Semiconductors on diamond substrates, precursors used in the preparation of semiconductors on diamond substrates, and methods for their manufacture - Patents.com

By forming a sacrificial carrier and nucleation layer with low dislocation density, the method enhances heat transfer in semiconductor-on-diamond substrates, addressing inefficiencies in existing technologies and improving thermal resistance.

JP7555332B2Active Publication Date: 2024-10-01UNIV OF BRISTOL
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021511614
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-31
Filing Date
2019-08-23
Publication Date
2024-10-01
Estimated Expiration
2039-08-23

AI Technical Summary

Technical Problem

Existing semiconductor wafers are limited in efficiency and capacity due to inadequate heat extraction, with diamond being a suitable candidate for improving heat transfer but requiring improved methods for nucleating and growing diamond layers on semiconductor devices.

Method used

A method involving the formation of a sacrificial carrier layer, a single crystal nucleation layer, and a device layer on a base substrate, followed by selective removal and diamond growth, ensuring lattice matching and low dislocation density to enhance heat transfer properties.

Benefits of technology

The method results in improved semiconductor-on-diamond substrates with reduced thermal resistance and enhanced heat transfer capabilities, surpassing conventional techniques by providing a better nucleation surface for diamond growth and maintaining high thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555332000004
    Figure 0007555332000004
  • Figure 0007555332000005
    Figure 0007555332000005
  • Figure 0007555332000006
    Figure 0007555332000006
Patent Text Reader

Abstract

The present invention provides a method 100 for producing a precursor 105a for use in producing a semiconductor-on-diamond substrate 110. The method includes: a) Start with the base substrate 112. b) forming a sacrificial carrier layer 114 on the base substrate, the sacrificial carrier layer comprising a single crystal semiconductor; c) forming a single crystal nucleation layer 116 on the sacrificial carrier layer, the single crystal nucleation layer being arranged to nucleate diamond growth; d) forming a device layer 118 on the single crystal nucleation layer, the device layer comprising a single crystal semiconductor layer or layers;
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to semiconductor-on-diamond substrates, precursors for use in preparing semiconductor-on-diamond substrates, and methods of making same. [Background technology]

[0002] Semiconductor wafers are used to manufacture components for electronic devices such as power, RF and microwave devices, as well as optical instruments such as light emitting diodes and laser diodes. Such devices are limited in efficiency and capacity by how much waste heat can be extracted from them. Diamond is a suitable candidate for heat extraction, especially for use as a heat transfer layer in such wafers.

[0003] FIG. 1 shows, in a schematic manner, a known method for fabricating semiconductors on diamond substrates 10. The substrate fabrication method begins with the provision of a growth structure including a Si (or other) substrate 12, on which one or more transition layers 14 are provided, on which a semiconductor device layer 16, such as a GaN device layer, which may include various epilayers such as GaN, AlGaN, InGaN, etc., is provided. The device layer is arranged such that electrical circuits are formed thereon, for example by deposition, removal, patterning, or modification of electrical properties. The transition layer 14 is arranged to provide some lattice or strain matching between the Si substrate 12 and the semiconductor device layer 16.

[0004] In step 40, the handle wafer 18 is attached to the device layer 16. This typically includes an attachment layer such as spin-on glass, or in other embodiments, attachment is provided by a wafer bond interface.

[0005] In step 42, the Si substrate 12 is removed.

[0006] In step 44, the or each transition layer 14 is removed.

[0007] In step 46, an amorphous nucleation layer 20 is deposited on the semiconductor device layer 16 on its exposed side, the side opposite to the side to which the handle wafer 18 is attached. The amorphous nucleation layer 20 is positioned to allow for the nucleation and growth of diamond.

[0008] In step 48 , a diamond layer 22 is grown on the amorphous nucleation layer 20 .

[0009] In step 50, the handle wafer 18 is removed. After removing the handle wafer 18, the semiconductor on diamond substrate 10 is provided. The exposed surface of the semiconductor device layer 16 can be prepared for further processing, for example by cleaning, for example to remove protective layers. The semiconductor on diamond substrate structure 10 is then available for processing of high-end RF and other devices. [Prior art documents] [Non-patent literature]

[0010] [Non-Patent Document 1] http: / / www.ioffe.ru / SVA / NSM / Semicond / Summary of the Invention [Means for solving the problem]

[0011] According to one aspect, the present invention provides a method of producing a precursor for use in producing a semiconductor-on-diamond substrate, the method comprising: a) Start with the base substrate. b) forming a sacrificial carrier layer over the base substrate, the sacrificial carrier layer comprising a single crystal semiconductor; c) forming a single crystal nucleation layer on the sacrificial carrier layer, the single crystal nucleation layer positioned to nucleate diamond growth. d) forming a device layer on the single crystal nucleation layer, the device layer comprising a single crystal semiconductor layer or a plurality of single crystal semiconductor layers;

[0012] Advantageously, the method of the present invention results in improved precursors, and subsequently results in better or more efficient production of final semiconductors on diamond substrates, compared to the prior art.The precursor is better because of how it is formed according to the method of the present invention.In particular, as will become clear, the surface interface between layers of precursor and at the exposed surface of precursor is better than that of conventional wafers for their subsequent intended use (use in combination with forming a suitable surface for nucleating diamond growth and providing a suitable device layer surface).

[0013] The method optionally includes successively growing a sacrificial carrier layer, then a nucleation layer, then a device layer to achieve steps b) through d). Optionally, the successive growing includes performing steps b) through d) in a growth chamber and not removing the produced precursor from the growth chamber while performing steps b) through d).

