Novel near-infrared luminous garnet fluorescent powder material and preparation method thereof
By introducing Si and Ge cations into the garnet structure, a new near-infrared luminescent garnet phosphor with Y3Ga(3-x)ZnGe(1-y)SiyO12:xCr3+ was solved, and the narrow emission peak and quantum of Cr3+ doped oxides were solved. The problem of low efficiency achieves the efficient performance of broadband near-infrared light sources and is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202410845089.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-01
AI Technical Summary
The narrow emission peak and low quantum efficiency of existing Cr3+ doped oxide near-infrared luminescent materials limit their application in near-infrared pc-LEDs.
By introducing different contents of Si and Ge cations into the garnet structure, replacing some or all of the gallium elements, forming a new near-infrared luminescent garnet phosphor with Y3Ga(3-x)ZnGe(1-y)SiyO12:xCr3+, and adjusting it Light emitting performance and realize broadband near-infrared light sources.
It has achieved wide emission peaks and high quantum efficiency, breaking through the technical bottleneck of fast-responsive, broadband near-infrared light sources, and is suitable for biomedical, night vision systems and plant growth lighting.
Smart Images

Figure CN118879320A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic luminescent materials, and in particular to a novel near-infrared luminescent garnet phosphor material and a preparation method thereof. Background Art
[0002] Near-infrared light refers to electromagnetic waves with a wavelength between 700-1700nm, which is between visible light and far infrared. In recent years, near-infrared light has shown great application prospects in biomedicine, night vision systems, plant growth lighting, non-destructive testing and other fields. Traditional near-infrared light sources such as halogen lamps, infrared light-emitting diodes and lasers, especially high-power lasers, all have inherent defects. Halogen tungsten lamps have the disadvantages of short life, slow response, large size, high energy consumption, and low efficiency; infrared lasers have a narrow half-peak width of emission peak and high cost, and often require a large cooling system and safety devices, making the overall equipment large; and infrared light-emitting diodes have a narrow half-peak width of emission peak, the emission peak will be blue-shifted or red-shifted, and the luminous intensity is seriously reduced at high temperatures, which cannot be widely used in near-infrared technology. On the contrary, in recent years, due to the invention of the blue light chip InGaN, the research on near-infrared phosphorescent conversion light-emitting diodes (pc-LEDs) has developed rapidly. The combination of blue light LED chips and excellent near-infrared phosphors has the advantages of low cost, adjustable spectrum, high thermal stability, miniaturization, and rapid response, and has become a research hotspot.
[0003] In pc-LEDs technology, near-infrared luminescent phosphors, as key components, play a vital role in determining the overall optical performance. Therefore, it is of great research value to explore luminescent materials that can be effectively excited by InGaN blue chips and produce broadband near-infrared emission with high efficiency and good thermal stability. At present, various rare earth or transition metal ions such as Eu 2+ , Yb 3+ 、Ni 2+ , Mn 2+ or Cr 3+ etc. are introduced into a suitable matrix as a luminescent center to achieve near-infrared emission. 3+ It is considered to be the most ideal activator because of its unique 3 The d3 electronic configuration can produce a broad near-infrared emission band in the range of 600-1400nm in a weak covalent environment. 3+ Doped Y3Ga5O 12The luminescence performance in the garnet structure can be effectively excited by blue light and can be used as a near-infrared light material. However, this type of phosphor generally has shortcomings such as narrow emission peak and low quantum efficiency, which greatly reduces the comprehensive performance of near-infrared pc-LEDs, thereby limiting its commercial application. By replacing some or all of the atoms in the garnet structure, a wider emission peak and higher quantum efficiency can be produced. Among them, LP Jiang et al. partially replaced gallium with silicon and magnesium elements to improve its luminescence performance (Inorg. Chem., 2023, DOI: 10.1021 / acs.inorgchem.2c04319.). Summary of the invention
[0004] In view of the above shortcomings, the present invention proposes a new type of Cr 3+ Doped garnet structure broadband near-infrared phosphor, which has a wide emission peak wavelength, solves the problem of Cr 3+ A new type of near-infrared luminescent garnet phosphor material with fast response and broadband near-infrared light source has been developed to overcome the shortcomings of doped oxides such as narrow emission peak and low quantum efficiency.
[0005] To achieve the above object, the present invention provides the following technical solution: a novel near-infrared luminescent garnet phosphor material, the chemical expression of which is Y3Ga (3-x) ZnGe (1-y) Si y O 12 :xCr 3+ , where x=0.01-0.09, y=0-1.
