Inspection method for piezoelectric elements
The use of a slightly adhesive sheet with defined properties stabilizes piezoelectric elements during electrical testing, addressing stress-induced cracks and misalignment, enhancing inspection reliability and yield.
Patent Information
- Application Number
- JP2023037207
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-12
- Filing Date
- 2023-03-10
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2038-09-10
AI Technical Summary
Existing methods for evaluating piezoelectric elements face issues such as stress-induced cracks and unstable contact during electrical characteristic testing due to adhesive sheets or tray-based handling, leading to potential misalignment and inspection failures.
A piezoelectric element testing method using a slightly adhesive sheet with specific physical properties (surface resistance ≥10 Ω, Young's modulus 5.0-10.0 MPa, thermal conductivity ≥0.05 W/mK, holding force 0.50 kgf/cm², and heat resistance ≥90°C) to adhere and hold piezoelectric elements, allowing for stable alignment and displacement during voltage application.
The method ensures stable inspection of piezoelectric elements even under shock conditions, preventing displacement inhibition and improving yield by reducing cracks and misalignment issues.
Smart Images

Figure 0007555443000002 
Figure 0007555443000005 
Figure 0007555443000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for inspecting a piezoelectric element, which evaluates the electrical characteristics of the piezoelectric element. [Background technology]
[0002] Conventionally, in characteristic inspection of piezoelectric elements, a voltage is applied to the piezoelectric element to cause a displacement in the piezoelectric element, thereby evaluating the electrical characteristics of the piezoelectric element (defect inspection, etc.). For example, in Patent Document 1, the electrical characteristics of the piezoelectric elements are evaluated in a state in which a plurality of piezoelectric elements are attached to an adhesive sheet. In Patent Document 2, the piezoelectric elements are placed in recesses in a tray, and the electrical characteristics of the piezoelectric elements are evaluated. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-190457 A [Patent Document 2] JP 2014-181126 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the method described in Patent Document 1, the adhesive sheet prevents the displacement of the piezoelectric element that occurs when a voltage is applied to the piezoelectric element, which increases the stress generated in the piezoelectric element when a voltage is applied, and this stress may cause cracks in the piezoelectric element.
[0005] In the method using the tray described in Patent Document 2, as shown in Fig. 7A, the planar size of the recess 104 must be slightly larger than the planar size of the piezoelectric element 100 so that the piezoelectric element 100 can be easily inserted and removed from the recess 104 of the tray 102. Therefore, the piezoelectric element 100 may be turned upside down or lost during handling due to the shock of transporting the tray 102 between processes or mounting the tray 102 on equipment. In addition, as shown in Fig. 7B, when a voltage is applied to the piezoelectric element 100, the position of the piezoelectric element 100 may be shifted within the recess 104, causing unstable contact between the probe 106 and the terminal 108, which may result in defective inspection.
[0006] The present invention has been made in consideration of the above problems, and has an object to provide a method for inspecting a piezoelectric element which has the following effects. (a) Even if an impact is applied to a tray on which a plurality of piezoelectric elements are aligned and placed, the aligned state of the piezoelectric elements is maintained while a characteristic inspection can be performed. (b) The displacement (deformation) of the piezoelectric element that occurs when a voltage is applied is not impeded. [Means for solving the problem]
[0007] [1] A method for inspecting a piezoelectric element according to the present invention is a method for inspecting a piezoelectric element, which applies a voltage to a piezoelectric element to evaluate the electrical characteristics of the piezoelectric element, comprising a first step of adhering and holding a lower surface of the piezoelectric element on a flat, non-hole-shaped, weakly adhesive sheet, and a second step of applying a voltage to the piezoelectric element held on the weakly adhesive sheet to evaluate the electrical characteristics of the piezoelectric element, the physical property value of the weakly adhesive sheet being a surface resistance of 10 16 ohms or more, Young's modulus 5.0~10.0MPa, thermal conductivity 0.05W / mK or more, retention force 0.50kgf / cm 2 The following is characterized by its heat resistance of 90°C or higher.
