter appearance.

[0023] Here, the term "forming the protrusions P so as to be uniform" means that the thickness t of the upper layer 14 is equal to or larger than the height h of the highest protrusion P among the heights h of the multiple protrusions P, as shown in FIG. max This means forming the upper layer so that the thickness is larger than t. That is, t>h max , preferably t≧2h max , more preferably t≧2.5h max , most preferably t≧3h max This means that the upper layer is formed so that the thickness t of the upper layer 14 satisfies the following condition. As long as this condition is met and the effect of the present invention is not hindered, it is permissible that some unevenness is formed on the surface of the upper layer. max , preferably t<12h max This allows the anchor effect of the hard particles to be fully exerted. This anchor effect allows the upper layer to be firmly bonded to the lower layer, making it possible to withstand strong shear forces.

[0024] In addition, if the thickness of the upper layer is not uniform, the thickness of the thinnest part t min Based on t min >h max , preferably t min ≧2h max , more preferably t min ≧2.5h max , most preferably t min ≧3h max The upper layer may be formed so as to satisfy the above condition.

[0025] The planar shape of the flooring material of the present invention may be either a floor tile or a floor sheet, but may be the same as the shape used for known resin tiles, for example, a rectangular shape such as a square, rectangle, or rhombus. Since floor sheets are often formed in a long length and stored or transported in a rolled state, it is preferable to use an ultraviolet-curing resin for the protective layer that is flexible enough not to break when rolled. On the other hand, floor tiles do not have such restrictions, but the ultraviolet-curing resin can be designed taking into account the occurrence of warping, etc.

[0026] The size of the flooring material of the present invention can be changed depending on, for example, the construction location, the desired design, etc. For example, it can be a rectangular tile shape with a length of 10 to 150 cm and a width of 10 to 150 cm, but is not limited to this.

[0027] 2) Each layer constituting the flooring material of the present invention In the following, in addition to the resin-containing hard layer, surface layer and anti-warping layer which are essential for the flooring material of the present invention, layers which are optionally laminated will also be described.

[0028] Base material layer In the flooring material of the present invention, the base layer serves as a core material and has a function in particular of supporting the protective layer and the like.

[0029] The composition of the base layer is not limited as long as it contains a resin component, but a composition containing a resin component and a plasticizer is particularly suitable. Therefore, for example, a composition containing 1 to 40 parts by weight of a plasticizer per 100 parts by weight of the resin component can be preferably used.

[0030] Examples of the resin component include various synthetic resins such as vinyl chloride resins, polyolefin resins, polyurethane resins, acrylic resins, etc. In particular, at least one of vinyl chloride resins and polyolefin resins is preferably used in terms of obtaining desired flexibility, processability, etc.

[0031] Examples of vinyl chloride resins include vinyl chloride resins, as well as copolymers containing vinyl chloride as a copolymerization component, such as vinyl chloride-vinyl acetate copolymers, ethylene-vinyl chloride copolymers, etc. Examples of polyolefin resins include polypropylene resins, etc.

[0032] In the present invention, it is most preferable that the resin contains at least a vinyl chloride resin, since the resin is inexpensive, has excellent flexibility and durability, and is also excellent in processability. More specifically, examples of resins suitable for achieving the effects of the present invention include vinyl chloride resins having an average degree of polymerization of 1000 to 3000 and polypropylene resins having an average degree of polymerization of 800 to 1000.

[0033] The content of the resin component in the base layer is not limited, but is generally about 25 to 60% by weight, and preferably 30 to 57% by weight. Note that, when a plasticizer is contained, the above content refers to the total amount of the resin component and the plasticizer.

[0034] In addition, in the flooring material of the present invention, a filler can be contained in the base layer as necessary. As the filler, one that is mixed in a known or commercially available flooring material can be adopted. In the present invention, inorganic fillers are particularly preferred. Examples of inorganic fillers include oxides, hydroxides, carbonates, chlorides, and silicates of inorganic or metal elements. More specifically, examples of such fillers include calcium oxide, barium carbonate, magnesium hydroxide, aluminum hydroxide, clay, talc, mica, calcium carbonate, silica sand, and calcium silicate. The calcium carbonate may be either heavy calcium carbonate or light calcium carbonate. These can be used alone or in combination of two or more.

[0035] The filler can usually be used in a powder form, and the average particle size can be appropriately set within the range of about 1 to 300 μm.

[0036] The content of the filler in the base layer is not limited, but is usually about 0 to 70% by weight. By setting the content within such a range, the strength and hardness according to the application can be imparted to the base layer.

[0037] The base layer may contain other additives within the range that does not impair the effects of the present invention. For example, plasticizers, stabilizers, processing aids, antifungal agents, flame retardants, antioxidants, lubricants, colorants, etc. If these additives are inorganic compounds, the content of such additives is also included in the content of the filler.

