Anti-reflection laminate

The antireflection laminate with a layered structure of specific refractive index layers addresses high reflectance issues in optical displays, achieving low reflectance and high transmittance across a wide wavelength range, including infrared, suitable for optical displays and infrared safety sensors.

JP7554820B2Active Publication Date: 2024-09-20FUKUBI KAGAKU IND
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022515275
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-14
Filing Date
2021-03-26
Publication Date
2024-09-20
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing antireflection films for optical display devices have high reflectance levels, exceeding several percent in the visible light range, failing to meet the luminous average reflection characteristics required by modern displays.

Method used

An antireflection laminate comprising a base material, hard coat layer, and a layered structure of low, medium-low, medium, and high refractive index layers, with specific refractive indices and thicknesses, optimized to achieve low reflectance and high transmittance across a wide wavelength range, including the addition of a medium-low refractive index layer to enhance antireflection properties.

Benefits of technology

The laminate achieves a luminous average reflectance of 0.6% or less and transmittance of 95% or more across 380 to 780 nm, with infrared transmittance of 85% or more, suitable for applications in optical displays and safety sensors using infrared cameras.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554820000048
    Figure 0007554820000048
  • Figure 0007554820000047
    Figure 0007554820000047
  • Figure 0007554820000049
    Figure 0007554820000049
Patent Text Reader

Abstract

The present invention is an anti-reflection laminate that includes a base material (B), a hard coat layer (HC), and an anti-reflection layer (AR), in the stated order, wherein the anti-reflection layer (AR) includes a low refractive index layer (L) having a refractive index of 1.450 or less and a film thickness of 70-130 nm, a high refractive index layer (H) having a refractive index of 1.700-1.850 and a film thickness of 10-250 nm, a medium refractive index layer (M) having a refractive index of 1.550-1.810 and a film thickness of 20-150 nm, and a medium-low refractive index layer (ML) having a refractive index of 1.500-1.650 and a film thickness of 10-230 nm, and the refractive indices of the layers of the anti-reflection layer (AR) satisfy the condition RI(L)<RI(ML)<RI(M)≤RI(H), where RI(L) represents the refractive index of the low refractive index layer (L), RI(ML) represents the refractive index of the medium-low refractive index layer (ML), RI(M) represents the refractive index of the medium refractive index layer (M), and RI(H) represents the refractive index of the high refractive index layer (H). In addition, the present invention is an anti-reflection laminate having excellent anti-reflection properties and light transmittance, wherein the above-described layers are arranged in the order medium-low refractive index layer (ML), medium refractive index layer (M), high refractive index layer (H), low refractive index layer (L) from the hard coat layer (HC) side, and the average luminous reflectance of both surfaces at a wavelength of 380-780 nm is 0.6% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antireflection laminate provided to prevent reflection of external light on the surface of a window, a display, etc. In particular, the present invention relates to an antireflection laminate provided on the front panel of an optical display device such as an LED display (LED, OLED), a liquid crystal display (LCD), or a plasma display (PDP). [Background technology]

[0002] Patent Document 1 proposes an anti-reflection film consisting of three layers formed by coating on a light-transmitting substrate, each layer having a predetermined thickness. However, the minimum reflectance of this anti-reflection film is about 0.5% at a wavelength of 600 nm, and the average reflectance in the visible light range of 380 to 780 nm is estimated to exceed several percent. Therefore, there is room for further improvement in order to satisfy the luminous average reflectance characteristics required for recent optical display devices. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-182007 A Summary of the Invention [Problem to be solved by the invention]

[0004] SUMMARY OF THE PRESENT DISCLOSURE An object of the present invention is to provide an antireflection laminate having excellent antireflection properties and light transmittance. The present inventors have discovered that by providing a three-layer antireflection layer composed of a low refractive index layer (L), a high refractive index layer (H), and a medium refractive index layer (M) with a medium-low refractive index layer (ML) having a refractive index intermediate between the refractive indexes of the low refractive index layer (L) and the medium refractive index layer (M), an antireflection laminate can be obtained which has excellent luminous average reflectance on both sides in the wavelength range of 380 to 780 nm and excellent luminous average transmittance in the wavelength range of 380 to 780 nm, and have completed the present invention.

Means for Solving the Problem

[0005] That is, the present invention includes the following inventions. 1. An antireflection laminate including a substrate (B), a hard coat layer (HC), and an antireflection layer (AR) in this order, wherein the antireflection layer (AR) includes a low refractive index layer (L) having a refractive index of 1.450 or less and a film thickness of 70 to 130 nm, a high refractive index layer (H) having a refractive index of 1.700 to 1.850 and a film thickness of 10 to 250 nm, a medium refractive index layer (M) having a refractive index of 1.550 to 1.810 and a film thickness of 20 to 150 nm, and a medium-low refractive index layer (ML) having a refractive index of 1.500 to 1.650 and a film thickness of 10 to 230 nm, the refractive indices of the respective layers of the antireflection layer (AR) satisfy the condition of RI(L) < RI(ML) < RI(M) ≤ RI(H), where RI(L) represents the refractive index of the low refractive index layer (L), RI(ML) represents the refractive index of the medium-low refractive index layer (ML), RI(M) represents the refractive index of the medium refractive index layer (M), RI(H) represents the refractive index of the high refractive index layer (H), and the respective layers are arranged in the order of the medium-low refractive index layer (ML), the medium refractive index layer (M), the high refractive index layer (H), and the low refractive index layer (L) from the hard coat layer (HC) side, and the antireflection laminate having a visual average reflectance of 0.6% or less on both sides at a wavelength of 380 to 780 nm.

[0006] 2. The medium-low refractive index layer (ML) is based on 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolyzate thereof, (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolyzate thereof, and (iii) a radiation-curable resin.

Chemical formula

[0007] 3. The medium refractive index layer (M) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [ka] (wherein R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [ka] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group. n is 1 or 2. 2. The antireflection laminate according to item 1 above, which is made of a cured product of a composition containing 40 to 500 parts by mass of metal oxide particles and 1 to 20 parts by mass of a metal chelate compound.

[0008] 4. The high refractive index layer (H) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [ka] (wherein R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [ka] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group. n is 1 or 2. 2. The antireflection laminate according to item 1 above, which is made of a cured product of a composition containing 300 to 500 parts by mass of metal oxide particles and 10 to 20 parts by mass of a metal chelate compound.

[0009] 5. The low refractive index layer (L) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [ka] (wherein R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [ka] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group. n is 1 or 2. 2. The antireflection laminate according to item 1 above, which is made of a cured product of a composition containing 100 to 200 parts by mass of silica particles and 5 to 15 parts by mass of a metal chelate compound.

[0010] 6. The metal oxide particles are at least one oxide particle selected from the group consisting of titanium oxide, zirconium oxide, niobium pentoxide, antimony-doped tin oxide (ATO), indium oxide-tin oxide (ITO), phosphorus-doped tin oxide (PTO), fluorine-doped tin oxide (FTO) and antimony pentoxide. Item 2 to 4 above 13. The antireflection laminate according to claim 12.

[0011] 7. A protective layer (C) is provided on the antireflection layer (AR), and the protective layer (C) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [ka] (wherein R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [ka] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group. n is 1 or 2. 2. The antireflection laminate according to item 1 above, which is made of a cured product of a composition containing 10 to 30 parts by mass of silica particles and 5 to 15 parts by mass of a metal chelate compound.

[0012] 8. The antireflection laminate according to any one of the above items 1 to 7, which has an average luminous transmittance of 95% or more at a wavelength of 380 to 780 nm. 9. The antireflection laminate according to any one of the above items 1 to 8, which has an infrared transmittance of 85% or more at a wavelength of 900 nm. Effect of the Invention

[0013] The antireflection laminate of the present invention is excellent in antireflection property and light transmittance. The antireflection laminate of the present invention has a low reflectance in a wide wavelength range of 380 to 780 nm. As a result, the average luminous reflectance of both surfaces of the antireflection laminate of the present invention is 0.6% or less. Furthermore, the antireflection laminate of the present invention has excellent infrared transmittance, with a transmittance of at least 85% for light with a wavelength of 900 nm, i.e., infrared light, and is as high as 96%. Therefore, it is useful as a front panel or cover material for a safety sensor using an infrared camera or an infrared laser, or as an instrument panel or touch panel for an automobile. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a diagram showing an example of a layer structure of the antireflection laminate of the present invention. [Diagram 2] FIG. 2 is a reflectance distribution diagram of the antireflection laminate of Example 1. [Diagram 3] FIG. 2 is a reflectance distribution diagram of the antireflection laminate of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] <Base material (B)> The substrate (B) is preferably formed of a transparent resin that has excellent impact resistance and does not impede visibility. The total light transmittance of the substrate (B) at a wavelength of 380 to 780 nm is preferably 88% or more, more preferably 89% or more, and even more preferably 92% or more. From the viewpoint of transparency and impact resistance, the substrate (B) is preferably formed of at least one resin selected from the group consisting of acrylic resin, polycarbonate resin, polyethylene terephthalate resin, and triacetyl cellulose resin. A laminate substrate in which these resins are laminated may be used. For example, a laminate substrate of polycarbonate resin and polymethyl methacrylate resin may be used. The thickness of the substrate (B) is designed by appropriately selecting from the required transparency and impact strength, but is usually in the range of 0.2 to 2.0 mm. The upper limit of the thickness of the substrate (B) is preferably 1.0 mm, more preferably 1.5 mm, and further preferably 2 mm.

[0016] <Hard coat layer (HC)> The hard coat layer (HC) is preferably a layer containing a resin component obtained by curing a trifunctional or lower urethane acrylate and a tetrafunctional or higher urethane acrylate. The thickness of the hard coat layer (HC) is preferably 1 to 3 μm. That is, if the thickness is too thin, it becomes difficult to ensure the basic physical properties (e.g., hardness and strength) of the hard coat layer (HC), and if the thickness is too thick, the difference in physical properties (e.g., flexibility and elongation) from the substrate (B) becomes large, which results in molding defects such as cracks. The thickness of the hard coat layer (HC) is preferably 1.2 to 2.5 μm, more preferably 1.5 to 2 μm. The hard coat layer (HC) preferably contains a resin component obtained by curing a trifunctional or lower urethane acrylate and a tetrafunctional or higher urethane acrylate, a silane coupling component, silica particles, and a metal chelate compound.