[0008] As a result, since the piezoelectric elements are held by the weak adhesive sheet, even if an impact is applied to the tray on which the piezoelectric elements are aligned, the alignment of the piezoelectric elements is maintained and characteristic inspection can be performed without impeding the displacement of the piezoelectric elements that occurs when a voltage is applied.
[0009] [2] In the present invention, the flat-shaped weak adhesive sheet is attached to a base material, and the base material may have at least a flat surface to which the weak adhesive sheet is attached, and the weak adhesive sheet is attached within the surface. This prevents the weak adhesive sheet from being wrinkled or partially turned upside down due to air conditioning, and allows the sheet to stably hold multiple piezoelectric elements. In addition, the material of the base material is preferably made of metal from the viewpoint of processing accuracy and heat conduction during heating, and more preferably aluminum from the viewpoint of heat conduction.
[0010] [3] A method for inspecting a piezoelectric element according to the present invention is a method for inspecting a piezoelectric element, which applies a voltage to a piezoelectric element to evaluate the electrical characteristics of the piezoelectric element, and includes a first step of adhering and holding a lower surface of the piezoelectric element on a flat, slightly adhesive sheet, and a second step of applying a voltage to the piezoelectric element held on the slightly adhesive sheet to evaluate the electrical characteristics of the piezoelectric element, wherein the physical property value of the slightly adhesive sheet is a surface resistance of 10 16 ohms or more, Young's modulus 5.0~10.0MPa, thermal conductivity 0.05W / mK or more, retention force 0.50kgf / cm 2 The following describes a method for manufacturing a micro-adhesive sheet having a heat resistance of 90°C or higher, a flat plate-shaped sheet that is attached to a base material, the base material being made of metal or ceramics, the base material having at least a flat surface to which the micro-adhesive sheet is attached, and the micro-adhesive sheet being attached within the flat surface.
[0011] [4] In the method for inspecting a piezoelectric element of the present invention, the low-pressure adhesive sheet may not have holes.
[0012] [5] In the present invention, the piezoelectric element may have a first terminal and a second terminal formed on an upper surface, the first step may include holding the lower surface of the piezoelectric element opposite the upper surface on the low-adhesive sheet, and the second step may include applying a voltage between the first terminal and the second terminal of the piezoelectric element.
[0013] In the first step, one surface of the piezoelectric element and the opposing other surface are held by the weak adhesive sheet, so that in the second step, a voltage can be applied between the first terminal and the second terminal formed on one surface of the piezoelectric element to perform a characteristic inspection. In other words, the characteristic inspection of the piezoelectric element can be easily performed while the piezoelectric element is held by the weak adhesive sheet.
[0014] [6] In the present invention, the size of the piezoelectric element is preferably 0.2 to 0.4 mm in length, 0.8 to 1.2 mm in width, and 0.05 to 0.2 mm in thickness, so that cracks or the like do not occur in the piezoelectric element during characteristic testing, and yield can be improved.
[0015] [7] In the present invention, the piezoelectric element may generate a distortion of 1500 to 4000 ppm in the d31 direction (direction along the electrode surface) at an electric field of 2.0 to 4.0 kV / mm when a voltage is applied for the characteristic inspection.
[0016] [8] In the present invention, it is preferable that the low-pressure adhesive sheet holds the piezoelectric element and does not inhibit the displacement of the piezoelectric element that occurs when a voltage is applied.
[0017] As a result, even if a distortion of 1500 to 4000 ppm in the d31 direction occurs at an electric field of 2.0 to 4.0 kV / mm when a voltage is applied to the piezoelectric element, the piezoelectric element can be held on the low-adhesive sheet and characteristics inspection can be performed without hindering the displacement occurring in the piezoelectric element.