[0014] Optionally, the step of forming a monocrystalline nucleation layer comprises depositing the nucleation layer via 2D growth or 3D growth or layer-by-layer growth, preferably by 2D or layer-by-layer growth.

[0015] Optionally, successively growing includes reasonably lattice matching the sacrificial carrier layer with the single crystal nucleation layer, and the single crystal nucleation layer with the device layer.

[0016] This method optionally includes the following: Step b) is 10 9 cm -2 The method includes forming a single crystal sacrificial carrier layer having a dislocation density below a first threshold dislocation density, such as Step c) is 0.5×10 9 cm -2and forming a single crystal nucleation layer having a dislocation density less than a second threshold dislocation density, such as Step d) is 10 8 cm -2 and forming a single crystal device layer having a dislocation density below a third threshold dislocation density, such as

[0017] Optionally, after step a) and before step b), the method includes forming one or more transition layers between the base substrate and the sacrificial carrier layer, the one or more transition layers positioned to facilitate a transition from the base substrate to the sacrificial carrier layer, and optionally, promoting the transition includes relieving strain or nucleation growth, or both, in the sacrificial carrier layer.

[0018] The method optionally includes bonding or forming a handle layer on the device layer.

[0019] The method optionally includes removing the base substrate, and further optionally includes removing the base substrate by chemical or mechanical polishing, or by a combination thereof.

[0020] Optionally, the method includes selectively removing one or more transition layers, such as by selectively etching.

[0021] Optionally, the method includes selectively removing, such as by selectively etching, the sacrificial carrier layer, the selective removal process stopping at the nucleation layer or the transition layer.

[0022] Optionally, step b) includes forming a sacrificial carrier layer from a first material such that the sacrificial carrier layer has a first removal rate, and step c) includes forming a nucleation layer from a second material such that the nucleation layer has a second removal rate, where the first removal rate is different from the second removal rate.

[0023] According to another aspect, a method for manufacturing a semiconductor-on-diamond substrate is provided, the method comprising the method of the above aspect, further comprising growing a diamond layer, such as a synthetic diamond layer, on the nucleation layer after selectively removing the sacrificial carrier layer.Optionally, the method comprises pretreating the nucleation layer with plasma or the like before growing the diamond layer thereon.Further optionally, the method comprises pretreating the nucleation layer by treating the nucleation layer with N2 and / or H2 plasma for a period of time in the case of an AlN nucleation layer.

[0024] The method optionally includes removing, optionally selectively removing, the handle layer.

[0025] Optionally, step d) includes forming the device layer from a third material such that the device layer has a third removal rate, and bonding or forming the handle layer includes bonding or forming the handle layer with a fourth material such that the handle layer has a fourth removal rate, where the fourth removal rate is different from the third removal rate.

[0026] The method optionally includes one or more of the following:

[0027] The base substrate includes a Si substrate, a SiC substrate, an AlN composite, or a sapphire substrate.

[0028] The single crystal sacrificial carrier layer includes SiC, GaN, AlN, InN, AlGaN, InGaN, BN, BAlN, ScN, Si and alloys thereof, Ga2O3, Al2O3, MgO and alloys thereof, and optionally has a thickness greater than 100 nm.

[0029] The single crystal nucleation layer comprises an oxide-based material such as SiC, GaN, AlN, AlGaN, ScN, BN, HfN, ZrN, InN, Si, Ge, TiN or alloys thereof, and Ga2O3, Al2O3, MgO and alloys thereof, and optionally and / or having a thickness of 5 nm to 100 nm, such as 5 nm to 50 nm; The thermal conductivity is 5 to 600 W / mK.

[0030] The single crystal device layers include SiC, GaN, AlN, InN, BN, Si and their alloys, Ga2O3, Al2O3, MgO and their alloys, or multi-layer structures such as 25 nm AlGaN on a GaN layer, or a 3 nm GaN-20 nm AlGaN-GaN layer, or a combination of GaN-InGaN-GaN layers, optionally having a thickness of up to 5000 nm.

[0031] The one or more transition layers may include one or more of SiC, AlN, GaN, AlGaN or AlGaN / AlGaN, BN, Si and alloys thereof, Ga2O3, Al2O3, MgO and alloys thereof, e.g. AlN or AlGaN layers with thicknesses of 5 nm to 200 nm are grown in a 3D form on SiC or sapphire substrates for the subsequent growth of GaN sacrificial carrier layers. An AlN transition layer is grown on a Si substrate, followed by a GaN / AlN superlattice transition layer, for subsequent growth of a GaN sacrificial carrier layer. An AlN transition layer is grown on a Si substrate, followed by an AlN / AlGaN / GaN graded alloy transition layer for subsequent growth of a GaN sacrificial carrier layer.

[0032] According to another aspect, the present invention provides a layered precursor for subsequent use in preparing a semiconductor-on-diamond substrate, the precursor comprising, in sequence, a base substrate, a sacrificial single crystal semiconductor carrier layer, a single crystal nucleation layer, nucleating diamond growth, a single crystal semiconductor device layer or a semiconductor device multilayer structure.

[0033] Optionally, the layered precursor further includes one or more transition layers between the base substrate and the sacrificial carrier layer, the one or more transition layers positioned to facilitate a transition from the base substrate to the sacrificial carrier layer, and optionally, promoting the transition includes relieving strain or nucleation growth, or both, in the sacrificial carrier layer.