[0017] (Resin component) The resin component functions as a binder that forms a hard coat layer (HC). As such a binder, it is preferable to use a combination of a trifunctional or lower urethane acrylate and a quadrifunctional or higher urethane acrylate. That is, a trifunctional or lower urethane acrylate forms a relatively flexible part upon curing, and a quadrifunctional or higher urethane acrylate forms a hard part upon curing, and by using both in combination, a film that is moderately dense and has high hardness can be formed. Incidentally, urethane acrylate is obtained by reacting a terminal isocyanate compound obtained by reacting a polyisocyanate compound with a polyol compound having multiple hydroxyl groups, and then reacting the resulting compound with a hydroxyl group-containing (meth)acrylate. The (meth)acryloyl group in the urethane acrylate is the functional group; for example, a urethane acrylate having two (meth)acryloyl groups is bifunctional, and one having three is trifunctional.

[0018] Therefore, a trifunctional or lower functional urethane acrylate is one having at most three (meth)acryloyl groups. For example, a urethane acrylate in which one (meth)acryloyl group is introduced at each end by reacting pentaerythritol mono(meth)acrylate with a terminal isocyanate compound is used as a bifunctional urethane acrylate. In addition, a compound obtained by reacting pentaerythritol mono(meth)acrylate and pentaerythritol di(meth)acrylate with a terminal isocyanate compound to introduce one (meth)acryloyl group at one end of the isocyanate compound and two (meth)acryloyl groups at the other end is used as a trifunctional urethane acrylate.

[0019] Furthermore, a compound obtained by reacting pentaerythritol di(meth)acrylate with a terminal isocyanate compound to introduce two (meth)acryloyl groups at each of both ends of the isocyanate compound is used as a tetrafunctional urethane acrylate. Of course, the above example is just one example, and other urethane acrylates can be used as long as they are 3 or less functional. For example, hydroxyl group-containing (meth)acrylic acid esters such as monoesters and diesters of (meth)acrylic acid of ethylene glycol, diethylene glycol, and polyhydric alcohols having 3 or more valences can be used to introduce a desired number of (meth)acryloyl groups to obtain urethane acrylates having 3 or less functionalities.

[0020] The same applies to urethane acrylates with four or more functionalities; for example, by reacting pentaerythritol tri(meth)acrylate with an isocyanate at both ends (e.g., trihexadiethylene diisocyanate), a hexafunctional urethane acrylate having three (meth)acryloyl groups at each of the molecular chain ends can be obtained.

[0021] In the present invention, the above-mentioned trifunctional or lower urethane acrylate and tetrafunctional or higher urethane acrylate are preferably used in a weight ratio of 2 / 98 to 70 / 30, particularly 10 / 90 to 60 / 40. If the amount of trifunctional or lower urethane acrylate used is too large, the hardness of the obtained hard coat layer (HC) may be impaired, and the basic performance of the hard coat layer (HC) may be reduced.

[0022] (Silane coupling component) The hard coat layer (HC) preferably contains a silane coupling component, which is used to stably disperse and hold silica particles (described later) in the hard coat layer (HC) without dropping off, and at the same time, to ensure adhesion with the antireflection layer (AR).

[0023] That is, the silane coupling component is preferably a compound (silane coupling agent) represented by the following formula or a hydrolysate thereof. R 3 n -Si(OR 1 ) 4-n (In the formula, R 3is an alkyl or alkenyl group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom, and n is the number 1 or 2. The group R in the above formula 3 Examples of the alkyl group include alkyl groups such as a methyl group, an ethyl group, and a propyl group, and alkenyl groups such as a vinyl group. The alkyl group may be substituted with a functional group such as a halogen atom such as chlorine, a mercapto group, an amino group, a (meth)acryloyl group, or an oxirane ring-containing group. In addition, the group R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom, and is bonded to a silicon atom by a group OR 1 is a hydrolyzable group.

[0024] Specific examples of the silane coupling agent include vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, γ-(N-styrylmethyl-β-aminoethylamino)propyltrimethoxysilane hydrochloride, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, methyltrimethoxysilane, methyltrichlorosilane, and dimethyldichlorosilane. The hydrolyzate of such a silane coupling agent undergoes polycondensation simultaneously with hydrolysis to form a polymer connected in a network shape by Si-O-Si bonds. Therefore, the use of the hydrolyzate of such a silane coupling agent can also make the hard coat layer (HC) dense.

[0025] In the present invention, the content ratio of the above compound or its hydrolysate in the hard coat layer (HC) is set in the range of preferably 1 to 30 parts by mass, more preferably 5 to 20 parts by mass, per 100 parts by mass of the resin component formed from the above-mentioned urethane acrylate.

[0026] (Solid Silica Particles) The hard coat layer (HC) preferably contains solid silica particles. The solid silica particles in the hard coat layer (HC) preferably have a particle size of 5 to 500 nm and a refractive index of 1.44 to 1.5. In other words, by using such oxide fine particles, basic properties such as hardness can be uniformly imparted to the entire hard coat layer (HC).

[0027] The content of such solid silica particles is preferably 10 to 80 parts by mass, more preferably 20 to 60 parts by mass, per 100 parts by mass of the resin component formed from the above-mentioned urethane acrylate. By including such silica particles in the hard coat layer (HC) in such a range, the basic properties of the hard coat layer (HC) can be maintained while improving adhesion with the antireflection layer (AR) and effectively preventing cracks, etc.

[0028] (Metal chelate compounds) The hard coat layer (HC) preferably contains a metal chelate compound. The metal chelate compound is used to introduce a crosslinked structure into the hard coat layer (HC) and make the hard coat layer (HC) denser. That is, a crosslinked structure is also formed in the resin component of the urethane acrylate described above, but the denseness is reduced by using a low-functional urethane acrylate to impart flexibility. That is, the metal chelate compound is used to compensate for the decrease in denseness without impairing the flexibility of the hard coat layer (HC), in other words, to adjust mechanical properties such as hardness that are affected by the denseness of the film. In addition, such a metal chelate compound is also contained in the anti-reflective layer (AR), and therefore the use of the metal chelate compound further increases the adhesion between the hard coat layer (HC) and the anti-reflective layer (AR), and effectively prevents cracks during molding.

[0029] As such metal chelate compounds, compounds of titanium, zirconium, aluminum, tin, niobium, tantalum or lead containing a bidentate ligand are preferred. A bidentate ligand is a chelating agent having two coordination sites, i.e., two atoms that can be coordinated to a metal, and generally forms a 5- to 7-membered ring with O, N, and S atoms to form a chelate compound. Examples of such bidentate ligands include acetylacetonate, ethylacetoacetate, diethylmalonate, dibenzoylmethanate, salicylate, glycolate, catecholate, salicylaldehyde, oxyacetophenonate, biphenolate, pyromeconate, oxynaphthoquinonate, oxyanthraquinonate, tropolonate, binokitylate, glycinato, alaninato, anthroninato, picolinate, aminophenolate, and the like. Examples of the alkylamino groups include arylamino groups, ethanolamino groups, mercaptoethylamino groups, 8-oxyquinolinato groups, salicylaldiminato groups, benzoin oximato groups, salicylaldoximato groups, oxyazobenzenato groups, phenylazonaphtholato groups, β-nitroso-α-naphtholato groups, diazoaminobenzenato groups, biuretato groups, diphenylcarbazonato groups, diphenylthiocarbazonato groups, biguanidato groups, and dimethylglyoximato groups.

[0030] In the present invention, the metal chelate compound preferably used is represented by the following formula: M(Li) k (X) m-k In the formula, M is titanium, zirconium, aluminum, tin, niobium, tantalum, or lead; Li is a bidentate ligand, X is a monovalent group, preferably a hydrolyzable group; m is the valence of the metal M; k is a number of 1 or more in a range not exceeding the valence of the metal M; It is expressed as:

[0031] Among these, titanium, zirconium and aluminum are preferred as the metal M, and an alkoxy group is preferred as the group X. Specific examples of such metal chelate compounds include the following Ti chelate compounds, Zr chelate compounds and Al chelate compounds.

[0032] Ti chelates; Titanium triethoxy mono(acetylacetonate) Titanium tri-n-propoxy mono(acetylacetonate) Titanium tri-i-propoxy mono(acetylacetonate) Tri-n-butoxy mono(acetylacetonate) titanium Titanium tri-sec-butoxy mono(acetylacetonate) Titanium tri-t-butoxy mono(acetylacetonate) Titanium diethoxybis(acetylacetonate) Titanium di-n-propoxy bis(acetylacetonate) Titanium di-i-propoxy bis(acetylacetonate) Di-n-butoxybis(acetylacetonate)titanium Titanium di-sec-butoxybis(acetylacetonate) Titanium di-t-butoxybis(acetylacetonate) Monoethoxy tris(acetylacetonate) titanium Mono-n-propoxy tris(acetylacetonate) titanium Mono-i-propoxy tris(acetylacetonate) titanium Mono-n-butoxytris(acetylacetonate)titanium Mono-sec-butoxytris(acetylacetonate)titanium Mono-t-butoxytris(acetylacetonate)titanium Titanium tetrakis(acetylacetonate) Titanium triethoxy mono(ethyl acetoacetate) Titanium tri-n-propoxy mono(ethyl acetoacetate) Tri-i-propoxy mono(ethyl acetoacetate) titanium Tri-n-butoxy mono(ethylacetoacetate) titanium Tri-sec-butoxy mono(ethyl acetoacetate) titanium Tri-t-butoxy mono(ethyl acetoacetate) titanium Titanium diethoxybis(ethylacetoacetate) Titanium di-n-propoxy bis(ethylacetoacetate) Titanium di-i-propoxy bis(ethylacetoacetate) Di-n-butoxybis(ethylacetoacetate)titanium Di-sec-butoxy bis(ethylacetoacetate)titanium Di-t-butoxybis(ethylacetoacetate)titanium Monoethoxy tris(ethylacetoacetate) titanium Mono-n-propoxy tris(ethylacetoacetate) titanium Mono-i-propoxy tris(ethylacetoacetate) titanium Mono-n-butoxytris(ethylacetoacetate)titanium Mono-sec-butoxytris(ethylacetoacetate)titanium Mono-t-butoxytris(ethylacetoacetate)titanium Titanium tetrakis(ethylacetoacetate) Mono(acetylacetonato)tris(ethylacetoacetate)titanium Titanium bis(acetylacetonate)bis(ethylacetoacetate) Titanium tris(acetylacetonato)mono(ethylacetoacetate)