[0038] In particular, it is preferable to use a relatively small amount of plasticizer within a range that does not impede the effects of the present invention. The softness of the flooring material can be finely adjusted by blending a plasticizer. The plasticizer is not particularly limited, and examples thereof include at least one of dioctyl phthalate (DOP), diheptyl phthalate (DHP), diisononyl phthalate (DINP), trioctyl phosphate (TOP), triphenyl phosphate (TPP), dioctyl terephthalate (DOTP), dioctyl isophthalate (DOIP), and diisononyl cyclohexyl phthalate (DINCH). These can also be commercially available products.

[0039] The content of the plasticizer in the base layer is not limited, but is usually about 40% by weight or less. By setting the content within this range, the strength and hardness according to the application can be more reliably imparted to the base layer.

[0040] The thickness of the base layer is not particularly limited, but may be, for example, about 1 to 10 mm, and particularly 1.5 to 5 mm. By setting the thickness within the above range, the strength and hardness of the base layer can be ensured.

[0041] The method for forming the substrate layer is not particularly limited, but a preformed sheet can usually be used. That is, a sheet for the substrate layer can be obtained by melting the resin composition as the starting material and forming it into a sheet. In addition, two or more such sheets can be laminated. The method for forming into a sheet is not particularly limited, and various methods such as extrusion molding, blow molding, and calendar molding can be adopted. In addition, the substrate layer and the adjacent layer can be formed by simultaneous extrusion lamination. In addition, the substrate layer for floor tiles can be formed by punching or cutting these sheets to the desired dimensions.

[0042] protective layer In the flooring material of the present invention, a protective layer is laminated on the surface of the base material layer. The formation of the protective layer can impart durability to the flooring material against external frictional forces, and at the same time, the smoothness of the surface can provide the flooring material with a highly designable, excellent appearance, antifouling properties, etc. In this respect, it is desirable that the protective layer is disposed on the outermost surface of the flooring material of the present invention and constitutes the surface exposed to the outside. This can more reliably protect the hard flooring material against external pressure, friction, etc.

[0043] In addition, since the protective layer contains ultraviolet-curable resin as a main component, it is usually transparent. If the protective layer is transparent or translucent, the discernibility of the design layer formed thereunder can be further improved. When the protective layer is transparent, the transparency is not limited, but is usually preferably 40% or less in terms of haze value, more preferably 30% or less, and even more preferably 20% or less. By setting such values, it is possible to make the surface of the layer (e.g., the design layer) underlying the protective layer more reliably visible. The lower limit of the haze value is not limited, but it is usually sufficient to set it to about 1%.

[0044] In the present invention, the protective layer is composed of at least two layers, and includes, for example, a lower layer on the substrate layer side and an upper layer formed on the surface of the lower layer as shown in FIG.

[0045] lower layer The lower layer contains an ultraviolet curable resin and hard particles. By including hard particles having such a predetermined size, as shown in FIG. 2, at least some of the hard particles can be partially protruded from the upper surface of the lower layer to form a protruding portion. As described above, when the upper layer is formed, the protruding portion will bite into the upper layer, which brings about an anchor effect and firmly bonds the lower layer and the upper layer. As a result, high abrasion resistance can be imparted not only to the lower layer but also to the upper layer. In addition, this anchor effect can more reliably maintain the predetermined layer structure against strong shear forces.

[0046] In addition, the lower end of the hard particle forming the protrusion is preferably located near the base layer. Located near the base layer means that the lower end of the hard particle is in contact with or slightly separated from the base layer, and specifically, it is desirable that the lower end of the hard particle is located at a distance of 3 μm or less from the surface (upper surface) of the base layer. Since the hard particle protrudes upward from the lower end of the lower layer through the entire lower layer, the hard particle is less likely to fall off, and the anchor effect is increased, and the bonding strength between the lower layer and the upper layer is also increased, so that durability and wear resistance can be improved.

[0047] The ultraviolet curable resin is not particularly limited. For example, ultraviolet curable resins such as unsaturated polyesters such as condensates of unsaturated dicarboxylic acids and polyhydric alcohols, methacrylates such as polyester methacrylate, polyether methacrylate, polyol methacrylate, melamine methacrylate, and acrylates such as polyester acrylate, epoxy acrylate, urethane acrylate, polyether acrylate, polyol acrylate, melamine acrylate, and the like can be used. These can be publicly known or commercially available.

[0048] The content of the ultraviolet-curable resin in the lower layer is not particularly limited, but is usually about 65 to 90% by weight, and preferably 70 to 85% by weight.

[0049] As the hard particles, inorganic particles can be suitably used. As the inorganic particles, for example, oxides, carbonates, hydroxides, etc. can be used. More specifically, alumina (aluminum oxide), silicon oxide, titanium oxide, calcium carbonate, barium carbonate, magnesium hydroxide, aluminum hydroxide, clay, talc, mica, heavy calcium carbonate, silica sand, light calcium carbonate, etc. can be mentioned. Among these, alumina is particularly preferred because it can impart high hardness and excellent durability and abrasion resistance. These can be used alone or in combination of two or more.