[0034] The layered precursor optionally comprises any one or more of the following:

[0035] The base substrate includes a Si substrate, a SiC substrate, an AlN composite, or a sapphire substrate.

[0036] The single crystal sacrificial carrier layer includes SiC, GaN, AlN, InN, AlGaN, InGaN, BN, BAlN, ScN, Si and alloys thereof, Ga2O3, Al2O3, MgO and alloys thereof, and optionally has a thickness greater than 100 nm.

[0037] The single crystal nucleation layer comprises an oxide-based material such as SiC, GaN, AlN, AlGaN, ScN, BN, HfN, ZrN, InN, Si, Ge, TiN or alloys thereof, and Ga2O3, Al2O3, MgO and alloys thereof, and optionally and / or having a thickness of 5 nm to 100 nm, such as 5 nm to 50 nm; The thermal conductivity is 5 to 600 W / mK.

[0038] the single crystal device layer comprises SiC, GaN, AlN, InN, BN, Si and alloys thereof, Ga2O3, Al2O3, MgO and alloys thereof, or the semiconductor device multi-layer structure comprises a multi-layer structure such as 25 nm AlGaN on a GaN layer, or a 3 nm GaN-20 nm AlGaN-GaN layer, or a combination of GaN-InGaN-GaN layers, optionally having a thickness of up to 5000 nm; The one or more transition layers may include one or more of SiC, AlN, GaN, AlGaN or AlGaN / AlGaN, BN, Si and alloys thereof, Ga2O3, Al2O3, MgO and alloys thereof, e.g. AlN layers with thicknesses of 5 nm to 200 nm are grown in a 3D morphology on SiC or sapphire substrates for the subsequent growth of GaN sacrificial carrier layers. An AlN transition layer is grown on a Si substrate, followed by a GaN / AlN superlattice transition layer, for subsequent growth of a GaN sacrificial carrier layer.

[0039] On a Si substrate, an AlN transition layer is grown followed by an AlN / AlGaN / GaN graded alloy transition layer for GaN sacrificial carrier layer growth.

[0040] The layered precursor optionally comprises: The single crystal sacrificial carrier layer has a dislocation density less than a first threshold dislocation density of 10 9 cm -2 and the dislocation density is The single crystal nucleation layer is 0.5 × 10 9 cm -2 and having a dislocation density less than a second threshold dislocation density, such as The single crystal device layer or the semiconductor device multilayer structure is 8 cm -2 and so on, having a dislocation density below a third threshold dislocation density.

[0041] According to another aspect, the present invention provides a semiconductor substrate on diamond, comprising a single crystal device layer or semiconductor device multilayer structure, a single crystal nucleation layer arranged to nucleate diamond growth, and a diamond layer having an interfacial thermal resistance. The distance between the device layer or semiconductor device multilayer structure and the diamond layer is improved compared to previous systems. Improved results achievable using the present invention are specified in Table 1 of the following description. [Brief description of the drawings]

[0042] The invention will now be described, by way of example only, with reference to the accompanying drawings in which: [Figure 1] FIG. 1 (PRIOR ART) illustrates a schematic diagram of a known technique for forming a semiconductor on a diamond substrate. [Diagram 2] FIG. 1 shows a schematic diagram of a method for forming a semiconductor on a diamond substrate, including a method for forming a precursor, according to one embodiment of the present invention. [Diagram 3] FIG. 2 shows a schematic diagram of a method for forming a semiconductor on a diamond substrate, including a method for forming a precursor according to another embodiment of the present invention. [Figure 4] FIG. 2 shows a schematic diagram of a method for forming a semiconductor on a diamond substrate, including a method for forming a precursor according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] In one embodiment, the present invention provides a method 100 for forming a semiconductor on a diamond substrate 110. The first part of the method 100 includes a method 100a for producing a precursor 105a for subsequent use in producing a semiconductor on the diamond substrate 110. Advantageously, the method 100a of the present invention results in an improved precursor 105a, which subsequently results in a better or more efficiently produced final semiconductor on the diamond substrate 110 compared to the prior art. The precursor 105a is better because of how it is formed according to the method 100a of the present invention. In particular, as will become clear, the surface boundaries between layers of the precursor 105a and at the exposed surface of the precursor 105a are better than conventional wafers due to their subsequent intended use (use of the combination of forming a suitable surface for nucleating diamond growth and providing a suitable device layer surface).

[0044] The method 100a of manufacturing the precursor 105a begins by starting with a base substrate 112. The base substrate may comprise any suitable material that can be used for the growth of subsequent layers. The base substrate may comprise any one of a Si substrate, a SiC substrate, a GaN substrate, an AlN substrate, an AlN composite, or a sapphire substrate. Alternatives include oxide-based substrates such as Ga2O3, MgO, etc. SiC substrates typically provide the highest quality GaN layer, but Si or AlN composite substrates significantly reduce manufacturing costs at the expense of a slightly increased defect density in the GaN layer.

[0045] The next step in the method 100 a includes forming a sacrificial carrier layer 114 on the base substrate 112 .

[0046] There are multiple known methods to form or deposit layers. Layers can be deposited or grown. Two commonly used growth options are metalorganic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE). MOCVD is often used for growth on several large substrates in a single reactor. The experienced reader will be able to use and adapt the standard techniques for layer formation. Different layers and layer compositions, e.g., GaN, AlN, InN, ScN, BN and their alloys, can be created by changing the raw materials or precursors in the growth system, oxide-based layers can also be considered. Other methods such as pulsed laser deposition, sputtering, magnetic sputtering, atomic layer deposition (ALD) (part or all of the epi can be grown in thin layers using this method) can also be used.