[0033] Zr chelates; Triethoxyzirconium mono(acetylacetonate) Tri-n-propoxy mono(acetylacetonate)zirconium Tri-i-propoxy mono(acetylacetonate)zirconium Tri-n-butoxy-mono(acetylacetonate)zirconium Tri-sec-butoxy mono(acetylacetonate)zirconium Tri-t-butoxyzirconium mono(acetylacetonate) Zirconium diethoxybis(acetylacetonate) Di-n-propoxy bis(acetylacetonate)zirconium Di-i-propoxy bis(acetylacetonate)zirconium Di-n-butoxy bis(acetylacetonate)zirconium Di-sec-butoxy bis(acetylacetonate)zirconium Di-t-butoxy bis(acetylacetonate)zirconium Monoethoxy tris(acetylacetonate)zirconium Mono-n-propoxy tris(acetylacetonate)zirconium Mono-i-propoxy tris(acetylacetonate)zirconium Mono-n-butoxy tris(acetylacetonate)zirconium Mono-sec-butoxy tris(acetylacetonate)zirconium Mono-t-butoxy tris(acetylacetonate)zirconium Tetrakis(acetylacetonate)zirconium Triethoxyzirconium mono(ethylacetoacetate) Tri-n-propoxy-mono(ethylacetoacetate)zirconium Tri-i-propoxy-mono(ethylacetoacetate)zirconium Tri-n-butoxy-mono(ethylacetoacetate)zirconium Tri-sec-butoxy mono(ethylacetoacetate)zirconium Tri-t-butoxy-mono(ethylacetoacetate)zirconium Zirconium diethoxybis(ethylacetoacetate) Di-n-propoxy bis(ethylacetoacetate)zirconium Di-i-propoxy bis(ethylacetoacetate)zirconium Di-n-butoxy bis(ethylacetoacetate)zirconium Di-sec-butoxy bis(ethylacetoacetate)zirconium Di-t-butoxy bis(ethylacetoacetate)zirconium Monoethoxy tris(ethylacetoacetate)zirconium Mono-n-propoxy tris(ethylacetoacetate)zirconium Mono-i-propoxy tris(ethylacetoacetate)zirconium Mono-n-butoxy tris(ethylacetoacetate)zirconium Mono-sec-butoxy tris(ethylacetoacetate)zirconium Mono-t-butoxy tris(ethylacetoacetate)zirconium Tetrakis(ethylacetoacetate)zirconium Mono(acetylacetonato)tris(ethylacetoacetate)zirconium Bis(acetylacetonato)bis(ethylacetoacetate)zirconium Tris(acetylacetonato)mono(ethylacetoacetate)zirconium

[0034] Al chelates; Aluminum diethoxy mono(acetylacetonate) Monoethoxy bis(acetylacetonate)aluminum Di-i-propoxy mono(acetylacetonate)aluminum Mono-i-propoxy bis(acetylacetonate)aluminum Mono-i-propoxy-bis(ethylacetoacetate)aluminum Aluminum monoethoxy bis(ethylacetoacetate) Aluminum diethoxy mono(ethyl acetoacetate) Aluminum di-i-propoxy mono(ethyl acetoacetate) Aluminum tris(acetylacetonate) Bis(ethylacetoacetate)mono(acetylacetonate)aluminum

[0035] The above-mentioned metal chelate compound is used in an amount of preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, per 100 parts by mass of the resin component formed from the urethane acrylate. By using the metal chelate compound within this range, it is possible to improve the adhesion between the hard coat layer (HC) and the antireflection layer (AR) formed on the hard coat layer (HC).

[0036] (Formation of hard coat layer (HC)) The hard coat layer (HC) can be formed by applying a coating liquid containing a monomer or oligomer for forming a resin component onto the substrate (B), forming a coating film on the substrate (B), drying the coating film as necessary, and then irradiating the coating film with ionizing radiation such as ultraviolet light or an electron beam to cause a curing reaction of the monomer or oligomer for forming the resin component.

[0037] <Anti-reflection layer (AR)> The anti-reflection layer (AR) includes a low refractive index layer (L), a high refractive index layer (H), a medium refractive index layer (M), and a medium-low refractive index layer (ML). Each layer is arranged in the order of the medium-low refractive index layer (ML), the medium refractive index layer (M), the high refractive index layer (H), and the low refractive index layer (L) from the hard coat layer (HC) side. For the anti-reflection layer (AR), the refractive indices of each layer satisfy the condition of RI(L) < RI(ML) < RI(M) ≤ RI(H). Here, RI(L) represents the refractive index of the low refractive index layer (L), RI(ML) represents the refractive index of the medium-low refractive index layer (ML), RI(M) represents the refractive index of the medium refractive index layer (M), RI(H) represents the refractive index of the high refractive index layer (H). In the present invention, there are an embodiment satisfying RI(M) = RI(H) and an embodiment satisfying RI(M) < RI(H).

[0038] 〔Medium-low refractive index layer (ML)〕 The refractive index of the medium-low refractive index layer (ML) is 1.500 to 1.650. The lower limit of the refractive index is preferably 1.51, more preferably 1.55. The upper limit of the refractive index is preferably 1.61, more preferably 1.60. The film thickness of the medium-low refractive index layer (ML) is 10 to 230 nm. The lower limit of the film thickness is preferably 15 nm, more preferably 45 nm. The upper limit of the film thickness is preferably 190 nm, more preferably 175 nm. The medium-low refractive index layer (ML) preferably consists of a cured product of a composition containing a binder component and metal oxide particles. Also, the medium-low refractive index layer (ML) preferably consists of a cured product of a composition containing a binder component, metal oxide particles, and a metal chelate compound. The medium-low refractive index layer (ML) preferably consists of a cured product of a composition containing 40 to 500 parts by mass of metal oxide particles and 10 parts by mass or less of a metal chelate compound with respect to 100 parts by mass of the binder component.

[0039] (Binder component) Examples of the binder component include (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof, and (iii) an ionizing radiation curable resin.

[0040] (Formula (1)) The binder component includes (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof. [ka] In the formula, R is an alkylene group. The number of carbon atoms in the alkylene group is preferably 1 to 9, and more preferably 1 to 5. Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a propylene group, a butylene group, a tetramethylene group, a pentylene group, and a hexylene group. R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group or a halogen atom. The number of carbon atoms in the alkyl group is preferably 1 to 9, and more preferably 1 to 5. Examples of the alkyl group include a methyl group, an ethyl group, a trimethyl group, a propyl group, a butyl group, a tetramethyl group, a pentyl group, and a hexyl group. The number of carbon atoms in the alkoxyalkyl group is preferably 1 to 9, more preferably 1 to 5. Examples of the alkoxy group in the alkoxyalkyl group include a methoxy group, an ethoxy group, a propoxy group, etc. Examples of the alkyl group in the alkoxyalkyl group include a methyl group, an ethyl group, a trimethyl group, a propyl group, a butyl group, a tetramethyl group, a pentyl group, a hexyl group, etc. The number of carbon atoms in the acyloxy group is preferably 1 to 9, more preferably 1 to 5. Examples of the acyloxy group include an acetyloxy group and a benzoyloxy group. Examples of halogen atoms include fluorine, chlorine, bromine, and iodine.

[0041] (Formula (2)) The binder component includes (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof. [ka] In formula (2), R 1 is the same as formula (1). n is 1 or 2. R 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group. The number of carbon atoms in the alkyl group is preferably 1 to 9, and more preferably 1 to 5. Examples of the alkyl group include a methyl group, an ethyl group, a trimethyl group, a propyl group, a butyl group, a tetramethyl group, a pentyl group, and a hexyl group. The number of carbon atoms in the alkenyl group is preferably 1 to 9, more preferably 1 to 5. Examples of the alkenyl group include an ethenyl group, a propenyl group, a butenyl group, a penyl group, and a hexenyl group. The number of carbon atoms in the alkoxyalkyl group is preferably 1 to 9, more preferably 1 to 5. Examples of the alkoxy group in the alkoxyalkyl group include a methoxy group, an ethoxy group, a propoxy group, etc. Examples of the alkyl group in the alkoxyalkyl group include a methyl group, an ethyl group, a trimethyl group, a propyl group, a butyl group, a tetramethyl group, a pentyl group, a hexyl group, etc.

[0042] (Ionizing radiation curable resin) Examples of the binder component include (iii) ionizing radiation curable resins. Examples of the ionizing radiation curable resins include urethane acrylates. Urethane acrylates are obtained by reacting a terminal isocyanate compound obtained by reacting a polyisocyanate compound with a polyol compound having multiple hydroxyl groups, and then reacting the resulting compound with a hydroxyl group-containing (meth)acrylate. The (meth)acryloyl group in the urethane acrylate is a functional group; for example, a urethane acrylate having two (meth)acryloyl groups is bifunctional, and one having three is trifunctional. Examples of the urethane acrylate include bifunctional to hexafunctional urethane acrylates. An example of a bifunctional urethane acrylate is one in which a terminal isocyanate compound is reacted with pentaerythritol mono(meth)acrylate to introduce one (meth)acryloyl group into each of both ends.

[0043] An example of a trifunctional urethane acrylate is one obtained by reacting pentaerythritol mono(meth)acrylate and pentaerythritol di(meth)acrylate with a terminal isocyanate compound to introduce one (meth)acryloyl group at one end of the isocyanate compound and two (meth)acryloyl groups at the other end. An example of a tetrafunctional urethane acrylate is one obtained by reacting pentaerythritol di(meth)acrylate with a terminal isocyanate compound to introduce two (meth)acryloyl groups at each of both ends of the isocyanate compound. An example of a hexafunctional urethane acrylate is one in which three (meth)acryloyl groups are introduced to each of the molecular chain terminals by reacting pentaerythritol tri(meth)acrylate with isocyanate at both ends (for example, trihexadiethylene diisocyanate). Further, examples include urethane acrylates in which a desired number of (meth)acryloyl groups are introduced into a hydroxyl group-containing (meth)acrylic acid ester such as a monoester or diester of (meth)acrylic acid of ethylene glycol, diethylene glycol, or a trihydric or higher polyhydric alcohol. A trifunctional or lower urethane acrylate and a quadruple or higher functional urethane acrylate can also be used in combination. The trifunctional or lower urethane acrylate and the quadruple or higher functional urethane acrylate are preferably used in a weight ratio of 2 / 98 to 70 / 30, particularly 10 / 90 to 60 / 40.

[0044] (metal oxide particles) The metal oxide particles may have a refractive index of 1.50 or more. For example, at least one oxide particle selected from the group consisting of titanium oxide, zirconium oxide, niobium pentoxide, antimony-doped tin oxide (ATO), indium oxide-tin oxide (ITO), phosphorus-doped tin oxide (PTO), fluorine-doped tin oxide (FTO) and antimony pentoxide is preferable. More specifically, the metal oxide particles include zirconium oxide particles (refractive index = 2.40), composite zirconium metal oxide particles in which zirconium oxide is combined with other oxides such as silicon oxide at the molecular level to adjust the refractive index, titanium oxide particles (refractive index = 2.71), composite titanium metal oxide particles in which titanium oxide is combined with other oxides such as silicon oxide or zirconium oxide at the molecular level to adjust the refractive index, etc. These metal oxide particles are appropriately combined to adjust the layer to the desired refractive index. Such particles are known per se and are commercially available. The average particle size of the metal oxide particles is preferably 1 to 100 nm, more preferably 1 to 70 nm.The refractive index of the metal oxide particles is preferably 1.70 to 2.80, more preferably 1.90 to 2.50. The content of the metal oxide particles in the solution for forming the medium-low refractive index layer (ML) is preferably 40 to 500 parts by mass with respect to 100 parts by mass of the binder component.