[0050] The size of the hard particles may be within a range in which protrusions are formed in the lower layer and do not protrude onto the surface of the upper layer. The shape of the hard particles is not limited, and any of a substantially spherical shape, a flake shape, a fibrous shape, an irregular shape, and the like may be adopted. In the present invention, an irregular shape is preferable in that it can be more firmly fixed in the protective layer, and an irregular shape having corners such as a crushed product is particularly preferable.

[0051] The size of the hard particles is generally set to a particle size in the range of about 20 to 150 μm, and particularly preferably in the range of 30 to 70 μm. When the particle shape is non-spherical, such as an irregular shape, the particle size can be determined by observing the hard particles with a scanning electron microscope (SEM) and dividing the sum of the maximum and minimum widths by 2 to calculate the average value.

[0052] Furthermore, the size of the hard particles is preferably smaller than the total thickness of the protective layer. Although it depends on the particle size distribution and shape of the hard particles, as a general guideline, it is preferable to set the average particle size D of the hard particles to satisfy 0.24T≦D≦0.8T with respect to the total thickness T of the protective layer. By setting it in this way, it is possible to reliably eliminate or reduce the hard particles protruding from the surface of the protective layer (upper layer), and as a result, it is possible to form a flat surface.

[0053] The content of the hard particles in the lower layer is not particularly limited, but is usually about 10 to 35% by weight, and preferably 15 to 30% by weight, which can provide higher abrasion resistance, durability, etc.

[0054] If necessary, other additives may be blended into the lower layer, such as plasticizers, stabilizers, processing aids, antifungal agents, flame retardants, antioxidants, lubricants, and colorants.

[0055] The thickness of the lower layer is not particularly limited, but is preferably 20 to 60 μm, more preferably 30 to 50 μm. By setting the thickness in this range, the hard particles can be firmly supported while the protrusions can be efficiently formed.

[0056] The lower layer may be one layer (single layer) or may be a multi-layer consisting of two or more layers laminated together. A single layer is preferred because it is easy to mold and the lower layer can be made strong.

[0057] upper layer The upper layer includes an ultraviolet-curable resin. The upper layer plays a role in leveling the lower layer, which has an uneven surface caused by protrusions, and forming a smooth surface. For example, as shown in FIG. 2, the upper layer covers the protrusions formed by hard particles partially protruding from the upper surface of the lower layer, canceling out the uneven surface caused by the protrusions and creating a relatively flat surface. Such an upper layer is supported by multiple protrusions present at scattered points, and therefore can exhibit high resistance to friction.

[0058] The ultraviolet curable resin is not particularly limited. For example, ultraviolet curable resins such as unsaturated polyesters such as condensates of unsaturated dicarboxylic acids and polyhydric alcohols, methacrylates such as polyester methacrylate, polyether methacrylate, polyol methacrylate, melamine methacrylate, and acrylates such as polyester acrylate, epoxy acrylate, urethane acrylate, polyether acrylate, polyol acrylate, melamine acrylate, and the like can be used. These can be publicly known or commercially available. In this case, the ultraviolet curable resin used in the upper layer may be the same as or different from the ultraviolet curable resin used in the lower layer.

[0059] The content of the ultraviolet curable resin in the upper layer can be appropriately set within the range of, for example, about 65 to 100% by weight, but is not limited to this.

[0060] In addition, other additives can be blended in the upper layer as necessary within a range that does not significantly impair smoothness. Therefore, it is preferable that the upper layer does not contain hard particles with a particle size of 20 μm or more. In addition, examples of other additives include plasticizers, stabilizers, processing aids, antifungal agents, flame retardants, antioxidants, lubricants, colorants, etc. When these other additives are solids (particles), it is preferable that they do not contain additives with a particle size of 20 μm or more.

[0061] The thickness of the upper layer is not particularly limited, but is preferably 50 to 120 μm, more preferably 70 to 100 μm. By setting the thickness in this range, it is possible to more reliably form a smooth surface as well as high abrasion resistance.

[0062] The upper layer may be one layer (single layer) or may be a multi-layer consisting of two or more layers. In the case of one layer, the upper layer can be easily formed. In the case of two or more layers, an optimal ultraviolet curing resin can be selected for each layer, and various functions such as antifouling properties can be imparted.

[0063] The protective layer (upper layer and lower layer) can be formed, for example, by applying a coating liquid containing the above-mentioned resin component and then curing it. The coating method is not limited, and for example, a roll coater, a curtain coater, a bar coater, a die coater, an air knife coater, a flow coater, spray coating, etc. can be used. In particular, a roll coater, a flow coater, a curtain coater, etc. are preferred because of their excellent processability.

[0064] The curing method may be appropriately selected depending on the type of resin component, etc., and is preferably performed by UV irradiation. Therefore, when a coating liquid containing a UV-curable resin is used, the coating film can be cured by UV irradiation to form a desired protective layer.