[0047] The sacrificial carrier layer 114 comprises a single crystal semiconductor. The sacrificial carrier layer 114 in this embodiment comprises any suitable material that a) adheres to the substrate 112 and b) can be selectively removed relative to the adjacent nucleation layer 116 later in the process (described below). The sacrificial carrier layer 114 comprises one of single crystal GaN, single crystal AlN, single crystal InN, single crystal AIGaN, single crystal InGaN, single crystal BN, single crystal BAlN, and oxide-based materials are also contemplated. In this embodiment, the single crystal sacrificial carrier layer has a thickness greater than 100 nm. However, depending on the etch selectivity, the thickness may be less than 100 nm. When the sacrificial layer and the substrate are the same material, in some embodiments, the growth of the sacrificial layer can be omitted.

[0048] For the purposes of this specification, a single crystal layer means a layer formed substantially from one crystal. It may contain defects such as dislocations, slip planes, point defects, etc., but can also be described as a single crystal layer. The density of said defects is sufficiently low to provide improved thermal transport and growth characteristics compared to conventional techniques. The layer is formed of single or multiple single crystal parts (with or without defects). The advantage of this is that by maintaining the crystallinity, a better quality interface between the layers is provided. It is necessary to have a single crystal layer (or as close as possible through multiple single crystal parts) to seed further single crystal material layers later in the process (which does not include growing a diamond layer).

[0049] If the intermediate layer (nucleation layer) is lattice matched (strained), no additional dislocations will be created in the subsequently grown layers. If instead a lattice-mismatched layer were grown, dislocations would be created that would propagate to the device layers and adversely affect electrical and thermal properties, which is undesirable. Therefore, it is advantageous for the intermediate layer to match the crystal lattice of the layers above and below.

[0050] The single crystal sacrificial carrier layer 114 in this embodiment has a dislocation density that is less than a first threshold dislocation density. In this example, the first threshold dislocation density is less than 10 9 cm -2In some embodiments, the first threshold dislocation density is 10 10 cm -2 and 10 12 cm -2 However, it can be made lower.

[0051] The next step of the method 100a includes forming a monocrystalline nucleation layer 116 on the sacrificial carrier layer 114. The monocrystalline nucleation layer 116 is configured to allow for (at a later stage) diamond nucleation and growth. In particular, in this embodiment, the monocrystalline nucleation layer includes any material suitable for nucleating synthetic diamond growth. The monocrystalline nucleation layer includes any one of AlN, GaN, InN, AlGaN, ScN, BN, HfN, ZrN, Ge or alloys thereof, and includes an oxide-based layer. In other embodiments, the nucleation layer includes metals such as Ir, W, Mo, and Nb. Ir can be grown monocrystalline on a material such as MgO. As previously mentioned, the monocrystalline nature of this layer allows for enhanced bonding (better surface connection and better transition properties) with the adjacent monocrystalline sacrificial carrier layer. The monocrystalline nucleation layer has a thickness of 5 nm to 100 nm, such as 5 nm to 50 nm. In some exemplary embodiments, when the nucleation layer is an AlN layer, there is a potential advantage to relaxing it, as it helps suppress the formation of parasitic lateral leakage channels. This will require some dislocations. However, it is not necessary to significantly increase the density of threading dislocations, as they will bend into the plane of the layer to release the strain. In fact, a relaxed AlN interlayer may be used as a growth tool to reduce the threading dislocation density by bending the dislocations, binding and terminating them, thus reducing the strain. Thus, in such examples, the thickness is 5-8 nm for strained layers, which are thick enough to act as an etch stop, or 8-50 nm for relaxed layers. From a thermal transport perspective, a thin dislocation-free (strained) layer is preferred. This would be in the low 5-8 nm range for the AlN example. A thicker layer containing dislocations (relaxed) would have a higher thermal resistance. In other examples, the use of AlGaN as a nucleation layer may require straining the layer to avoid a large thermal resistance, as the critical thickness before relaxation occurs is thicker.

[0052] The thermal conductivity of the nucleation layer is between 5 and 400 W / (m·K). In some exemplary embodiments, the thermal conductivity is 300 W / (m·K) for AlN nucleation layers, or 400 W / (m·K) for BN nucleation layers (this is the value in the basal plane direction). It is close to 10 W / (m·K) in the through-plane direction (heat flow direction), or 10 W / (m·K) for ScN nucleation layers, or 50 W / (m·K) for ZrN nucleation layers. The higher the thermal conductivity of the material, the better it is for heat transport within the device. It is also important to consider the lattice mismatch between the nucleation layer and the sacrificial carrier layer. Preferably, this should be kept below 15%. However, it is usually only a few percent to minimize extra dislocations introduced into the growth of the nucleation layer.

[0053] In another example, the thermal conductivities based on these bulk thermal conductivity values ​​at 300K are as follows:

[0054] AlN: Approximately 20 W / mK at a thickness of 5 nm, approximately 180 W / mK at a thickness of 100 nm, BN: Approximately 12 W / mK at a thickness of 5 nm, approximately 27 W / mK at a thickness of 100 nm.

[0055] Other examples will be apparent to the skilled reader. Preferably, the single crystal nucleation layer has a dislocation density less than a second threshold dislocation density. In this example, the second threshold dislocation density is less than 0.5x10 9 cm -2 This level may be advantageous for example GaN HEMTs. In some embodiments, the second threshold dislocation density is 0.5×10 10 cm -2 and 0.5x10 11 cm -2 However, it can be lower. For example, when manufacturing for laser diodes or microelectronic applications, the second threshold dislocation density is lower, for example 10 4 cm -2 or 10 8 cm -2 It is possible that.

