Manufacturing method of cold rolled steel sheet and manufacturing method of steel parts
By controlling the size and density of Nb, Ti, and V-based carbides through specific manufacturing processes, cold-rolled steel sheets achieve enhanced toughness and hardness, addressing the limitations of existing methods in achieving both properties simultaneously.
Patent Information
- Application Number
- JP2023102642
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-18
- Filing Date
- 2023-06-22
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2042-06-10
AI Technical Summary
Existing methods struggle to achieve both high hardness and toughness in cold-rolled steel sheets, as grain refinement techniques using Nb addition either saturate or lead to void generation, limiting the effectiveness of carbides in improving toughness.
Control the size and density of Nb, Ti, and V-based carbides in cold-rolled steel sheets by specific manufacturing processes, including controlled heating, hot rolling, annealing, and multiple stages of cold rolling, to enhance toughness and hardness.
The method results in cold-rolled steel sheets with improved toughness and hardness, suitable for applications requiring durability like textile machinery, bearing parts, and cutlery, by optimizing carbide distribution and density.
Smart Images

Figure 0007555080000001 
Figure 0007555080000002 
Figure 0007555080000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a cold-rolled steel sheet, and in particular to a cold-rolled steel sheet capable of producing steel parts having excellent toughness. The present invention also relates to a steel part using the cold-rolled steel sheet, a manufacturing method of the cold-rolled steel sheet, and a manufacturing method of the steel part. [Background technology]
[0002] Cold-rolled steel sheets are widely used as materials for manufacturing various steel parts. In particular, cold-rolled steel sheets made of high carbon steel have high hardness and are used in applications requiring wear resistance, such as textile machinery parts, bearing parts, and machine and household knives.
[0003] On the other hand, steel parts such as textile machinery parts, bearing parts, and machine and household knives are repeatedly subjected to shocks caused by reciprocating motion during use. Therefore, steel parts are required to have excellent toughness to prevent damage caused by shocks caused by reciprocating motion.
[0004] However, metal materials become more brittle as their hardness increases, making it difficult to achieve both hardness and toughness. For example, quenching and tempering are commonly used to improve the toughness of steel parts, but quenching and tempering reduces the hardness of the steel, so conventional quenching and tempering processes cannot achieve both high levels of hardness and toughness.
[0005] Therefore, various methods have been proposed to achieve both hardness and toughness.
[0006] For example, Patent Documents 1 and 2 disclose techniques for improving the toughness of high carbon cold-rolled steel sheets by utilizing the grain refining effect of Nb addition.
[0007] In addition, Patent Document 3 proposes a technology for improving the wear resistance of cold-rolled steel sheet by dispersing coarse Nb-containing carbides at high density in a matrix consisting of a ferrite phase, and for improving toughness by utilizing the grain refinement effect of adding Nb.
[0008] Patent Document 4 proposes a technology for improving the wear resistance and toughness of cold-rolled steel sheet by dispersing coarse Nb·Ti carbides at high density in the matrix and reducing the number density of voids.
[0009] Patent Document 5 proposes a technology for improving the spheroidization rate of carbides such as cementite by annealing a steel plate containing 0.5 to 0.7 mass% carbon before final quenching and tempering, thereby improving toughness.
[0010] Patent Document 6 proposes a technology for producing a soft high-carbon steel sheet with excellent punchability by performing an annealing finish at a stage immediately before the final hardening and tempering treatment, thereby increasing the number density of voids formed in the material.
[0011] Patent Document 7 proposes a technology for improving impact toughness and wear resistance in a high carbon steel plate by controlling the generation of cementite carbide, which does not contain niobium, titanium, or vanadium carbides, and adjusting the spheroidization rate and number density of the cementite carbide to desired values. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Japanese Patent Application Publication No. 05-345952 [Patent Document 2] JP 2017-036492 A [Patent Document 3] JP 2015-190036 A [Patent Document 4] JP 2017-190494 A [Patent Document 5] JP 2009-024233 A [Patent Document 6] JP 2011-012316 A [Patent Document 7] Patent No. 6880245 Summary of the Invention [Problem to be solved by the invention]
[0013] The techniques proposed in Patent Documents 1 and 2 improve the toughness of high carbon cold rolled steel sheets by utilizing the grain refining effect of Nb addition. However, the grain refining effect of Nb is saturated at a Nb content of about 0.1 mass%, so the required toughness cannot be obtained by the grain refining effect alone.
[0014] In addition, the technology proposed in Patent Document 3 also improves toughness by utilizing the grain refinement effect of Nb addition. However, in Patent Document 3, Nb-containing carbide is used to improve wear resistance, and Nb-containing carbide is a factor that reduces toughness. Therefore, the effect of Nb addition and the effect of Nb-containing carbide cancel each other out, and the required toughness cannot be obtained.
[0015] As in Patent Document 3, the technology proposed in Patent Document 4 also utilizes the effect of improving wear resistance by dispersing hard Nb·Ti carbides at high density. However, when Nb·Ti carbides are dispersed at high density, voids are generated between the matrix and the carbides during cold rolling, resulting in a decrease in toughness. Therefore, Patent Document 4 suppresses the generation of voids by limiting the reduction ratio in cold rolling. However, this method limits the reduction ratio, which inevitably limits the thickness and mechanical properties of the cold-rolled steel sheet that can be manufactured, and therefore cannot be said to be an essential solution.