[0006] Compared with the prior art, the advantages of the present invention are: the present invention discloses a new type of Cr 3+ Doping garnet structure broadband near-infrared phosphor improves its luminescence performance, thereby producing a wider emission peak and higher quantum efficiency, breaking through the technical bottleneck of miniaturization, rapid response, and broadband near-infrared light source. The luminescence performance and experimental optical band gap of the phosphor can be regularly adjusted by replacing Si and Ge cations with different contents, achieving Cr 3+ Precise control of emission spectra.
[0007] The broadband near-infrared phosphor of the present invention has room for composition selection and adjustment, is easier to prepare, can be prepared by a variety of conventional preparation methods, can be prepared by a traditional high-temperature solid phase method, but is not limited thereto, and is easy to mass produce.
[0008] The broadband near-infrared phosphor of the present invention generates good broadband near-infrared light under the excitation of the blue light chip InGaN, has the characteristics of stable physical and chemical properties and stable luminescence properties, and shows great application potential in the fields of biomedicine, night vision systems, plant growth lighting, non-destructive testing, etc.
[0009] As an improvement, the phosphor material comprises: Y2O3, Ga2O3, ZnO, SiO2, GeO2, and the doped transition metal ion raw material is Cr2O3.
[0010] As an improvement, the mass percentage of Y2O3 is 42-44.5%, the mass percentage of Ga2O3 is 34.4-36.4%, the mass percentage of ZnO is 10.1-10.7%, the mass percentage of SiO2 is 0-7.9%, the mass percentage of GeO2 is 0-13%, and the mass percentage of transition oxide Cr2O3 is 0.5%. Its chemical expression is Y3Ga3ZnGe (1-y) Si y O 12 :0.05Cr 3+ , where x=0.05, y=0-1, the luminescence performance of the near-infrared phosphor is improved by replacing cations of different masses. Considering the cost of raw materials, replacing Ge by cation Si can greatly save production costs.
[0011] As an improvement, the mass percentage of Y2O3 is 42%, the mass percentage of Ga2O3 is 34-34.8%, the mass percentage of ZnO is 10.1%, the mass percentage of GeO2 is 13%, and the mass percentage of transition oxide Cr2O3 is 0.5%-0.9%. Its chemical formula is Y3Ga (3-x) ZnGe (1-y) Si y O12: xCr 3+ , where x = 0.01-0.09, y = 0. When x = 0.05, the near-infrared phosphor has good optical properties and stable physical and chemical properties, and is an excellent component for manufacturing excellent performance near-infrared pc-LEDs.
[0012] As an improvement, the mass percentage of Y2O3 is 44.5%, the mass percentage of Ga2O3 is 36-36.8%, the mass percentage of ZnO is 10.7%, the mass percentage of SiO2 is 7.9%, and the mass percentage of transition oxide Cr2O3 is 0.1-0.9%. Its chemical formula is Y3Ga (3-x) ZnGe (1-y) Si y O 12 :xCr 3+ , where x = 0.01-0.09, y = 1. When x = 0.05, the near-infrared phosphor has good optical properties and stable physical and chemical properties, and is an excellent component for manufacturing excellent performance near-infrared pc-LEDs.
[0013] As an improvement, after the garnet structure near-infrared phosphor material is excited by 400-480nm ultraviolet light or blue light, the near-infrared light wavelength is 650-900nm, and the half-peak width is 100-150nm. The excitation range of the phosphor is relatively wide, with the strongest excitation peak at around 450nm. Therefore, it is very suitable for InGaN blue light LED excitation and can be widely used in biomedicine, night vision systems, plant growth lighting, non-destructive testing and other fields.
[0014] As an improved method for preparing a novel near-infrared luminescent garnet phosphor material, the method comprises the following steps:
[0015] S1: According to the chemical formula Y3Ga (3-x) ZnGe (1-y) Si y O 12 :xCr 3+ After the molar weight raw materials Y2O3, Ga2O3, ZnO, SiO2, GeO2, and transition oxide Cr2O3 are added, a proper amount of anhydrous ethanol is added to the above raw materials and ground to mix them uniformly;
[0016] S2: After the anhydrous ethanol in step S1 is completely volatilized, the dry powder is placed in a crucible, and then placed in a muffle furnace to increase the temperature through a heating atmosphere, and then the temperature is increased to a set sintering temperature and then kept warm;
[0017] S3: After the sintered product obtained in step S2 is naturally cooled to room temperature, the sintered product is fully ground to obtain a novel near-infrared luminescent garnet phosphor.