[0056] Generally, preferably, the dislocation density is reduced by the device structure, but in some cases, it may actually increase in between at one of the layer boundaries. Thus, in some other instances, the second threshold dislocation density may be higher than the first threshold density, because extra dislocations may form due to large strain mismatch. For example, when AlN is grown on a GaN sacrificial layer, as the AlN gets thicker, defects may occur, increasing the defect density. However, as mentioned above, in certain scenarios, if there is bending of dislocations, the defect density may also decrease. In general, it is desirable to keep the defect density low.

[0057] In some examples covered by the present invention, the defect density in the sacrificial layer is 10 8 cm -2 and in the AlN layer is 10 9 cm -2 Even if the dislocation density in the nucleation layer is greater than the dislocation density in the sacrificial carrier layer, the final product can still benefit from the method of the present invention.

[0058] We considered a critical thickness for the nucleation interlayer: AlN can be grown on GaN to a thickness of about 10 nm before strain relaxation occurs. Going thicker than this may not provide significant gains because the relationship between thermal conductivity and thermal conductivity of the layer is nonlinear; that is, the thermal resistance of the layer increases even if the thermal conductivity of the thick layer is high.

[0059] The next step of the method of method 100a includes forming a single crystal device layer 118 on the single crystal nucleation layer 116. The device layer 118 includes a single crystal semiconductor. The device layer 118 is any single crystal semiconductor that achieves the desired effect of providing a suitable surface for forming electrical circuits therein or thereon. The device layer 118 can include any one of GaN, AIN, InN, BN and alloys thereof, and oxide-based materials such as Ga2O3, MgO, and the like. In some embodiments, the single crystal device layer has a thickness of 100 nm to 5000 nm. In other embodiments, the device layer is a multi-layer structure. For example, the device layer is a GaN / AIGaN layer (e.g., this type of layer is suitable for forming transistors). In other embodiments, the device layer is a GaN / InGaN / GaN layer (e.g., this type of layer is useful for light emitting devices). In such an example, each different layer of the multi-layer structure is a single crystal layer. The multi-layer device layers may include, for example, 25 nm AlGaN on a GaN layer, or a combination of 3 nm GaN-20 nm AlGaN-GaN layers or GaN-InGaN-GaN layers, and in some embodiments may also include SiC-based device structures or Ga2O3 and related device structures. The single crystal device layers, in this embodiment, have a dislocation density below the third threshold dislocation density. The third threshold dislocation density in this example is 10 8 cm -2 In other embodiments, the third threshold dislocation density may be lower or higher. Generally, the third threshold dislocation density is 10 10 cm -2 If the dislocation density is greater than 100, the device will not function properly. The present invention helps to more efficiently produce high quality finished devices thanks to improved precursor manufacturing methods with the possibility of adding a nucleation layer to control the dislocation density in the device structure.

[0060] In FIG. 2, the starting structure includes an additional layer between the base substrate 112 and the sacrificial carrier layer 114. In most, but not all, embodiments, a transition layer (or layers) 113 is provided before the sacrificial carrier layer is formed. The transition layer 113 is formed between the base substrate 112 and the sacrificial carrier layer 114. The one or more transition layers 113 are positioned to facilitate a smooth growth transition from the base substrate 112 to the sacrificial carrier layer 114. The transition layer provides strain relief to ensure that the layers grow sufficiently. Facilitating the transition includes relieving strain and / or nucleating growth of the sacrificial carrier layer 114 or both. The transition layer may include any one or more of AIN, GaN, AIGaN or AIGaN / AIGaN, BN or alloys thereof. In some embodiments, the transition layer has a 3D morphology and includes a 5 nm to 200 nm thick AIN or AlGaN layer grown on a SiC or sapphire substrate (for subsequent GaN sacrificial carrier layer growth). In another example, the transition layer includes, on a silicon substrate, an AlN transition layer followed by a GaN / AlN superlattice, a transition layer for subsequent GaN or other material sacrificial carrier layer growth (112). In yet another example, on a Si substrate, the transition layer includes an AlN transition layer followed by an AlN / AlGaN / GaN graded alloy transition layer (used for subsequent GaN sacrificial carrier layer growth). In one example, the transition layer is a very thin, e.g., 10 nm, highly defect dense single crystal semiconductor layer. In some GaN on Si embodiments, the transition layer is as thin as 4 microns. In GaN on SiC embodiments, the transition layer can be between 10 nm and 30 nm. This layer nucleates the growth of the GaN sacrificial carrier layer.

[0061] Alternatively, each transition layer may assist in any one or combination of lattice matching, strain matching, and nucleation between adjacent layers.

[0062] In some embodiments, there is no transition layer between the substrate and the sacrificial carrier layer.

[0063] In this embodiment, the sacrificial carrier layer 114, the nucleation layer 116, and the device layer 118 are grown sequentially on the substrate, or on the substrate and the transition layer. In this example, the sequential growth involves performing the relevant formation steps in a growth chamber and not removing the precursors being fabricated from the growth chamber during the performance of the steps.

[0064] In some embodiments, during production, precursors can be moved from one growth chamber to another under controlled conditions to ensure consistent growth. For example, in two connected growth chambers connected via a vacuum channel, the growth of the precursor can be stopped in one chamber and the precursor moved to the other chamber to continue growth.

