Fluoride phosphors, composites and light-emitting devices

A fluoride phosphor with controlled particle size distribution and manufacturing methods addresses the challenge of forming uniform films, enhancing quantum efficiency and film smoothness for miniaturized LED and display applications.

JP7554833B2Active Publication Date: 2024-09-20DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022544460
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-25
Filing Date
2021-08-16
Publication Date
2024-09-20
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

Conventional fluoride phosphors struggle to form smooth and uniform phosphor films, particularly in applications requiring thin films for miniaturized LEDs and display technologies, due to issues with film uniformity and quantum efficiency.

Method used

A fluoride phosphor composition represented by A2M(1-n)F6:Mn4+ n, with specific particle size distribution parameters (D50 of 0.1-9.5 μm and D90 of 0.5-16 μm) and manufacturing methods that prevent excessive crystal growth, ensuring uniformity and high quantum efficiency.

Benefits of technology

The solution enables the formation of smooth and uniform phosphor films with improved quantum efficiency, facilitating applications in micro LEDs, mini LEDs, and wavelength conversion elements while suppressing variations in light emitting characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554833000003
    Figure 0007554833000003
  • Figure 0007554833000002
    Figure 0007554833000002
  • Figure 0007554833000001
    Figure 0007554833000001
Patent Text Reader

Abstract

A fluoride phosphor, the composition of which is represented by general formula (1) and in which, when the cumulative 50% value is taken as D50 and the cumulative 90% value is taken as D90 in a volume-based particle size distribution curve determined by a laser diffraction scattering method, D50 is 0.1-9.5 μm and D90 is 0.5-16 μm. General formula (1): A2M(1-n)F6:Mn4+ n In general formula (1), element A is one or more alkali metal elements containing K, element M is an Si simple substance, a Ge simple substance, or a combination of Si and one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf, and 0 < n ≦ 0.1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a fluoride phosphor, a composite, and a light-emitting device.

Background Art

[0002] As a phosphor capable of converting blue light emitted from a blue light-emitting diode into red light, a fluoride phosphor represented by K2SiF6:Mn 4+ is known (often abbreviated as "KSF phosphor", etc.). This phosphor is efficiently excited by blue light. Further, the half-value width of the emission spectrum of this phosphor is narrow and sharp. Therefore, by using this phosphor as a red phosphor, excellent color rendering properties and color reproducibility can be realized without reducing the brightness of a white LED.

[0003] As a prior art of fluoride phosphors, for example, Patent Document 1 can be cited. In Patent Document 1, a fluoride phosphor having a composition represented by the general formula A2M (1-n) F6:Mn 4+ n is described, having a bulk density of 0.80 g / cm 3 or more and a mass median diameter of 30 μm or less. In the general formula, 0 < n ≦ 0.1, element A is one or more alkali metal elements containing K, and element M is a combination of Si alone, Ge alone, or one or more elements selected from the group consisting of Si and Ge, Sn, Ti, Zr, and Hf.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] Due to their excellent luminescence properties, fluoride phosphors such as KSF phosphors are being considered for use in a variety of applications, including displays in addition to lighting.

[0006] In conventional lighting applications, a composite capable of converting blue light into other colors is typically created by using the "potting method," in which a fluorescent agent made by mixing powdered fluoride phosphor and resin is dropped onto a substrate with a dispenser and allowed to harden. On the other hand, in consideration of new applications of fluoride phosphors, such as the miniaturized LEDs of recent years and display applications (mini LED displays), it is preferable to be able to form a relatively thin phosphor film by coating, printing, or other methods rather than by potting.

[0007] However, according to the inventor's preliminary investigation, when attempting to form a phosphor layer using conventional fluoride phosphors by coating, printing, or other methods, it was sometimes impossible to form a sufficiently smooth and uniform phosphor film. In particular, in recent years, with the miniaturization and complexity of devices, there has been a demand for providing thin phosphor films, but conventional fluoride phosphors have not been able to satisfactorily meet this demand.

[0008] The present invention has been made in view of the above circumstances, and one of the objects of the present invention is to provide a fluoride phosphor that can be suitably applied to the formation of a smooth and uniform phosphor film. [Means for solving the problem]

[0009] The present inventors have completed the invention provided below and solved the above problems.

[0010] The fluoride phosphor of the present invention is The composition is represented by the following general formula (1): The cumulative 50% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is D 50 , cumulative 90% value D 90 When D 50 is 0.1 to 9.5 μm, and D 90is 0.5 to 16 μm. General formula (1): A2M (1-n) F6:Mn 4+ n In general formula (1), Element A is one or more alkali metal elements containing K, the element M is Si alone, Ge alone, or a combination of Si with one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf; 0 <n≦0.1である。

[0011] The composite of the present invention comprises the above-mentioned fluoride phosphor and a sealing material that seals the fluoride phosphor.

[0012] The light emitting device of the present invention comprises a light emitting element that emits excitation light, and the above composite that converts the wavelength of the excitation light. [Effects of the Invention]

[0013] According to the present invention, a fluoride phosphor is provided that is preferably applicable to the formation of a smooth and uniform phosphor film. [Brief explanation of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram illustrating an example of a composite / light-emitting device. [Figure 2] FIG. 10 is a diagram illustrating another example of a composite / light-emitting device. DETAILED DESCRIPTION OF THE INVENTION

[0015] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only, and the shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products. In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."