[0018] The preparation method of a novel near-infrared luminescent garnet phosphor material of the present invention only requires grinding and mixing the required raw materials according to a specified molar ratio, heating and cooling, and then grinding again to obtain the novel near-infrared luminescent garnet phosphor. The production process is simple and convenient for large-scale production.
[0019] As an improvement, in step S2, the heating rate in the muffle furnace is 5-10°C / min, and the heating atmosphere is air atmosphere.
[0020] As an improvement, in step S2, the sintering temperature is 1400-1500° C. and the holding time is 5-6 hours.
[0021] As an improvement, the room temperature in step S3 is 20±5°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0023] Figure 1 is the X-ray diffraction (XRD) pattern of the near-infrared phosphor of Example 1;
[0024] Figure 2 The luminescence spectrum of the near-infrared phosphor of Example 1 (λ em =783nm,λ ex =453nm);
[0025] Figure 3 is the X-ray diffraction (XRD) pattern of the near-infrared phosphor of Example 2;
[0026] Figure 4 The luminescence spectrum of the near-infrared phosphor of Example 2 (λ em =783nm,λ ex =453nm);
[0027] Figure 5 is the X-ray diffraction (XRD) pattern of the near-infrared phosphor of Example 3;
[0028] Figure 6 The luminescence spectrum of the near-infrared phosphor of Example 3 (λ em =783nm,λ ex =453nm);
[0029] Figure 7 This is a graph showing the dependence of substitution concentration on half-peak width and emission intensity in Example 3;
[0030] Figure 8 This is a graph showing the relationship between the substitution concentration and the experimental optical band gap of the phosphor in Example 3. DETAILED DESCRIPTION
[0031] In the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "planar direction", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0032] Example 1
[0033] like Figure 1 , 2 As shown, a new transition metal Cr 3+ Doped Y3Ga3ZnSiO 12 :xCr 3+A new type of near-infrared luminescent garnet phosphor, wherein x=0.01-0.09, and the masses of the raw materials are respectively Y2O3: 0.33871g, Ga2O3: 0.27273-0.28023g, ZnO: 0.08138g, SiO2: 0.06008g, and Cr2O3: 0.00076-0.00684g.
[0034] When x=0.01, the preparation steps of the novel near-infrared luminescent garnet phosphor are as follows:
[0035] S1. Use an electronic balance to weigh the raw materials Y2O3: 0.33871g, Ga2O3: 0.28023g, ZnO: 0.08138g, SiO2: 0.06008g, Cr2O3: 0.00076g, put the raw materials into an agate bowl, add appropriate amount of anhydrous ethanol and grind them to make them evenly mixed.
[0036] S2. After the dry powder is evenly mixed and the anhydrous ethanol is completely volatilized, pour it into an alumina crucible, place the alumina crucible in a KF1700 box-type muffle furnace, set the heating rate to 5°C / min, heat to 1400°C and continue to keep warm for 5h;
[0037] S3. When cooled to room temperature, take out and grind for 5-10 minutes to obtain a novel near-infrared luminescent garnet phosphor.
[0038] The XRD spectrum of the novel near-infrared luminescent garnet phosphor obtained in Example 1 is as follows: Figure 1 As shown, the diffraction peaks of all samples are observed to be consistent with those of Y3Ga5O 12 The standard card matched well, and no impurity peak was observed, indicating that the novel near-infrared luminescent garnet phosphor of Example 1 was successfully obtained.
[0039] The fluorescence test of Example 1 was carried out, and its excitation and emission spectra were as follows: Figure 2 As shown. Under the excitation of 453nm wavelength, the new near-infrared luminescent garnet phosphor emits near-infrared light, and along with Cr 3+ With the increase of doping concentration, the peak position and half-peak width of the excitation emission spectrum do not change significantly, and the emission intensity shows a pattern of first increasing and then decreasing, reaching the maximum at x=0.05, with a half-peak width of 128nm.
[0040] Example 2
[0041] like Figure 3 , Figure 4 As shown, a new transition metal Cr 3+ Doped Y3Ga3ZnGeO 12 :xCr 3+A new type of near-infrared luminescent garnet phosphor, wherein x=0.01-0.09, and the masses of the raw materials are respectively Y2O3: 0.33871g, Ga2O3: 0.27273-0.28023g, ZnO: 0.08138g, GeO2: 0.10464g, and Cr2O3: 0.00076-0.00684g.