[0045] (Anti-static function) When the mid-low refractive index layer (ML) contains at least one type of conductive particle selected from the group consisting of antimony-doped tin oxide (ATO), indium oxide-tin oxide (ITO), phosphorus-doped tin oxide (PTO), fluorine-doped tin oxide (FTO) and antimony pentoxide, the mid-low refractive index layer (ML) can be endowed with an antistatic function. In this case, the content of the conductive particles is preferably 100 to 500 parts by mass, more preferably 200 to 500 parts by mass, and further preferably 300 to 500 parts by mass, relative to 100 parts by mass of the binder component. The average particle size of the conductive particles is preferably 1 to 50 nm, and more preferably 1 to 30 nm. When the medium-low refractive index layer (ML) is provided with an antistatic function, the thickness of the medium-low refractive index layer (ML) is preferably 10 to 50 nm. The lower limit of the thickness is preferably 15 nm, more preferably 20 nm. The upper limit of the thickness is preferably 50 nm, more preferably 48 nm.

[0046] When the medium-low refractive index layer (ML) does not require an antistatic function, it may contain at least one oxide particle selected from the group consisting of titanium oxide, zirconium oxide, and niobium pentoxide. In this case, the content of the metal oxide particles is preferably 10 to 100 parts by mass, more preferably 20 to 60 parts by mass, and even more preferably 30 to 60 parts by mass, relative to 100 parts by mass of the binder component. The average particle size of the metal oxide particles is preferably 10 to 100 nm, more preferably 20 to 80 nm. The thickness of the medium-low refractive index layer (ML) is preferably 50 to 200 nm. The lower limit of the thickness is preferably 60 nm, more preferably 80 nm. The upper limit of the thickness is preferably 200 nm, more preferably 180 nm.

[0047] (Metal chelate compounds) The metal chelate compound is contained for the purpose of increasing the denseness, strength, and hardness of the layer. The metal chelate compound is a compound in which a chelating agent, typically a bidentate ligand, is coordinated to a metal such as titanium, zirconium, or aluminum.

[0048] Specifically, titanium chelate compounds such as triethoxy mono(acetylacetonate)titanium, tri-n-propoxy mono(acetylacetonate)titanium, diethoxy bis(acetylacetonate)titanium, monoethoxy tris(acetylacetonate)titanium, tetrakis(acetylacetonate)titanium, triethoxy mono(ethylacetoacetate)titanium, diethoxy bis(ethylacetoacetate)titanium, monoethoxy tris(ethylacetoacetate)titanium, mono(acetylacetonate)tris(ethylacetoacetate)titanium, bis(acetylacetonate)bis(ethylacetoacetate)titanium, and tris(acetylacetonate)mono(ethylacetoacetate)titanium; Zirconium chelate compounds such as triethoxy mono(acetylacetonate)zirconium, tri-n-propoxy mono(acetylacetonate)zirconium, diethoxy bis(acetylacetonate)zirconium, monoethoxy tris(acetylacetonate)zirconium, tetrakis(acetylacetonate)zirconium, triethoxy mono(ethylacetoacetate)zirconium, diethoxy bis(ethylacetoacetate)zirconium, monoethoxy tris(ethylacetoacetate)zirconium, tetrakis(ethylacetoacetate)zirconium, mono(acetylacetonate)tris(ethylacetoacetate)zirconium, bis(acetylacetonate)bis(ethylacetoacetate)zirconium, and tris(acetylacetonate)mono(ethylacetoacetate)zirconium; Examples of aluminum chelate compounds include diethoxy mono(acetylacetonate)aluminum, monoethoxy bis(acetylacetonate)aluminum, di-i-propoxy mono(acetylacetonate)aluminum, mono-i-propoxy bis(ethylacetoacetate)aluminum, monoethoxy bis(ethylacetoacetate)aluminum, diethoxy mono(ethylacetoacetate)aluminum, tris(acetylacetonate)aluminum, and bis(ethylacetoacetate)mono(acetylacetonate)aluminum.

[0049] The content of the metal chelate compound in the solution for forming the medium-low refractive index layer (ML) is preferably 10 parts by mass or less relative to 100 parts by mass of the binder component. The lower limit of the content is preferably 1 part by mass, more preferably 3 parts by mass, relative to 100 parts by mass of the binder component. The upper limit of the content is preferably 8 parts by mass, more preferably 6 parts by mass, relative to 100 parts by mass of the binder component. When the medium-low refractive index layer (ML) contains at least one type of conductive particle selected from the group consisting of antimony-doped tin oxide (ATO), indium oxide-tin oxide (ITO), phosphorus-doped tin oxide (PTO), fluorine-doped tin oxide (FTO) and antimony pentoxide to impart an antistatic function, it is not necessary to contain a metal chelate compound.

[0050] (Formation of low and medium refractive index layer (ML)) The medium-low refractive index layer (ML) is formed by dissolving the above-mentioned components in specific amounts, and further optional components, in the following solvents for the purpose of viscosity adjustment and easy application to prepare a coating solution for the medium-low refractive index layer (ML), applying this solution to the hard coat layer (HC), drying it, and then heating and curing it. Curing can be performed by irradiating it with ionizing radiation such as ultraviolet rays (UV) or electron beams (EB).

[0051] Suitable solvents for use in the coating solution for the medium-low refractive index layer (ML) include alcohol compounds such as methyl alcohol, ethyl alcohol, and propyl alcohol, aromatic compounds such as toluene and xylene, ester compounds such as ethyl acetate, butyl acetate, and isobutyl acetate, and ketone compounds such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), and diacetone alcohol. In addition, solvents such as methylene glycol monomethyl ether acetate, ethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate, as well as cellosolve compounds such as methyl cellosolve, ethyl cellosolve, and propylene glycol monomethyl ether can also be used. Each of the above components constituting the coating solution for the low and medium refractive index layer (ML) is usually arbitrarily mixed and stirred near room temperature to form a solution. When a commercially available particle dispersion is used, the solvent as the dispersion medium will inevitably be mixed into the solution. The solvent in the coating solution for the low and medium refractive index layer (ML) and the solvent separately blended are removed in the drying and curing processes.

[0052] The method of coating the solution onto the hard coat layer (HC) is not particularly limited, and methods such as dip coating method, roll coating method, die coating method, flow coating method, spray method, etc. are adopted. From the viewpoints of appearance quality and film thickness control, the dip coating method is preferred. Then, it is dried, and then heated and thermally cured to form the low and medium refractive index layer (ML). Also, the low and medium refractive index layer (ML) can be formed by performing a curing reaction by irradiating ionizing radiation such as ultraviolet rays and electron beams.

[0053] 〔Medium refractive index layer (M)〕 The refractive index of the medium refractive index layer (M) is 1.550 to 1.810. The lower limit of the refractive index is preferably 1.550, more preferably 1.580. The upper limit of the refractive index is preferably 1.800, more preferably 1.770. The film thickness of the medium refractive index layer (M) is 20 to 150 nm. The lower limit of the film thickness is preferably 25 nm, more preferably 50 nm. The upper limit of the film thickness is preferably 130 nm, more preferably 110 nm. When RI(M) < RI(H), that is, when the refractive index of the medium refractive index layer (M) is smaller than the refractive index of the high refractive index layer (H), the lower limit of the refractive index of the medium refractive index layer (M) is preferably 1.550, more preferably 1.580. The upper limit of the refractive index of the medium refractive index layer (M) is preferably 1.730, more preferably 1.710, and even more preferably 1.700. When RI(M)=RI(H), that is, when the refractive index of the medium refractive index layer (M) is the same as that of the high refractive index layer (H), the lower limit of the refractive index of the medium refractive index layer (M) is preferably 1.750, more preferably 1.760. The upper limit of the refractive index of the medium refractive index layer (M) is preferably 1.810, more preferably 1.790, and even more preferably 1.770.

[0054] The medium refractive index layer (M) is preferably made of a cured product of a composition containing a binder component, metal oxide particles, and a metal chelate compound. The medium refractive index layer (M) is preferably made of a cured product of a composition containing 40 to 500 parts by mass of metal oxide particles and 1 to 20 parts by mass of a metal chelate compound per 100 parts by mass of the binder component.

[0055] (Binder component) The binder component is preferably at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by formula (2) or a hydrolysate thereof. Formulas (1) and (2) are as described in the section on the mid-low refractive index layer (ML).

[0056] (metal oxide particles) The metal oxide particles used in the medium refractive index layer (M) can be the same type of metal oxide particles as those used to form the medium-low refractive index layer (ML), and can be selected from among them.

[0057] (Metal chelate compounds) The metal chelate compound used in the medium refractive index layer (M) can be the same type as the metal chelate compound used to form the medium-low refractive index layer (ML), and can be selected from among them.

[0058] (Formation of medium refractive index layer (M)) The medium refractive index layer (M) can be formed by dissolving specific amounts of each of the above components, as well as any optional components, in a solvent to prepare a solution for the medium refractive index layer (M), applying this solution to the medium-low refractive index layer (ML), drying it, and then heating and heat-curing it. The solvent used in the coating solution for the medium refractive index layer (M) is the same as that used in the coating solution for the medium-low refractive index layer (ML). The thickness of the layer is set in the range of 20 to 150 nm from the viewpoint of anti-reflection performance. The mixing order and mixing conditions of the above components constituting the solution for the medium refractive index layer (M), and further the coating method on the medium-low refractive index layer (ML) are not particularly limited.

[0059] [High refractive index layer (H)] The antireflection layer (AR) has a high refractive index layer (H) between a medium refractive index layer (M) and a low refractive index layer (L) in order to exhibit an extremely high antireflection effect. The refractive index of the high refractive index layer (H) is 1.700 to 1.850. The lower limit of the refractive index is preferably 1.710, more preferably 1.730. The upper limit of the refractive index is preferably 1.830, more preferably 1.810. The high refractive index layer (H) has a thickness of 10 to 250 nm. The lower limit of the thickness is preferably 15 nm, more preferably 50 nm. The upper limit of the thickness is preferably 210 nm, more preferably 150 nm. The high refractive index layer (H) is preferably made of a cured product of a composition containing a binder component, metal oxide particles, and a metal chelate compound. The high refractive index layer (H) is preferably made of a cured product of a composition containing 300 to 500 parts by mass of metal oxide particles and 10 to 20 parts by mass of a metal chelate compound per 100 parts by mass of the binder component.