[0016] <Fluoride phosphor> The composition of the fluoride fluorescent material of this embodiment is represented by the following general formula (1). General formula (1): A2M (1-n) F6:Mn 4+ n

[0017] In general formula (1), Element A is one or more alkali metal elements containing K, the element M is Si alone, Ge alone, or a combination of Si with one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf; 0 <n≦0.1である。

[0018] In addition, the cumulative 50% value in the volume-based particle size distribution curve of the fluoride fluorescent material of this embodiment obtained by the laser diffraction scattering method is D 50 , cumulative 90% value D 90 When D 50 is 0.1 to 9 μm, and D 90 is 0.5 to 16 μm.

[0019] The fluoride phosphor of this embodiment has a composition represented by general formula (1), and converts blue light emitted from a blue LED into red light. Also, D 50 is 0.1 to 9.5 μm, and D 90 Since the thickness is 0.5 to 16 μm, the fluoride phosphor of this embodiment is preferably applied to the formation of a smooth and uniform phosphor film. 50 is 9 μm or less, and D 90 The fact that D is 16 μm or less means that the fluoride phosphor of this embodiment does not contain many relatively large particles that may hinder the formation of a smooth and uniform phosphor film. 50 is 9 μm or less, and D 90 By keeping the thickness of the phosphor layer to 16 μm or less, it is possible to form a smooth and uniform phosphor film.

[0020] Furthermore, a phosphor film made using the fluoride phosphor of this embodiment can have good optical properties. Specifically, a phosphor film made using the fluoride phosphor of this embodiment tends to have poor transmittance of blue light, which is excitation light (because the small particle size of the phosphor improves dispersibility in the phosphor film, making it difficult for blue light to transmit). Such optical properties mean that the fluoride phosphor of this embodiment can be preferably applied to, for example, micro LEDs, mini LEDs, wavelength conversion elements for projectors, etc., which will be described later.

[0021] By the way, D 50 is 0.1 μm or more, and D 90 is 0.5 μm or more (i.e., the particles constituting the fluoride phosphor are "large enough"), which makes it easy to prevent an excessive decrease in the quantum efficiency of the fluoride phosphor. In other words, the fluoride phosphor of this embodiment is preferably applicable to the formation of a smooth and uniform phosphor film, while also having good quantum efficiency.

[0022] The fluoride phosphor of this embodiment can be produced by using appropriate raw materials and employing appropriate production methods and production conditions. Details will be described later, but for example, when controlling the saturation of an aqueous solution to precipitate a fluoride phosphor, a production method in which water is added to the system in a short time to instantly increase the saturation can be used to prevent crystal growth from proceeding more than necessary. By using such a production method, D 50 is 0.1 to 9.5 μm, and D 90 It is possible to produce a fluoride phosphor having a particle size of 0.5 to 16 μm. For reference, if a known manufacturing method or manufacturing conditions do not employ such a method, the D 50 and / or D 90 tends to be large.

[0023] The fluoride phosphor of this embodiment will be further described.

[0024] (Composition: General formula (1)) Element A is one or more alkali metal elements containing K. Specifically, it can be potassium alone or a combination of potassium and one or more alkali metal elements selected from lithium (Li), sodium (Na), rubidium (Rb), and cesium (Cs). From the perspective of chemical stability, it is preferable that the potassium content ratio in element A is high (for example, 50 mol% or more in element A is potassium), and it is more preferable that element A is potassium alone.

[0025] Element M is silicon alone, germanium alone, or a combination of silicon and one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf. From the perspective of chemical stability, it is preferable that the silicon content ratio in element M is high (for example, 50 mol% or more in element M is silicon), and it is more preferable that element M is silicon alone.

[0026] In general formula (1), n may be 0 < n ≤ 0.1, but from the perspective of better luminescence characteristics, it is preferably 0.015 ≤ n ≤ 0.04.

[0027] (D 50 ) For the fluoride phosphor of this embodiment, D 50 may be 0.1 to 9.5 μm, preferably 1 to 9.5 μm, more preferably 3 to 9.2 μm, still more preferably 5 to 9 μm, and particularly preferably 7 to 9 μm. When D 50 is moderately large, a phosphor film that is smooth and uniform can be formed while having sufficient quantum efficiency.

[0028] (D 90 ) For the fluoride phosphor of this embodiment, D 90 may be 0.5 to 16 μm, preferably 3 to 16 μm, more preferably 5 to 16 μm, still more preferably 7 to 15 μm, particularly preferably 10 to 14 μm, and especially preferably 11 to 13 μm. D 90By appropriately large, it is possible to form a smooth and uniform phosphor film with sufficient quantum efficiency. 90 By making D appropriately small, the smoothness and uniformity of the phosphor film can be further improved. 90 Since the thickness is appropriately small, it is easy to obtain a smooth and uniform phosphor film even when a thin phosphor film is formed.