[0016] Moreover, even in the techniques proposed in Patent Documents 5 to 7, the toughness is still insufficient.
[0017] The present invention has been made in view of the above circumstances, and has an object to achieve even better toughness in a cold-rolled steel sheet in which the hardness has been improved by using carbides such as Nb. [Means for solving the problem]
[0018] The present inventors have investigated methods for solving the above problems and have come to the following findings.
[0019] (1) By appropriately controlling the size and density of Nb·Ti·V carbides in cold-rolled steel sheets, the toughness of the cold-rolled steel sheets after quenching and tempering can be effectively improved, and as a result, it becomes possible to manufacture steel parts that have both high levels of hardness and toughness.
[0020] (2) By appropriately controlling the chemical composition of the steel slab used and the manufacturing conditions of the cold-rolled steel sheet, the size and density of Nb·Ti·V carbides in the cold-rolled steel sheet can be appropriately controlled.
[0021] The present invention has been completed based on the above findings, and the gist of the present invention is as follows.
[0022] 1. In mass percent, C: 0.6~1.25%, Si: 0.10-0.55%, Mn: 0.20-2.0%, P: 0.0005~0.05%, S: 0.03% or less, Al: 0.001 to 0.1%, N: 0.001 to 0.009%, Cr: 0.1-1.0%, and Contains one or more of Ti: 0.01-1.0%, Nb: 0.05-0.5%, and V: 0.01-1.0%, Heating a steel slab having a composition with the balance being Fe and unavoidable impurities; The heated steel slab is hot-rolled under the condition of a finish rolling inlet temperature of 1000°C or more to obtain a hot-rolled steel sheet; The hot-rolled steel sheet is cooled under the conditions of a time from the end of the hot rolling to the start of cooling: 2 seconds or less, an average cooling rate: 25 ° C. / s or more, and a cooling stop temperature: 720 ° C. or less, The cooled hot-rolled steel sheet is coiled. The hot-rolled steel sheet after coiling is subjected to a first annealing under the conditions of an annealing temperature of 650°C or more and 780°C or less and an annealing time of 3 hours or more; The hot-rolled steel sheet after the first annealing is subjected to cold rolling at a rolling ratio of 15% or more and second annealing at an annealing temperature of 600 to 800 ° C. and a heating rate of 150 ° C. / h or less, which are repeated at least twice, and then subjected to final cold rolling at a rolling ratio of 20% or more. The average grain size of carbides containing at least one of Nb, Ti, and V present in ferrite grains is 0.10 μm or more, and the number density of the carbides having a grain size of 0.10 μm or more is 100 pieces / mm 2 The method for producing the cold-rolled steel sheet as described above.
[0023] 2. The composition of the components is, in mass%, Sb: 0.1% or less, Hf: 0.5% or less, REM: 0.1% or less, Cu: 0.5% or less, Ni: 3.0% or less, Sn: 0.5% or less, Mo: 1% or less Zr: 0.5% or less, B: 0.005% or less, and The method for producing a cold-rolled steel sheet according to 1 above, further comprising: adding 1 or more selected from the group consisting of W: 0.01% or less.
[0024] 3. The method for producing a cold-rolled steel sheet according to 1 above, wherein the heating rate in the second annealing is 50° C. / h or more.
[0025] 4. The method for producing a cold-rolled steel sheet according to 2 above, wherein the heating rate in the second annealing is 50° C. / h or more.
[0026] 5. A method for producing a steel part, comprising quenching a cold-rolled steel sheet produced by the method described in any one of 1 to 4 above at a quenching temperature of 700°C to 900°C for a holding time of 1 minute to less than 60 minutes, and then tempering the same at a tempering temperature of 150 to 400°C for a holding time of 20 minutes to 3 hours.
[0027] The main configuration of another embodiment of the present invention is as follows.
[0028] 1. In mass percent, C: 0.6~1.25%, Si: 0.10-0.55%, Mn: 0.20-2.0%, P: 0.0005~0.05%, S: 0.03 or less, Al: 0.001 to 0.1%, N: 0.001 to 0.009%, Cr: 0.1-1.0%, and Contains one or more of Ti: 0.01-1.0%, Nb: 0.05-0.5%, and V: 0.01-1.0%, The balance is Fe and unavoidable impurities. The average grain size of carbides containing at least one of Nb, Ti, and V present in ferrite grains is 0.1 μm or more, and Among the carbides, those having a particle size of 0.1 μm or more have a number density of 100 pieces / mm 2 This is the above cold-rolled steel sheet.
[0029] 2. The composition of the components is, in mass%, Sb: 0.1% or less, Hf: 0.5% or less, REM: 0.1% or less, Cu: 0.5% or less, Ni: 3.0% or less, Sn: 0.5% or less, Mo: 1% or less Zr: 0.5% or less, B: 0.005% or less, and The cold rolled steel sheet according to 1 above, further comprising one or more selected from the group consisting of: W: 0.01% or less.
[0030] 3. A steel part obtained by subjecting the cold-rolled steel sheet according to 1 or 2 above to quenching and tempering treatment.
[0031] 4. The steel part according to claim 3, which is any one of a textile machine part, a bearing part, and a blade.