[0060] (Binder component) The binder component is preferably at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by formula (2) or a hydrolysate thereof. Formulas (1) and (2) are as described in the section on the mid-low refractive index layer (ML).

[0061] (metal oxide particles) The metal oxide particles used in the high refractive index layer (H) can be the same type of metal oxide particles as those used to form the medium-low refractive index layer (ML), and can be selected from among them.

[0062] (Metal chelate compounds) The metal chelate compound used in the high refractive index layer (H) can be the same type as the metal chelate compound used to form the medium-low refractive index layer (ML), and can be selected from among them.

[0063] (Formation of high refractive index layer (H)) The high refractive index layer (H) can be formed by dissolving each component, and further any optional components, in various solvents used in forming the medium-low refractive index layer (ML) to prepare a coating solution for the high refractive index layer (H), applying this solution to the medium refractive index layer (M), drying it, and then heating and curing it. The thickness of the layer is set in the range of 10 to 250 nm from the viewpoint of anti-reflection performance. The mixing order and mixing conditions of the above components constituting the coating solution for the high refractive index layer (H), and further the method of coating onto the medium refractive index layer (M) are not particularly limited, and the method used when forming the medium-low refractive index layer (ML) can be used. The antireflection layers (medium-low refractive index layer, medium refractive index layer, high refractive index layer and low refractive index layer) formed by applying and then curing the coating solution in the above-mentioned solution state by a so-called wet method have superior infrared transmittance compared to antireflection layers formed by a dry method. The reason for this is considered to be as follows. The high refractive index layer produced by the wet method has a lower refractive index than that produced by the dry method due to the presence of a binder component, and as a result, the low reflection design in the visible range can suppress a sudden increase in reflectance in the outer visible range. As a result, the wet method provides low reflectance in a wide range of the visible and outer visible light ranges, and a relatively high transmittance in the infrared range.

[0064] [Low refractive index layer (L)] The refractive index of the low refractive index layer (L) is 1.450 or less. The lower limit of the refractive index is preferably 1.300, more preferably 1.320. The upper limit of the refractive index is preferably 1.440, more preferably 1.430. The low refractive index layer (L) has a thickness of 70 to 130 nm. The lower limit of the thickness is preferably 75 nm, more preferably 80 nm. The upper limit of the thickness is preferably 120 nm, more preferably 110 nm. The low refractive index layer (L) is preferably made of a cured product of a composition containing a binder component, silica particles, and a metal chelate compound. The low refractive index layer (L) is preferably made of a cured product of a composition containing 100 to 200 parts by mass of silica particles and 5 to 15 parts by mass of a metal chelate compound per 100 parts by mass of the binder component.

[0065] (Binder component) The binder component is preferably at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by formula (2) or a hydrolysate thereof. Formulas (1) and (2) are as described in the section on the mid-low refractive index layer (ML).

[0066] (Silica particles) From the viewpoint of exerting an anti-reflection effect, it is preferable to use hollow silica particles having a space inside. The average particle size is preferably 10 to 150 nm. Since the hollow silica particles are particles with a cavity inside, their density is lower than other silica particles, and is, for example, usually 1.5 g / cm. 3 The following is the result. Such hollow silica particles are known per se, and are commercially available, for example, produced by synthesizing silica in the presence of a surfactant that serves as a template, and finally calcining to decompose and remove the surfactant. Note that, in such commercially available products, the hollow silica particles are dispersed in a solvent such as water or alcohol, so that these solvents are inevitably mixed into the low refractive index layer (L) forming solution prepared to form the low refractive index layer (L). However, during drying and curing after coating, these solvents are volatilized and removed together with the solvent that is separately mixed to make the coating solution. It is preferable to use hollow silica particles, but solid silica particles that do not have internal cavities can also be used.

[0067] The content of the silica particles in the low refractive index layer (L) forming solution is preferably 100 to 200 parts by mass, more preferably 110 to 190 parts by mass, and further preferably 120 to 185 parts by mass, based on 100 parts by mass of the binder component.

[0068] (Metal chelate compounds) The metal chelate compound is contained for the purpose of increasing the denseness, strength, and hardness of the layer. The metal chelate compound is a compound in which a chelating agent, typically a bidentate ligand, is coordinated to a metal such as titanium, zirconium, or aluminum.

[0069] Specifically, titanium chelate compounds such as triethoxy mono(acetylacetonate)titanium, tri-n-propoxy mono(acetylacetonate)titanium, diethoxy bis(acetylacetonate)titanium, monoethoxy tris(acetylacetonate)titanium, tetrakis(acetylacetonate)titanium, triethoxy mono(ethylacetoacetate)titanium, diethoxy bis(ethylacetoacetate)titanium, monoethoxy tris(ethylacetoacetate)titanium, mono(acetylacetonate)tris(ethylacetoacetate)titanium, bis(acetylacetonate)bis(ethylacetoacetate)titanium, and tris(acetylacetonate)mono(ethylacetoacetate)titanium; Zirconium chelate compounds such as triethoxy mono(acetylacetonate)zirconium, tri-n-propoxy mono(acetylacetonate)zirconium, diethoxy bis(acetylacetonate)zirconium, monoethoxy tris(acetylacetonate)zirconium, tetrakis(acetylacetonate)zirconium, triethoxy mono(ethylacetoacetate)zirconium, diethoxy bis(ethylacetoacetate)zirconium, monoethoxy tris(ethylacetoacetate)zirconium, tetrakis(ethylacetoacetate)zirconium, mono(acetylacetonate)tris(ethylacetoacetate)zirconium, bis(acetylacetonate)bis(ethylacetoacetate)zirconium, and tris(acetylacetonate)mono(ethylacetoacetate)zirconium; Examples of aluminum chelate compounds include diethoxy mono(acetylacetonate)aluminum, monoethoxy bis(acetylacetonate)aluminum, di-i-propoxy mono(acetylacetonate)aluminum, mono-i-propoxy bis(ethylacetoacetate)aluminum, monoethoxy bis(ethylacetoacetate)aluminum, diethoxy mono(ethylacetoacetate)aluminum, tris(acetylacetonate)aluminum, and bis(ethylacetoacetate)mono(acetylacetonate)aluminum.

[0070] The content of the metal chelate compound in the low refractive index layer (L) forming solution is preferably 5 to 15 parts by mass, more preferably 5 to 13 parts by mass, and further preferably 5 to 10 parts by mass, based on 100 parts by mass of the binder component.

[0071] (Formation of low refractive index layer (L)) The low refractive index layer (L) can be formed by dissolving specific amounts of the above-mentioned components, as well as any optional components, in the following solvents for the purpose of adjusting viscosity and making it easier to apply to prepare a coating solution for the low refractive index layer (L), applying this solution to the hard coat layer (HC), drying it, and then heating and thermally curing it.

[0072] Suitable solvents for use in the coating solution for the low refractive index layer (L) include alcohol compounds such as methyl alcohol, ethyl alcohol, and propyl alcohol; aromatic compounds such as toluene and xylene; ester compounds such as ethyl acetate, butyl acetate, and isobutyl acetate; and ketone compounds such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), and diacetone alcohol. In addition, solvents such as methylene glycol monomethyl ether acetate, ethylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether acetate, as well as cellosolve compounds such as methyl cellosolve, ethyl cellosolve, and propylene glycol monomethyl ether can also be used. The above components constituting the coating solution for the low refractive index layer (L) are usually mixed and stirred at room temperature to form a solution. When a commercially available particle dispersion is used, the solvent, which is the dispersion medium, is inevitably mixed into the solution. The solvent in the coating solution for the low refractive index layer (L) and any other solvents added separately are removed in the drying and curing steps. The method for applying the solution onto the high refractive index layer (H) is not particularly limited, and methods such as dip coating, roll coating, die coating, flow coating, and spraying can be used. From the viewpoint of appearance quality and film thickness control, the dip coating method is preferred.

[0073] <Protective layer (C)> The antireflective laminate of the present invention may have a protective layer (C) on the antireflective layer (AR). The refractive index of the protective layer (C) is preferably 1.450 to 1.550. The lower limit of the refractive index is preferably 1.460, more preferably 1.470. The upper limit of the refractive index is preferably 1.530, more preferably 1.520.

[0074] The thickness of the protective layer (C) is 5 to 50 nm. The lower limit of the thickness is preferably 10 nm, more preferably 15 nm. The upper limit of the thickness is preferably 40 nm, more preferably 30 nm. The protective layer (C) is preferably made of a cured product of a composition containing a binder component, silica particles, and a metal chelate compound. The protective layer (C) is preferably made of a cured product of a composition containing 10 to 30 parts by mass of solid silica particles and 5 to 15 parts by mass of a metal chelate compound per 100 parts by mass of the binder component.

[0075] (Binder component) The binder component is preferably at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by formula (2) or a hydrolysate thereof. Formulas (1) and (2) are as described in the section on the mid-low refractive index layer (ML).

[0076] (Solid Silica Particles) The protective layer (C) preferably contains solid silica particles. The solid silica particles in the protective layer (C) preferably have a particle size of 5 to 500 nm and a refractive index of 1.44 to 1.5. In other words, by using such oxide fine particles, basic properties such as hardness can be uniformly imparted to the entire protective layer (C).

[0077] (Metal chelate compounds) The metal chelate compound used in the protective layer (C) can be the same as the metal chelate compound used in forming the medium-low refractive index layer (ML), and can be selected from these.

[0078] (Formation of protective layer (C)) The protective layer (C) is formed by dissolving each component, and further optional components, in various solvents used in forming the medium-low refractive index layer (ML) to prepare a coating solution for the protective layer (C), applying this solution to the low refractive index layer (L), drying it, and then heating and curing it. From the viewpoint of antireflection performance, the thickness of the layer is preferably 5 to 100 nm, more preferably 20 to 70 nm, and even more preferably 30 to 50 nm.

[0079] The mixing order and mixing conditions of the above components constituting the coating solution for the protective layer (C), as well as the method of coating onto the low refractive index layer (L), are not particularly limited, and the method used when forming the medium-low refractive index layer (ML) can be used.

[0080] <Antistatic layer (AS)> The antireflection laminate of the present invention may have an antistatic layer (AS) between the hard coat layer (HC) and the medium-low refractive index layer (ML). The antistatic layer (AS) is preferably made of a cured product of a composition containing a binder component and conductive particles. The antistatic layer (AS) is preferably made of a cured product of a composition containing 100 to 500 parts by mass of conductive particles per 100 parts by mass of the binder component. The thickness of the antistatic layer (AS) is preferably from 10 to 200 nm, more preferably from 20 to 150 nm, further preferably from 30 to 100 nm, and even more preferably from 40 to 80 nm.