[0029] (D 97 , D 100 ) D of the fluoride phosphor of this embodiment 97 (cumulative 97% value in a volume-based particle size distribution curve determined by a laser diffraction scattering method) is preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 17 μm or less. 97 The lower limit is, for example, 10 μm, specifically 12 μm, and more specifically 14 μm. In addition, the D of the fluoride phosphor of this embodiment 100 (cumulative 97% value in a volume-based particle size distribution curve determined by a laser diffraction scattering method) is preferably 40 μm or less, more preferably 35 μm or less, and even more preferably 30 μm or less. 100 The lower limit is, for example, 15 μm, specifically 18 μm, and more specifically 20 μm. D 97 and D 100 If the thickness is not too large, the smoothness and uniformity of the phosphor film can be further improved. Also, even when a thin phosphor film is formed, a smooth and uniform phosphor film can be easily obtained.

[0030] (D 10 ) D of the fluoride phosphor of this embodiment 10 (cumulative 10% value in a volume-based particle size distribution curve determined by a laser diffraction scattering method) is preferably 5.5 μm or more, and more preferably 6 μm or more. 10 There is no particular upper limit to the thickness, but it is, for example, 10 μm or less, specifically 8 μm or less. D 10A relatively large value of D means that the proportion of microparticles with low luminous efficiency is small. 10 When ρ is a relatively large value, the quantum efficiency tends to be further increased.

[0031] By the way, D 10 is 5.5 μm or more, and D 50 is 0.1 to 9.5 μm and D 90 A fluoride phosphor having a particle size of 0.5 to 16 μm is preferably produced by the method of precipitating from an aqueous solution, which will be described later. 50 and D 90 If you try to make the size smaller, a lot of fine powder will be generated, and as a result, D 10 Fluoride phosphors that contain a large amount of fine powder due to pulverization tend to have low luminous efficiency.

[0032] (γ:(D 90 -D 50 ) / D 50 ) In the fluoride phosphor of this embodiment, (D 90 -D 50 ) / D 50 The value of γ defined by the following formula is preferably 0.5 or less, more preferably 0.46 or less. There is no particular lower limit, but it is, for example, 0.25 or more, specifically 0.35 or more. γ is D 50 Relative D based on 90 is an index that can be interpreted as the value of D 50 and D 90 In addition to setting the value of γ itself within the above range, by appropriately adjusting the value of γ, the smoothness and uniformity of the phosphor film can be further improved.

[0033] (δ:(D 90 -D 10 ) / D 50 ) In the fluoride phosphor of this embodiment, (D 90 -D 10 ) / D 50The value of δ defined by the following formula is preferably 0.75 or less, more preferably 0.73 or less. There is no particular lower limit, but it is, for example, 0.30 or more, specifically 0.50 or more. δ can be considered an index that represents the "width" of the particle size distribution. A narrow particle size distribution of a fluoride phosphor means that the particles that make up the fluoride phosphor have a relatively "uniform" particle size. Therefore, by setting δ to 0.75 or less, the smoothness and uniformity of the phosphor film can be further improved.

[0034] As mentioned above, D 10 In order to increase the D, it is preferable to use a method of precipitating the fluoride fluorescent material from an aqueous solution (details will be described later) without mechanical pulverization. 10 If δ is large, δ becomes small. Therefore, from the viewpoint of making δ 0.75 or less, it is preferable to adopt a method of precipitating a fluoride fluorescent material from an aqueous solution as the manufacturing method.

[0035] (quantum efficiency) The internal quantum efficiency of the fluoride phosphor of this embodiment is preferably 70% or more, more preferably 75% or more. There is no particular upper limit to the internal quantum efficiency, but in reality the upper limit is, for example, 95%, specifically 90%. The external quantum efficiency of the fluoride phosphor of this embodiment is preferably 45% or more, more preferably 46.5% or more, and even more preferably 48% or more. There is no particular upper limit to the external quantum efficiency, but in reality it is, for example, 70%, specifically 65%, and more specifically 61%. Generally, the quantum efficiency of a fluoride phosphor having a small particle size tends to be low, but the fluoride phosphor of this embodiment exhibits a relatively good quantum efficiency. 10 By setting δ within the above-mentioned ranges, it is easy to obtain a smooth and uniform phosphor film having good quantum efficiency.

[0036] <Manufacturing method> The method for producing the fluoride phosphor of this embodiment is not limited. The fluoride phosphor of this embodiment can be produced by using appropriate materials and selecting appropriate production methods and conditions. Specific examples of production methods are described in the Examples below, but two production patterns will be described below as "Production Method 1" and "Production Method 2."

[0037] (Manufacturing method 1) The manufacturing method 1 mainly includes a dissolution step and a precipitation step. These steps are described below. These steps can be performed at room temperature.

[0038] ·Dissolution process In the dissolution step, (i) a raw material that supplies element A (such as K), (ii) a raw material that supplies element M (preferably Si), and (iii) a raw material that supplies F are usually dissolved in hydrofluoric acid. One raw material may serve as two or more of (i) to (iii). For example, K2SiF6, which will be described later, serves as all of the raw materials (i) to (iii). The concentration of hydrogen fluoride in hydrofluoric acid before dissolving the raw materials (i) to (iii) is preferably 50 to 60 mass %.

[0039] As a raw material for supplying element A, a compound of element A is preferable in view of chemical stability. For example, an oxide, hydroxide, fluoride, or carbonate of element A can be used. The source material for F can be a fluoride of other elements (A, M, Mn). Fluorine can also be supplied from hydrogen fluoride in hydrofluoric acid used as a solvent.