[0065] In addition, the upper layer may be applied without curing the lower layer, and then all layers may be cured simultaneously. Alternatively, the lower layer and the upper layer may be cured or semi-cured separately, and finally, all layers may be completely cured.

[0066] The lower layer and the upper layer can be formed by such a method. Even if each layer is formed separately by coating or the like, for example, each layer may be substantially or visually integrated (the boundaries between layers may become unrecognizable) by being composed of the same composition, and such a case is also included in the protective layer of the present invention.

[0067] Other layers As described above, the flooring material of the present invention requires a base material layer and a protective layer, but may contain other layers within the scope of the present invention without impeding the effects of the present invention. For example, an adhesive layer, a design layer, a reinforcing layer, an anti-warping layer, etc. can be mentioned. Therefore, as an embodiment example of the flooring material of the present invention, for example, a laminate such as "base material layer / design layer / protective layer (lower layer / upper layer)", "anti-warping layer / base material layer / design layer / protective layer (lower layer / upper layer)", "anti-warping layer / base material layer / protective layer (lower layer / upper layer)", " / base material layer / reinforcing layer / design layer / protective layer (lower layer / upper layer)", "anti-warping layer / base material layer / reinforcing layer / design layer / protective layer (lower layer / upper layer)", "anti-warping layer / base material layer / reinforcing layer / protective layer (lower layer / upper layer)", "anti-warping layer / base material layer / reinforcing layer / protective layer (lower layer / upper layer)" can be adopted. In addition, the adhesive layer can be appropriately used for bonding between each layer. The specific configuration of each optional layer will be described below.

[0068] Reinforcement layer The reinforcing layer has the function of reinforcing the flooring material of the present invention in the planar or vertical direction. As such a reinforcing layer, in particular, at least one of a) a woven or nonwoven sheet of organic or inorganic fibers (hereinafter also referred to as "fiber sheet") and b) a composite material containing the fiber sheet and a resin component of the base layer can be preferably used.

[0069] The fiber sheet of the above a) includes woven or nonwoven fabrics of synthetic fibers made of polymeric organic compounds, as well as natural fibers, glass fibers, carbon fibers, metal fibers, etc. Nonwoven fabrics also include, for example, spunbond, felt, etc.

[0070] The composite material of b) above can be a material obtained by impregnating the fiber sheet of b) above with a synthetic resin. Also usable is a material obtained by laminating a sheet of the foam material of a) above and the fiber sheet of b) above.

[0071] The thickness of the reinforcing layer can be set appropriately depending on the type of material that constitutes the reinforcing layer, but is usually within the range of about 0.2 to 1 mm. By setting the thickness of the reinforcing layer within this range, the flooring material can be sufficiently reinforced while keeping the overall thickness of the flooring material relatively thin.

[0072] The method of forming the reinforcing layer may be to laminate a preformed sheet for the reinforcing layer at a predetermined position. The lamination may be performed by adhesion using an adhesive layer as described above, or a sheet for the reinforcing layer containing a resin component having heat sealability as a resin component may be joined to another layer by heat sealing (thermal fusion). For this reason, the reinforcing layer (particularly the fiber sheet) may be laminated on the resin-containing hard layer, or may be embedded in the resin-containing hard layer.

[0073] A higher anti-warping effect can be obtained by arranging the reinforcing layer in the center of the flooring material of the present invention, and configuring the layer structure of the flooring material so that the surface layer such as a protective layer and the anti-warping layer are symmetrical in the vertical direction. This is thought to be because with such a layer structure, there is no difference in dimensional change between the front and back surfaces of the flooring material, and the reinforcing layer also suppresses dimensional change of the entire flooring material. In this structure, for example, if a hard polyvinyl chloride resin is used for the surface layer and the anti-warping layer, the anti-warping effect and the dimensional change suppression effect can be further improved.

[0074] Design layer The design layer is a layer that has the function of expressing a desired design, such as a picture, design, pattern, or letter, and imparting design to the flooring material of the present invention. By providing the design layer, the desired design can be imparted to the flooring material of the present invention easily and inexpensively. In addition, the design layer may be a single colored layer or a colored layer consisting of two or more types of colored regions.

[0075] The design layer is preferably formed from a resin composition containing a thermoplastic resin that can be easily bonded to a layer disposed above or below it. Examples of the thermoplastic resin include vinyl chloride resins, olefin resins, ethylene-vinyl acetate copolymers, ethylene-methacrylate resins and other acrylic resins, amide resins, ester resins, vinyl acetate resins, olefin elastomers, styrene elastomers and other elastomers, rubbers, and the like.

[0076] Among these, it is preferable that the layer be formed from a resin composition containing a vinyl chloride resin, since this provides better flexibility and allows various designs to be easily formed by adding a colorant or by printing, making it possible to form the design layer inexpensively and easily.