[0018] [9] In the present invention, the slightly adhesive sheet preferably has a relationship between the thickness ta and the dielectric tangent tan θ that satisfies (a) to (d). (a) When 0.03 mm ≦ ta ≦ 0.05 mm, tan θ ≦ 0.20 (b) 0.05 mm <ta≦0.10mmのとき、tanθ≦0.15 (c) 0.10 mm <ta≦0.20mmのとき、tanθ≦0.10 (d) 0.20 mm <ta≦0.50mmのとき、tanθ≦0.05 Effect of the Invention
[0019] The method for manufacturing a piezoelectric element according to the present invention provides the following advantages. (a) Even if an impact is applied to a tray on which a plurality of piezoelectric elements are aligned and placed, the aligned state of the piezoelectric elements is maintained while a characteristic inspection can be performed. (b) The displacement of the piezoelectric element that occurs when a voltage is applied is not impeded. [Brief description of the drawings]
[0020] [Figure 1] 1 is a perspective view showing an example of a piezoelectric element whose characteristics are inspected by a method for inspecting a piezoelectric element according to an embodiment of the present invention; [Diagram 2] 4 is a flowchart showing a method for inspecting a piezoelectric element according to the present embodiment. [Diagram 3] FIG. 3A is a perspective view showing an example of a low-pressure adhesive sheet attached to a base material, and FIG. 3B is a cross-sectional view taken along line IIIB-IIIB in FIG. 3A. [Figure 4] Figure 4A is a cross-sectional view, with some parts omitted, showing multiple piezoelectric elements held on a weak adhesive sheet attached to a base material, and Figure 4B is a cross-sectional view, with some parts omitted, showing a state in which a voltage is applied to multiple piezoelectric elements held on the weak adhesive sheet. [Diagram 5] Table 1 shows the details and evaluation results for Samples 1 to 22. [Figure 6] FIG. 2 is a graph showing the relationship between thickness and dielectric tangent (tan θ) in Table 1. [Figure 7]FIG. 7A is an explanatory diagram showing an example of a disadvantage when using a conventional tray, and FIG. 7B is an explanatory diagram showing another example of a disadvantage when using a conventional tray. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of a method for inspecting a piezoelectric element according to the present invention will be described with reference to Fig. 1 to Fig. 6. In this specification, the symbol "to" indicating a range of values is used to mean that the values before and after the symbol "to" are included as the lower limit and upper limit.
[0022] 1, a piezoelectric element 10 that is an object of inspection by the method for inspecting a piezoelectric element according to the present embodiment has an element body 12 having a perovskite structure or the like, and a pair of electrodes 14a and 14b formed, for example, on the upper and lower surfaces of the element body 12. The piezoelectric element 10 has a structure in which the element body 12 has a laminated structure, for example, and the pair of electrodes 14a and 14b are formed in a comb-like shape. In this case, the pair of electrodes 14a and 14b are formed so as to appear on the upper surface of the element body 12.
[0023] In the method for inspecting a piezoelectric element according to the present embodiment, the piezoelectric element 10 (see FIG. 1) is held on a flat, slightly adhesive sheet 30 (see FIGS. 3A and 3B) as shown in step S1 of FIG. 2. Then, in step S2, a voltage is applied to the piezoelectric element 10 held on the slightly adhesive sheet 30 to measure the deformation and natural frequency of the piezoelectric element 10, thereby evaluating the electrical characteristics of the piezoelectric element 10.
[0024] The piezoelectric element 10 is fabricated, for example, by following the procedure below. That is, a green laminate composed of a green sheet and an electrode film is fired to fabricate a large piezoelectric substrate (not shown). The large piezoelectric substrate is then subjected to a piezoelectric treatment and separated into a plurality of pieces to fabricate a plurality of piezoelectric elements 10. Of course, the large piezoelectric substrate may be separated into a plurality of pieces (piezoelectric substrate pieces), and then each piezoelectric substrate piece may be subjected to a piezoelectric treatment to fabricate a plurality of piezoelectric elements 10.