[0040] A particularly preferred raw material (other than hydrofluoric acid in hydrofluoric acid) used in the dissolution step is K2SiF6.

[0041] ·Precipitation process In the precipitation step, the raw material for supplying Mn and an appropriate amount of water are added to the system as quickly as possible. This causes the system to rapidly become supersaturated, and the fluoride phosphor having the composition represented by general formula (1) is precipitated. Here, "as quickly as possible" refers to adding about 1.5 L of water to the system in about 3 seconds, although this depends on the scale of the system. For example, if 1 L of hydrofluoric acid is used in the dissolution step, the raw material for supplying Mn is preferably added in the required amount all at once. This operation (rapidly bringing the system into a supersaturated state) prevents crystal growth from proceeding more than necessary, and D 50 is 0.1 to 9.5 μm, and D 90 It is believed that a fluoride phosphor having a particle size of 0.5 to 16 μm can be obtained.

[0042] Raw materials for supplying Mn in the precipitation process include hexafluoromanganates, permanganates, oxides (excluding permanganates), fluorides (excluding hexafluoromanganates), chlorides, sulfates, and nitrates. Among these, fluorides are preferred because they can efficiently substitute Mn for the Si sites in the fluoride phosphor, resulting in good luminescence characteristics. Among fluorides, hexafluoromanganates are preferred. Examples of hexafluoromanganates include Na2MnF6, K2MnF6, Rb2MnF6, MgMnF6, CaMnF6, SrMnF6, and BaMnF6. K2MnF6 is particularly preferred because it can simultaneously supply F and K (corresponding to element A), which constitute the fluoride phosphor, in addition to Mn.

[0043] The fluoride phosphor obtained in the precipitation step is recovered by solid-liquid separation such as filtration and washed with an organic solvent such as methanol, ethanol, or acetone. Washing the fluoride phosphor with water can hydrolyze a portion of it to produce a brown manganese compound, which can degrade the properties of the fluoride phosphor. For this reason, it is preferable to use an organic solvent in the washing step. Furthermore, washing the phosphor several times with a hydrofluoric acid reaction solution before washing with an organic solvent can dissolve and remove trace amounts of impurities. The concentration of hydrofluoric acid in the hydrofluoric acid reaction solution used for washing is preferably 5% by mass or more to suppress decomposition of the fluoride phosphor, and preferably 60% by mass or less to ensure the solubility of the fluoride phosphor. After the washing step, it is preferable to dry the fluoride phosphor to thoroughly evaporate the washing solution. Furthermore, classification may be carried out using a sieve with a predetermined mesh size, and coarse particles may be removed.

[0044] (Manufacturing method 2) Although Production Method 2 differs from Production Method 1, it is similar in that the system is rapidly brought to a supersaturated state, thereby precipitating a fluoride phosphor having a composition represented by general formula (1). Production Method 2 mainly includes a dissolving step, a step of introducing raw materials that supply Mn, and a precipitating step. These steps are described below. These steps can be performed at room temperature.

[0045] ·Dissolution process The dissolving step in Production Method 2 can be the same as in Production Method 1.

[0046] -Mn supply raw material input process In the step of adding a raw material for supplying Mn, the "raw material for supplying Mn" described in the precipitation step of Production Method 1, such as K2MnF6, is added to the solution obtained in the dissolving step, and the mixture is stirred and dissolved.

[0047] ·Precipitation process In the precipitation step in manufacturing method 2, for example, an aqueous solution containing about 10 to 40 g / L of potassium hydrofluoride (KHF2) is added to the system as quickly as possible. This rapidly brings the system into a supersaturated state, and a fluoride phosphor having a composition represented by general formula (1) is precipitated. Here, "as quickly as possible" means that, although it depends on the scale of the system, for example, if 1 L of hydrofluoric acid aqueous solution is used in the dissolution step, preferably about 1.5 L of the above aqueous solution is added to the system in about 3 seconds. By rapidly bringing the system into a supersaturated state in this way, crystal growth is prevented from proceeding more than necessary, and D 50 is 0.1 to 9.5 μm, and D 90 It is believed that a fluoride phosphor having a particle size of 0.5 to 16 μm can be obtained. In the precipitation step, a potassium source such as KF may be used instead of KHF2.

[0048] In the production method 2, similarly to the production method 1, it is preferable to carry out filtration, washing, classification using a sieve / removal of coarse particles, and the like.

[0049] <Composite, light-emitting device> The composite of this embodiment includes the above-described fluoride phosphor and a sealant that seals the fluoride phosphor. The light emitting device of this embodiment includes a light emitting element that emits excitation light, and the above-described composite that converts the wavelength of the excitation light.

[0050] An example of a composite and a light-emitting device will be described below with reference to Fig. 1. Also, a composite and a light-emitting device different from those in Fig. 1 will be described with reference to Fig. 2.

[0051] (Figure 1) FIG. 1 is a schematic diagram of a light emitting device 1. As shown in FIG. The light emitting device 1 includes a composite 10 and a light emitting element 20. The composite 10 is provided in contact with the upper part of the light emitting element 20. The light emitting element 20 is typically a blue LED. Terminals are present on the bottom of the light emitting element 20. When the terminals are connected to a power source, the light emitting element 20 can emit light. The excitation light emitted from the light-emitting element 20 is wavelength-converted by the complex 10. When the excitation light is blue light, the blue light is wavelength-converted to red light by the complex 10 containing a fluoride fluorescent material.