[0032] 5. Heating a steel slab having the composition described in 1 or 2 above, The heated steel slab is hot-rolled under the condition of a finish rolling entry temperature of Ac3 point or higher to obtain a hot-rolled steel sheet; The hot-rolled steel sheet is cooled under the conditions of a time from the end of the hot rolling to the start of cooling: 2 seconds or less, an average cooling rate: 25 ° C. / s or more, and a cooling stop temperature: 720 ° C. or less, The cooled hot-rolled steel sheet is coiled. The hot-rolled steel sheet after coiling is subjected to a first annealing under the conditions of an annealing temperature of 650°C or more and 780°C or less and an annealing time of 3 hours or more; A method for producing a cold-rolled steel sheet, comprising the steps of: cold rolling at a rolling ratio of 15% or more and second annealing at an annealing temperature of 600 to 800°C on the hot-rolled steel sheet after the first annealing, the cold-rolling being repeated at least twice, and then final cold rolling at a rolling ratio of 20% or more.
[0033] 6. The method for producing a cold-rolled steel sheet according to 5 above, wherein the heating rate in the second annealing is 50° C. / h or more.
[0034] 7. A method for manufacturing a steel part, comprising quenching the cold-rolled steel sheet manufactured by the manufacturing method described in 5 or 6 above at a quenching temperature of 700°C to 800°C for a holding time of 1 minute to less than 60 minutes, and then tempering the same at a tempering temperature of 150 to 300°C for a holding time of 20 minutes to 3 hours. Effect of the Invention
[0035] According to the present invention, it is possible to obtain even better toughness after quenching and tempering in a cold-rolled steel sheet in which the hardness is improved by using carbides such as Nb. Therefore, the cold-rolled steel sheet of the present invention can be extremely suitably used as a material for various steel parts, including parts for textile machines, bearing parts, and machine and household knives. Furthermore, according to the present invention, it is possible to provide steel parts using the cold-rolled steel sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The present invention will be described in detail below. Note that the present invention is not limited to this embodiment. In addition, the present invention focuses on carbides that are present in ferrite grains and contain at least one of Nb, Ti, and V. Therefore, in the following description, "carbides that are present in ferrite grains and contain at least one of Nb, Ti, and V" may be simply referred to as "carbides".
[0037] [Component composition] The cold-rolled steel sheet of the present invention has the above-mentioned composition. The reasons for the limitations will be described below. In the following description, "%" as a unit of content refers to "mass%" unless otherwise specified.
[0038] C: 0.6 to 1.25% C is an element necessary for improving hardness after quenching and tempering. C is also an element necessary for forming carbides together with cementite, Nb, Ti, V, and other elements. In order to form the necessary carbides and obtain the strength after quenching and tempering, the C content must be 0.6% or more. Therefore, the C content is 0.6% or more, preferably 0.7% or more. On the other hand, if the C content exceeds 1.25%, the hardness increases excessively and the material becomes brittle. Also, if the C content exceeds 1.25%, the surface scale becomes strong during heating, resulting in deterioration of the surface properties. Therefore, the C content is 1.25% or less, preferably 1.20% or less.
[0039] Silicon: 0.10 to 0.55% Si is an element that has the effect of increasing strength by solid solution strengthening. In order to obtain the above effect, the Si content is set to 0.10% or more, preferably 0.12% or more, and more preferably 0.14% or more. On the other hand, if the Si content is excessive, Si oxides are generated and toughness is reduced. On the other hand, if the Si content is excessive, the generation and grain growth of ferrite are promoted, the precipitation of carbides at grain boundaries is promoted, and the precipitation of carbides within grains is suppressed. In addition, if Si is excessive, the surface scale during heating becomes strong, resulting in deterioration of surface properties. Therefore, the Si content is set to 0.55% or less, preferably 0.50% or less, and more preferably 0.45% or less.
[0040] Mn: 0.20~2.0% Mn is an element that has the effect of promoting quenching and suppressing temper softening, thereby improving hardness. In order to suppress temper softening, it is necessary to suppress the formation of C as cementite or to delay dislocation recovery, but Mn has both effects, and by adding Mn, a high-hardness structure with high dislocation density can be maintained even after tempering. In order to obtain the above effect, the Mn content is set to 0.20% or more, preferably 0.25% or more. On the other hand, if the Mn content exceeds 2.0%, a band-shaped structure is formed due to the segregation of Mn. In particular, abnormal grain growth and heterogeneity of the structure are likely to occur in the segregated part of MnS, and local precipitation occurs at the ferrite grain boundary, suppressing the formation of carbides within the grains. In addition, it causes cracks and shape defects during processing. Therefore, the Mn content is set to 2.0% or less, preferably 1.95% or less.
[0041] P: 0.0005~0.05% By adding a small amount of P, the strength improving effect due to solid solution strengthening can be obtained. To obtain this effect, the P content is set to 0.0005% or more, preferably 0.0008% or more. On the other hand, if the P content exceeds 0.05%, the toughness decreases due to grain boundary embrittlement. Therefore, the P content is set to 0.05% or less, preferably 0.045% or less.
[0042] S: 0.03% or less S forms sulfides with Mn, thereby reducing toughness. Therefore, the S content is set to 0.03% or less, preferably 0.02% or less. On the other hand, from the viewpoint of improving toughness, the lower the S content, the better, so the lower limit of the S content is not particularly limited and may be 0%. However, since excessive reduction leads to an increase in manufacturing costs, from the viewpoint of industrial production, the S content is preferably set to 0.0005% or more, and more preferably set to 0.001% or more.