[0025] As shown in Figures 3A and 3B, the flat-plate-shaped weak adhesive sheet 30 is attached to a base material 32 made of metal or ceramics. It is preferable that at least the surface of the base material 32 to which the weak adhesive sheet 30 is attached is flat, and the weak adhesive sheet 30 is attached within the above surface. This prevents the weak adhesive sheet 30 from being wrinkled or partially turned inside out due to air conditioning wind, etc., and allows the plurality of piezoelectric elements 10 to be stably held. In addition, the material of the base material 32 is more preferably metal from the viewpoint of processing accuracy and heat conduction during heating, and more preferably aluminum from the viewpoint of heat conduction.
[0026] Therefore, in step S1, for example, an alignment jig is used to align and hold the plurality of piezoelectric elements 10 on the weak adhesive sheet 30 as shown in Fig. 4A. The alignment is preferably performed, for example, in a matrix shape in which the plurality of piezoelectric elements 10 are aligned vertically and horizontally. Furthermore, it is preferable that the weak adhesive sheet 30 maintains the aligned state of the plurality of piezoelectric elements 10 even when an impact is applied through the base material 32 or to the weak adhesive sheet 30 itself.
[0027] On the other hand, the inspection process in step S2 is performed with a plurality of piezoelectric elements 10 aligned on the weak adhesive sheet 30 as shown in Fig. 4B. For example, one voltage application device 40 is used to inspect the electrical characteristics of the plurality of piezoelectric elements 10 in sequence. Of course, a plurality of voltage application devices 40 may be connected to inspect the electrical characteristics of the plurality of piezoelectric elements 10 at once or in several batches. When the electrical characteristics of each piezoelectric element 10 are inspected, a distortion of 1500 to 4000 ppm occurs in the d31 direction (direction along the electrode surface) at an electric field of 2.0 to 4.0 kV / mm.
[0028] Therefore, it is preferable that the weak adhesive sheet 30 has a holding force that is not inhibiting the distortion (displacement) of the multiple piezoelectric elements 10 that occurs during the characteristic inspection in step S2. In other words, the holding of the piezoelectric elements 10 by the weak adhesive sheet 30 corresponds to physical adhesion (secondary bonding, intermolecular bonding), which is one of the adhesive principles.
[0029] The physical properties of the weakly adhesive sheet 30 are a surface resistance of 10 16 ohms or more, Young's modulus 5.0~10.0MPa, thermal conductivity 0.05W / mK or more, retention force 0.50kgf / cm 2 The heat resistance is preferably 90° C. or higher. The holding power of the low-pressure adhesive sheet 30 is 0.10 kgf / cm 2 The above is preferred. EXAMPLES
[0030] [First Example] In the first example, a preferable relationship between the thickness ta (see FIG. 3B) of the low-pressure adhesive sheet 30 and the dielectric tangent tan θ was confirmed.
[0031] Specifically, samples 1 to 22 (weak adhesive sheets 30) were prepared, and the resistance value (Ω: ohms) of each sample was measured at a resonance frequency (7.2 to 7.9 MHz). The details of each sample are shown in Table 1 of FIG.
[0032] [Sample 1-3] The low-pressure adhesive sheets 30 of Samples 1 to 3 all have a thickness ta of 0.03 mm. Sample 1 has a dielectric loss tangent (tan θ) of 0.23 and is made of fluororubber. Sample 2 has a dielectric loss tangent (tan θ) of 0.20 and is made of fluororubber. Sample 3 has a dielectric loss tangent (tan θ) of 0.17 and is made of fluororubber.
[0033] [Sample 4-6] The low-pressure adhesive sheets 30 of Samples 4 to 6 all have a thickness ta of 0.10 mm. Sample 4 has a dielectric loss tangent (tan θ) of 0.25 and is made of fluororubber. Sample 5 has a dielectric loss tangent (tan θ) of 0.15 and is made of fluororubber. Sample 6 has a dielectric loss tangent (tan θ) of 0.03 and is made of fluororesin.
[0034] [Sample 7, 8] The low-pressure adhesive sheets 30 of Samples 7 and 8 both have a thickness ta of 0.15 mm. Sample 7 has a dielectric loss tangent (tan θ) of 0.25 and is made of fluororubber. Sample 8 has a dielectric loss tangent (tan θ) of 0.23 and is made of fluororubber.
