Large hollow porous quartz glass base material and its manufacturing method
By controlling the rotational speed and using a wobbling condition to adjust density distributions, the method addresses the challenge of producing large hollow porous quartz glass cylinders with uniform properties and easy target extraction, reducing defects and non-uniformities.
Patent Information
- Application Number
- JP2020121187
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-15
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-07-15
AI Technical Summary
The existing methods for producing large hollow porous quartz glass cylinders face challenges in extracting the target from the soot body without causing scratches or cracks, especially when the soot body and target are firmly attached, leading to local defects and non-uniform density distributions that affect the quality of the final product.
The method involves controlling the rotational speed of the soot body during growth to maintain a constant surface circumferential speed by adjusting the frequency coefficient γ within a specific range (0.13 ≦ γ < 1.0), and using a wobbling condition to disperse the burner return positions, thereby minimizing density variations and facilitating easy extraction of the target.
This approach allows for the production of large hollow porous quartz glass cylinders with uniform chlorine and OH group content concentrations, reducing the risk of cracks and ensuring homogeneous optical and thermophysical properties, enabling easy target extraction.
Smart Images

Figure 0007555208000011 
Figure 0007555208000009 
Figure 0007555208000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a large hollow porous quartz glass base material and a manufacturing method thereof, and a hollow synthetic quartz glass cylinder using the same and a manufacturing method thereof, and in particular to a large, heavy hollow porous quartz glass base material having an outer diameter exceeding 300 mm, a manufacturing method for a hollow porous quartz glass base material that can suitably manufacture such a large hollow porous quartz glass base material, and a hollow synthetic quartz glass cylinder using the same and a manufacturing method thereof. [Background technology]
[0002] Synthetic quartz glass is widely used in the optical, semiconductor and chemical industries, particularly as a lens material for projection and exposure systems in microlithography, as a material for semiconductor manufacturing tools and optical fibers.
[0003] The general method for manufacturing hollow synthetic quartz glass cylinders is to manufacture a hollow porous synthetic quartz glass base material (soot body) and then sinter it to make it transparent. The OVD (Outside Vapor Deposition) method is known for manufacturing soot bodies, and the soot body is manufactured by converting silicon-containing raw materials into fine SiO2 particles by flame hydrolysis or pyrolysis and depositing them on the outer surface of a target rotating around its long axis.
[0004] Before sintering, the hollow porous quartz glass base material (soot body) needs to have the target removed, and this is done by rotating the target and the hollow soot body relative to each other or moving them in the longitudinal direction. This is extremely difficult if the soot body and the target are stuck together. Furthermore, even if it is possible to remove the target by applying a large force, scratches will be created on the inner surface of the soot body during the process, and these scratches will remain as localized defects in the quartz cylinder after sintering, resulting in defective parts.
[0005] In recent years, the demand for larger quartz cylinders has been increasing due to the increasing diameter of semiconductor wafers and the increasing size of optical fiber preforms. In order to manufacture large quartz cylinders, the hollow porous quartz glass preform (soot body), which is an intermediate product in the manufacturing process, must also be made larger and heavier. However, the increase in weight and diameter of the soot body has created a problem in that it becomes difficult to extract the target from the soot body. This means that it is difficult to realize both the fact that the target and the soot body are integrated during the growth of the soot body, and the soot body rotates following the target, and that the target can be extracted from the soot body after the soot growth is complete.
[0006] In the OVD method, a plurality of burners for synthesizing glass particles are arranged at regular intervals, and the row of burners is moved back and forth (swinged) relative to a rotating starting member (target) to deposit glass particles in layers on the target, thereby obtaining a soot body. At the turning point of the swing, the swing speed becomes zero instantaneously, so the time during which the flame is actually irradiated is longer than in the part swinging at a steady speed. Therefore, at the turning point, the amount of glass particles deposited is large, and unevenness occurs in the longitudinal direction. For this reason, Patent Document 1 describes a traverse method in which the turning point of the swing is moved by a predetermined distance in order to distribute the deposition in the longitudinal direction, thereby obtaining a soot body with a uniform outer diameter in the longitudinal direction, and such a traverse method is known as a method for distributing the deposition amount and density distribution.
[0007] In addition, in the OVD method, deposition is performed on the outer surface of the target while rotating it around its long axis. Therefore, if the rotation speed of the soot body is constant, the peripheral speed of the outer surface of the soot body increases with the growth of the outer diameter of the soot body, and the irradiation time per unit area becomes shorter, making it impossible to obtain a radially homogeneous soot body. Recently, as the diameter and thickness of the soot body are increased in order to improve productivity and reduce costs, the effect is particularly noticeable for large-diameter soot bodies with an outer diameter of more than 300 mm, and it is necessary to control the rotation speed to be lower as the outer diameter of the soot body grows so that the peripheral speed is constant. Furthermore, even if the peripheral speed is constant, if the speed is faster than a certain level, vibrations will occur due to slight eccentricity of the radial center of gravity when the outer diameter becomes large in the later stage of growth, and the load on the rotating device will increase, making stable production impossible. Furthermore, if the peripheral speed is faster than a certain level, the soot body will not follow the rotation of the target and will spin freely at the interface between the soot body and the target, causing the problem that the soot body cannot rotate stably at a constant speed. This problem can be avoided by strengthening the adhesion of the soot body to the target, but in that case, the target extraction work described above becomes extremely difficult, and even if the target can be extracted, local defects will occur. Therefore, a constant peripheral speed at a low rotation speed is essential.
[0008] However, when the size was increased and the rotation conditions were slowed down to keep the peripheral speed constant, cracks and ruptures frequently occurred during or after growth. Even if it did not reach that stage, if treatment with a chlorinating agent was performed, the chlorine content concentration distribution of the synthetic quartz glass cylinder after sintering became non-uniform, and if treatment with a chlorinating agent was not performed, the OH group content concentration distribution became non-uniform, making it impossible to obtain a quartz glass cylinder with optically homogeneous physical properties.
[0009] In the manufacture of optical fibers, the difference in chlorine concentration in the radial and circumferential directions is important, and recent research has revealed that fiber curl can be improved by reducing the difference in chlorine concentration distribution in the circumferential direction. When drawing large-diameter preforms, the amount of drawing per unit length increases and the deformation time in the drawing furnace increases, so the local homogeneity of the cladding affects the properties of the fiber. Therefore, as the size of the cladding glass base material increases, the stability of the chlorine concentration over a smaller range becomes important.
[0010] Quartz glass cylinders manufactured without chlorination treatment are often used as materials for quartz glass jigs and lamps used in semiconductor manufacturing equipment. To obtain such quartz glass materials, they are molded and heat-processed to the desired size, but if there is a large difference in OH group concentration during this process, viscosity distribution occurs within the cylinder, causing shape instability problems such as uneven thickness, siding, and ovalization. As with the optical fiber mentioned above, this becomes more pronounced as the glass size becomes larger, so it is important to stabilize the OH group concentration over a small area.
[0011] Regarding the reciprocating motion of the burner and the rotation of the support in the OVD method, Patent Document 2 describes that the base temperature of the surface is maintained between 1050°C and 1350°C, the average peripheral speed is maintained between 8m / min and 15m / min, and the translation speed (swing speed) of the burner row is maintained between 300mm / min and 800mm / min, thereby enabling the production of a base material with almost no local axial density fluctuation. However, in the method described in Patent Document 2, for example, if the swing distance is 100mm, the swing speed is 800mm / min, and the average peripheral speed is 9m / min, the rotation speed needs to be increased from 19.1rpm to 6.4rpm to grow the outer diameter (hereinafter, the outer diameter is also referred to as OD) of the deposit from 100mm to 300mm. However, if production is performed under these conditions, cracks will occur during growth and growth cannot continue.