[0077] Various additives can be blended into the resin composition as necessary. Known or commercially available additives can be used as the additives. For example, fillers, plasticizers, flame retardants, stabilizers, antioxidants, lubricants, colorants, foaming agents, etc. can be mentioned. Therefore, for example, a resin composition containing a resin component, a plasticizer, and a stabilizer can be adopted.

[0078] The thickness of the design layer is not particularly limited, but is, for example, about 2 μm to 1.50 mm, preferably 3 μm to 1.00 mm, and more preferably 5 μm to 15 μm.

[0079] The method for forming the design layer is not particularly limited, and may be formed, for example, by directly printing a pattern on the upper surface of the thermoplastic resin sheet by a known printing method, or by laminating a printed pattern film on the upper surface of the thermoplastic resin sheet. In addition, the design layer may be formed from a resin composition containing a colorant and a thermoplastic resin, or may be formed by preparing and kneading together a plurality of resin compositions containing colorants and thermoplastic resins of different colors.

[0080] Methods for directly printing a pattern on the upper surface of a thermoplastic resin sheet include, for example, methods using various devices such as gravure printing, screen printing, and flexographic printing, as well as printing with a transfer sheet. In addition, a method of laminating a printed film on which a design layer has been formed in advance on a resin film can also be used.

[0081] The method of attaching a printed pattern film to the upper surface of a thermoplastic resin sheet is a preferred method from the viewpoint of easily expressing various patterns. For example, the pattern film can easily and inexpensively impart complex designs such as stone patterns, wood grain patterns, and geometric patterns to the flooring material of the present invention. The thickness of the pattern film is usually preferably about 0.04 to 0.20 mm, and more preferably 0.05 to 0.16 mm. If the thickness of the pattern film is too thin, light may pass through and the surface of the thermoplastic resin sheet laminated on the lower surface may be seen through, and the design of the pattern film may not be fully expressed. On the other hand, if the thickness of the pattern film is too thin, the boundary part of the flooring material may be noticeable when the flooring material is laid.

[0082] Furthermore, by replacing the pattern film, the flooring material of the present invention can be easily made to have different appearance elements such as patterns, brightness, saturation, and color tone, using the same production equipment. By laying flooring materials with different appearance elements irregularly, a unique design can be expressed in an integrated manner on the entire floor surface. An example of a case where a unique design is expressed in an integrated manner using flooring materials with different appearance elements is, for example, a case where the texture of the floor surface formed using various wood materials is expressed in an integrated manner on the entire floor surface by changing the brightness, saturation, or color tone of the stone pattern. If flooring materials with different appearance elements are laid irregularly in this way, even if the flooring materials are partially replaced, no sense of incongruity in design occurs, and the texture of the floor surface formed using various wood materials can be expressed in an integrated manner on the entire floor surface.

[0083] adhesive layer The adhesive layer may be formed as necessary to bond the layers together. The adhesive layer may be formed, for example, using an adhesive. Any known or commercially available adhesive may be used as the adhesive.

[0084] The type of adhesive can be appropriately selected depending on the material of each layer. For example, an adhesive containing one or a mixture of two or more types selected from urethane resin, vinyl acetate resin, styrene-butadiene copolymer resin, acrylic resin, vinyl chloride resin, and epoxy resin as an adhesive component is exemplified. Among these, an adhesive containing a urethane resin as an adhesive component can be preferably used from the viewpoint of excellent moisture resistance, etc.

[0085] In addition, the curing type of the adhesive is not limited, and various types of adhesives such as one-liquid adhesives, two-liquid adhesives, thermosetting adhesives, hot melt adhesives, and ultraviolet curing adhesives can be used. Among these adhesives, it is preferable to use a hot melt adhesive because it has a short curing time and high productivity. More preferably, a reactive hot melt adhesive is preferable. This makes it possible to more effectively suppress deterioration over time, and as a result, it is possible to maintain strong adhesion for a long period of time. Therefore, in the present invention, a reactive hot melt adhesive containing a urethane resin as an adhesive component can be preferably used. This is resistant to humidity and has stable quality for a long period of time, and does not require any special equipment such as UV irradiation, and flooring materials can be manufactured with simple equipment or work.

[0086] In the present invention, by using an adhesive, it is possible to prevent the product from being thermally deteriorated during the production process, and it is also possible to suitably bond the layers even when they are made of different materials.

[0087] The thickness of the adhesive layer is not particularly limited, but is usually about 1 to 200 μm, and preferably 30 to 100 μm. By setting the thickness within such a range, it becomes possible to bond each layer more effectively.

[0088] The adhesive layer can be formed, for example, by applying the adhesive to the lower surface of the substrate sheet that will become the hard resin-containing layer, and then curing the adhesive. The curing method can be appropriately selected depending on the curing type of the adhesive used, and various processes such as aging, drying, heating, and ultraviolet irradiation can be used. The conditions for these processes can be in accordance with known methods.