[0035] [Sample 9-12] The low-adhesive sheets 30 of Samples 9 to 12 all have a thickness ta of 0.20 mm. Sample 9 has a dielectric loss tangent (tan θ) of 0.25 and is made of fluororubber. Sample 10 has a dielectric loss tangent (tan θ) of 0.15 and is made of fluororubber. Sample 11 has a dielectric loss tangent (tan θ) of 0.05 and is made of olefin. Sample 12 has a dielectric loss tangent (tan θ) of 0.03 and is made of fluororesin.
[0036] [Sample 13-15] The low-pressure adhesive sheets 30 of Samples 13 to 15 all have a thickness ta of 0.30 mm. Sample 13 has a dielectric loss tangent (tan θ) of 0.20 and is made of fluororubber. Sample 14 has a dielectric loss tangent (tan θ) of 0.05 and is made of olefin. Sample 15 has a dielectric loss tangent (tan θ) of 0.03 and is made of fluororesin.
[0037] [Sample 16-19] The low-pressure adhesive sheets 30 of Samples 16 to 19 all have a thickness ta of 0.40 mm. Sample 16 has a dielectric loss tangent (tan θ) of 0.15 and is made of fluororubber. Sample 17 has a dielectric loss tangent (tan θ) of 0.15 and is made of olefin. Sample 18 has a dielectric loss tangent (tan θ) of 0.05 and is made of olefin. Sample 19 has a dielectric loss tangent (tan θ) of 0.03 and is made of fluororesin.
[0038] [Sample 20-22] The low-pressure adhesive sheets 30 of Samples 20 to 22 all have a thickness ta of 0.50 mm. Sample 20 has a dielectric loss tangent (tan θ) of 0.15 and is made of olefin. Sample 21 has a dielectric loss tangent (tan θ) of 0.05 and is made of olefin. Sample 22 has a dielectric loss tangent (tan θ) of 0.03 and is made of fluororesin.
[0039] [evaluation] Among the samples, those with a resistance value of 200 (Ω) or more at the resonant frequency (7.2 to 7.9 MHz) were rated as "A," and those with a resistance value of less than 200 (Ω) were rated as "B."
[0040] The evaluation results of each sample are shown in Table 1 of Figure 5 and Figure 6. Figure 6 is a graph showing the relationship between the thickness ta and the dielectric tangent (tan θ) in Table 1. In Figure 6, the relationship with the evaluation "A" is marked with "○" and the relationship with the evaluation "B" is marked with "×".
[0041] From the above evaluation results, it is preferable that the low-pressure adhesive sheet 30 has a relationship between the thickness ta and the dielectric tangent tan θ of (a) to (d). (a) When 0.03 mm ≦ ta ≦ 0.05 mm, tan θ ≦ 0.20 (b) 0.05 mm <ta≦0.10mmのとき、tanθ≦0.15 (c) 0.10 mm <ta≦0.20mmのとき、tanθ≦0.10 (d) 0.20 mm <ta≦0.50mmのとき、tanθ≦0.05
[0042] [Second Example] In the second embodiment, the yield and retry rate were confirmed for the embodiment and the comparative example.
[0043] In the embodiment, 100 piezoelectric elements 10 were aligned and held on the weak adhesive sheet 30 of sample 6 described above using an alignment device, the surface temperature of the base material 32 to which the weak adhesive sheet 30 was attached was set to 90±5°C, and a voltage of 53±2V was applied between the pair of electrodes 14a and 14b of each piezoelectric element 10 to perform a characteristic test.
[0044] In addition, a capacitance test and a resonance test were performed to evaluate the electrical characteristics. The capacitance test was performed by using an LCR meter to measure the electrostatic capacitance by contacting a probe with the electrodes 14a and 14b of each piezoelectric element 10 and applying a measurement signal with a voltage of 0.5 V and a frequency of 1 kHz.