[0043] Al: 0.001 to 0.1% Al is an element necessary for deoxidation during steelmaking. Therefore, the Al content is set to 0.001% or more. On the other hand, if Al is excessive, nitrides are formed, which promotes the formation of cracks and voids originating from the nitrides, resulting in a decrease in toughness. Therefore, the Al content is set to 0.1% or less, preferably 0.08% or less, and more preferably 0.06% or less.
[0044] N: 0.001 to 0.009% Nitrogen is an element that refines grain size and improves toughness by forming fine nitrides. Therefore, the N content is set to 0.001% or more. On the other hand, if N is excessive, it bonds with Al to form nitrides, which promotes the formation of cracks and voids originating from the nitrides, resulting in a decrease in toughness. Therefore, the N content is set to 0.009% or less, preferably 0.008% or less.
[0045] Cr: 0.1-1.0% Cr is an element that enhances the hardenability and strength of steel. To obtain the above effects, the Cr content is set to 0.1% or more, preferably 0.12% or more. On the other hand, excessive Cr forms coarse Cr carbides and Cr nitrides, which generate voids around the Cr carbides and Cr nitrides, resulting in a decrease in toughness. Therefore, the Cr content is set to 1.0% or less, preferably 0.95% or less.
[0046] The above-mentioned composition contains one or more selected from Ti: 0.01-1.0%, Nb: 0.05-0.5%, and V: 0.01-1.0%. In order to obtain a desired number density of carbides, it is necessary to add at least one of Ti, Nb, and V in the amount mentioned above.
[0047] Ti: 0.01 to 1.0% Ti is an element that has the effect of forming carbides within grains and improving toughness. When Ti is added, the Ti content is set to 0.01% or more, preferably 0.015% or more, in order to obtain the above effect. On the other hand, if Ti is added in excess, the austenitization temperature becomes high, and ferrite is more likely to form on the surface of the steel sheet due to the temperature drop during hot rolling. The ferrite formed on the surface remains even after the subsequent cold rolling and annealing, and as a result of the priority being given to the formation of carbides on the grain boundaries, the formation of carbides within the grains is suppressed. Therefore, the Ti content is set to 1.0% or less, preferably 0.9% or less.
[0048] Nb: 0.05-0.5% Nb is an element that has the effect of forming carbides within grains and improving toughness. Nb is also an element that has a large effect on grain refinement. When Nb is added, the Nb content is set to 0.05% or more in order to obtain the above effect. On the other hand, when Nb is added in excess, carbides are formed at grain boundaries and the number density of carbides formed within grains decreases. Carbides formed at grain boundaries become the starting points of voids and cracks, thereby reducing toughness. Therefore, the Nb content is set to 0.5% or less, preferably 0.45% or less.
[0049] V: 0.01 to 1.0% V is an element that has the effect of forming carbides within grains and improving toughness. V also has the effect of improving hardenability, improving the strength of steel. In order to suppress tempering softening, it is necessary to suppress the formation of C as cementite or to delay dislocation recovery, but V has both of these functions, and by adding V, the processed structure can be maintained even after tempering, improving toughness. When V is added, the V content is set to 0.01% or more in order to obtain the above effect. On the other hand, if V is added in excess, the carbides formed at the grain boundaries become coarse, and the carbides formed at the grain boundaries become the starting points of voids and cracks, thereby reducing toughness. Therefore, the V content is set to 1.0% or less, preferably 0.95% or less.
[0050] A cold-rolled steel sheet according to one embodiment of the present invention has a composition comprising the above components with the remainder being Fe and unavoidable impurities.
[0051] In another embodiment of the present invention, the above-mentioned composition may further contain one or more selected from the group consisting of Sb: 0.1% or less, Hf: 0.5% or less, REM: 0.1% or less, Cu: 0.5% or less, Ni: 3.0% or less, Sn: 0.5% or less, Mo: 1% or less, Zr: 0.5% or less, B: 0.005% or less, and W: 0.01% or less.
[0052] Sb: 0.1% or less Sb is an element effective in improving corrosion resistance, but if added in excess, it forms an Sb-rich layer under the scale formed during hot rolling, causing surface scuffs (scratches) on the steel sheet after hot rolling. Therefore, the Sb content is set to 0.1% or less. On the other hand, the lower limit of the Sb content is not particularly limited, but from the viewpoint of enhancing the effect of addition, it is preferable that the Sb content be 0.0003% or more.
[0053] Hf: 0.5% or less Hf is an element effective in improving corrosion resistance, but if added in excess, it forms a Hf-rich layer under the scale formed during hot rolling, causing surface scuffs (scratches) on the steel sheet after hot rolling. Therefore, the Hf content is set to 0.5% or less. On the other hand, the lower limit of the Hf content is not particularly limited, but from the viewpoint of enhancing the effect of addition, it is preferable that the Hf content be 0.001% or more.
[0054] REM: 0.1% or less REM (rare earth metal) is an element that improves the strength of steel. However, excessive addition of REM can delay the spheroidization of cementite and promote inhomogeneous deformation during cold working, which can deteriorate the surface properties. Therefore, the REM content is set to 0.1% or less. On the other hand, although there is no particular lower limit for the REM content, from the viewpoint of enhancing the effect of addition, it is preferable that the REM content be 0.005% or more.