[0089] 2. Manufacturing method for wear-resistant flooring The flooring material of the present invention can be manufactured by forming or laminating each layer by the method described above. That is, for laminating each layer, in addition to a method of applying an adhesive, a method of bonding layers by heat fusion without applying an adhesive can also be used.

[0090] In particular, the present invention relates to a method for producing a wear-resistant flooring, comprising the steps of: (1) A step of forming a coating film for an underlayer by applying a coating liquid containing an ultraviolet-curable resin and hard particles to a base layer containing a resin component or a layer laminated thereon (underlayer forming step); (2) A step of forming an upper layer coating film by applying a coating liquid containing an ultraviolet curable resin to the lower layer coating film (upper layer forming step); (3) A step of curing the lower layer coating film and the upper layer coating film by irradiating the lower layer coating film and the upper layer coating film with ultraviolet light (curing step). The wear-resistant flooring material can be produced more efficiently and reliably by the manufacturing method thereof, which is characterized by comprising the steps of:

[0091] Lower layer formation process In the lower layer forming step, a coating liquid containing an ultraviolet curable resin and hard particles (preferably hard particles having a particle size of 20 to 150 μm, more preferably 30 to 70 μm) is applied to a base layer containing a resin component or a layer laminated thereon to form a coating film for the lower layer.

[0092] The layer to which the coating liquid is applied may be a base layer, or when another layer is laminated on the base layer, the other layer may be the other layer. Examples of the other layer include a design layer.

[0093] The coating liquid contains ultraviolet curable resin and hard particles. The ultraviolet curable resin, hard particles, the ratio of the two, additives, etc. can be set in accordance with the contents described in "1. Wear-resistant flooring material" above.

[0094] The coating liquid may contain a solvent as necessary. Examples of the solvent include 1) alcohol-based solvents such as ethanol, methanol, isopropyl alcohol, and benzyl alcohol; 2) ketone-based solvents such as acetone, methyl ethyl ketone, and cyclohexanone; 3) ether-based solvents such as isopropyl ether, methyl cellosolve, ethyl cellosolve, and tetrahydrofuran (THF); 4) ester-based solvents such as ethyl acetate, methyl acetate, butyl acetate, and cellosolve acetate; and 5) glycol-based solvents such as ethylene glycol and diethylene glycol. These may be used alone or in combination.

[0095] The solid content of the coating liquid may be appropriately set within the range of, for example, 10 to 90% by weight so as to obtain the desired coatability, but is not limited thereto.

[0096] As described above, the coating method can be, for example, a roll coater, a curtain coater, a bar coater, a die coater, an air knife coater, a flow coater, spray coating, etc. In particular, a roll coater can be suitably used for forming the lower layer from the viewpoint of excellent coatability, etc.

[0097] The coating may be a single layer coating or two or more layers coating, so long as the desired thickness of the lower layer is obtained.

[0098] The amount of the coating liquid to be applied may be appropriately set so that the bottom layer to be finally formed has a predetermined thickness, which may be adjusted within the range of, for example, about 20 to 60 μm, but is not limited thereto.

[0099] Upper layer formation process In the upper layer forming step, a coating liquid containing an ultraviolet curable resin is applied to the lower layer coating to form an upper layer coating.

[0100] The coating liquid contains an ultraviolet curable resin. The ultraviolet curable resin, additives, etc. can be set in accordance with the contents described in "1. Wear-resistant flooring material" above. Therefore, it is preferable to use a coating liquid that contains, for example, an ultraviolet curable resin and does not contain solid particles with a particle size of 20 μm or more.

[0101] The coating liquid may contain a solvent as necessary. Examples of the solvent include 1) alcohol-based solvents such as ethanol, methanol, isopropyl alcohol, and benzyl alcohol; 2) ketone-based solvents such as acetone, methyl ethyl ketone, and cyclohexanone; 3) ether-based solvents such as isopropyl ether, methyl cellosolve, ethyl cellosolve, and tetrahydrofuran (THF); 4) ester-based solvents such as ethyl acetate, methyl acetate, butyl acetate, and cellosolve acetate; and 5) glycol-based solvents such as ethylene glycol and diethylene glycol. These may be used alone or in combination.

[0102] The solid content of the coating liquid may be appropriately set within the range of, for example, 10 to 90% by weight so as to obtain the desired coatability, but is not limited thereto.

[0103] As described above, the coating method may be, for example, a roll coater, curtain coater, bar coater, die coater, air knife coater, flow coater, spray coating, etc. In particular, a curtain coater is preferably used for forming the upper layer, from the viewpoint of being able to increase the film thickness and having excellent surface smoothness. When using a curtain coater, floor tiles are more preferable than floor sheets as the flooring material of the present invention, since the equipment does not need to be large and coating can be easily performed.

[0104] The coating may be a single layer coating or two or more layers coating, so long as the desired upper layer thickness is obtained.