[0012] Furthermore, Patent Document 3 describes a method in which the turning point of the reciprocating motion is moved in a constant direction by a predetermined distance and then moved in the opposite direction at a predetermined position, in which the rotation speed is kept constant and conditions are set to satisfy the following relationship, thereby suppressing external shape fluctuations (irregularities in the axial direction of the soot). The value expressed as A=(r / v)×L is 40≧A≧8 [r = rotation speed (rpm), v = reciprocating speed (mm / min), L = burner spacing]
[0013] In the method described in Patent Document 3, for example, when the swing speed is 850 mm / min and the swing width is 100 mm, the rotation speed r (rpm) needs to be 68≦r≦320 to set A within the specified range. However, when the outer diameter of the deposition body is large, for example, when the OD is 300 mm, the surface peripheral speed p (m / min) is fast at 64≦p≦301, and a strong centrifugal force is generated. The force increases as the weight and diameter increase, so vibration occurs, and the device and target need to be rigid enough to withstand the centrifugal force, which makes them expensive, and there is a problem that cracks occur during growth. Furthermore, Patent Document 3 is a method of depositing silica glass particles on the surface of a starting rod to manufacture a solid optical fiber preform, but it is not a method of manufacturing a hollow porous silica glass base material. In the method described in Patent Document 3, in order to manufacture a soot body with an outer diameter of 300 mm or more without idling between the interface of the target, it is necessary to firmly fix the target and the soot body, but in that case, there is also a problem that it is difficult to extract the target.
[0014] Patent Document 4 also describes that fluctuations in the longitudinal diameter can be suppressed by setting the reciprocating movement speed (swing speed) and rotation speed so that the rotational position of the starting rod is shifted half a period from its original position when the relative reciprocating movement (swing) of the starting rod and the burner makes one round trip and returns to its original position, and describes the following conditions. (L / V)×N(rpm)=n+0.5±0.1 [L = travel distance (mm), V = reciprocating speed (mm / min), N = rod rotation speed (rpm), n: any integer]
[0015] In the method described in Patent Document 4, the rotational position is shifted by 0.5 rotational period (180°) when the rod goes back and forth once, so that when the rod goes back and forth twice, the rotational position is shifted by one rotation (360°). For example, when the swing speed is 850 mm / min and the swing width is 100 mm, the above formula is satisfied when the rotation speed is 12.75 rpm (100 mm / 850 mm / min×12.75 rpm=1.5). However, in the case of 12.75 rpm, the timing of the swing turn-back position and one rotation coincides once every three rotations, and a density distribution is formed in the soot body in both the long axis direction and the radial direction. Furthermore, Patent Document 4 is also a method of depositing glass particles on the surface of a starting rod to manufacture a solid glass particle deposit body, but is not a method of manufacturing a hollow porous quartz glass base material.
[0016] As mentioned above, none of the patent documents are inventions that show the local density distribution of a soot body under low rotation speed conditions that enables extraction of a target from a large-diameter soot body with an outer diameter exceeding 300 mm, and further solve this problem to suppress the occurrence of cracks. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] Japanese Patent Application Publication No. 3-228845 [Patent Document 2] Special Publication No. 2001-504426 [Patent Document 3] JP 2002-167228 A [Patent Document 4] JP 2013-43810 A Summary of the Invention [Problem to be solved by the invention]
[0018] The present invention aims to provide a large hollow synthetic quartz glass porous base material and a manufacturing method thereof, as well as a hollow synthetic quartz glass cylinder and a manufacturing method thereof, which can produce a soot body without significantly increasing the load on the apparatus, such as centrifugal force generated during growth, even when the soot body has an outer diameter of more than 300 mm, and which eliminates the local density distribution of the soot body under constant low peripheral rotation speed conditions that accompany the increase in the diameter of the soot body when the outer diameter exceeds 300 mm, and which does not cause cracks or ruptures in the soot body even when produced at low rotation speeds, and which makes it easy to extract a target from the increased diameter soot body. [Means for solving the problem]
[0019] In order to solve the above problem, the soot body was investigated, and it was found that there is a difference not only in the amount of deposition but also in the density of the deposited layer at the turning point of the reciprocating movement of the burner in the soot body. In the present invention, the reciprocating movement of the burner is called a swing. Figure 4 is a graph showing the turning point of the reciprocating movement (swing) of the burner and the density distribution of the deposited layer in the longitudinal direction of the soot body. As shown in Figure 4, at the turning point of the burner, the density is higher than when the swing speed is moving at a steady speed, and by repeatedly depositing this, an axial density distribution is generated in the soot body.
[0020] Further investigation revealed that localized density differences were formed not only in the axial direction but also in the radial direction. A detailed analysis of this localized radial density variation revealed that the swing turning point and one rotation coincided at the same time. Figure 5 is a graph showing the density distribution in the radial direction of the soot body. As shown in Figure 5, the swing turning points where density is high are usually distributed in the circumferential direction, but when the swing turning point and one rotation coincide and the soot body grows for a certain period of time, the high density areas do not disperse and high density areas and low density areas overlap in the circumferential direction, resulting in extremely low density areas. In Figure 5, γ is a frequency coefficient calculated by the following formula (1). γ = S / (L N m ) · · · (1) [In the above formula (1), S is the burner moving speed (mm / min), L is the burner moving distance (mm), N m is the minimum value (rpm) at which the soot body can vary.
[0021] In other words, it was found that not only the deposition amount and density distribution in the axial direction but also the local density distribution occurs in the radial direction in the soot body, and various problems such as cracks, chlorine concentration distribution, and OH group concentration distribution occur as a result of the influence. Furthermore, it was found that by controlling the rotational peripheral speed of the soot body during growth to be substantially constant and setting the frequency coefficient γ to be within a predetermined range, it is possible to create a soot body even with an outer diameter of more than 300 mm without significantly increasing the load on the device, such as the centrifugal force generated during growth, and further to suppress the occurrence of cracks and the non-uniformity of the chlorine concentration and the OH group concentration. Furthermore, it was found that by setting the above, it is possible to easily extract a target from a soot body with a large diameter.
[0022] That is, the method for producing a hollow porous quartz glass base material of the present invention includes the steps of arranging multiple burners for synthesizing glass particles at a predetermined interval, moving the burners back and forth, and depositing glass particles on a rotating target to grow a soot body, and extracting the target from the soot body to produce a hollow porous quartz glass base material, and is characterized in that the rotational peripheral speed of the soot body is controlled to be essentially constant by varying the rotation speed of the soot body based on the outer diameter of the soot body which varies during growth, and the frequency coefficient γ calculated by the following formula (1) is set to be in the range of the following formula (2) when the outer diameter of the soot body exceeds 250 mm. γ = S / (L N m ) · · · (1) 0.13≦γ<1.0 (2) [In the formula (1), S is the moving speed of the burner (mm / min), L is the moving distance of the burner (mm), N m is the minimum value (rpm) of the rotational speed of the soot body.
[0023] When the turning position in the reciprocating movement of the burner is moved by a predetermined distance under wobbling conditions, it is preferable to set the turning position in the reciprocating movement of the burner to be within the range of the above formula (2) when the amount of movement of the turning position in one reciprocating movement of the burner is 1 / 3 or less of the flame diameter of the burner irradiated to the soot body. In the present invention, moving the turning position in the reciprocating movement of the burner by a predetermined distance is called wobbling. In the method of the present invention, by performing wobbling under the above-mentioned conditions, a hollow porous quartz glass base material with an extremely small density fluctuation can be obtained. Note that, under wobbling conditions, when the amount of movement of the turning position exceeds 1 / 3 of the flame diameter, the turning positions are dispersed, so heat is also dispersed, and problems such as cracks and non-uniform physical properties are relatively unlikely to occur.
[0024] The frequency coefficient γ is preferably 0.13 or more and 0.3 or less. By setting the frequency coefficient γ to 0.3 or less, it is possible to obtain a hollow synthetic quartz glass cylinder that is free from cracks or ruptures in the soot body, has a uniform distribution of the chlorine concentration and the OH group concentration, and is extremely homogeneous in terms of optical properties and thermal properties.