[0055] Cu: 0.5% or less Cu is an effective element for improving corrosion resistance, but if added in excess, it will form a Cu-rich layer under the scale formed during hot rolling, causing surface scuffs (scratches) on the steel sheet after hot rolling. Therefore, the amount of Cu added is set to 0.5% or less. On the other hand, the lower limit of the Cu content is not particularly limited, but from the viewpoint of enhancing the effect of addition, it is preferable that the Cu content be 0.01% or more.
[0056] Ni: 3.0% or less Ni is an element that improves the strength of steel. However, excessive addition of Ni can promote inhomogeneous deformation during cold working and deteriorate the surface properties. Therefore, the Ni content is set to 3.0% or less. On the other hand, the lower limit of the Ni content is not particularly limited, but from the viewpoint of enhancing the effect of addition, the Ni content is preferably set to 0.01% or more.
[0057] Sn: 0.5% or less Sn is an effective element for improving corrosion resistance, but if added in excess, it forms a Sn-rich layer under the scale formed during hot rolling, which causes surface scuffs (scratches) on the steel sheet after hot rolling. Therefore, the Sn content is set to 0.5% or less. On the other hand, the lower limit of the Sn content is not particularly limited, but from the viewpoint of enhancing the effect of addition, it is preferable that the Sn content be 0.0001% or more.
[0058] Mo: 1% or less Mo is an element that improves the strength of steel. However, excessive addition of Mo can delay the spheroidization of cementite and promote inhomogeneous deformation during cold working, which can deteriorate the surface properties. Therefore, the Mo content is set to 1% or less. On the other hand, the lower limit of the Mo content is not particularly limited, but from the viewpoint of enhancing the effect of addition, the Mo content is preferably set to 0.001% or more.
[0059] Zr: 0.5% or less Zr is an effective element for improving corrosion resistance, but if added in excess, it will form a Zn-rich layer under the scale formed during hot rolling, causing surface scuffs (scratches) on the steel sheet after hot rolling. Therefore, the Zr content is set to 0.5% or less. On the other hand, the lower limit of the Zr content is not particularly limited, but from the viewpoint of enhancing the effect of addition, it is preferable that the Zr content be 0.01% or more.
[0060] B: 0.005% or less B is an element that has the effect of improving hardenability and can be added as desired. However, if the B content exceeds 0.005%, cracks are likely to occur on the surface during hardening. Therefore, the B content is set to 0.005% or less. On the other hand, although there is no particular lower limit for the B content, from the viewpoint of enhancing the effect of addition, when B is added, the B content is preferably set to 0.0001% or more.
[0061] W: 0.01% or less W is an element that has the effect of improving hardenability and can be added as desired. However, if the W content exceeds 0.01%, cracks are likely to occur on the surface during hardening. Therefore, the W content is set to 0.01% or less. On the other hand, although there is no particular lower limit for the W content, from the viewpoint of enhancing the effect of addition, when W is added, the W content is preferably set to 0.001% or more.
[0062] [carbide] Next, the carbides contained in the cold-rolled steel sheet of the present invention will be described.
[0063] Average particle size: 0.10μm or more Count density: 100 pieces / mm 2 End A structure in which Nb, Ti, and V-based carbides are formed within the grains is created before cold rolling, which is a pre-process before the start of part processing. After that, the processed structure is generated during cold rolling, and then quenching and tempering are performed, whereby some of the fine Nb, Ti, and V-based carbides are reprecipitated at the subgrain boundaries. This structure increases the resistance to strain introduced by repeated deformation, improving the toughness of the final product. To achieve this effect, the average grain size of the carbides containing at least one of Nb, Ti, and V present within the ferrite grains must be 0.10 μm or more. For the same reason, the number density of the carbides with a grain size of 0.10 μm or more must be 100 pieces / mm 2 It needs to be more than that.
[0064] If the average grain size of the carbides is less than 0.10 μm, the amount of fine Nb, Ti, and V carbides that precipitate after quenching and tempering is insufficient, and a high toughness improvement effect cannot be obtained. 2 If it is less than this, as in the case of the average grain size, the amount of fine Nb, Ti, and V carbides that precipitate after quenching and tempering is insufficient, and a high toughness improvement effect cannot be obtained.
[0065] Plate Thickness The thickness of the cold rolled steel sheet is not particularly limited and may be any thickness, but is preferably 0.1 mm or more, and more preferably 0.2 mm or more. The upper limit of the thickness is also not particularly limited, but is preferably 2.5 mm or less, more preferably 1.6 mm or less, and even more preferably 0.8 mm or less. When the thickness is 0.2 mm or more and 0.8 mm or less, it can be particularly suitably used as a material for textile machine parts such as knitting needles.
[0066] [Method of manufacturing cold-rolled steel sheets] Next, a method for producing a cold-rolled steel sheet according to an embodiment of the present invention will be described.
[0067] The cold-rolled steel sheet can be produced by sequentially carrying out the following steps on a steel slab having the above-mentioned composition. (1)Heating (2) Hot rolling (3) Cooling (4) Winding (5) First annealing (6) Cold rolling (7) Second annealing (8) Final cold rolling The above steps (6) and (7) are then repeated two or more times. Each step will now be described.