[0042] When x=0.01, the preparation steps of the novel near-infrared luminescent garnet phosphor are as follows:
[0043] S1. Use an electronic balance to weigh the raw materials Y2O3: 0.33871g, Ga2O3: 0.28023g, ZnO: 0.08138g, GeO2: 0.10464g, Cr2O3: 0.00076g, put the raw materials into an agate bowl, add appropriate amount of anhydrous ethanol and grind them to make them evenly mixed;
[0044] S2. After the dry powder is evenly mixed and the anhydrous ethanol is completely volatilized, pour it into an alumina crucible, place the alumina crucible in a KF1700 box-type muffle furnace, set the heating rate to 5°C / min, heat to 1400°C and continue to keep warm for 5h;
[0045] S3. When cooled to room temperature, take out and grind for 5-10 minutes to obtain a novel near-infrared luminescent garnet phosphor.
[0046] The XRD spectrum of the novel near-infrared luminescent garnet phosphor obtained in Example 2 is as follows: Figure 3 It is observed that the diffraction peaks of all samples are consistent with those of Y3Ga5O 12 The standard card matched well and no impurity peak was observed, indicating that the novel near-infrared luminescent garnet phosphor of Example 2 was successfully obtained.
[0047] The fluorescence test of Example 2 was carried out, and its excitation and emission spectra were as follows: Figure 4 As shown in Figure 2, under the excitation of 453nm wavelength, the new near-infrared luminescent garnet phosphor emits near-infrared light, and along with the Cr 3+ With the increase of doping concentration, the peak position and half-peak width of the excitation emission spectrum do not change significantly, and the emission intensity shows a pattern of first increasing and then decreasing, reaching the maximum at x=0.05, with a half-peak width of 128nm.
[0048] Example 3
[0049] like Figure 5 , Figure 6 As shown, a new transition metal Cr 3+ Doped Y3Ga3ZnGe (1-y) Si y O 12 :0.05Cr3+ A new type of near-infrared luminescent garnet phosphor, wherein y=0-1, and the masses of the raw materials are respectively Y2O3: 0.33871g, Ga2O3: 0.27648g, ZnO: 0.08138g, GeO2: 0-0.10464g, SiO2: 0-0.06008g, and Cr2O3: 0.00380g.
[0050] When y=0.2, the preparation steps of the novel near-infrared luminescent garnet phosphor are as follows:
[0051] S1. Use an electronic balance to weigh the raw materials Y2O3: 0.33871g, Ga2O3: 0.28023g, ZnO: 0.08138g, GeO2: 0.08371g, SiO2: 0.02403g, Cr2O3: 0.00380g, put the raw materials into an agate bowl, add appropriate amount of anhydrous ethanol and grind them to make them evenly mixed;
[0052] S2. After the dry powder is evenly mixed and the anhydrous ethanol is completely volatilized, pour it into an alumina crucible, place the alumina crucible in a KF1700 box-type muffle furnace, set the heating rate to 5°C / min, heat to 1400°C and continue to keep warm for 5h;
[0053] S3. When cooled to room temperature, take out and grind for 5-10 minutes to obtain a novel near-infrared luminescent garnet phosphor.
[0054] The XRD spectrum of the novel near-infrared luminescent garnet phosphor obtained in Example 3 is as follows: Figure 5 As shown, the diffraction peaks of all samples are observed to be consistent with those of Y3Ga5O 12 The standard card matched well and no impurity peak was observed, indicating that the novel near-infrared luminescent garnet phosphor of Example 3 was successfully obtained.
[0055] The fluorescence test of Example 3 was carried out, and its emission spectrum was as follows Figure 6 As shown, under the excitation of 453nm wavelength, the new near-infrared luminescent garnet phosphor emits near-infrared light.
[0056] like Figure 7 As shown, it can be seen that in Example 3, as the content of Si replacing Ge increases, the near-infrared emission intensity of the new near-infrared luminescent garnet phosphor will show a trend of first increasing and then decreasing. When y=0.2, the intensity of the emission peak reaches the maximum; while the peak position and half-peak width of the excitation emission spectrum of the sample do not change significantly.
[0057] like Figure 8As shown, it can be seen that in Example 3, the variation law of the experimental optical band gap of the novel near-infrared luminescent garnet phosphor during the substitution process from Ge to Si, in which the band gap value decreases regularly.