[0025] The method for producing a synthetic quartz glass cylinder of the present invention is characterized by using a hollow porous quartz glass preform obtained by the method for producing a hollow porous quartz glass preform of the present invention.
[0026] A first embodiment of the hollow porous quartz glass base material of the present invention is a large cylindrical hollow porous quartz glass base material having an outer diameter exceeding 300 mm and a length of 2 m or more, the average density of the entire base material being 0.55 g / cm 3 The above is also characterized in that the density variation per unit length at four points equidistant from the inner surface in the radial direction in four directions every 90° on the cylindrical cross section is 10% / cm or less compared to the average value of the four points, and that the material does not contain cracks.
[0027] A second embodiment of the hollow porous quartz glass base material of the present invention is a large cylindrical hollow porous quartz glass base material having an outer diameter of 500 mm or more and a length of 1.0 m or more, the average density of the entire base material being 0.55 g / cm 3 The above is also characterized in that the density variation per unit length at four points equidistant from the inner surface in the radial direction in four directions every 90° on the cylindrical cross section is 10% / cm or less compared to the average value of the four points, and that the material does not contain cracks.
[0028] The large-sized hollow porous quartz glass base material is suitably obtained by the method for producing a hollow porous quartz glass base material.
[0029] A third aspect of the hollow porous quartz glass base material of the present invention is a hollow porous quartz glass base material obtained by the manufacturing method of the hollow porous quartz glass base material, which is manufactured under the above-mentioned wobbling conditions and under conditions in which the movement amount of the turning position during one round trip of the burner is less than 1 / 3 of the flame diameter of the burner irradiated to the soot body, and is characterized in that the density variation per unit length at four points equidistant from the inner surface in the radial direction in four directions every 90° on the cylindrical cross section is 2% / cm or less compared to the average value of the four points.
[0030] A first embodiment of the hollow synthetic quartz glass cylinder of the present invention is obtained by dehydrating and vitrifying the hollow porous quartz glass base material, and is characterized in that it has an outer diameter of 200 to 500 mm, a length of 0.7 to 3.5 m, an OH group concentration of less than 5 ppm, and a chlorine content concentration of 500 ppm or more and 3000 ppm or less, and is free of appearance defects caused by cracks in the porous member.
[0031] In the first embodiment of the hollow synthetic quartz glass cylinder, it is preferable that the "maximum-minimum difference" of the chlorine concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder and spaced every 90° in the circumferential direction is within 15% of the average value of the four positions.
[0032] A second embodiment of the hollow synthetic quartz glass cylinder of the present invention is obtained by pre-sintering and vitrifying the hollow porous quartz glass base material, and is characterized in that it has an outer diameter of 200 to 500 mm, a length of 0.7 m to 3.5 m, an OH group concentration of 50 ppm or more and 500 ppm or less, and is free of appearance defects caused by cracks in the porous member.
[0033] In a second embodiment of the hollow synthetic quartz glass cylinder, it is preferable that the "maximum-minimum difference" of the OH group concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder and spaced every 90° in the circumferential direction is within 15% of the average value of the four positions.
[0034] A third embodiment of the hollow synthetic quartz glass cylinder of the present invention is a hollow synthetic quartz glass cylinder obtained by vitrifying the third embodiment of the hollow porous quartz glass base material, characterized in that the "maximum-minimum difference" of the chlorine concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, spaced at 90° intervals in the circumferential direction, is 10% or less of the average value of the four positions.
[0035] A fourth embodiment of the hollow synthetic quartz glass cylinder of the present invention is a hollow synthetic quartz glass cylinder obtained by vitrifying the hollow porous quartz glass base material of the third embodiment, characterized in that the "maximum-minimum difference" of the OH group concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, spaced at 90° intervals in the circumferential direction, is 10% or less of the average value of the four positions. Effect of the Invention
[0036] According to the present invention, a soot body can be produced even for a soot body with an outer diameter of more than 300 mm without significantly increasing the load on the apparatus, such as centrifugal force generated during growth, and further, the local density distribution of the soot body under constant peripheral speed and low rotation speed conditions that accompanies the increase in the diameter of a soot body exceeding 300 mm can be eliminated, and there is no crack or rupture in the soot body even when produced at a low rotation speed, and the target can be easily extracted from the increased diameter soot body, which has the remarkable effect of providing a large hollow synthetic quartz glass porous base material and a manufacturing method thereof, as well as a hollow synthetic quartz glass cylinder and a manufacturing method thereof. Furthermore, according to the present invention, it is possible to obtain a large hollow synthetic quartz glass cylinder having a uniform chlorine content or OH group content and extremely homogeneous optical and thermal properties. [Brief description of the drawings]
[0037] [Figure 1] FIG. 1 is a schematic explanatory diagram showing a method for producing a hollow porous quartz glass base material according to the present invention. [Diagram 2] 1A and 1B are schematic explanatory diagrams showing the movement of a burner in a method for producing a hollow porous quartz glass base material of the present invention, where (a) shows a non-wobbling condition and (b) shows a wobbling condition. [Diagram 3] FIG. 2 is a schematic explanatory diagram showing burner irradiation in the method for producing a hollow porous quartz glass base material of the present invention. [Figure 4] 1 is a graph showing the turning point of the reciprocating movement of a burner and the density distribution of a deposited layer in the longitudinal direction of a soot body. [Diagram 5] 1 is a graph showing a density distribution in a radial direction of a soot body. [Figure 6] FIG. 2 is a schematic explanatory diagram showing a method for measuring the density of the hollow porous quartz glass base material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The following describes the embodiments of the present invention, but these embodiments are shown by way of example only, and it goes without saying that various modifications are possible without departing from the technical spirit of the present invention. In the drawings, the same members are represented by the same reference numerals.
[0039] Fig. 1 is a schematic diagram showing the method for producing a hollow porous quartz glass base material of the present invention. The method for producing a hollow porous quartz glass base material of the present invention is a method for producing a hollow porous quartz glass base material by arranging a plurality of glass particle synthesis burners 16a, reciprocating the burners 16a, depositing glass particles on a rotating target 14, and growing a soot body 12, and controlling the rotational speed of the soot body 12 to be practically constant by varying the rotation speed of the soot body 12 based on the outer diameter of the soot body 12 that varies during growth, and setting the frequency coefficient γ calculated by the following formula (1) to be within the range of the following formula (2) when the outer diameter of the soot body exceeds 250 mm. Note that practically constant means ±5%. γ = S / (L N m ) · · · (1) 0.13≦γ<1.0 (2) [In the above formula (1), S is the moving speed of the burner 16a (mm / min), L is the moving distance of the burner 16a (mm), N m is the minimum value (rpm) of the fluctuating rotation speed of the soot body 12.
[0040] In Figure 1, the symbol 10 denotes a manufacturing apparatus for producing a hollow porous quartz glass base material, and includes a target holding and rotation mechanism 20 that rotates and holds a target 14 and controls the rotation speed (rpm), a glass particle synthesis burner group 16 in which a plurality of glass particle synthesis burners 16a are arranged at predetermined intervals, and a burner group movement control device 18 that controls the swing and up and down movement of the burner group 16.
[0041] As shown in Figure 1, a target holding and rotation mechanism 20 that controls the rotation speed of the target 14 and a group of glass particle synthesis burners 16 whose swing (reciprocating movement) and up-down movement are controlled by a burner group movement control device 18 are used to control the rotation speed of the soot body 12 based on the outer diameter of the soot body 12 that changes during growth, thereby controlling the rotational peripheral speed of the soot body 12 to be practically constant, and under conditions set so that the frequency coefficient γ calculated by the above formula (1) is 0.13 or more and less than 1.0, glass particles generated by a hydrolysis reaction caused by the flame of a glass particle synthesis burner 16a to which a glass raw material (SiCl4, etc.) is supplied are deposited on the outer surface of the rod-shaped target 14, whose rotation speed is controlled and held by the target holding and rotation mechanism 20, to grow the soot body 12, and then the target 14 is extracted from the soot body 12, thereby producing the hollow porous quartz glass base material of the present invention.