[0068] (1)Heating First, a steel slab having the above-mentioned composition is heated. The steel slab can be produced by any method without any particular limitation. For example, the composition of the steel slab may be adjusted by a blast furnace converter method or an electric furnace method. Moreover, casting of the molten steel into a slab may be performed by a continuous casting method or a blooming rolling method.
[0069] The heating can be carried out by any method, but is preferably carried out using a heating furnace.
[0070] When the heating is performed using a heating furnace, the temperature inside the heating furnace is not particularly limited, but from the viewpoint of homogenizing the steel components and dissolving the segregated and undissolved carbides in the steel slab, it is preferable to set the temperature at 1100°C or higher.
[0071] The holding time during the heating is not particularly limited, but from the viewpoint of sufficiently dissolving undissolved carbides, the holding time is preferably 1 hour or more.
[0072] (2) Hot rolling The heated steel slab is then hot-rolled to produce a hot-rolled steel sheet. In the hot-rolling, rough rolling and finish rolling can be performed according to a conventional method.
[0073] Finish rolling entry temperature: Ac3 point or higher If the finish rolling entry temperature in the hot rolling is lower than the Ac3 point, extended ferrite is generated in the steel sheet after hot rolling, and this extended ferrite remains in the finally obtained cold-rolled steel sheet. As a result, the generation of grain boundary carbides is promoted and the generation of intragranular carbides is suppressed, resulting in a decrease in toughness. Therefore, the finish rolling entry temperature in the hot rolling is set to the Ac3 point or higher. On the other hand, the upper limit of the finish rolling entry temperature is not particularly limited, but it is preferably set to 1200°C or lower.
[0074] The Ac3 point (° C.) is calculated by the following formula (1). Ac3(℃) = 910 - (203 * C 1 / 2 ) + (44.7 × Si) - (30 × Mn) - (11 × Cr) + (400 × Ti) + (460 × Al) + (700 × P) +(104 × V) + 38 …(1) Here, the element symbols in the above formula (1) indicate the content (mass%) of each element, and are set to zero when the element is not contained.
[0075] (3) Cooling Time from the end of hot rolling to the start of cooling: 2 seconds or less Next, the hot-rolled steel sheet is cooled. At that time, if a long time passes between the end of hot rolling and the start of cooling, coarse ferrite is generated, and carbides containing at least one of Ti, Nb, and V are heterogeneously precipitated at the grain boundaries. This heterogeneous structure is not homogenized in the subsequent cold rolling and annealing, and hinders the generation of carbides within the grains. Therefore, the time from the end of hot rolling to the start of cooling is set to 2 seconds or less. On the other hand, from the above viewpoint, the shorter the time from the end of hot rolling to the start of cooling, the better, so the lower limit is not particularly limited. However, from the viewpoint of industrial production, it may be 0.5 seconds or more, or may be 0.8 seconds or more.
[0076] Average cooling rate: 25℃ / s or more If the average cooling rate in the cooling is less than 25°C / s, the ferrite grains become coarse and the generated carbides become localized, so that when the subsequent cold rolling and annealing are repeated, the generation of carbides is concentrated at the grain boundaries, and the generation of intragranular carbides is suppressed. Therefore, the average cooling rate is set to 25°C / s or more. On the other hand, although there is no particular upper limit for the average cooling rate, if the cooling rate is excessively high, the coiled shape becomes poor due to volume expansion caused by transformation during the subsequent coiling. Therefore, from the viewpoint of obtaining a good coiled shape, the average cooling rate is preferably set to 160°C / s or less, and more preferably set to 150°C / s or less.
[0077] Cooling stop temperature: 720℃ Also, if the cooling stop temperature in the cooling is too high, the ferrite grains will coarsen, and the formation of carbides in the grains will be suppressed when cold rolling and annealing are repeated. Therefore, the cooling stop temperature is set to 720°C or lower. On the other hand, although there is no particular limit to the lower limit of the cooling stop temperature, if the cooling stop temperature is excessively low, the coiling shape will be poor due to volume expansion caused by transformation during the subsequent coiling. Therefore, the cooling stop temperature is preferably set to 620°C or higher, and more preferably 640°C or higher.
[0078] (4) Winding After the cooling is stopped, the cooled hot-rolled steel sheet is wound into a coil. At this time, the coiling temperature is not particularly limited, but is preferably 600 to 730° C. By setting the temperature at this temperature, plate-shaped cementite is precipitated, and the wound shape of the coil is stabilized.
[0079] (5) First annealing Annealing temperature: 650℃ or higher, 780℃ or lower Annealing time: 3 hours or more The hot-rolled steel sheet after coiling is subjected to a first annealing under the conditions of an annealing temperature of 650°C or more and 780°C or less, and an annealing time of 3 hours or more. The structure of the hot-rolled steel sheet after coiling is a pearlite structure in which carbides and ferrite formed in a plate shape are arranged. Since the pearlite structure is stable, it will not be homogenized unless it is held at a high temperature for a long time. In order to break down the pearlite structure and generate desired carbides within the grains in the subsequent cold rolling and annealing processes, it is necessary to set the annealing temperature to 650°C or more and the annealing time to 3 hours or more. On the other hand, if the annealing temperature is higher than 780°C, phase transformation starts preferentially from a part, resulting in a locally coarse structure and an inhomogeneous structure, making it difficult to obtain intragranular carbides, and the desired carbide number density cannot be obtained. The upper limit of the annealing time is not particularly limited, but if it is too long, the productivity will decrease and the effect will saturate. Therefore, it is preferable to set it to 20 hours or less.