[0045] The resonance test was performed by using a network analyzer to measure the frequency dependency of impedance by contacting a probe with the electrodes 14a and 14b of each piezoelectric element 10 and applying a measurement signal of +4 dBm. Then, by referring to the waveform of the frequency characteristics near the resonance frequency of each piezoelectric element 10, it was determined that there was no crack when the impedance peak value at the resonance frequency exceeded a predetermined threshold. Also, it was determined that there was a crack when the impedance peak value at the resonance frequency did not exceed the predetermined threshold.
[0046] In the comparative example, a characteristic test was performed using a tray 102 shown in Fig. 7A. 100 recesses 104 were formed in the tray 102. 100 piezoelectric elements 100 were inserted using an insertion jig so that one piezoelectric element 100 was inserted into each of the 100 recesses 104. Then, a voltage of 53±2V was applied between a pair of electrodes of each piezoelectric element 100 to perform a characteristic test. Furthermore, in the comparative example, a capacitance test and a resonance test were performed in the same manner as in the above example.
[0047] [evaluation] For each of the examples and the comparative examples, the percentage of the number of piezoelectric substrate pieces that were normally polarized among 100 piezoelectric elements was calculated, i.e., (normal number / 100)×100(%), and the calculated result was regarded as the yield, which was 80% for the example and 60% for the comparative example.
[0048] The retry rate of the polarization process was also confirmed for the Example and Comparative Example. The Comparative Example had 200 retries for 1000 inspection pieces, resulting in a retry rate of 0.2. In contrast, the Example had 30 retries for 1000 inspection pieces, resulting in a low retry rate of 0.03.
[0049] In the examples and comparative examples, a retry refers to a process of contacting a probe with each piezoelectric element and performing a polarization process or a measurement process (retest) again when the characteristic value measured by contacting the probe with the piezoelectric element is incorrect. Also, a retry rate refers to the ratio of the number of retries to the number of tests, that is, the number of retries / number of tests.
[0050] The retry rate of the inspection judgment was confirmed for the embodiment and the comparative example. In the comparative example, the number of retests was 100 out of 1000 pieces in the capacitance inspection, and the retry rate was 0.1. In contrast, in the embodiment, the number of retests was 8 out of 1000 pieces in the capacitance inspection, and the retry rate was 0.008. Furthermore, in the comparative example, the number of retests was 300 out of 1000 pieces in the resonance inspection, and the retry rate was 0.3. In contrast, in the embodiment, the number of retests was 30 out of 1000 pieces in the resonance inspection, and the retry rate was 0.03.
[0051] From the above results, it was confirmed that the retry rate is reduced and the yield is improved when the piezoelectric element 10 is fixed to the weak adhesive sheet 30 as shown in FIG. 7A, compared to when the weak adhesive sheet 30 is not used and the piezoelectric element 100 is held only by the frame of the tray 102.
[0052] Incidentally, the method for inspecting a piezoelectric element according to the present invention is not limited to the above-mentioned embodiment, and it goes without saying that various configurations can be adopted without departing from the gist of the present invention.
Claims
1. A method for inspecting a piezoelectric element, comprising: applying a voltage to a piezoelectric element (10) to evaluate electrical characteristics of the piezoelectric element (10); A first step of attaching the lower surface of the piezoelectric element (10) to a flat, non-hole-containing, slightly adhesive sheet (30) to hold a plurality of the piezoelectric elements (10) in an aligned state on the slightly adhesive sheet (30); A second step of applying a voltage to the piezoelectric element (10) held on the low-pressure adhesive sheet (30) to evaluate the electrical characteristics of the piezoelectric element (10), The physical properties of the low-pressure adhesive sheet (30) are as follows: surface resistance is 10 16 ohms or more, Young's modulus 5.0-10.0MPa, thermal conductivity 0.05W / mK or more, retention force 0.50kgf / cm 2 The following is a method for inspecting a piezoelectric element, characterized in that the element has a heat resistance of 90° C. or higher.