[0042] The cause of cracks is a local density difference that occurs within the soot body, which occurs when the timing of one rotation of the soot body and the timing of the burner swing turn coincide. Now consider the case where Y rotations are made during X swings (X / 2 round trips). The time required to swing X times is X(L / S), and conversely, the time required to rotate Y times is Y / N. Here, L is the burner travel distance (mm), S is the burner travel speed (mm / min), and N is the soot body rotation speed (rpm). The timing of the swing and rotation coincide, so X(L / S)=Y / N, and X / Y=S / (LN). This X / Y is called the frequency coefficient γ. γ shown in Figure 5 is the frequency coefficient.
[0043] For example, if two rotations occur between two swings, then γ = X / Y = 2 / 2 = 1. In this case, the timing of the rotation and swing will match at the left end of the swing during one turn, and the timing will match at the right end during the next turn. Since multiple burners are placed at equal intervals, the rotation and swing will match every turn, taking into account adjacent burners. The areas where they match will have a high density, while areas where they do not will have an extremely low density. This large density difference will cause cracks to appear during growth or after growth has finished. In the present invention, by controlling the surface speed of the soot body to be substantially constant and setting γ to less than 1.0 in the range where the outer diameter of the soot body exceeds 250 mm, a large hollow porous quartz glass preform free from cracks and ruptures can be obtained. In the present invention, the surface speed of the soot body is preferably 5 to 50 m / min, more preferably 5 to 10 m / min.
[0044] In addition, by using the same concept, even if not every time, the rotation and the turnaround match once every few times, and this also has an effect. Table 1 shows the frequency with which the rotation and the swing match when swing X=2 and rotation Y is an even number, and Table 2 shows the frequency with which the rotation and the swing match when swing X=2 and rotation Y is an odd number.
[0045] [Table 1]
[0046] [Table 2]
[0047] In the case of γ=2 / 3=0.667, where there are three rotations during two swings (one round trip), the turning point of the swing coincides with the turning point of one rotation once every three rotations, resulting in a density difference, although it is minor compared to when they coincide every time. In the case of γ=2 / 4=0.5, where there are four rotations during two swings (one round trip), the turning point of the swing coincides with the turning point of one rotation twice every four rotations, resulting in a density difference. As the density difference is not as great as when they coincide every time, cracks are unlikely to occur, but the density difference causes the distribution of chlorine concentration and OH group concentration to become non-uniform, making it impossible to obtain optically homogeneous quartz glass.
[0048] Therefore, in the frequency coefficient γ expressed as X / Y=S / (LN), N is the minimum value N m By setting the swing distance, swing speed, and rotation number so that the value of the frequency coefficient γ at this time is γ≦0.3, it is possible to create a condition in which the timing of the rotation and swing do not coincide, and as a result, a quartz glass cylinder can be obtained that is free of cracks and has a small chlorine content concentration distribution and a small OH group content concentration distribution. Since the present invention controls the rotational peripheral speed of the soot body to be practically constant, the rotation number of the soot body decreases as the soot body grows. Therefore, in the present invention, when the rotation number N is set to the minimum value N m It is defined by the frequency coefficient γ at
[0049] Furthermore, by setting the frequency coefficient γ to 0.13 or more, a soot body can be produced without causing vibration of the growing soot body or vibration of the apparatus even when deposition is performed with an outer diameter exceeding 250 mm. In the present invention, the frequency coefficient γ is 0.13 or more and less than 1.0, and more preferably 0.13 or more and 0.3 or less. By setting γ to less than 1.0, cracks and ruptures of the soot body are eliminated, and further, by setting γ to 0.3 or less, it is possible to obtain a quartz glass cylinder that is free of cracks and ruptures of the soot body, has a uniform distribution of the chlorine concentration and the OH group concentration, and is optically and thermally homogeneous.
[0050] In the method of the present invention, the swing turning position may be moved in a fixed direction by a predetermined distance (α) and then moved in the opposite direction at a predetermined position, so-called wobbling conditions, or non-wobbling conditions may be used. Figure 2 is a schematic diagram showing the movement of the burner in the manufacturing method of the hollow porous quartz glass base material of the present invention, where (a) shows the non-wobbling condition and (b) shows the wobbling condition. In Figure 2, L is the swing distance, b is the burner interval, and α is the wobbling shift amount. Note that, although Figure 2 shows the case where the swing distance and the burner interval are the same, in the present invention, the swing distance and the burner interval may be the same or different.
[0051] When performing under wobbling conditions, it is preferable to set the movement amount α of the turning position in one round trip of the burner so that it falls within the range of the above formula (2) when it is 1 / 3 or less of the flame diameter of the burner irradiated to the soot body. In the method of the present invention, by performing wobbling under the above conditions, it is possible to obtain a homogeneous hollow porous quartz glass base material with an extremely small density fluctuation amount. Note that, under wobbling conditions, when the movement amount of the turning position exceeds 1 / 3 of the flame diameter, the turning positions are dispersed, so heat is also dispersed, and problems such as cracks and non-uniform physical properties are relatively unlikely to occur.
[0052] 3 is a schematic diagram showing the irradiation of a burner in the method for producing a hollow porous quartz glass base material of the present invention, where d is the flame irradiation diameter. Even when wobbling is used, if the amount of movement α of the turning position in each swing is 1 / 3 or less of the flame irradiation diameter d irradiated from the burner to the deposit and spreads, the overlap between layers is large, so the method of the present invention is effective. The flame irradiation diameter d can be measured by image analysis of the flame during the growth of the soot body.
[0053] The method of the present invention can provide a large hollow porous quartz glass preform having an outer diameter of more than 300 mm, with small density fluctuation and no cracks or ruptures. Specifically, it can provide a large hollow porous quartz glass preform having an outer diameter of more than 300 mm and an axial length of 2 m or more, or a large hollow porous quartz glass preform having an outer diameter of 500 mm or more and an axial length of 1.0 m or more. The method of the present invention can also provide a large hollow porous quartz glass preform weighing 100 kg or more. Furthermore, the method of the present invention can make it extremely easy to extract the target even if the soot body is large in diameter and weight.
[0054] In the first embodiment of the hollow porous quartz glass base material of the present invention, the average density of the entire base material is 0.55 g / cm 3 The above is a large-sized hollow porous quartz glass base material having small density fluctuation, containing no cracks, an outer diameter exceeding 300 mm, and a length of 2 m or more. In a second embodiment of the hollow porous quartz glass base material of the present invention, the average density of the entire base material is 0.55 g / cm 3 The present invention provides a large-sized hollow porous quartz glass base material having small density fluctuations, no cracks, an outer diameter of 500 mm or more, and a length of 1.0 m or more.
[0055] In the first and second aspects of the hollow porous quartz glass base material, the average density of the entire base material is 0.55 g / cm 3 More than 0.56g / cm 3 More than 0.77g / cm 3 Less than 0.59 g / cm is preferred. 3 More than 0.68g / cm 3 The following is more preferred:
[0056] 6 is a schematic diagram showing a method for measuring the density variation in the hollow porous quartz glass base material of the present invention. As shown in FIG. 6, the density variation was measured at 1 cm from each of four points (a to d) equidistant (X mm) from the inner surface in the radial direction on four perpendicular lines (A to D) at 90° intervals in four directions of the cylindrical cross section of the hollow porous quartz glass base material 12 of the present invention. 3The density per unit length is measured, and the density variation is defined as the difference between the maximum and minimum density values at the four points (a to d). The density variation per unit length of the hollow porous quartz glass base material 12 of the present invention is 10% / cm or less, preferably 5% / cm or less, and more preferably 2% / cm or less, relative to the average value of the four points (a to d) in the four directions (A to D).