[0080] It is also preferable to subject the hot-rolled steel sheet to pickling prior to the first annealing.
[0081] (6) Cold rolling (7) Second annealing Plate-shaped carbides are formed in the steel sheet after hot rolling. Since the plate-shaped carbides are stable, they tend to remain for a long time, and the plate-shaped carbides that remain eventually cause voids and cracks, thereby reducing toughness. Therefore, in order to turn the plate-shaped carbides into particles and remelt them by heating during annealing, and to precipitate the carbides within the grains, the hot-rolled steel sheet after the first annealing is subjected to cold rolling and second annealing two or more times.
[0082] Rolling ratio: 15% or more If the rolling reduction rate in the cold rolling is less than 15%, the carbides at the grain boundaries will become coarse, and the number density of the carbides generated within the grains will decrease and the grain size of the intragranular carbides will become small. Therefore, the rolling reduction rate is set to 15% or more. On the other hand, the upper limit of the rolling reduction rate is not particularly limited, but it is preferably set to 70% or less.
[0083] Annealing temperature: 600~800℃ If the annealing temperature in the second annealing is higher than 800°C, the carbides at the grain boundaries will become coarse, and the number density of the carbides generated within the grains will decrease, and the grain size of the intragranular carbides will become small. Therefore, the annealing temperature is set to 800°C or lower. On the other hand, if the annealing temperature is lower than 600°C, the generation of intragranular carbides will be suppressed, and the desired grain size will not be obtained. Therefore, the annealing temperature is set to 600°C or higher.
[0084] The heating rate in the second annealing is not particularly limited, but if the heating rate is too slow, carbides are likely to form at the ferrite grain boundaries, and the formation of carbides within the grains is suppressed. Therefore, from the viewpoint of further enhancing the toughness improvement effect, it is preferable that the heating rate in the second annealing is 50° C. / hr or more. On the other hand, the upper limit of the heating rate is not particularly limited, but it is preferable that it is 200° C. / s or less.
[0085] The cold rolling and the second annealing are repeated two or more times. By repeating the cold rolling and the annealing two or more times, the generation of carbides is promoted, and the desired size and number density of carbides in the grains can be finally achieved. The upper limit of the number of repetitions is not particularly limited, but since the effect is saturated even if the number of repetitions is more than five, it is preferable that the number of repetitions is five or less.
[0086] (8) Final cold rolling Rolling ratio 20% or more After repeating the cold rolling and second annealing two or more times as described above, final cold rolling is further performed at a rolling reduction of 20% or more. By performing final cold rolling at a rolling reduction of 20% or more, carbides of a desired number density are precipitated in the grains during quenching and tempering, improving toughness. A larger rolling reduction in the final cold rolling is better, but if it is 65% or more, the shape of the steel sheet may become unstable. Therefore, the rolling reduction is preferably less than 65%.
[0087] By satisfying the above conditions, it is possible to produce a cold-rolled steel sheet having excellent toughness after quenching and tempering. The finally obtained cold-rolled steel sheet may be further subjected to an arbitrary surface treatment.
[0088] [Manufacturing method for steel parts] In one embodiment of the present invention, a steel part can be manufactured by quenching and tempering the cold rolled steel sheet manufactured by the above manufacturing method. The conditions of the quenching and tempering are not particularly limited, but in order to obtain higher toughness, it is preferable to perform quenching under the conditions of a quenching temperature of 700°C or more and 900°C or less, and a holding time of 1 minute or more and less than 60 minutes, and then tempering under the conditions of a tempering temperature of 150 to 400°C, and a holding time of 20 minutes or more and 3 hours or less. It is more preferable that the quenching temperature is 750°C or more and 850°C or less. It is more preferable that the tempering temperature is 200 to 300°C.
[0089] The cooling method in the quenching is not particularly limited and can be any method, for example, air cooling, water quenching, or oil quenching.
[0090] Prior to the quenching and tempering, the cold rolled steel sheet may be optionally processed to have a desired shape. EXAMPLES
[0091] In order to confirm the effects of the present invention, cold-rolled steel sheets were produced according to the procedure described below, and the toughness of the obtained cold-rolled steel sheets after quenching and tempering was evaluated.
[0092] First, steel having the chemical composition shown in Table 1 was melted in a converter and made into a steel slab by a continuous casting method. The steel slab was then successively subjected to heating, hot rolling, cooling, coiling, first annealing, cold rolling, second annealing, and final cold rolling to obtain a cold-rolled steel sheet having a final thickness of about 0.4 mm. Each process was carried out under the conditions shown in Tables 2 and 3, and the cold rolling and second annealing were repeated the number of times shown in Tables 2 and 3.
[0093] (Method of measuring carbide) A test piece for microstructure observation was taken from the obtained cold-rolled steel sheet. After polishing the rolling direction cross section (L cross section) of the test piece for microstructure observation, the polished surface was corroded with 1 to 3 vol% nital solution to reveal the structure. Next, the surface of the test piece for microstructure observation was photographed at a magnification of 3000 times using a SEM (Scanning Electron Microscope) to obtain a microstructure image. From the obtained microstructure image, the grain size of Nb, Ti, and V-based carbides generated within the grains was measured by a cutting method, and the number density was calculated by counting the carbides within the measurement field of view. The average value of three fields of view was calculated as the grain size and number density. The measurement results are shown in Tables 4 and 5. The Nb, Ti, and V-based carbides were identified using SEM-EDS (Energy Dispersive x-ray Spectroscopy) analysis. Element mapping was performed on the observation field of view to separate cementite and other carbides, and the other carbides were determined to be Nb, Ti, and V-based carbides.