[0105] The amount of the coating liquid to be applied may be appropriately set so that the upper layer to be finally formed has a predetermined thickness, which may be adjusted within the range of, for example, about 50 to 120 μm, but is not limited thereto.

[0106] Curing process In the curing step, the underlayer coating film and the overlayer coating film are irradiated with ultraviolet light to cure the underlayer coating film and the overlayer coating film.

[0107] In the present invention, the upper layer may be applied before the lower layer is cured, and all layers may be cured simultaneously by irradiating ultraviolet rays, or the lower layer and the upper layer may be cured or semi-cured separately, and then all layers may be completely cured at the end. The curing method may be appropriately selected based on the coating method used for each layer and the optimum method.

[0108] The ultraviolet irradiation can be carried out using a known or commercially available ultraviolet irradiation device. The irradiation conditions are, for example, an integrated light amount of 50 to 5000 mJ / cm at an ultraviolet wavelength of 365 nm. 2 It can be, but is not limited to, the degree.

[0109] Other processes As steps other than those described above, steps such as coating with an adhesive, forming or laminating other layers (such as a design layer) can be additionally carried out as necessary.

[0110] The other layers can be formed by the method described above in "1. Wear-resistant floor material."

[0111] In the case of applying an adhesive, the adhesive layer may be any of those described above. The adhesive layer may be formed by applying an adhesive to one surface of the layers to be joined, or by applying an adhesive to both surfaces of the layers to be joined.

[0112] In the present invention, when the layers are bonded by heat fusion without applying an adhesive, the method of heat fusion is not particularly limited. For example, the layers can be bonded by melting and softening them under heat and pressure while overlapping them. More specifically, the layers can be bonded by heat pressing or continuous pressing in which the layers are continuously pressed. Bonding by heat fusion is advantageous in that the materials of the layers are not plasticized, are not easily deteriorated over time, and can be firmly bonded for a long period of time.

[0113] When bonding is performed by heat fusion, it is preferable that at least one of the layers to be bonded contains a component having heat fusion properties (heat sealability), such as polyethylene or polypropylene.

[0114] Furthermore, when the layers are joined by heat fusion, two or more layers can be molded by extrusion lamination. The laminate thus obtained can be used as a part of the layer structure of the flooring material of the present invention.

[0115] After laminating the layers, the laminate may be cut, processed, etc., according to a known method, if necessary.

[0116] 3.Floor structure The present invention includes a floor structure in which a plurality of floor materials of the present invention are laid on a floor substrate. For example, a single or a plurality of sheets of the floor material of the present invention having a substantially rectangular shape (such as a substantially square, substantially rectangular, substantially rhombus, substantially parallelogram, etc.) can be prepared and placed on a floor substrate (such as a floor slab, such as a concrete slab) to form a floor structure made of the floor material of the present invention. In particular, in the present invention, a floor structure can be formed by laying the floor material of the present invention directly on such a floor substrate.

[0117] When the flooring material of the present invention is installed on a floor base, it may be installed in the same manner as the installation method used when installing publicly known or commercially available flooring materials. For example, it may be installed using adhesives, pressure sensitive adhesives, adhesive tapes (double-sided adhesive tapes), etc. These adhesives, etc. may also be commercially available products.

[0118] The floor structure constructed in this manner can be suitably used as flooring in various areas, such as indoors, corridors, verandas, balconies, bathrooms, dressing rooms, toilets, etc. of commercial facilities such as shops and hotels, residences (houses), hospitals, offices, etc. EXAMPLES

[0119] The features of the present invention will be described in more detail below with reference to examples and comparative examples, although the scope of the present invention is not limited to the examples.

[0120] Example 1 We produced a flooring material consisting of a laminate "base layer / protective layer (lower layer / upper layer)" as shown in Figure 1. The base layer was a hard polyvinyl chloride resin sheet (thickness 3.0 mm) with a composition consisting of 45% by weight of polyvinyl chloride resin, 6% by weight of plasticizer, 46% by weight of filler, and 3% by weight of other additives.

[0121] A coating liquid (solvent-free type) containing 100 parts by weight of ultraviolet-curable resin mainly composed of urethane acrylate and 30 parts by weight of hard particles (alumina particles, particle size #280 (average particle size 68 μm), irregular shape) was applied to one side of the sheet using a roll coater to form a coating film for the lower layer. The alumina particle size was based on the particle size of abrasives for grinding wheels specified in "Japanese Industrial Standards JIS R6001".

[0122] Next, a coating liquid containing an ultraviolet-curable resin mainly composed of urethane acrylate and not containing alumina particles was applied to the surface of the lower layer coating film using a curtain coater to form an upper layer coating film.

[0123] Then, ultraviolet light was applied from above the upper layer coating using a commercially available ultraviolet irradiation device, causing the lower layer coating and the upper layer coating to harden almost simultaneously, thereby producing a flooring material in which a lower layer (thickness 45 μm) and an upper layer (80 μm) were laminated onto the base layer.