[0057] A third embodiment of the hollow porous quartz glass preform of the present invention is a hollow porous quartz glass preform in which the density variation per unit length at four points equidistant from the inner surface in the radial direction in four directions every 90° on the cylindrical cross section is 2% / cm or less relative to the average value of the four points. In the method for producing the hollow porous quartz glass preform, the hollow porous quartz glass preform is produced under wobbling conditions in which the movement amount of the turning position in one round trip of the burner is 1 / 3 or less of the flame diameter of the burner irradiated to the soot body, whereby a homogeneous hollow porous quartz glass preform with the aforementioned density variation is extremely small at 2% / cm or less can be obtained.
[0058] The method for producing a synthetic quartz glass cylinder of the present invention uses a hollow porous quartz glass base material obtained by the method of the present invention. The method for producing the synthetic quartz glass cylinder is not particularly limited, and it is sufficient to use the hollow porous quartz glass base material to produce a synthetic quartz glass cylinder by a known method, but a method of obtaining a synthetic quartz glass cylinder by dehydration treatment and sintering and vitrifying, or a method of obtaining a synthetic quartz glass cylinder by pre-sintering and vitrifying, is preferred. The method of the present invention makes it possible to preferably obtain a large synthetic quartz glass cylinder with an outer diameter of 200 mm or more that does not include any defective appearance caused by cracks in the porous member, is free from cracks and ruptures, and is free of such defects.
[0059] Specifically, as the large synthetic quartz glass cylinder, a hollow synthetic quartz glass cylinder with an outer diameter of 200 mm or more can be obtained by using a cylindrical large hollow porous quartz glass base material with an outer diameter of more than 300 mm, and a hollow synthetic quartz glass cylinder with an outer diameter of 300 mm or more can be obtained by using a cylindrical large hollow porous quartz glass base material with an outer diameter of 500 mm or more. In particular, hollow synthetic quartz glass cylinders with an outer diameter of 200 mm or more but less than 300 mm and an axial length of 2.3 mm or more, and hollow synthetic quartz glass cylinders with an outer diameter of 300 mm or more and an axial length of 0.7 mm or more are more suitable.
[0060] In the present invention, by using a hollow porous quartz glass base material obtained under conditions where γ is set to less than 1.0 in the range where the outer diameter of the soot body exceeds 250 mm, a large quartz glass cylinder that does not include appearance defects caused by cracks in the porous member and is free of cracks and ruptures can be easily obtained. This quartz glass cylinder is particularly suitable as a material for semiconductor manufacturing jigs, which are desired to be large. Furthermore, by using a hollow porous quartz glass base material obtained under conditions where γ is set to 0.3 or less, a quartz glass cylinder that is free of cracks and ruptures, has a uniform distribution of the chlorine content concentration and the OH group content concentration, and is extremely homogeneous in terms of optical and thermal properties.
[0061] A first embodiment of the hollow synthetic quartz glass cylinder of the present invention is a hollow synthetic quartz glass cylinder having an outer diameter of 200 to 500 mm and a length of 0.7 to 3.5 m, which is obtained by dehydrating and vitrifying the large hollow porous quartz glass base material by chlorine treatment, and which is characterized in that it has an OH group concentration of less than 5 ppm, a chlorine content concentration of 500 ppm or more and 3000 ppm or less, preferably 1000 ppm or more and 2500 ppm or less, and is free of appearance defects caused by cracks in the porous member.
[0062] In the first embodiment of the hollow synthetic quartz glass cylinder, the "maximum-minimum difference" of the chlorine concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder and spaced every 90° in the circumferential direction is preferably within 15% of the average value of the four positions, and more preferably within 10%.
[0063] A second embodiment of the synthetic quartz glass cylinder of the present invention is a hollow synthetic quartz glass cylinder having an outer diameter of 200 to 500 mm and a length of 0.7 to 3.5 m, which is obtained by pre-sintering and vitrifying the large hollow porous quartz glass base material without chlorine treatment, and which is characterized in that the OH group concentration is 50 ppm or more and 500 ppm or less, preferably 100 ppm or more and 300 ppm or less, and is free of appearance defects caused by cracks in the porous member.
[0064] In a second embodiment of the hollow synthetic quartz glass cylinder, the "maximum-minimum difference" of the OH group concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder and spaced every 90° in the circumferential direction is preferably within 15% of the average value of the four positions, and more preferably within 10%.
[0065] The third embodiment of the synthetic quartz glass cylinder of the present invention is a hollow synthetic quartz glass cylinder obtained by vitrifying the third embodiment of the hollow porous quartz glass base material, characterized in that the "maximum-minimum difference" of the chlorine concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, every 90° in the circumferential direction, is 10% or less of the average value of the four positions. The OH group concentration of the synthetic quartz glass cylinder is preferably less than 5 ppm, and more preferably does not substantially contain OH groups. Note that "substantially does not contain OH groups" means that the content of OH groups in the synthetic quartz glass cylinder is 0 ppm or more and less than 1 ppm. The method for vitrifying the hollow porous quartz glass base material is not particularly limited, and any known method can be used, but a method in which the base material is dehydrated and sintered to obtain a synthetic quartz glass cylinder is preferred, and a method in which the base material is dehydrated in a chlorine atmosphere and then sintered to obtain a synthetic quartz glass cylinder is even more preferred.
[0066] The fourth embodiment of the synthetic quartz glass cylinder of the present invention is a hollow synthetic quartz glass cylinder obtained by vitrifying the hollow porous quartz glass base material of the third embodiment, characterized in that the "maximum-minimum difference" of the OH group concentration at four positions equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, every 90° in the circumferential direction, is 10% or less of the average value of the four positions. It is preferable that the synthetic quartz glass cylinder is substantially free of chlorine. Note that "substantially free of chlorine" means that the chlorine content in the synthetic quartz glass cylinder is 0 ppm or more and less than 20 ppm. The method for vitrifying the hollow porous quartz glass base material is not particularly limited, and any known method can be used, but a method in which the base material is dehydrated and sintered into a synthetic quartz glass cylinder, or a method in which the base material is pre-sintered and vitrified into a synthetic quartz glass cylinder, is preferred, and a method in which the base material is dehydrated by heating without being chlorinated, and then sintered into a synthetic quartz glass cylinder is more preferred.
[0067] Conventionally, when the size is increased and the rotation speed is set to be constant during the growth of the soot body, there was a problem that if dehydration treatment is performed in a chlorine atmosphere during the manufacture of a synthetic quartz glass cylinder, the chlorine content concentration distribution in the circumferential direction of the synthetic quartz glass cylinder becomes non-uniform, and if dehydration is performed by heating without chlorine treatment, the OH group content concentration distribution in the circumferential direction of the synthetic quartz glass cylinder becomes non-uniform. However, in the method of the present invention, by using a hollow porous quartz glass base material obtained under conditions in which the γ is set to 0.3 or less, it is possible to obtain an extremely homogeneous synthetic quartz glass cylinder in which the chlorine content concentration distribution is small even when dehydration treatment is performed in a chlorine atmosphere, and the difference in the OH group content concentration distribution is small even when dehydration is performed by heating without chlorine treatment.
[0068] Such extremely homogeneous synthetic quartz glass cylinders are particularly suitable as materials for optical applications, optical fiber applications, and materials for quartz glass jigs and lamps used in semiconductor manufacturing equipment. In particular, it was found that if the difference between the maximum and minimum values of the chlorine concentration distribution at each of the four points in the circumferential direction inside the cylinder cross section is within 15% of the average value of the four points, there is no effect on the characteristics of the optical fiber, including fiber curl.
[0069] The chlorine content distribution of a synthetic quartz glass cylinder that has been dehydrated and sintered to transparency in a chlorine atmosphere is preferably such that the difference between high and low concentrations in four directions around the circumference of the cylinder is 300 ppm or less, more preferably 200 ppm or less.