2. 2. The method for inspecting a piezoelectric element according to claim 1, The flat low-pressure adhesive sheet (30) is attached to a base material (32), The method for inspecting a piezoelectric element is characterized in that at least the surface of the base material (32) to which the weak adhesive sheet (30) is attached is flat, and the weak adhesive sheet (30) is attached within the flat surface.
3. A method for inspecting a piezoelectric element, comprising: applying a voltage to a piezoelectric element (10) to evaluate electrical characteristics of the piezoelectric element (10); A first step of attaching the lower surface of the piezoelectric element (10) to a flat, slightly adhesive sheet (30) to hold a plurality of the piezoelectric elements (10) in an aligned state on the slightly adhesive sheet (30); A second step of applying a voltage to the piezoelectric element (10) held on the low-pressure adhesive sheet (30) to evaluate the electrical characteristics of the piezoelectric element (10), The physical properties of the low-pressure adhesive sheet (30) are as follows: surface resistance is 10 16 ohms or more, Young's modulus 5.0-10.0MPa, thermal conductivity 0.05W / mK or more, retention force 0.50kgf / cm 2The heat resistance is 90°C or higher. The flat low-pressure adhesive sheet (30) is attached to a base material (32), The base material (32) is made of metal or ceramics, The method for inspecting a piezoelectric element is characterized in that at least the surface of the base material (32) to which the weak adhesive sheet (30) is attached is flat, and the weak adhesive sheet (30) is attached within the flat surface.
4. 4. The method for inspecting a piezoelectric element according to claim 3, A method for inspecting a piezoelectric element, wherein the weak adhesive sheet has no holes.
5. The method for inspecting a piezoelectric element according to any one of claims 1 to 4, The piezoelectric element (10) has a first terminal (14a) and a second terminal (14b) formed on an upper surface thereof, The first step includes holding the lower surface of the piezoelectric element (10), which faces the upper surface, on the weak adhesive sheet (30); The method for inspecting a piezoelectric element is characterized in that the second step applies a voltage between the first terminal (14a) and the second terminal (14b) of the piezoelectric element (10).
6. The method for inspecting a piezoelectric element according to any one of claims 1 to 5, The method for inspecting a piezoelectric element is characterized in that the size of the piezoelectric element (10) is 0.2 to 0.4 mm in length, 0.8 to 1.2 mm in width, and 0.05 to 0.2 mm in thickness.
7. The method for inspecting a piezoelectric element according to any one of claims 1 to 6, The method for inspecting a piezoelectric element is characterized in that, when a voltage is applied to the piezoelectric element (10) for evaluating the electrical characteristics, a distortion in the d31 direction of 1500 to 4000 ppm occurs at an electric field of 2.0 to 4.0 kV / mm.
8. The method for inspecting a piezoelectric element according to any one of claims 1 to 7, The method for inspecting a piezoelectric element is characterized in that the weak adhesive sheet (30) holds the piezoelectric element (10) and does not hinder the displacement of the piezoelectric element (10) that occurs when a voltage is applied.
9. The method for inspecting a piezoelectric element according to any one of claims 1 to 8, The method for inspecting a piezoelectric element is characterized in that the relationship between the thickness ta and the dielectric tangent tanθ of the slightly adhesive sheet (30) is (a) to (d). (a) When 0.03 mm≦ta≦0.05 mm, tan θ≦0.20 (b) When 0.05 mm<ta≦0.10 mm, tan θ≦0.15 (c) When 0.10 mm<ta≦0.20 mm, tan θ≦0.10 (d) When 0.20 mm<ta≦0.50 mm, tan θ≦0.05
Citation Information
Patent Citations
Method for manufacturing and handling element having directivity
JP2002190457A
Manufacturing method of piezoelectric element
JP2013161970A
Component aligning apparatus, alignment tray, and component aligning method
JP2014181126A
Laminated ceramic structure, manufacturing method therefor, and piezoelectric actuator
WO2015060132A1
Ceramic device and joined body
WO2015194461A1