[0124] Example 2 A flooring material was produced in the same manner as in Example 1, except that the thickness of the lower layer was set to 30 μm.

[0125] Example 3 A flooring material was produced in the same manner as in Example 1, except that the thickness of the lower layer was set to 20 μm.

[0126] Comparative Example 1 A flooring material was produced in the same manner as in Example 1, except that alumina was not blended into the lower layer.

[0127] Comparative Example 2 A flooring material was produced in the same manner as in Example 1, except that the lower layer was not formed.

[0128] Test Example 1 The abrasion resistance of the protective layer of the flooring material obtained in each of the Examples and Comparative Examples was examined. The results are shown in Tables 2 to 4. The Taber abrasion test is a test to measure abrasion resistance. Specifically, based on the test method compliant with the Japanese Industrial Standard "JIS A1453", abrasive paper S-42 was attached to a Taber abrasion tester, and the sample surface was abraded by rotating at a rotation speed of 70 rpm. The abraded surface was visually observed to determine the number of rotations until the protective layer was 100% worn away and disappeared. In addition, the abrasion resistance as a flooring material was judged from the number of rotations in the Taber abrasion test, according to the criteria shown in Table 1.

[0129] [Table 1]

[0130] [Table 2]

[0131] [Table 3]

[0132] As is clear from the results in Tables 2 and 3, by forming a predetermined protective layer, it is possible to exhibit better abrasion resistance.

[0133] Test Example 2 The cross section of the flooring material obtained in Example 1 was observed. The flooring material was cut and the cut surface was observed with a scanning electron microscope. The results are shown in Figure 3. The transparent vinyl chloride layer in Figure 3 is the surface layer and corresponds to a part of the base layer of the present invention.

[0134] As shown in Figure 3, it can be seen that a protective layer is formed on the base layer, alumina particles, which are hard particles, are fixed to the lower side (base layer side) of the protective layer, a layer of a specified thickness is formed to cover the upper side, and the unevenness caused by the alumina particles is smoothed to make the protective layer surface flat. It can also be seen that the protective layer has a two-layer structure in which a layer that does not contain alumina particles is laminated on top of the layer that fixes the alumina particles.

Claims

1. A flooring material comprising a base layer containing a resin component and a protective layer thereon, (1) The protective layer includes a lower layer including an ultraviolet curable resin and hard particles, and an upper layer including an ultraviolet curable resin, (2) the upper layer is directly laminated on the lower layer, (3) At least some of the hard particles have protrusions formed by partially protruding from the upper surface of the lower layer, (4) The upper layer is formed to smooth out the protruding portion, (5) 1) the lower layer has a thickness of 20 to 60 μm and contains hard particles having a particle size of 20 to 150 μm; 2) the upper layer has a thickness of 70 to 120 μm; (6) The thickness t of the upper layer and the height hmax of the highest protrusion P among the heights h of the multiple protrusions P satisfy t ≧ 2hmax, (7) The lower ends of the hard particles forming the protrusions are located in the vicinity of the base layer. A wear-resistant flooring material characterized by the above.

2. An abrasion-resistant flooring material as described in claim 1, wherein the particle size of the hard particles is 20 to 70 μm.

3. 3. The wear-resistant flooring material according to claim 1, wherein the content of the hard particles in the lower layer is 10 to 35% by weight.

4. A wear-resistant flooring material as described in any of claims 1 to 3, wherein, when the thickness of the upper layer is not uniform, the thickness tmin of the thinnest part and the height hmax of the highest protrusion P among the heights h of the multiple protrusions P satisfy tmin ≧ 2hmax.

5. A method for producing a wear-resistant floor covering, comprising the steps of: (1) A step of forming a coating film for an underlayer by applying a coating liquid containing an ultraviolet curable resin and hard particles to a base layer containing a resin component or a layer laminated thereon in such a manner that at least a part of the hard particles partially protrude from the upper surface of the underlayer to form a protruding portion; (2) forming an upper layer coating film by applying a coating liquid containing an ultraviolet curable resin to the lower layer coating film; (3) A process of curing the lower layer coating film and the upper layer coating film by irradiating the lower layer coating film and the upper layer coating film with ultraviolet light to form an upper layer and a lower layer in which the thickness of the lower layer is 20 to 60 μm, the thickness of the upper layer is 70 to 120 μm, and the thickness t of the upper layer and the height hmax of the highest protrusion P among the heights h of the multiple protrusions P satisfy t ≧ 2hmax. A method for producing an abrasion-resistant flooring material, comprising:

Citation Information

Patent Citations

  • Decorative material with wear resistance

    JP2000094625A

  • Method for laminating surface-protective film and decorative material with surface protective film produced by the same

    JP2002119910A

  • Decorative sheet for floor

    JP2003034011A

  • Energy ray-curable resin composition for synthetic resin floor covering, and synthetic resin flooring material having film composed of the composition

    JP2005213296A

  • Synthetic resin floor tile

    JP2007046302A