[0070] The distribution of OH group concentration in a synthetic quartz glass cylinder that has been dehydrated by heating without chlorine treatment is preferably such that the difference between the high and low OH group concentrations in the four circumferential directions of the cylinder is 50 ppm or less, and more preferably 25 ppm or less. EXAMPLES
[0071] Example 1 In the so-called OVD method, in which a plurality of burners for synthesizing glass particles are arranged at regular intervals, a row of burners is moved back and forth (swinged) relative to a rotating target [ceramic tube with an outer diameter (OD) of 50 mm], glass particles are deposited in layers on the target, and a glass particle deposit body is produced, a soot body is produced under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 140 mm / min (constant), and a surface peripheral speed of 11 m / min (constant), and the target is removed from the soot body to obtain a hollow porous quartz glass base material. The production conditions are shown in Table 3, the results of the obtained hollow porous quartz glass base material are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Tables 5 and 6, respectively.
[0072] [Table 3]
[0073] If the soot body is grown from a target OD of 50 mm to an outer diameter (OD) of 400 mm, the rotation speed will be slowed down from 70.1 rpm to 8.8 rpm under the above conditions. The minimum rotation speed N m is 8.8 rpm and γ = S / (L N m )=0.16. As a result, although there was slight vibration during growth of the equipment, growth proceeded without any problems, and there were no cracks in the soot body. A large hollow porous quartz glass preform (soot body) with an outer diameter of 400 mm, a total axial length of 3,500 mm, and a weight of 247 kg was successfully created.
[0074] The average density and density variation of the obtained soot body were measured. The density variation was calculated by calculating the density per unit length at four points (a to d) at X = 105 mm in Figure 6, defining the difference between the maximum and minimum density values at the four points (a to d) as the density variation amount, and calculating the ratio to the average value of the four points.
[0075] [Table 4]
[0076] The average density of the entire soot body is 0.57 g / cm 3 The density variation per unit length at four points 105 mm from the inner surface in four directions was 4.4% / cm relative to the average value of the four points, and a hollow porous quartz glass preform with extremely small density variation was obtained.
[0077] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The chlorine concentration was measured in each of the four directions by fluorescent X-ray analysis. The analytical device used for measuring the chlorine concentration was a fluorescent X-ray analyzer SPECTRO MIDEX manufactured by Spectro (lower detection limit of the device: chlorine concentration 20 ppm). The OH group concentration (OH group) was measured by FT-IR analysis. The analytical device used for measuring the OH group concentration was a Fourier transform infrared spectrometer Nicolet iS10 FT-IR manufactured by Thermo Fisher Scientific (lower detection limit of the device: OH group concentration 1 ppm). The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum values of the chlorine concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and the ratio to the average value of the four points was calculated. The results are shown in Table 5.
[0078] [Table 5]
[0079] The chlorine concentration was measured in four circumferential directions of the cylinder, and was found to be 1540-1720 ppm. The difference in the four directions was small, at a maximum of 180 ppm, and the variation in the average value of the four directions was 10.9%, resulting in a homogeneous concentration. The OH group concentration (OH group) was less than 1 ppm.
[0080] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. The results are shown in Table 6.
[0081] [Table 6]
[0082] When the OH group concentration was measured in four directions around the cylinder, it was found to be 230 to 255 ppm, with a small difference of a maximum of 25 ppm between the four directions, and the variation from the average value of the four directions was 10.2%, showing uniformity. The chlorine concentration was less than 20 ppm.
[0083] Example 2 A hollow porous quartz glass preform was obtained in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 200 mm / min (constant), and a surface peripheral speed of 9 m / min (constant), and the target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Tables 5 and 6, respectively.
[0084] If the target OD is to grow from 50 mm to 400 mm, the rotation speed will be slowed down from 57.3 rpm to 7.2 rpm under the above conditions. The minimum rotation speed N m is 7.2 rpm, so γ = 0.28. As a result, the growth was possible without any vibrations during the growth of the equipment, there were no cracks in the soot body, and a large hollow porous quartz glass preform with an outer diameter of 400 mm, a total length of 3500 mm, and a weight of 247 kg was successfully created.
[0085] The average density and density variation of the entire soot body obtained were measured. The density variation was calculated by calculating the density per unit length at four points of X=105 mm in Figure 6. The average density of the entire soot body was 0.57 g / cm 3 The density variation per unit length at 105 mm from the inner surface in four directions was 3.8% / cm relative to the average value of the four points, and a hollow porous quartz glass base material with extremely small density variation was obtained.
[0086] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum values of the chlorine concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. The chlorine concentration was measured in four circumferential directions of the cylinder, and was found to be 1740-1960 ppm. The difference between the four directions was small, at a maximum of 220 ppm, and the variation from the average value of the four directions was 11.7%, resulting in a homogeneous concentration. The OH group concentration (OH group) was less than 1 ppm.
[0087] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. When the OH group concentration was measured in four directions around the cylinder, it was found to be 225 to 255 ppm, with a small difference of a maximum of 30 ppm between the four directions, and the variation from the average value of the four directions was 12.4%, showing uniformity. The chlorine concentration was less than 20 ppm.
[0088] Example 3 A hollow porous quartz glass preform was obtained in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 600 mm / min (constant), and a surface peripheral speed of 9 m / min (constant), and the target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Table 5.
[0089] If the target OD is to grow from 50 mm to 400 mm, the rotation speed will be slowed down from 57.3 rpm to 7.2 rpm under the above conditions. The minimum rotation speed N m is 7.2 rpm, so γ = 0.84. As a result, the growth was possible without any vibrations during the growth of the equipment, there were no cracks in the soot body, and a large hollow porous quartz glass preform with an outer diameter of 400 mm, a total length of 3500 mm, and a weight of 247 kg was successfully created.
[0090] The average density and density variation of the entire soot body obtained were measured. The density variation was calculated by calculating the density per unit length at four points of X=105 mm in Figure 6. The average density of the entire soot body was 0.57 g / cm 3 The density variation per unit length at 105 mm from the inner surface in four directions was 9.5% / cm relative to the average value of the four points.
[0091] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum chlorine concentrations at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value. The chlorine concentration was measured in four circumferential directions of the cylinder, and the chlorine concentration was 1640 to 2330 ppm. The difference between the four directions was as large as 690 ppm, and the variation from the average value of the four directions was 34.9%, which showed a decrease in homogeneity compared to Examples 1 and 2. The OH group concentration (OH group) was less than 1 ppm.
[0092] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value. When the OH group concentration was measured in four directions in the cylinder circumferential direction, it was found that the OH group concentration was 195 to 255 ppm, the difference between the four directions was as large as 60 ppm at maximum, and the variation from the average value of the four directions was 26.7%, indicating that the homogeneity was lower than in Examples 1 and 2. In addition, the chlorine concentration was less than 20 ppm.
[0093] Example 4 A hollow porous quartz glass preform was obtained in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 200 mm / min (constant), a surface peripheral speed of 9 m / min (constant), and a wobbling shift amount α of 4 mm per swing (the flame irradiation diameter at this time was 28 mm, so the wobbling shift amount was 1 / 7 of the flame irradiation diameter. The flame diameter was measured by image analysis of the flame during the growth of the soot body). The target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Table 5.
[0094] If the target OD is to grow from 50 mm to 400 mm, the rotation speed will be slowed down from 57.3 rpm to 7.2 rpm under the above conditions. The minimum rotation speed N m is 7.2 rpm, so γ = 0.28. As a result, the growth was possible without any vibrations during the growth of the equipment, there were no cracks in the soot body, and a large hollow porous quartz glass preform with an outer diameter of 400 mm, a total length of 3500 mm, and a weight of 247 kg was successfully created. The average density and density variation of the entire soot body obtained were measured. The density variation was calculated by calculating the density per unit length at four points of X=105 mm in Figure 6. The average density of the entire soot body was 0.57 g / cm 3 The density variation per unit length at 105 mm from the inner surface in four directions was 1.6% / cm relative to the average value of the four points, and a hollow porous quartz glass base material with extremely small density variation was obtained.