[0052] The composite 10 can be composed of the above-mentioned fluoride phosphor and a sealing material that seals the fluoride phosphor. As the encapsulant, for example, various curable resin materials (materials that are cured by heat and / or light) can be used. Any curable resin material can be used as long as it is sufficiently transparent and can provide the optical properties required for displays and lighting devices. Examples of the sealing material include silicone resin materials. Regarding silicone resin materials, curable materials are supplied by companies such as Dow Corning Toray Co., Ltd. and Shin-Etsu Chemical Co., Ltd. Silicone resin materials are preferred from the viewpoints of high transparency and excellent heat resistance. Other examples of the sealing material include epoxy resin materials and urethane resin materials. The amount of the particles of the fluoride fluorescent material in the composite 10 is, for example, 10 to 70 mass %, and preferably 25 to 55 mass %.

[0053] There is no particular limitation on the size or shape of the light emitting element 20. Depending on the application of the light emitting device 1, the light emitting element 20 can have any size or shape.

[0054] The light emitting device 1 can be, for example, a micro LED or mini LED for manufacturing a self-luminous display. A micro LED typically refers to an LED with a chip size of less than 100 μm square that constitutes the pixels of a self-luminous display. A mini LED refers to an LED with a chip size of 100 μm or more (more specifically, 100 μm or more and 200 μm or less) that constitutes the pixels of a self-luminous display. A self-luminous display can be manufactured by using multiple micro LEDs or mini LEDs.

[0055] Specifically, by using the light-emitting device 1 as a pixel (typically a red pixel) and combining it with a micro LED or mini LED that emits blue light and a micro LED or mini LED that emits green light, a self-luminous display capable of color display can be constructed. For information on micro LED displays and mini LED displays, you can refer to documents such as "2019 Survey on the Latest Trends in Next-Generation Display Technology and Related Materials / Processes (Fuji Chimera Research Institute)," "Appl. Sci. 2018, 8, 1557," and "Journal of the Institute of Image Information and Television Engineers Vol. 73, No. 5, pp. 939-942 (2019)."

[0056] In this embodiment, D 50 is 0.1 to 9.5 μm, and D 90 By using a fluoride phosphor having a particle size of 0.5 to 16 μm, it becomes easier to improve the smoothness and uniformity of the composite 10, and it becomes easier to make the composite 10 thinner. Providing a smooth and uniform composite 10 can provide effects such as improving the yield of the light emitting device 1 and suppressing variations in the light emitting characteristics of the light emitting device 1. The effect of "suppressing variations" is particularly desirable when the light emitting device 1 is applied to a self-luminous display. In a self-luminous display in which variations in the light emitting characteristics of the light emitting device 1 are suppressed, the light emitting characteristics between pixels can be "uniformed." Furthermore, being able to thin the composite 10 also contributes to reducing the size of the entire light emitting device 1. That is, being able to thin the composite 10 makes it easier to manufacture a "small light emitting device 1" such as a micro LED or a mini LED.

[0057] Incidentally, the light emitted from the fluoride phosphor of this embodiment tends to have a relatively large x value in the chromaticity diagram, which is also why it is preferable to use the fluoride phosphor of this embodiment to construct a self-luminous display.

[0058] (Figure 2) 2 is a diagram schematically illustrating a wavelength conversion member of a projector, which is an example of the composite of this embodiment. This wavelength conversion member is a so-called transmission type rotating fluorescent plate (phosphor wheel).

[0059] In this wavelength conversion member, a phosphor layer 200 (composite) is formed along the rotation direction of a disk-shaped substrate 1 that is driven to rotate by a motor 300. The region where the phosphor layer 2 is formed includes a blue light incident region where blue light (typically blue laser light) from a blue light source is incident. When the substrate 100 is rotated around the rotation axis by the motor 300, the blue light incident region moves relative to the substrate 100 around the rotation axis.

[0060] The phosphor layer 200 is a composite material including phosphor particles and a sealant that seals the phosphor particles. Examples of the sealing material for forming the phosphor layer 200 (composite) include the same materials as those described for the light emitting device in Fig. 1. The amount of phosphor particles in the phosphor layer 200 (composite) is, for example, 10 to 70 mass %, and preferably 25 to 55 mass %.

[0061] The substrate 100 is preferably made of a material that transmits visible light. Examples of materials for the substrate 100 include quartz glass, quartz crystal, sapphire, optical glass, and transparent resin. A dielectric multilayer film (not shown) may be provided between the substrate 100 and the phosphor layer 200. The dielectric multilayer film functions as a dichroic mirror, transmitting blue light with a wavelength of around 450 nm and reflecting light of 490 nm or more, which includes the wavelength range of the fluorescence emitted from the phosphor layer 200 (490 nm to 750 nm). The shape of the substrate 100 is typically a disk, but is not limited to a disk shape.