[0081] (Conductive particles) Suitable conductive particles include indium oxide, indium oxide-tin oxide (ITO), tin oxide, antimony-doped tin oxide (ATO), phosphorus-doped tin oxide (PTO), fluorine-doped tin oxide (FTO), zinc oxide, aluminum-doped zinc oxide (AZO), and gallium-doped zinc oxide (GZO). Among them, tin oxide-based conductive particles have absorption that is positively correlated with wavelength, and the light transmission absorption loss of the formed antireflection laminate is reduced by Q 450 550 650 This can be easily done. The antistatic layer (AS) preferably contains at least one type of conductive particles selected from the group consisting of indium oxide-tin oxide (ITO), antimony-doped tin oxide (ATO), phosphorus-doped tin oxide (PTO) and fluorine-doped tin oxide (FTO). Organic conductive particles can also be used.

[0082] ​​The content of the conductive particles is preferably 200 to 500 parts by mass, more preferably 300 to 500 parts by mass, based on 100 parts by mass of the binder component. The particle size of the conductive particles is preferably 1 nm to 100 nm. The particle size is preferably 1 to 50 nm, more preferably 1 to 30 nm, and even more preferably 1 to 15 nm.

[0083] (Binder component) The binder component of the antistatic layer (AS) is preferably formed by curing a urethane acrylate having four or more functional groups. An example of a tetrafunctional or higher urethane acrylate is a hexafunctional urethane acrylate having three (meth)acryloyl groups at each of the molecular chain terminals, which is obtained by reacting pentaerythritol tri(meth)acrylate with an isocyanate at both ends (e.g., trihexadiethylene diisocyanate).

[0084] The monomer or oligomer serving as the binder component is preferably a urethane acrylate having four or more functionalities. An example of a urethane acrylate having four functionalities is one in which pentaerythritol di(meth)acrylate is reacted with a terminal isocyanate compound to introduce two (meth)acryloyl groups to each of both ends of the isocyanate compound. An example of a urethane acrylate having six functionalities (a2) is one in which pentaerythritol tri(meth)acrylate is reacted with a terminal isocyanate (e.g., trihexadiethylene diisocyanate) to introduce three (meth)acryloyl groups to each of the molecular chain ends.

[0085] If necessary, a solvent and various additives can be added to the coating liquid. The solvent is appropriately selected from aromatic hydrocarbons such as toluene, xylene, cyclohexane, and cyclohexylbenzene; hydrocarbons such as n-hexane; ethers such as dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, dioxane, dioxolane, trioxane, tetrahydrofuran, anisole, and phenetole; ketones such as methyl isobutyl ketone, methyl butyl ketone, acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methyl cyclopentanone, and methyl cyclohexanone; esters such as ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, and γ-butyrolactone; and cellosolves such as methyl cellosolve, cellosolve, butyl cellosolve, and cellosolve acetate, taking into consideration suitability for coating. The coating liquid may also contain additives such as a surface conditioner, a refractive index adjuster, an adhesion improver, and a hardener.

[0086] (Formation of antistatic layer (AS)) The antistatic layer (AS) can be formed by applying a coating liquid containing conductive particles and a monomer or oligomer for forming a binder component onto the substrate (B), forming a coating film on the substrate (B), drying the coating film as necessary, and then irradiating the coating with ionizing radiation such as ultraviolet light or an electron beam to cause a curing reaction of the monomer or oligomer for forming the resin component.

[0087] The coating liquid can be applied using a roll coater, reverse roll coater, gravure coater, microgravure coater, knife coater, bar coater, wire bar coater, die coater or dip coater.

[0088] In addition, when the coating liquid for forming the antistatic layer (AS) is cured by ultraviolet light, it is preferable to add a photopolymerization initiator to the coating liquid for forming the antistatic layer (AS). The photopolymerization initiator may be any one that generates radicals when irradiated with ultraviolet light, and for example, acetophenones, benzoins, benzophenones, phosphine oxides, ketals, anthraquinones, and thioxanthones can be used. The amount of the photopolymerization initiator added is preferably 1 to 10 parts by mass, more preferably 1 to 7 parts by mass, based on 100 parts by mass of the urethane acrylate having 4 or more functional groups.

[0089] <Anti-stain layer (AF)> Depending on the application, an antifouling layer (AF) may be laminated on the outermost surface. When an antifouling layer is provided, dirt (such as human fingerprints) attached to the antireflection laminate can be easily removed. In order to fully exert its function, the antifouling layer is preferably a layer that constitutes the outermost surface of the functional layer. The antifouling layer (AF) can be formed by coating with a fluororesin-based antifouling agent. Examples of fluororesin-based compounds include organosilicon compounds having one or more groups selected from the group consisting of polyfluoropolyether groups, polyfluoroalkylene groups, and polyfluoroalkyl groups. The polyfluoropolyether group is a divalent group having a structure in which polyfluoroalkylene groups and etheric oxygen atoms are alternately bonded. Specific examples of antifouling agents that are commercially available and easily available include the "SURECO (registered trademark) AF" series manufactured by AGC, the "SHIN-ETSU SUBELYN (registered trademark)" series manufactured by Shin-Etsu Chemical Co., Ltd., the "OPTOOL" series manufactured by Daikin Industries, Ltd., the "FLUOROSURF (registered trademark)" series manufactured by FluoroTechnology, the "DURASURF" series manufactured by Harbeth, and the "Ftergent" series manufactured by NEOS. The thickness of the antifouling layer (AF) is preferably 2 to 20 nm, more preferably 2 to 15 nm, and further preferably 2 to 10 nm.

[0090] <Layer structure of the antireflection laminate of the present invention> The antireflection laminate of the present invention is arranged in the order of substrate (B) / hard coat layer (HC) / medium / low refractive index layer (ML) / medium refractive index layer (M) / high refractive index layer (H) / low refractive index layer (L). A protective layer (C) may be provided on the surface of the low refractive index layer (L) opposite to the substrate (B). An antistatic layer (AS) may be provided between the hard coat layer (HC) and the medium-low refractive index layer (ML). The antireflection laminate of the present invention may have an antifouling layer (AF) on the outermost surface. In the present invention, each layer has the following characteristics. Feature 1: The low-medium refractive index layer (ML) has an antistatic function. Feature 2: The medium-low refractive index layer (ML) does not have an antistatic function. Feature 3: Refractive index of medium refractive index layer (M) < Refractive index of high refractive index layer (H) Feature 4: Refractive index of medium refractive index layer (M) = Refractive index of high refractive index layer (H) Feature 5: Has a protective layer. Feature 6: Has an antistatic layer. The antireflection laminates shown in the examples have the following characteristics. Examples 1 to 18: Feature 1 + Feature 3 Examples 19-20: Feature 2 + Feature 3 Example 21: Feature 1 + Feature 3 + Feature 5 Example 22: Feature 2 + Feature 3 Example 23: Feature 2 + Feature 4 Example 24: Feature 2 + Feature 3 + Feature 6 Example 25: Feature 2 + Feature 4 + Feature 6 Example 26: Feature 2 + Feature 4

[0091] <Characteristics of anti-reflection laminate> [Average visual reflectance on both sides] The average luminous reflectance of both surfaces of the antireflection laminate of the present invention at wavelengths of 380 to 780 nm is 0.6% or less, preferably 0.55% or less, and more preferably 0.5% or less. As is clear from a comparison of the reflectance distribution of the antireflection laminate of Example 1 shown in FIG. 2 with the reflectance distribution of the antireflection laminate of Comparative Example 1 shown in FIG. 3, the antireflection laminate of the present invention exhibits low reflectance over a wide wavelength range.

[0092] [Luminous average transmittance] The average luminous transmittance of the antireflection laminate of the present invention at a wavelength of 380 to 780 nm is preferably 95% or more, more preferably 96% or more, and further preferably 97% or more. [Infrared transmittance] The transmittance at a wavelength of 900 nm of the antireflection laminate of the present invention is preferably 85% or more, more preferably 87% or more, and further preferably 90% or more. EXAMPLES

[0093] For example, in the numbers of the tables in the examples, there are [Table 2-1] and [Table 2-2], which are divisions of [Table 2], and both may be referred to as [Table 2]. <Characteristics> The properties of the anti-reflection laminate were measured by the following methods. (Average visual reflectance on both sides) The average luminous reflectance of both surfaces was measured by the following method: Using an ultraviolet-visible spectrophotometer V-650 manufactured by JASCO Corporation, measurements were taken at 380 nm to 780 nm, and the result was calculated by multiplying by a weighting coefficient. (Luminous average transmittance) The average luminous transmittance was measured by the following method: Using an ultraviolet-visible spectrophotometer V-650 manufactured by JASCO Corporation, measurements were taken at 380 nm to 780 nm, and the result was calculated by multiplying by a weighting coefficient. (Infrared transmittance) The infrared transmittance was measured by the following method. A PbS detector was attached to an ultraviolet, visible, near infrared spectrophotometer: V-570 manufactured by JASCO Corporation, and the transmittance was measured from 380 to 1000 nm. From the obtained transmittance values, the transmittance value at a wavelength of 900 nm was taken as the infrared transmittance. The obtained transmittance value is the transmittance at each wavelength in 1 nm increments. (Refractive index of each layer) The refractive index of each layer was measured by the following method. Each layer was coated on an acrylic substrate, and the peak or bottom value was measured using a UV-Visible Spectrophotometer: V-650 manufactured by JASCO Corporation. The refractive index of each layer was calculated using the measured value.

[0094] <Solution for forming hard coat layer> The components shown in Table 1 below were mixed to prepare a solution for forming a hard coat layer. [Table 1]

[0095] <Anti-reflection layer (AR) forming solution> (Solution for forming low and medium refractive index layers (ML)) The components shown in Table 2 below were mixed in the amounts shown in Table 2 to prepare solutions for forming the medium-low refractive index layers (ML) (ml-1 to ml-6 and co-ml-1 to co-ml-2). (Medium refractive index layer (M) forming solution) The components shown in Table 3 below were mixed in the amounts shown in Table 3 to prepare solutions for forming a medium refractive index layer (M) (m-1 to m-7 and co-m-1 to co-m-2).

[0096] (Solution for forming high refractive index layer (H)) The components shown in Table 4 below were mixed in the amounts shown in Table 4 to prepare solutions for forming a high refractive index layer (H) (h-1 to h-4 and co-h-1). (Low refractive index layer (L) forming solution) The components shown in Table 5 below were mixed in the amounts shown in Table 5 to prepare solutions (l-1 to l-6 and co-l-1) for forming a low refractive index layer (L).