[0095] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum values of the chlorine concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. The chlorine concentration was measured in four circumferential directions of the cylinder, and the chlorine concentration was 1860 to 1995 ppm. The difference between the four directions was extremely small, at a maximum of 135 ppm, and the variation from the average value of the four directions was 6.9%, resulting in a homogeneous concentration. In addition, the OH group concentration (OH group) was less than 1 ppm.
[0096] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 210 mm, an inner diameter of 45 mm or less, and a length of 3.4 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. When the OH group concentration was measured in four directions around the cylinder, it was found to be 200 to 215 ppm, with a small difference of a maximum of 15 ppm between the four directions, and the variation from the average value of the four directions was also homogeneous at 7.1%. The chlorine concentration was also less than 20 ppm.
[0097] Example 5 A hollow porous quartz glass preform was obtained in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 200 mm / min (constant), and a surface peripheral speed of 13 m / min (constant), and the target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Table 5.
[0098] If the target OD is to grow from 50 mm to 600 mm, the rotation speed will be slowed down from 82.8 rpm to 6.9 rpm under the above conditions. The minimum rotation speed N m is 6.9 rpm, so γ = 0.29. As a result, the growth was possible without any vibrations during the growth of the equipment, there were no cracks in the soot body, and a large hollow porous quartz glass preform with an outer diameter of 600 mm, a total length of 2500 mm, and a weight of 402 kg was successfully created. The average density and density variation of the entire soot body obtained were measured. The density variation was calculated by calculating the density per unit length at four points of X=200 mm in Figure 6. The average density of the entire soot body was 0.57 g / cm 3 The density variation per unit length at a position 200 mm from the inner surface in each of the four directions was 3.7% / cm relative to the average value of the four points, and a hollow porous quartz glass preform with an extremely small density variation was obtained.
[0099] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 350 mm, an inner diameter of 45 mm or less, and a length of 1.9 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum chlorine concentrations at four positions 100 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. The chlorine concentration was measured in four circumferential directions of the cylinder, and the chlorine concentration was 1890 to 2170 ppm. The difference between the four directions was small, at a maximum of 280 ppm, and the variation from the average value of the four directions was 14.1%, resulting in a homogeneous concentration. In addition, the OH group concentration (OH group) was less than 1 ppm.
[0100] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 350 mm, an inner diameter of 45 mm or less, and a length of 1.9 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. When the OH group concentration was measured in four directions around the cylinder, it was found to be 225 to 245 ppm, with a small difference of a maximum of 25 ppm between the four directions, and the variation from the average value of the four directions was also homogeneous at 10.5%. The chlorine concentration was also less than 20 ppm.
[0101] Example 6 A hollow porous quartz glass preform was obtained in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 400 mm / min (constant), and a surface peripheral speed of 9 m / min (constant), and the target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Table 5.
[0102] If the target OD is to be grown from 50 mm to 600 mm, the rotation speed will be slowed down from 57.3 rpm to 4.8 rpm under the above conditions. The minimum rotation speed N m is 4.8 rpm, so γ = 0.84. As a result, the growth was possible without any vibrations during the growth of the equipment, there were no cracks in the soot body, and a large hollow porous quartz glass preform with an outer diameter of 600 mm, a total length of 2500 mm, and a weight of 402 kg was successfully created. The average density and density variation of the entire soot body obtained were measured. The density variation was calculated by calculating the density per unit length at four points of X=200 mm in Figure 6. The average density of the entire soot body was 0.57 g / cm 3 The density variation per unit length at 200 mm from the inner surface in four directions was 8.3% / cm relative to the average value of the four points.
[0103] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 350 mm, an inner diameter of 45 mm or less, and a length of 1.9 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum chlorine concentrations at four positions 100 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. The chlorine concentration was measured in four circumferential directions of the cylinder, and the chlorine concentration was 1725 to 2340 ppm. The difference in the four directions was as large as 615 ppm, and the amount of variation relative to the average value in the four directions was 29.1%, indicating that the homogeneity was lower than in Examples 4 and 5. In addition, the OH group concentration (OH group) was less than 1 ppm.
[0104] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 350 mm, an inner diameter of 45 mm or less, and a length of 1.9 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. When the OH group concentration was measured in four directions in the cylinder circumferential direction, it was found that the OH group concentration was 200 to 250 ppm, the difference between the four directions was relatively large at a maximum of 50 ppm, and the variation from the average value of the four directions was 21.7%, indicating that the homogeneity was lower than in Examples 4 and 5. In addition, the chlorine concentration was less than 20 ppm.
[0105] Example 7 A hollow porous quartz glass preform was obtained in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 200 mm / min (constant), a surface peripheral speed of 13 m / min (constant), and a wobbling shift amount α of 4 mm per swing (the flame irradiation diameter at this time was 28 mm, so the wobbling shift amount was 1 / 7 of the flame irradiation diameter), and the target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4, and the measurement results of the synthetic quartz glass cylinder are shown in Table 5.
[0106] If the target OD is to grow from 50 mm to 600 mm, the rotation speed will be slowed down from 82.8 rpm to 6.9 rpm under the above conditions. The minimum rotation speed N m is 6.9 rpm γ =0.29. As a result, the growth was possible without any vibrations during the growth of the equipment, there were no cracks in the soot body, and a large hollow porous quartz glass preform with an outer diameter of 600 mm, a total length of 2500 mm, and a weight of 402 kg was successfully created. The average density and density variation of the entire soot body obtained were measured. The density variation was calculated by calculating the density per unit length at four points of X=200 mm in Figure 6. The average density of the entire soot body was 0.57 g / cm 3 The density variation per unit length at a position 200 mm from the inner surface in four directions was 1.8% / cm relative to the average value of the four points, and a hollow porous quartz glass preform with extremely small density variation was obtained.
[0107] The obtained hollow porous quartz glass base material was dehydrated and sintered to make it transparent in a chlorine atmosphere to obtain a synthetic quartz glass cylinder with an outer diameter of 350 mm, an inner diameter of 45 mm or less, and a length of 1.9 m. The obtained synthetic quartz glass cylinder had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the chlorine concentration was measured by measuring the difference between the maximum and minimum chlorine concentrations at four positions 100 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. The chlorine concentration was measured in four circumferential directions of the cylinder, and the chlorine concentration was 1770 to 1935 ppm. The difference in the four directions was small, at a maximum of 165 ppm, and the variation from the average value of the four directions was 8.8%, resulting in a homogeneous concentration. In addition, the OH group concentration (OH group) was less than 1 ppm.
[0108] Furthermore, a soot body produced under the same conditions was dehydrated by heating without chlorine treatment, and then sintered and clarified to obtain a synthetic quartz glass cylinder with an outer diameter of 350 mm, an inner diameter of 45 mm or less, and a length of 1.9 m. The synthetic quartz glass cylinder obtained had a good appearance without any defects caused by cracks in the porous member. The chlorine concentration and OH group concentration of the obtained quartz glass cylinder were measured. The fluctuation of the OH group concentration was measured by measuring the difference between the maximum and minimum values of the OH group concentration at four positions 50 mm from the inner surface of the cylindrical cross section at 90° intervals in the circumferential direction, and calculating the ratio to the average value of the four points. When the OH group concentration was measured in four directions around the cylinder, it was found to be 205 to 225 ppm, with a maximum difference of 20 ppm in the four directions, and the variation from the average value in the four directions was also small at 9.4%, indicating homogeneity. The chlorine concentration was also less than 20 ppm.