[0062] The phosphor layer 200 rotates together with the substrate 1 during use. In such a substrate 100, when blue light (laser light) is incident on the phosphor layer 200, a portion of the phosphor layer 200 corresponding to the blue light incident region generates heat. Then, as the substrate 100 rotates, this heated portion (heat-generating portion) moves in a circle around the rotation axis and returns to the blue light incident region again, repeating this cycle. In this way, by successively changing the irradiation position of the blue light on the phosphor layer 200, excessive heat generation is suppressed.

[0063] At least a portion of the blue light incident on the wavelength conversion member is wavelength-converted to red light by the phosphor layer 200. At least a portion of the red light is emitted in the direction opposite to the side where the blue light is incident.

[0064] By using the above-mentioned fluoride phosphor and sealing material, it is possible to provide a smooth and uniform phosphor layer 200 (composite), which contributes to, for example, improving the yield of wavelength conversion members.

[0065] A projector (light-emitting device) that uses a blue light source typically includes a blue light source such as a blue laser, a wavelength conversion element that converts the wavelength of the blue light emitted from the blue light source, a modulation element that modulates the light emitted from the wavelength conversion element using an image signal, and our optical system that projects the light modulated by the modulation element. For specific configurations of the wavelength conversion element and the projector, reference can be made to Fig. 1 and its explanation in JP 2013-162021 A, the description in JP 2013-92796 A, etc. In addition, known techniques can be applied as appropriate to configure the wavelength conversion element and the projector.

[0066] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention. Below, examples of reference forms are given. 1. The composition is represented by the following general formula (1): The cumulative 50% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is D 50 , cumulative 90% value D 90 When D 50 is 0.1 to 9.5 μm, and D 90 Fluoride phosphors having a particle size of 0.5 to 16 μm. General formula (1):A 2 M (1-n) F 6 :Mn 4+ n In general formula (1), Element A is one or more alkali metal elements containing K, the element M is Si alone, Ge alone, or a combination of Si with one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf; 0 <n≦0.1である。 2. 1. The fluoride phosphor according to claim 1, γ=(D 90 -D 50 ) / D 50 A fluoride phosphor having a γ value of 0.5 or less, as defined by 3. 1. or 2. The fluoride phosphor according to The cumulative 10% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is D 10 Then, δ=(D 90 -D 10 ) / D 50 A fluoride phosphor having a δ value of 0.75 or less, as defined by the following formula: 4. The fluoride phosphor according to any one of 1. to 3. The cumulative 97% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is D 97 When D 97 Fluoride phosphor having a particle size of 20 μm or less. 5. 1. The fluoride phosphor according to any one of 1. to 4. The cumulative 10% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is D 10 When D 10 Fluoride phosphor having a diameter of 5.5 μm or more. 6. The fluoride phosphor according to any one of 1. to 5., A fluoride phosphor with an external quantum efficiency of 45% or more when excited with light having a wavelength of 455 nm. 7. A composite comprising the fluoride phosphor according to any one of 1. to 6. and a sealing material that seals the fluoride phosphor. 8. A light-emitting device comprising: a light-emitting element that emits excitation light; and the composite according to 7. that converts the wavelength of the excitation light. [Example]

[0067] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, it should be noted that the present invention is not limited to the Examples.

[0068] In the following, the following raw materials were used. Hydrofluoric acid: Stella Chemifa K2SiF6: Solid / Morita Chemical Co., Ltd. K2MnF6: Prepared by the method described in paragraph 0042 of JP2019-1897A KHF2: Fujifilm Wako Pure Chemical Corporation, special grade reagent SiO2: High Purity Chemical Co., Ltd.

[0069] Example 1 At room temperature, 1000 mL of a 55% by mass aqueous solution of hydrofluoric acid was placed in a Teflon (registered trademark) beaker, to which 650 g of K2SiF was added, followed by stirring for 5 minutes to obtain a homogeneous solution. While continuing stirring, 6 g of K2MnF6 and 1500 mL of ion-exchanged water were simultaneously added to this homogeneous solution. The entire amount of K2MnF6 was added all at once, and the entire amount of ion-exchanged water was added over 3 seconds (i.e., at a rate of 500 mL / s). This initiated the precipitation of a yellow solid. Stirring was then continued for 5 minutes.

[0070] After stirring, the solution was allowed to stand to precipitate a yellow solid. After confirming the precipitation, the supernatant was removed, and the yellow solid was washed with hydrofluoric acid having a concentration of approximately 24% by mass, followed by washing with methanol. The washed solid was filtered to separate and recover the solid, and further dried to remove the remaining methanol by evaporation. After drying, a nylon sieve with 75 μm openings was used to classify and recover only the yellow powder that passed through this sieve. In this way, a fluoride phosphor was obtained.

[0071] <Example 2> A fluoride fluorescent material was obtained in the same manner as in Example 1, except that the stirring time after adding K2SiF6 to the hydrofluoric acid aqueous solution was changed from 5 minutes to 10 minutes.

[0072] Example 3 At room temperature, 1000 mL of hydrofluoric acid with a concentration of 55% by mass was placed in a Teflon (registered trademark) beaker, to which 650 g of K2SiF was added, and the mixture was stirred for 10 minutes to obtain a homogeneous solution. While continuing to stir, 6 g of K2MnF was added to this homogeneous solution and stirred for an additional 30 seconds. Then, a KHF2 aqueous solution (1500 mL of ion-exchanged water, 35 g of KHF2, and stirred for 5 minutes to achieve a uniform solution) was added, which had been prepared in a separate beaker. The entire amount of this aqueous solution was added in 3 seconds (i.e., at a rate of 500 mL / s). This initiated the precipitation of a yellow solid. Stirring was then continued for another 5 minutes.