[0097] [Table 2-1]

[0098] [Table 2-2]

[0099] [Table 3-1]

[0100] [Table 3-2]

[0101] [Table 4]

[0102] [Table 5-1]

[0103] [Table 5-2]

[0104] <Example 1> A hard coat layer (HC) and an anti-reflection layer (AR) were formed in this order on a 1 mm thick polymethyl methacrylate (PMMA) substrate (B) by the following method. The film thickness was adjusted by the pulling speed from the layer-forming solution into which the film had been dipped. The composition, film thickness, refractive index, average luminous reflectance at wavelengths of 380 to 780 nm, average luminous transmittance at wavelengths of 380 to 780 nm, and infrared transmittance at a wavelength of 900 nm for each layer are shown in Table 6.

[0105] [Formation of hard coat layer (HC)] The substrate (B) was dipped in the solution for forming a hard coat layer, then dried at 80°C for 10 minutes and cured with UV at 500 mJ to obtain a laminate (HC) in which a hard coat layer (HC) having a thickness of 2 μm was formed on the substrate (B).

[0106] [Formation of Anti-Reflection Layer (AR)] On the laminate (HC), a medium / low refractive index layer (ML), a medium refractive index layer (M), a high refractive index layer (H) and a low refractive index layer (L) were formed by the following procedure. (Formation of low and medium refractive index layer (ML)) The laminate (HC) was dipped in a solution for forming a medium-low refractive index layer (ml-1), then dried at 80°C for 10 minutes, and UV cured under a condition of 500 mJ to obtain a laminate (ML) with a medium-low refractive index layer (ML). (Formation of medium refractive index layer (M)) The laminate (ML) was dipped in a solution (m-1) for forming a medium refractive index layer, and then heat-treated at 100°C for 60 minutes to obtain a laminate (MLM) having a medium refractive index layer (M). (Formation of high refractive index layer (H)) The laminate (MLM) was then dipped into a high refractive index layer forming solution (h-1) and then heat-treated at 100°C for 60 minutes to obtain a laminate (MLMH) having a high refractive index layer (H). (Formation of low refractive index layer (L)) The laminate (MLMH) was then dipped in a solution (l-1) for forming a low refractive index layer, and then heat-treated at 100°C for 120 minutes to obtain a laminate (AR) with a low refractive index layer (L). Figure 2 shows the distribution of the average luminous reflectance.

[0107] <Example 2> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were as shown in Table 6.

[0108] <Example 3> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were as shown in Table 6.

[0109] <Examples 4 to 7> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness of each layer was set as shown in Table 6.

[0110] <Example 8> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness of each layer was set as shown in Table 6.

[0111] <Example 9> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness of each layer was set as shown in Table 6.

[0112] <Example 10> An antireflection laminate was produced in the same manner as in Example 1, except that l-2 was used as the low refractive index layer-forming solution and the film thickness and refractive index of each layer were set as shown in Table 6.

[0113] <Example 11> An antireflection laminate was produced in the same manner as in Example 1, except that l-3 was used as the low refractive index layer-forming solution and the film thickness and refractive index of each layer were set as shown in Table 6.

[0114] <Example 12> An antireflection laminate was produced in the same manner as in Example 1, except that h-2 was used as the high refractive index layer-forming solution and the film thickness and refractive index of each layer were as shown in Table 6.

[0115] <Example 13> An antireflection laminate was produced in the same manner as in Example 1, except that h-3 was used as the high refractive index layer-forming solution and the thickness and refractive index of each layer were as shown in Table 6.

[0116] <Example 14> An antireflection laminate was produced in the same manner as in Example 1, except that m-2 was used as the solution for forming the medium refractive index layer and the film thickness and refractive index of each layer were set as shown in Table 6.

[0117] <Example 15> An antireflection laminate was produced in the same manner as in Example 1, except that m-3 was used as the solution for forming the medium refractive index layer and the film thickness and refractive index of each layer were set as shown in Table 6.

[0118] <Example 16> An antireflection laminate was produced in the same manner as in Example 1, except that ml-2 was used as the solution for forming the medium to low refractive index layers and the film thickness and refractive index of each layer were set as shown in Table 6.

[0119] <Example 17> An antireflection laminate was produced in the same manner as in Example 1, except that ml-3 was used as the solution for forming the medium to low refractive index layers and the film thickness and refractive index of each layer were set as shown in Table 6.

[0120] <Example 18> An anti-reflection laminate was produced in the same manner as in Example 1, except that ml-4 was used as the solution for forming the medium and low refractive index layer, m-4 was used as the solution for forming the medium refractive index layer, and l-4 was used as the solution for forming the low refractive index layer, and the film thickness and refractive index of each layer were as shown in Table 6.

[0121] <Example 19> After dipping in ml-5 as a solution for forming a medium-low refractive index layer, the laminate (ML) was obtained by heat treatment at 100° C. for 60 minutes to form a medium-low refractive index layer (ML). An anti-reflection laminate was produced in the same manner as in Example 1, except that m-5 was used as a solution for forming a medium refractive index layer, h-4 was used as a solution for forming a high refractive index layer, and l-5 was used as a solution for forming a low refractive index layer, and the film thickness and refractive index of each layer were as shown in Table 6.

[0122] <Example 20> After dipping in ml-5 as a solution for forming a medium-low refractive index layer, a laminate (ML) was obtained by heat-treating at 100° C. for 60 minutes to form a medium-low refractive index layer (ML). An anti-reflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were as shown in Table 6. The composition, thickness, refractive index, average luminous reflectance at wavelengths of 380 to 780 nm, average luminous transmittance at wavelengths of 380 to 780 nm, and infrared transmittance at a wavelength of 900 nm of each layer of Examples 1 to 20 are shown in Table 6. The abbreviations in the table are as follows. γ-GPS: 3-glycidoxypropyltrimethoxysilane ATAA: Aluminum tris(acetylacetonate) PEA: Pentaerythritol acrylate

[0123] [Table 6-1]

[0124] [Table 6-2]

[0125] [Table 6-3]

[0126] [Table 6-4]

[0127] [Table 6-5]

[0128] <Example 21> With protective layer (Protective layer forming solution) As a solution for forming a protective layer, c-1 having the composition shown in Table 7 was prepared.

[0129] [Table 7] A hard coat layer (HC), an anti-reflection layer (AR) and a protective layer (C) were formed in this order on a 1 mm thick polymethyl methacrylate (PMMA) substrate (B) by the following method. The film thickness was adjusted by the withdrawal speed from the layer-forming solution into which the substrate was dipped.

[0130] [Formation of hard coat layer (HC)] The substrate (B) was dipped in the solution for forming a hard coat layer, then dried at 80°C for 10 minutes and cured with UV at 500 mJ to obtain a laminate (HC) in which a hard coat layer (HC) having a thickness of 2 μm was formed on the substrate (B). [Formation of Anti-Reflection Layer (AR)] A laminate (AR) was produced in the same manner as in Example 1, except that 1-6 was used as the low refractive index layer forming solution and the film thickness and refractive index of each layer were set as shown in Table 8. [Formation of protective layer (C)] The laminate (AR) was dipped in the protective layer forming solution (c-1) and then heat-treated at 100°C for 120 minutes to produce a laminate (C) having a protective layer (C) formed on the laminate (AR).

[0131] <Example 22> After dipping in ml-6 as a solution for forming a medium-low refractive index layer, the laminate (ML) was obtained by heat treatment at 100° C. for 60 minutes to form a medium-low refractive index layer (ML). An anti-reflection laminate was produced in the same manner as in Example 1, except that m-6 was used as a solution for forming a medium refractive index layer, h-4 was used as a solution for forming a high refractive index layer, and l-6 was used as a solution for forming a low refractive index layer, and the film thickness and refractive index of each layer were as shown in Table 8.

[0132] Example 23: Medium refractive index layer (M) = high refractive index layer (H) A low-medium refractive index layer (ML) was formed using ml-6 as a solution for forming a low-medium refractive index layer, a medium refractive index layer (M) was formed using m-7 as a solution for forming a medium refractive index layer, and a layer was formed thereon using a solution for forming a high refractive index layer h-4 to form a high refractive index layer (H). That is, the medium refractive index layer (M) and the high refractive index layer (H) were made exactly the same layer. The solution for forming a medium refractive index layer m-7 and the solution for forming a high refractive index layer h-4 have the same composition except for the solvent. Furthermore, a low refractive index layer (L) was formed using l-6 as a solution for forming a low refractive index layer. An anti-reflection laminate was manufactured in the same manner as in Example 1, except that the film thickness and refractive index of each layer were as shown in Table 8. The composition, thickness, refractive index, average luminous reflectance at wavelengths of 380 to 780 nm, average luminous transmittance at wavelengths of 380 to 780 nm, and infrared transmittance at a wavelength of 900 nm of each layer of Examples 21 to 23 are shown in Table 8. The abbreviations in Table 8 are as follows. γ-GPS: 3-glycidoxypropyltrimethoxysilane ATAA: Aluminum tris(acetylacetonate) PEA: Pentaerythritol acrylate

[0133] [Table 8]

[0134] <Example 24> With antistatic layer (AS) (Antistatic layer forming solution) The components shown in Table 9 below were mixed to prepare an antistatic layer-forming solution as-1.

[0135] [Table 9] A hard coat layer (HC), an antistatic layer (AS) and an antireflective layer (AR) were formed in this order on a 1 mm thick polymethyl methacrylate (PMMA) substrate (B) by the following method. The film thickness was adjusted by changing the withdrawal speed from the layer-forming solution into which the film was dipped.

[0136] [Formation of hard coat layer (HC)] The substrate (B) was dipped in the solution for forming a hard coat layer, then dried at 80°C for 10 minutes and cured with UV at 500 mJ to obtain a laminate (HC) in which a hard coat layer (HC) having a thickness of 2 μm was formed on the substrate (B). [Formation of antistatic layer (AS)] The laminate (HC) was dipped into the obtained solution and then heat-treated at 80°C for 10 minutes to obtain a laminate (AS) in which an antistatic layer (AS) having a thickness of 50 nm was formed on the laminate (HC). [Formation of Anti-Reflection Layer (AR)] The laminate (AS) was dipped in a solution for forming a medium to low refractive index layer (ml-6) and then heat-treated at 100°C for 60 minutes to obtain a laminate (ASML) having a medium to low refractive index layer (ML). After dipping in the medium refractive index layer forming solution (m-6), heat treatment was performed at 100° C. for 60 minutes to obtain a laminate (ASMLM) having a medium refractive index layer (M) formed thereon. Next, the laminate (ASMLM) was dipped into a high refractive index layer forming solution (h-4) and then heat-treated at 100°C for 60 minutes to obtain a laminate (ASMLMH) having a high refractive index layer (H). Next, the laminate (ASMLMH) was dipped into a solution for forming a low refractive index layer (l-6), and then heat-treated at 100°C for 120 minutes to obtain a laminate (ASAR) having a low refractive index layer (L).