[0109] Comparative Example 1 A hollow porous quartz glass base material was manufactured in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 140 mm / min (constant), and a surface peripheral speed of 18 m / min (constant).
[0110] When growing the soot body from a target OD of 50 mm to an OD of 400 mm, under the above conditions, the rotation speed would be slowed down from 114.6 rpm to 14.3 rpm. However, when the soot body OD exceeded 200 mm, the equipment began to vibrate, and when it exceeded 250 mm, the vibrations became so strong that production was stopped midway and it was not possible to continue production up to OD 400.
[0111] Comparative Example 2 A hollow porous quartz glass preform was manufactured in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 800 mm / min (constant), and a surface peripheral speed of 9 m / min (constant), and the target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4.
[0112] If the target OD is to grow from 50 mm to 400 mm, the rotation speed will be slowed down from 57.3 rpm to 7.2 rpm under the above conditions. The minimum rotation speed N m The rotation speed was 7.2 rpm, and γ was 1.12. As a result, the growth was possible without any vibration during the growth of the device, but when the soot body OD reached about 300 mm, a crack occurred in the soot body, and production could not be continued.
[0113] Comparative Example 3 A hollow porous quartz glass preform was manufactured in the same manner as in Example 1, except that the manufacturing conditions were changed as shown in Table 3. That is, a soot body was manufactured under the conditions of a burner interval of 100 mm, a swing distance L of 100 mm, a swing speed S of 800 mm / min (constant), a surface peripheral speed of 9 m / min (constant), and a wobbling shift amount α of 4 mm per swing (the flame irradiation diameter at this time was 28 mm, so the wobbling shift amount was 1 / 7 of the flame irradiation diameter. The flame diameter was measured by image analysis of the flame during the growth of the soot body). The target was extracted from the soot body to obtain a hollow porous quartz glass preform. The results of the obtained hollow porous quartz glass preform are shown in Table 4.
[0114] If the target OD is to grow from 50 mm to 400 mm, the rotation speed will be slowed down from 57.3 rpm to 7.2 rpm under the above conditions. The minimum rotation speed N m The rotation speed was 7.2 rpm, and γ was 1.12. As a result, the growth was possible without any vibration during the growth of the equipment, but when the soot body OD reached about 350 mm, a crack occurred in the soot body, and production could not be continued. [Explanation of symbols]
[0115] 10: manufacturing equipment, 12: soot body, 14: target, 16: group of burners for synthesizing glass microparticles, 16a: burner for synthesizing glass microparticles, 18: swing and up and down movement device for the group of burners for synthesizing glass microparticles, 20: target holding and rotating mechanism, 22: burner flame, d: flame irradiation diameter, L: swing distance, b: burner spacing, α: wobbling shift amount.
Claims
1. a step of arranging a plurality of burners for synthesizing glass particles at a predetermined interval, reciprocating the burners, and depositing glass particles on a rotating target to grow a soot body; extracting the target from the soot body to produce a hollow porous quartz glass base material; A method for producing a hollow porous quartz glass base material, comprising: A method for producing a hollow porous quartz glass base material, characterized in that the rotational peripheral speed of the soot body is controlled to be virtually constant by varying the rotation speed of the soot body based on the outer diameter of the soot body which varies during growth, and the frequency coefficient γ calculated by the following formula (1) is set to be within the range of the following formula (2) in the range in which the outer diameter of the soot body exceeds 250 mm. γ=S / (L・N) m )・・・(1) 0.13≦γ<1.0 (2) [In the formula (1), S is the moving speed of the burner (mm / min), L is the moving distance of the burner (mm), N m is the minimum value (rpm) of the rotational speed of the soot body.
2. A method for manufacturing a hollow porous quartz glass base material as described in claim 1, characterized in that the turning point in the reciprocating movement of the burner is moved by a predetermined distance, and the amount of movement of the turning point in one reciprocating movement of the burner is less than 1 / 3 of the flame diameter of the burner irradiated to the soot body.
3. 3. The method for producing a hollow porous quartz glass base material according to claim 1, wherein the frequency coefficient γ is 0.13 or more and 0.3 or less.
4. A method for producing a synthetic quartz glass cylinder, comprising using a hollow porous quartz glass base material obtained by the method according to any one of claims 1 to 3.
5. A large cylindrical hollow porous quartz glass base material having an outer diameter exceeding 300 mm and a length of 2 m or more, the average density of the entire base material being 0.55 g / cm 3 A large hollow porous quartz glass base material characterized in that, when the density variation is defined as the difference between the maximum and minimum density values per cm3 at four points equidistant (X mm) from the inner surface in the radial direction on four perpendicular lines every 90° on the cylindrical cross section, the density variation per unit length at a distance (X mm) from the inner surface is 10% / cm or less of the average value of the four points and that it does not contain cracks.
6. A large cylindrical hollow porous quartz glass base material having an outer diameter of 500 mm or more and a length of 1.0 m or more, the average density of the entire base material being 0.55 g / cm 3 A large hollow porous quartz glass base material characterized in that, when the density variation is defined as the difference between the maximum and minimum density values per cm3 at four points equidistant (X mm) from the inner surface in the radial direction on four perpendicular lines every 90° on the cylindrical cross section, the density variation per unit length at a distance (X mm) from the inner surface is 10% / cm or less of the average value of the four points and that it does not contain cracks.
7. 7. The hollow porous quartz glass base material according to claim 5 or 6, wherein the density variation per unit length at a distance (X mm) from the inner surface is 2% / cm or less of the average value of the four points, when the density variation is defined as the difference between the maximum and minimum density per cm3 at four points equidistant (X mm) from the inner surface in the radial direction on four perpendicular lines every 90° on the cylindrical cross section.
8. A hollow synthetic quartz glass cylinder obtained by vitrifying the hollow porous quartz glass base material according to any one of claims 5 to 7, A hollow synthetic quartz glass cylinder having an outer diameter of 200 to 500 mm, a length of 0.7 to 3.5 m, an OH group concentration of less than 5 ppm, a chlorine content concentration of 500 ppm to 3000 ppm, and no external defects.
9. A hollow synthetic quartz glass cylinder according to claim 8, characterized in that the "difference between the maximum value and the minimum value" of the chlorine concentration at four positions every 90° in the circumferential direction, which are equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, is within 15% of the average value of the four positions.
10. A hollow synthetic quartz glass cylinder obtained by vitrifying the hollow porous quartz glass base material according to any one of claims 5 to 7, A hollow synthetic quartz glass cylinder having an outer diameter of 200 to 500 mm, a length of 0.7 to 3.5 m, an OH group concentration of 50 ppm to 500 ppm, and no external defects.
11. A hollow synthetic quartz glass cylinder according to claim 10, characterized in that the "difference between maximum and minimum values" of OH group concentrations at four positions every 90° in the circumferential direction, equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, is within 15% of the average value of the four positions.
12. A hollow synthetic quartz glass cylinder obtained by vitrifying the hollow porous quartz glass base material according to claim 7, A hollow synthetic quartz glass cylinder, characterized in that the "difference between the maximum value and the minimum value" of the chlorine concentration at four positions every 90° in the circumferential direction, which are equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, is 10% or less of the average value of the four positions.
13. A hollow synthetic quartz glass cylinder obtained by vitrifying the hollow porous quartz glass base material according to claim 7, A hollow synthetic quartz glass cylinder, characterized in that the "difference between maximum value and minimum value" of OH group concentration at four positions every 90° in the circumferential direction, which are equidistant from the inner surface of the cylindrical cross section of the hollow synthetic quartz glass cylinder, is 10% or less of the average value of the four positions.
Citation Information
Patent Citations
Production of matrix for optical fiber preform
JP1991228845A
Method for manufacturing quartz glass body
JP2001504426A
Method of producing optical fiber preform
JP2002167228A
Method for producing glass fine particle deposited body
JP2013043810A
High-purity synthetic silica and products such as jigs manufactured from high-purity synthetic silica.