[0058] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various non-substantial improvements are made using the technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A novel near-infrared luminescent garnet phosphor material, characterized in that: The chemical expression of the phosphor material is Y3Ga (3-x) ZnGe (1-y) Si y O 12 :xCr 3+ , where x=0.01-0.09, y=0-1.
2. The novel near-infrared luminescent garnet phosphor material according to claim 1, characterized in that: The phosphor material comprises: Y2O3, Ga2O3, ZnO, SiO2, GeO2, and the doped transition metal ion raw material is Cr2O3.
3. The novel near-infrared luminescent garnet phosphor material according to claim 2, characterized in that: The mass percentage of Y2O3 is 42-44.5%, the mass percentage of Ga2O3 is 34.4-36.4%, the mass percentage of ZnO is 10.1-10.7%, the mass percentage of SiO2 is 0-7.9%, the mass percentage of GeO2 is 0-13%, and the mass percentage of transition oxide Cr2O3 is 0.5%. Its chemical expression is Y3Ga3ZnGe (1-y) Si y O 12 :0.05Cr 3+ , where x=0.05, y=0-1.
4. The novel near-infrared luminescent garnet phosphor material according to claim 2, characterized in that: The mass percentage of Y2O3 is 42%, the mass percentage of Ga2O3 is 34-34.8%, the mass percentage of ZnO is 10.1%, the mass percentage of GeO2 is 13%, and the mass percentage of transition oxide Cr2O3 is 0.5%-0.9%. Its chemical formula is Y3Ga (3-x) ZnGe (1-y) Si y O12: xCr 3+ , where x=0.01-0.09, y=0.
5. The novel near-infrared luminescent garnet phosphor material according to claim 2, characterized in that: The mass percentage of Y2O3 is 44.5%, the mass percentage of Ga2O3 is 36-36.8%, the mass percentage of ZnO is 10.7%, the mass percentage of SiO2 is 7.9%, and the mass percentage of transition oxide Cr2O3 is 0.1-0.9%. Its chemical formula is Y3Ga (3-x) ZnGe (1-y) oeLh 12 :xCr 3+ , where x=0.01-0.09, y=1.
6. The novel near-infrared luminescent garnet phosphor material according to claim 1, characterized in that: After the garnet structure near-infrared phosphor material is excited by ultraviolet light or blue light of 400-480nm, the wavelength of the near-infrared luminescence is 650-900nm and the half-peak width is 100-150nm.
7. A method for preparing a novel near-infrared luminescent garnet phosphor material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: According to the chemical formula Y3Ga (3-x) ZnGe (1-y) Si y O 12 :xCr 3+ After weighing the raw materials Y2O3, Ga2O3, ZnO, SiO2, GeO2, and transition oxide Cr2O3 according to the molar ratio in the above, adding a proper amount of anhydrous ethanol to the above raw materials and grinding them to mix them uniformly; S2: After the anhydrous ethanol in step S1 is completely volatilized, the dry powder is placed in a crucible, and then placed in a muffle furnace to increase the temperature through a heating atmosphere, and then the temperature is increased to a set sintering temperature and then kept warm; S3: After the sintered product obtained in step S2 is naturally cooled to room temperature, the sintered product is fully ground to obtain a novel near-infrared luminescent garnet phosphor.
8. The method for preparing a novel near-infrared luminescent garnet phosphor material according to claim 7, characterized in that: In step S2, the heating rate in the muffle furnace is 5-10°C / min, and the heating atmosphere is air atmosphere.
9. The method for preparing a novel near-infrared luminescent garnet phosphor material according to claim 7, characterized in that: In step S2, the sintering temperature is 1400-1500° C., and the holding time is 5-6 hours.
10. The method for preparing a novel near-infrared luminescent garnet phosphor material according to claim 7, characterized in that: The room temperature in step S3 is 20±5°C.
Citation Information
Patent Citations
Cr<3+>-doped germanium-containing garnet phase broadband near-infrared fluorescent powder and preparation method thereof
CN111778027A
Near-infrared fluorescent powder, preparation method and near-infrared light source using near-infrared fluorescent powder
CN114276807A
Cited By
Cr < 3 + >-doped gallium germanate broadband near-infrared luminescent material as well as preparation method and application thereof
CN119391421A
Near-infrared luminescent material with zero ultra-high-temperature luminescence loss and quantum yield close to 100% as well as preparation method and application of near-infrared luminescent material
CN120059748A