[0137] Example 25: With antistatic layer (AS), medium refractive index layer (M) = high refractive index layer (H) A low-medium refractive index layer (M) was formed using ml-6 as a solution for forming a low-medium refractive index layer, a medium refractive index layer (M) was formed using m-7 as a solution for forming a medium refractive index layer, and a high refractive index layer (H) was formed on the medium refractive index layer using a solution for forming a high refractive index layer h-4. That is, the medium refractive index layer (M) and the high refractive index layer (H) were exactly the same layer. The medium refractive index layer forming solution m-7 and the high refractive index layer forming solution h-4 have the same composition except for the solvent. Furthermore, a low refractive index layer (L) was formed using l-6 as a solution for forming a low refractive index layer. An anti-reflection laminate was produced in the same manner as in Example 24, except that the film thickness and refractive index of each layer were as shown in Table 10.

[0138] The composition, thickness, refractive index, average luminous reflectance at wavelengths of 380 to 780 nm, average luminous transmittance at wavelengths of 380 to 780 nm, and infrared transmittance at a wavelength of 900 nm of each layer of Examples 24 to 25 are shown in Table 10. The abbreviations in Table 10 are as follows. γ-GPS: 3-glycidoxypropyltrimethoxysilane ATAA: Aluminum tris(acetylacetonate) PEA: Pentaerythritol acrylate

[0139] [Table 10]

[0140] Example 26: Medium refractive index layer (M) = high refractive index layer (H) A low-medium refractive index layer (ML) was formed using ml-6 as a solution for forming a low-medium refractive index layer, a medium refractive index layer (M) was formed using m-7 as a solution for forming a medium refractive index layer, and a high refractive index layer (H) was formed on the medium refractive index layer using a solution for forming a high refractive index layer h-1. The medium refractive index layer (M) and the high refractive index layer (H) had exactly the same refractive index and film thickness. Furthermore, a low refractive index layer (L) was formed using l-6 as a solution for forming a low refractive index layer. An anti-reflection laminate was produced in the same manner as in Example 1, except that the film thickness and refractive index of each layer were as shown in Table 8. Table 8 shows the composition, thickness, refractive index, average luminous reflectance at wavelengths of 380 to 780 nm, average luminous transmittance at wavelengths of 380 to 780 nm, and infrared transmittance at a wavelength of 900 nm of each layer of Example 26.

[0141] <Comparative Example 1> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were as shown in Table 11. This is an example in which the thickness of the low refractive index layer (L) was increased. Figure 3 shows the distribution of the average luminous reflectance.

[0142] <Comparative Example 2> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the thickness of the low refractive index layer (L) was reduced.

[0143] <Comparative Example 3> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the thickness of the high refractive index layer (H) was increased.

[0144] <Comparative Example 4> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the thickness of the high refractive index layer (H) was reduced.

[0145] <Comparative Example 5> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the thickness of the medium refractive index layer (M) was increased.

[0146] <Comparative Example 6> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were as shown in Table 11. This is an example in which the thickness of the medium refractive index layer (M) was reduced.

[0147] <Comparative Example 7> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were as shown in Table 11. This is an example in which the thickness of the medium-low refractive index layer (ML) was increased.

[0148] <Comparative Example 8> An antireflection laminate was produced in the same manner as in Example 1, except that the thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the thickness of the medium-low refractive index layer (ML) was reduced.

[0149] <Comparative Example 9> An antireflection laminate was produced in the same manner as in Example 1, except that co-l-1 was used as the low refractive index layer-forming solution and the film thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the refractive index of the low refractive index layer (L) was increased.

[0150] <Comparative Example 10> An antireflection laminate was produced in the same manner as in Example 1, except that co-h-1 was used as the high refractive index layer-forming solution and the film thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the refractive index of the high refractive index layer (H) was reduced.

[0151] <Comparative Example 11> An antireflection laminate was produced in the same manner as in Example 1, except that co-m-1 was used as the solution for forming the medium refractive index layer, and the film thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the refractive index of the medium refractive index layer was increased.

[0152] <Comparative Example 12> An antireflection laminate was produced in the same manner as in Example 1, except that co-m-2 was used as the solution for forming the medium refractive index layer, and the film thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the refractive index of the medium refractive index layer was reduced.

[0153] <Comparative Example 13> An antireflection laminate was produced in the same manner as in Example 1, except that co-ml-1 was used as the solution for forming the medium to low refractive index layers, and the film thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the refractive index of the medium to low refractive index layers was increased.

[0154] <Comparative Example 14> An antireflection laminate was produced in the same manner as in Example 1, except that co-ml-2 was used as the solution for forming the medium to low refractive index layer, and the film thickness and refractive index of each layer were set as shown in Table 11. This is an example in which the refractive index of the medium to low refractive index layer was reduced.

[0155] The composition, thickness, refractive index, average luminous reflectance at wavelengths of 380 to 780 nm, average luminous transmittance at wavelengths of 380 to 780 nm, and infrared transmittance at a wavelength of 900 nm of each layer of Comparative Examples 1 to 14 are shown in Table 11. The abbreviations in Table 11 are as follows. γ-GPS: 3-glycidoxypropyltrimethoxysilane ATAA: Aluminum tris(acetylacetonate) PEA: Pentaerythritol acrylate

[0156] Table 12 shows the average luminous reflectance at wavelengths of 380 to 780 nm, the average luminous transmittance at wavelengths of 380 to 780 nm, the infrared transmittance at a wavelength of 900 nm, the thickness of each layer, and the refractive index of the antireflection laminates of Examples 1 to 26 and Comparative Examples 1 to 14.

[0157] [Table 11-1]

[0158] [Table 11-2]

[0159] [Table 11-3]

[0160] [Table 11-4]

[0161] [Table 12-1]

[0162] [Table 12-2]

[0163] [Table 12-3] [Industrial Applicability]

[0164] The antireflection laminate of the present invention can be used for front panels of optical display devices such as LED displays (LED, OLED), liquid crystal displays (LCD), and plasma displays (PDP), front panels and cover materials of safety sensors using infrared cameras and infrared lasers, instrument panels of automobiles, and touch panels of car navigation systems and electrical appliances. [Explanation of symbols]

[0165] L: Low refractive index layer H: High refractive index layer M: Medium refractive index layer ML: Medium to low refractive index layer HC: Hard coat layer B: Base material

Claims

1. An antireflection laminate comprising a substrate (B), a hard coat layer (HC) and an antireflection layer (AR) in this order, The anti-reflection layer (AR) is A low refractive index layer (L) having a refractive index of 1.450 or less and a film thickness of 70 to 130 nm; A high refractive index layer (H) having a refractive index of 1.700 to 1.850 and a film thickness of 10 to 250 nm; A medium refractive index layer (M) having a refractive index of 1.550 to 1.810 and a film thickness of 20 to 150 nm; A medium-low refractive index layer (ML) having a refractive index of 1.500 to 1.650 and a film thickness of 10 to 230 nm; the refractive index of each layer of the antireflection layer (AR) satisfies the condition RI(L)<RI(ML)<RI(M)≦RI(H); Where: RI(L) is the refractive index of the low refractive index layer (L), RI(ML) is the refractive index of the medium-low refractive index layer (ML), RI(M) is the refractive index of the medium refractive index layer (M); RI(H) represents the refractive index of the high refractive index layer (H); The layers are arranged in the following order from the hard coat layer (HC) side: medium-low refractive index layer (ML), medium refractive index layer (M), high refractive index layer (H), and low refractive index layer (L); The antireflection laminate has an average luminous reflectance of 0.6% or less on both sides in the wavelength range of 380 to 780 nm.

2. The medium-low refractive index layer (ML) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof, and (iii) an ionizing radiation curable resin, [Formula 1] (Wherein, R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [chemical 2] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group; and n is 1 or 2.

2. The anti-reflection laminate according to claim 1, which is made of a cured product of a composition containing 40 to 500 parts by mass of metal oxide particles and 10 parts by mass or less of a metal chelate compound.

3. The medium refractive index layer (M) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [C3] (Wherein, R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [C4] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group; and n is 1 or 2.

2. The anti-reflection laminate according to claim 1, which is formed from a cured product of a composition containing 40 to 500 parts by mass of metal oxide particles and 1 to 20 parts by mass of a metal chelate compound.

4. The high refractive index layer (H) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [C5] (Wherein, R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [C6] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group; and n is 1 or 2.

2. The anti-reflection laminate according to claim 1, which is made of a cured product of a composition containing 300 to 500 parts by mass of metal oxide particles and 10 to 20 parts by mass of a metal chelate compound.

5. The low refractive index layer (L) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof, and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [C7] (Wherein, R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [C8] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group; and n is 1 or 2.

2. The anti-reflection laminate according to claim 1, which is formed from a cured product of a composition containing 100 to 200 parts by mass of silica particles and 5 to 15 parts by mass of a metal chelate compound.

6. The antireflection laminate according to any one of claims 2 to 4, wherein the metal oxide particles are at least one type of oxide particles selected from the group consisting of titanium oxide, zirconium oxide, niobium pentoxide, antimony-doped tin oxide (ATO), indium oxide-tin oxide (ITO), phosphorus-doped tin oxide (PTO), fluorine-doped tin oxide (FTO) and antimony pentoxide.

7. A protective layer (C) is provided on the antireflection layer (AR), and the protective layer (C) contains, per 100 parts by mass of at least one binder component selected from the group consisting of (i) an alkoxysilane compound represented by the following formula (1) or a hydrolysate thereof and (ii) an alkoxysilane compound represented by the following formula (2) or a hydrolysate thereof: [C9] (Wherein, R is an alkylene group, R 1 is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. [C10] (In the formula, R 1 R is an alkyl group, an alkoxyalkyl group, an acyloxy group, or a halogen atom. 2 is an alkyl group, an alkenyl group, or an alkoxyalkyl group; and n is 1 or 2.

2. The anti-reflection laminate according to claim 1, which is formed from a cured product of a composition containing 10 to 30 parts by mass of silica particles and 5 to 15 parts by mass of a metal chelate compound.

8. The antireflection laminate according to any one of claims 1 to 7, which has an average luminous transmittance of 95% or more in the wavelength range of 380 to 780 nm.

9. The antireflection laminate according to any one of claims 1 to 8, which has an infrared transmittance of 85% or more at a wavelength of 900 nm.

Citation Information

Patent Citations

  • Formation of antireflection layer

    JP1991256003A

  • Optical parts

    JP1992191801A

  • Reflection-preventing article

    JP1995060855A

  • Durable reflection preventing film

    JP2002182007A

  • Method for producing laminate

    JP2006206832A