[0073] After the stirring was completed, the solid matter was collected, washed, and so on in the same manner as in Example 1. A fluoride fluorescent material was obtained.

[0074] Example 4 A fluoride fluorescent material was obtained in the same manner as in Example 3, except that the KHF2 aqueous solution was prepared by adding 227 g of KHF2 to 1500 mL of ion-exchanged water and stirring for 5 minutes to obtain a uniform solution.

[0075] <Comparative Example 1> Comparative Example 1 is a production example corresponding to the production of a fluoride fluorescent material by the conventional poor solvent method. At room temperature, 1000 mL of a 55% by mass aqueous solution of hydrofluoric acid was placed in a Teflon (registered trademark) beaker, to which 650 g of K2SiF and 3 g of K2MnF were added, followed by stirring for 10 minutes to obtain a homogeneous solution. To this solution, 1500 mL of ion-exchanged water was added over 10 seconds (i.e., added at a rate of 150 mL / s). This initiated the precipitation of a yellow solid. Thereafter, stirring was continued for 5 minutes.

[0076] After the stirring was completed, the solid matter was collected, washed, and so on in the same manner as in Example 1. A fluoride fluorescent material was obtained.

[0077] <Comparative Example 2> Comparative Example 2 is an example of the production of a fluoride fluorescent material by a conventional production method called the silica addition method. At room temperature, 700 mL of 55% by mass hydrofluoric acid was added to a Teflon (registered trademark) beaker. 293.8 g of KHF was added and stirred for 15 minutes. 4.0 g of KMnF was then added and stirred for 30 seconds. 24 g of SiO was then added and stirred for 10 minutes.

[0078] After the stirring was completed, the solid matter was collected, washed, and so on in the same manner as in Example 1. A fluoride fluorescent material was obtained.

[0079] <Comparative Example 3> Comparative Example 3 is also an example of producing a fluoride fluorescent material by a conventional method called the silica addition method. A fluoride fluorescent material was obtained in the same manner as in Comparative Example 2, except that the stirring time after adding 4.0 g of K2MnF was changed from 30 seconds to 45 seconds.

[0080] <Identification: Crystal phase measurement, etc.> The X-ray diffraction patterns of the fluoride phosphors (yellow powders) obtained in Examples 1 to 4 were obtained using an X-ray diffractometer. The obtained X-ray diffraction patterns were identical to those of K2SiF6 crystals. (1-n)F6:Mn 4+ n It was confirmed that a single phase was obtained.

[0081] In addition to X-ray diffraction, the fluoride phosphor (yellow powder) obtained in Example 1 was dissolved using sodium carbonate and boric acid, respectively, and analyzed by ICP atomic emission spectroscopy to determine the contents of K, Si, and Mn. Furthermore, the F content was determined by dissolving 0.1 g of the fluoride phosphor (yellow powder) in water and analyzing it in accordance with the measurement method of "7.2 Purity" in JIS K 8821 "Sodium Fluoride (Reagent)." Based on these analyses, the value of n in the aforementioned general formula (1) was 0.03. Based on the ratio of raw materials used, the values ​​of n in Examples 2 to 4 are considered to be roughly the same.

[0082] <Particle size distribution measurement by laser diffraction scattering method> 30 mL of ethanol was weighed into a 50 mL beaker, and 0.03 g of fluoride fluorescent material was added thereto. The container was then placed in a homogenizer (manufactured by Nippon Seiki Seisakusho, trade name US-150E) whose output had been adjusted to "Altitude: 100%" in advance, and pretreatment was carried out for 3 minutes. The volume-based particle size distribution curve was obtained for the solution prepared in this manner using a laser diffraction / scattering particle size distribution analyzer (manufactured by Microtrackbell, product name MT3300EXII). 10 , D 50 , D 90 , D 57 and D 100 Then, γ=(D 90 -D 50 ) / D 50 and δ = (D 90 -D 10 ) / D 50 asked for.

[0083] <Emission characteristic evaluation (quantum efficiency and chromaticity)> A standard reflector (Spectralon, manufactured by Labsphere) with a reflectance of 99% was set in the side opening (φ10 mm) of an integrating sphere (φ60 mm). Monochromatic light separated to a wavelength of 455 nm from a light source (Xe lamp) was introduced into the integrating sphere via an optical fiber, and the spectrum of the reflected light was measured using a spectrophotometer (MCPD-7000, manufactured by Otsuka Electronics Co., Ltd.). The number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 to 465 nm. Next, a concave cell filled with fluoride phosphor to create a smooth surface was placed in the opening of an integrating sphere and irradiated with monochromatic light at a wavelength of 455 nm. The excitation reflected light and fluorescence spectra were measured using a spectrophotometer. The number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) were calculated from the obtained spectral data. The excitation reflected light photon count was calculated over the same wavelength range as the excitation light photon count, and the fluorescence photon count was calculated over the 465-800 nm range. The absorptivity (= (Qex - Qref) / Qex × 100), internal quantum efficiency (= Qem / (Qex - Qref) × 100), and external quantum efficiency (= Qem / Qex × 100) were calculated from the obtained three types of photon counts. Based on the data obtained from this measurement, the x and y values ​​of the fluorescence emitted from the fluoride phosphor were calculated in the xy chromaticity diagram using the analysis software provided with the device.