[0065] In other embodiments, the precursor 105a may not be grown continuously.

[0066] Successive growth of these layers advantageously provides precursors with good surface matching properties between the layers. Not removing the precursors from the growth chamber during successive growth provides further advantages, such as preventing surface reconstruction or contamination. In conjunction with the use of single crystalline carrier layers, nucleation layers and device layers, precursors with good strain and lattice matching properties are provided.

[0067] In this example, the nucleation layer 116 is deposited by layer-by-layer growth in 2D. In other embodiments, 3D growth can be used. 2D growth of the nucleation layer is preferred to avoid introducing defects in this layer. The 3D growth option can be considered more practical for the growth of the transition layer 113.

[0068] In this example, the successive growth involves a reasonably lattice-matched (in some embodiments, the lattice constants of the two materials differ by less than 15%; preferably less than 1-3%, but more is possible) sacrificial carrier layer lattice-matched to the single crystal nucleation layer, and the single crystal nucleation layer lattice-matched to the device layer. For example, for AlN, the difference in lattice constants can be 2.4%, which allows for an intermediate layer approximately 10 nm thick.

[0069] In this embodiment, the method 100a further includes a step 140 of bonding or forming a handle layer 120 on the device layer 118. The handle layer includes any layer suitable for later gripping the device layer or device at a later stage of the manufacturing process. In some embodiments, spin-on-glass attaches the handle layer to the device layer. The handle layer is also a type of sacrificial layer. Within this specification, a sacrificial layer is a layer that is removed at a later stage of the manufacturing process and is not present in the final semiconductor on the diamond substrate 110. Examples of handle wafers may include Si, GaAs, Ge (although Si is most often used because it is relatively cheap and easy to remove).

[0070] The method 100a further includes a step 142 of removing the base substrate 112. In this example, the base substrate is removed via a chemical or mechanical polishing process, or a combination thereof. This can be a selective or non-selective removal process.

[0071] In embodiments where one or more transition layers 113 are present, the method 100a includes removing step 144 or each transition layer 113. In this example, removal 144 of the transition layer 113 is accomplished by selectively removing, such as by selectively etching the transition layer 113. Selective etching techniques include, for example, reactive ion etching and liquid-based etching using custom gases for the GaN / AIN interface. Selective removal, such as selective etching, for purposes of this specification is the removal of one material from adjacent materials where the materials have significantly different removal rates from one another for a particular removal process. For example, GaN has a significantly different removal rate relative to AIN for a particular gas or liquid, i.e., reactive ion etching or wet etching process, respectively. An example of a liquid-based etch might include KOH under UV irradiation (photon energy > band gap GaN (but smaller than band gap AlN, SiC, BN, etc.)). Selective removal techniques will be apparent to the skilled reader familiar with cleanroom processes.

[0072] In contrast, non-selective removal is accomplished by, for example, mechanical etching or polishing or non-selective chemical processes.

[0073] Method 100a in step 144 includes removing sacrificial carrier layer 114 along with any transition layer 113 that may be present in some embodiments. Following step 144, in this example, precursor 105a is formed (see FIG. 2). In other examples (see FIGS. 3 and 4), the precursor is considered to have been formed at an earlier stage, as discussed in more detail below.

[0074] In this example, the sacrificial carrier layer 114 is formed from a first material such that the sacrificial carrier layer has a first removal rate. The nucleation layer 116 is formed from a second material such that the nucleation layer has a second removal rate. The first removal rate is different from the second removal rate, and a selective removal technique, such as a selective etching removal technique, can be used to cleanly and efficiently remove the sacrificial carrier layer, leaving a good, clean, atomically smooth nucleation layer surface for subsequent diamond growth. Advantageously, the method 100a of the present invention provides such an advantage that is not present in other known methods. This advantage is due to the nature of the growth of an initial monocrystalline layer in the first stage, as shown diagrammatically in FIG. 2. The nucleation layer is sandwiched between the device layer and the sacrificial carrier layer, which has removal properties, such that subsequent selective etching (step 144) is efficiently possible. This arrangement allows for the use of an efficient technique (selective removal) to provide a high quality nucleation surface. It also allows for the fabrication of on-diamond semiconductors, such as GaN device layers, with well-defined thicknesses without the use of timed etching. With the current state of the art, the thickness of the GaN layer in the final product can mostly only be controlled by timed etching. The introduction of selective etching at critical stages is a technological advantage. Avoiding the use of timed etching facilitates manufacturing.

[0075] The method 100 of manufacturing a semiconductor on a diamond substrate 110 further includes step 146 of growing a diamond layer 122 on the nucleation layer 116 after selectively removing the sacrificial carrier layer 114. In this example, the diamond layer comprises a synthetic diamond layer. The diamond layer can be efficiently grown without the need for further preparation of the nucleation surface according to step 144 of this example. In other examples, minimal or no preparation work is required between steps 144 and 146, especially when compared to previous techniques for growing diamond on differently prepared nucleation surfaces.

[0076] In one example, the preparation includes treating the AlN nucleation surface with plasma. The plasma treatment includes treating the AlN nucleation surface with N2 and / or H2 plasma. In one particular case, the treatment includes treating the AlN nucleation layer with 10% N2 / H2 plasma for 10 minutes. This pretreatment is shown by the inventors to increase the oxygen content of the AlN nucleation surface. Such a pretreated surface allows for the growth of a thick diamond layer thereon (in some examples >10 μm, or in some examples >50 μm, or in some examples >100 μm).