[0094] (Toughness after quenching and tempering) Next, in order to evaluate the toughness of the obtained cold-rolled steel sheet after quenching and tempering, the following test was performed, and the impact value in a Charpy impact test was measured. First, the obtained cold-rolled steel sheet was quenched and tempered. The quenching was performed by holding the cold-rolled steel sheet for 10 minutes in a furnace previously heated to 800°C, and then oil quenching at 80°C. The tempering was performed by holding the quenched cold-rolled steel sheet for 1 hour in a furnace previously heated to 250°C, and then air-cooling.
[0095] Thereafter, a Charpy impact test was carried out to measure the impact value. The measurement results are shown in Tables 4 and 5. For the Charpy impact test, a test piece with a notch depth of 2.5 mm and a notch radius of 0.1 mm (notch width of 0.2 mm) was used, which was taken from a cold-rolled steel sheet after quenching and tempering. The U-notch of the test piece was formed by electric discharge machining. In the present invention, the impact value is 8 J / cm 2 When this value was met, it was determined that the toughness after quenching and tempering was excellent.
[0096] [Table 1]
[0097] [Table 2]
[0098] [Table 3]
[0099] [Table 4]
[0100] [Table 5]
[0101] As can be seen from the results shown in Tables 1 to 5, the cold-rolled steel sheet satisfying the conditions of the present invention has excellent toughness after quenching and tempering. According to the present invention, it is possible to achieve both high hardness due to Nb-Ti-V carbides and excellent toughness, so that by using the cold-rolled steel sheet of the present invention, steel parts having both high levels of hardness and toughness can be manufactured. Therefore, the cold-rolled steel sheet of the present invention can be extremely suitably used as a material for various steel parts such as textile machine parts, bearing parts, and blades.
Claims
1. In mass percent, C: 0.6-1.25%, Si: 0.10 to 0.55%, Mn: 0.20-2.0%, P: 0.0005-0.05%, S: 0.03% or less, Al: 0.001-0.1%, N: 0.001 to 0.009%, Cr: 0.1 to 1.0%, and Contains one or more of Ti: 0.01 to 1.0%, Nb: 0.05 to 0.5%, and V: 0.01 to 1.0%, Heating a steel slab having a composition with the balance being Fe and unavoidable impurities; The heated steel slab is hot-rolled under the condition of a finish rolling inlet temperature of 1000° C. or more to obtain a hot-rolled steel sheet. The hot-rolled steel sheet is cooled under the conditions of a time from the end of the hot rolling to the start of cooling: 2 seconds or less, an average cooling rate: 25 ° C. / s or more, and a cooling stop temperature: 720 ° C. or less, The cooled hot-rolled steel sheet is coiled. The hot-rolled steel sheet after coiling is subjected to a first annealing under the conditions of an annealing temperature of 650° C. or more and 780° C. or less and an annealing time of 3 hours or more; The hot-rolled steel sheet after the first annealing is subjected to cold rolling at a rolling ratio of 15% or more and second annealing at an annealing temperature of 600 to 800 ° C. and a heating rate of 150 ° C. / h or less, which are repeated at least twice, and then subjected to final cold rolling at a rolling ratio of 20% or more. The average grain size of carbides containing at least one of Nb, Ti, and V present in ferrite grains is 0.10 μm or more, and the number density of the carbides having a grain size of 0.10 μm or more is 100 pieces / mm 2 The method for producing the cold-rolled steel sheet as described above.
2. The composition of the components is, in mass%, Sb: 0.1% or less, Hf: 0.5% or less, REM: 0.1% or less, Cu: 0.5% or less, Ni: 3.0% or less, Sn: 0.5% or less, Mo: 1% or less, Zr: 0.5% or less, B: 0.005% or less, and The method for producing a cold-rolled steel sheet according to claim 1, further comprising: W: 0.01% or less.
3. The method for producing a cold-rolled steel sheet according to claim 1, wherein the heating rate in the second annealing is 50° C. / h or more.
4. The method for producing a cold-rolled steel sheet according to claim 2, wherein the heating rate in the second annealing is 50° C. / h or more.
5. A method for producing a steel part, comprising quenching the cold-rolled steel sheet produced by the method according to any one of claims 1 to 4 under conditions of a quenching temperature of 700°C to 900°C and a holding time of 1 minute to less than 60 minutes, and then tempering the cold-rolled steel sheet under conditions of a tempering temperature of 150 to 400°C and a holding time of 20 minutes to 3 hours.
Citation Information
Patent Citations
High carbon cold rolled steel sheet with high toughness
JP1993345952A
High carbon steel sheet excellent in hardenability, fatigue property and toughness, and method for producing the same
JP2009024233A
Steel for wear resistant quenched-tempered component, and method for producing the same
JP2010138453A
Soft high-carbon steel sheet superior in punchability and method for manufacturing the same
JP2011012316A
Steel sheet for fiber machine component and manufacturing method therefor
JP2015190036A