[0084] <Smoothness and uniformity of phosphor film, optical properties> First, a phenyl silicone resin (OE-6630, manufactured by Dow Corning Corporation) and a fluoride phosphor were mixed using a mixer (ARE-310, manufactured by Thinky Corporation) while degassing. This resulted in a mixture for forming a phosphor film. The amount of the fluoride phosphor used was set so that the ratio of the fluoride phosphor in the mixture was 40 mass%. Next, the mixture was applied between two 100 μm thick PFA (fluororesin) films and passed through a roller set to a thickness of 50 μm. It was then heat-treated at 150°C for 1 hour. After cooling, the PFA film was peeled off and the film was cut into a size of 20 mm x 20 mm. In this way, a sheet-shaped phosphor film (composite) was obtained.

[0085] The obtained phosphor film was visually inspected and rated as good (○) if no unevenness was visible and the film was smooth, bad (×) if unevenness was clearly visible, and somewhat poor (△) if unevenness was not apparent at first glance but was visible upon careful inspection.

[0086] The obtained phosphor film was placed on a blue LED with an emission wavelength of 455 nm, and the blue LED was allowed to emit light. The brightness of the light emitted on the side of the phosphor film opposite the blue LED was evaluated using a total luminous flux measurement system HM9100 (manufactured by Otsuka Electronics Co., Ltd.). Using Example 1 as the standard, a case in which the same brightness as Example 1 was obtained was evaluated as good (○), a case in which the brightness was brighter than Example 1 was evaluated as very good (◎), a case in which the brightness was slightly darker than Example 1 was evaluated as slightly poor (△), and a case in which the brightness was significantly darker than Example 1 was evaluated as poor (×).

[0087] The various measurement / evaluation results are summarized in the table below.

[0088] [Table 1]

[0089] As shown in the table above, the fluoride phosphors of Examples 1 to 4 (D 50 is 0.1 to 9.5 μm, and D 90 The phosphor films formed using the fluorine-containing film (D) were smooth and no non-uniformity was observed in the films (Examples 1 to 4). 50 is more than 9.5 μm, or D 90 The phosphor film formed using a fluoride phosphor with a particle size of more than 16 μm showed non-uniformity.

[0090] Furthermore, the phosphor films formed using the fluoride phosphors of Examples 1 to 4 exhibited good optical properties (brightness). Furthermore, the quantum efficiency of the fluoride phosphors of Examples 1 to 4 was comparable to that of Comparative Examples 1 to 3.

[0091] This application claims priority based on Japanese Patent Application No. 2020-141416, filed on August 25, 2020, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]

[0092] 1. Light-emitting device 10 Complex 20 Light-emitting element 100 boards 200 Phosphor layer (composite) 300 motor

Claims

1. The composition is represented by the following general formula (1): The cumulative 10% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is designated as D 10 , and the cumulative 50% value is designated as D 50 , cumulative 90% value D 90 When D 10 is 5.5 to 8 μm, D 50 is 7 to 9.5 μm, and D 90 A fluoride phosphor having a diameter of 10 to 16 μm. General formula (1): A 2 M (1-n) F 6 :Mn 4+ n In general formula (1), Element A is K alone, The element M is simple Si; 0.015≦n≦0.

04.

2. 2. The fluoride phosphor according to claim 1 , γ = (D 90 -D 50 ) / D 50 A fluoride phosphor having a γ value of 0.5 or less, as defined by the following formula:

3. 3. The fluoride phosphor according to claim 1, δ = (D 90 -D 10 ) / D 50 A fluoride phosphor having a δ value of 0.75 or less, as defined by the following formula:

4. The fluoride phosphor according to any one of claims 1 to 3, The cumulative 97% value in the volume-based particle size distribution curve obtained by the laser diffraction scattering method is D 97 When this is done, D 97 A fluoride phosphor having a diameter of 20 μm or less.

5. The fluoride phosphor according to any one of claims 1 to 4, A fluoride phosphor having an external quantum efficiency of 45% or more when excited with light having a wavelength of 455 nm.

6. A composite comprising the fluoride phosphor according to any one of claims 1 to 5 and a sealing material that seals the fluoride phosphor.

7. A light emitting device comprising: a light emitting element that emits excitation light; and the composite according to claim 6 that converts the wavelength of the excitation light.

Citation Information

Patent Citations

  • Mn ACTIVATED COMPLEX FLUORIDE FLUOPHOR AND MANUFACTURING METHOD THEREFOR

    JP2018012825A

  • Fluoride phosphor and light-emitting device using the same

    JP2019001897A

  • Wavelength-conversion member and light-emitting device

    JP2019186537A

  • Hexafluoromanganate (IV), complex fluoride phosphor, and methods respectively for producing said products

    WO2015115188A1

  • Fluorescent sheet, light-emitting element using same, light source unit, display, and production method for light-emitting element

    WO2017094832A1