[0077] The method 100 further includes a step 148 of removing the handle layer 120. As will be appreciated, up until this stage, the handle layer 120 was required to be treated as a precursor during the manufacturing process to avoid damaging the device layer 118, which is part of the final semiconductor on the diamond substrate 110. In this particular example, the handle layer is removed by a selective removal process. In this example, the device layer 118 is formed from a third material such that the device layer has a third removal rate. The handle layer includes a fourth material such that the handle layer has a fourth removal rate. The fourth removal rate is different from the third removal rate, thus making selective removal of the handle layer from the device layer in step 148 efficient and possible. The semiconductor device layer 118 on the diamond substrate 110 has an exposed surface as shown in FIG. 2. For the selective removal process used in step 148, the exposed surface needs to be treated less (or in some cases, no further treatment of the exposed surface) to prepare it for later use in its role as a device layer.

[0078] In some embodiments, the top surface of the device layer is protected, for example with SiN, prior to attachment of the handle wafer. Once the handle wafer (or spin-on glass used to attach the handle wafer) is removed, this SiN layer (sometimes broadly referred to as a protective layer) is removed prior to device processing on the wafer. This protective layer protects the top surface of the device grade material. In some embodiments, the SiN layer is retained during device fabrication.

[0079] In other embodiments, the precursor 105 may be considered to have been formed at an earlier stage.

[0080] In the example of FIG. 3, the precursor can be considered to be formed prior to removal of the sacrificial carrier layer 114 , ie, before step 144 and after step 142 .

[0081] In the example of FIG. 4, the precursor can be considered to be formed before step 142 and after step 140, ie, before removal of base substrate 112.

[0082] In yet another embodiment, the precursor may be considered to be formed prior to the addition of the handle layer 120 , ie, prior to step 140 .

[0083] In these various examples and embodiments, the initial stage of providing a sandwich nucleation layer with a device layer 118 on one side and a sacrificial carrier layer 114 on the other side provides a useful and technically advantageous starting point for efficiently carrying out the following steps, a method not known from conventional precursors for fabricating semiconductors on diamond substrates.

[0084] Some specific exemplary embodiments of precursor configurations will now be described in more detail. Example 1 Substrate: Si Sacrificial carrier layer = single crystal GaN with an AlGaN-based strain relief layer. Its characteristics are thickness = 1 μm, dislocation density = 109 cm -2 Includes. Nucleation layer = single crystal AlN. Its characteristics are dislocation density = 10 9 cm -2 Includes. Device layer = single crystal GaN with 25 nm of AlGaN on top. Its characteristics are dislocation density = 10 9 cm -2 Includes.

[0085] Example 2 Substrate: SiC Sacrificial carrier layer = Single crystal GaN with AlN nucleation layer. Its characteristics are thickness = 1 μm, dislocation density = 10 8 cm -2 Includes. Nucleation layer = single crystal AlN. Its characteristics are dislocation density = 10 8 cm -2 Includes. Device layer = single crystal GaN with 25 nm of AlGaN on top. Its characteristics are dislocation density = 10 8 cm -2 Includes.

[0086] Example 3 Substrate and sacrificial carrier layer=GaN (a single GaN layer is formed and acts as both the substrate and the sacrificial carrier layer). Nucleation layer = single crystal AlN. Its characteristics are dislocation density = 10 6 cm -2 Includes. Device layer = Single crystal GaN incorporating InGaN quantum wells. Its characteristics are dislocation density = 10 6 cm -2 Includes.

[0087] Example 4 Substrate and sacrificial carrier layer=Ga2O3 (a single Ga2O3 layer is formed and serves as both the substrate and the sacrificial carrier layer). Nucleation layer = single crystal GaAlO. Its characteristics are dislocation density = 10 6 cm -2 Includes. Device layer = single crystal Ga2O3. Its characteristics are dislocation density = 10 6 cm -2 Includes.

[0088] The embodiments of the present invention allow for selective removal back to the nucleation layer. This provides a suitable nucleation surface for diamond growth and improves heat transfer in the final product. The advantage is that the selective etching stops at the nucleation layer, making the fabrication of a single crystal nucleation layer easy to implement. The nucleation layer, being single crystal, has a higher thermal conductivity in some instances (>10 W / mK) than commonly used amorphous nucleation layers such as SiO2 and Si3N4 of the prior art, aiding in the transfer of heat therethrough. Given that the surface of the nucleation layer thus produced is smooth, there is even less phonon scattering due to interface roughness, which can further impede heat transfer.

[0089] In some instances, the inventors have considered the thermal resistance of the interface between the GaN device layers and the diamond substrate.

[0090] Consideration Case (1)-Prior Art: For an amorphous nucleation layer (50 nm thick silicon nitride), the effective thermal resistance of this interface is 5×10 -8 m 2 K / W (this value is proportional to the layer thickness), which for example for an 8-finger, 125 μm wide GaN transistor with a device geometry of 35 μm gate finger spacing, accounts for about 40% of the total thermal resistance at chip level.

[0091] Consideration Case (2): For a GaN transistor with the same 8-finger, 125 μm wide, 35 μm gate finger spacing device geometry, a 10 nm thick crystalline AlN nucleation layer is estimated to have a thermal conductivity of about 20 W / mK (due to the reduced phonon mean free path). -9 m 2 An effective interfacial thermal resistance of K / W is obtained. The intrinsic thermal resistance (phonon mismatch) between GaN and diamond is about 2×10-9 m 2 It is K / W.

[0092] Thus, a thin crystalline AlN nucleation layer (effectively formed according to the present method) does not add appreciably to the thermal resistance of the device, and indeed this is true as long as the thermal conductivity of a 10 nm thick layer is >5 W / mK.

[0093] Comparing case (1), which is an example of the proposed inventive method, with the current state of the art, the inventors reduced the temperature rise on the chip by 40% (excluding packaging thermal resistance etc.).

[0094] The present invention can be used to manufacture components, such as electronic, optical and optoelectronic components.

[0095] As previously mentioned, the present invention allows for efficient fabrication of structures with excellent thermal conduction properties. The present invention provides a semiconductor-on-diamond substrate comprising a single crystal device layer or semiconductor device multi-layer structure, a single crystal nucleation layer arranged to nucleate diamond growth, and a diamond layer, where the thermal resistance of the interface between the device layer or semiconductor device multi-layer structure and the diamond layer is improved compared to conventional systems.

[0096] The inventors have investigated the expected thermal conductivity and thermal boundary resistance properties for the different proposed materials, as summarized in the table below.

[0097]

number

[0098] The thermal conductivity of thin films is calculated using the Landauer model applied to ballistic heat conduction in thin films. The effective phonon mean free path is calculated by multiplying the bulk phonon mean free path (l ph ) and the boundary length (L).

[0099]

number

[0100] The following table gives the thermal conductivity and effective thermal boundary resistance values ​​assuming a defect-free material. Most of these values ​​are taken from "Thermal Conductivity and Effective Thermal Boundary Resistances of Materials 1". Room temperature values ​​are used.

[0101] [Table 1]

[0102] In general, our investigations show that even low thermal conductivity materials such as Ga2O3 do not become a major thermal barrier at a thickness of 50 nm if the layer is free of dislocations / defects. This factor determines the maximum thickness that can be grown.

[0103] As used in this specification and claims, the terms "comprise" and "include" and variations thereof mean that the specified features, steps or integers are included. These terms are not to be interpreted as excluding the presence of other features, steps or components.

[0104] The features disclosed in the foregoing description, or the following claims, or the accompanying drawings, whether expressed in a particular form, or in terms of means for performing a disclosed function, or a method or process for achieving a disclosed result, may, as appropriate, be utilized to realize the invention in various of its forms, either separately or in any combination of such features.

Claims

1. 1. A method for manufacturing a semiconductor-on-diamond substrate, comprising: a) starting with a base substrate; b) forming a sacrificial carrier layer on the base substrate, the sacrificial carrier layer comprising a single crystal semiconductor; c) forming a single crystal nucleation layer on the sacrificial carrier layer, the single crystal nucleation layer arranged to nucleate diamond growth; d) forming a device layer on the single crystal nucleation layer, the device layer comprising a single crystal semiconductor layer or multiple single crystal semiconductor layers; e) removing the base substrate; f) selectively removing the sacrificial carrier layer, the process for selectively removing the sacrificial carrier layer stopping at the single crystal nucleation layer; g) selectively removing the sacrificial carrier layer and then growing a diamond layer on the single crystal nucleation layer; Equipped with Step b) includes forming the sacrificial carrier layer from a first material such that the sacrificial carrier layer has a first removal rate, and step c) includes forming the single crystal nucleation layer from a second material such that the single crystal nucleation layer has a second removal rate, the first removal rate being different from the second removal rate. A method comprising:

2. 2. The method of claim 1, comprising the steps of successively growing the sacrificial carrier layer, then the single crystal nucleation layer, then the device layer to accomplish steps b) to d).

3. 3. The method of claim 2, wherein the step of continuously growing comprises performing steps b) through d) in a growth chamber and not removing the precursor produced from the growth chamber while performing steps b) through d).

4. 4. The method of claim 1, wherein forming the monocrystalline nucleation layer comprises depositing the monocrystalline nucleation layer via 2D growth or 3D growth or layer-by-layer growth.

5. 4. The method of claim 2 or 3, wherein the step of successively growing includes the steps of reasonably lattice-matching the sacrificial carrier layer to the single crystal nucleation layer and reasonably lattice-matching the single crystal nucleation layer to the device layer.

6. Step b) includes forming a single crystal sacrificial carrier layer having a dislocation density less than a first threshold dislocation density of 10 cm; Step c) includes forming a single crystal nucleation layer having a dislocation density less than a second threshold dislocation density of 0.5×10 cm; 6. The method of claim 1, wherein step d) includes forming a single crystal device layer having a dislocation density less than a third threshold dislocation density of 10@8 cm@-2.

7. 7. The method of claim 1 , further comprising, after step a) and before step b), forming one or more transition layers between the base substrate and the sacrificial carrier layer, the one or more transition layers being arranged to facilitate a transition from the base substrate to the sacrificial carrier layer, wherein facilitating the transition comprises strain relaxation or nucleation growth of the sacrificial carrier layer, or both.

8. 8. The method of claim 1, further comprising bonding or forming a handle layer on the device layer.

9. The method of claim 7 including selectively removing the one or more transition layers.

10. The method of claim 8 including the step of removing the handle layer.

11. 11. The method of claim 8 or 10, wherein step d) comprises forming the device layer from a third material such that the device layer has a third removal rate, and wherein bonding or forming the handle layer comprises bonding or forming the handle layer with a fourth material such that the handle layer has a fourth removal rate, the fourth removal rate being different from the third removal rate.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method for the same

    JP2010067662A

  • Direct growth of diamond on back-side vias for GaNHEMT devices

    JP2015517205A

  • HEMT transistor

    JP2018503252A