How alcohol is produced
A catalyst system using specific metals on carriers like ZrO2 supports efficient and selective alcohol production from carboxylic acids under mild conditions, addressing the inefficiencies of high-pressure methods and providing an environmentally friendly solution.
Patent Information
- Application Number
- JP2020022162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-15
- Filing Date
- 2020-02-13
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-02-13
AI Technical Summary
Existing methods for reducing carboxylic acids to alcohols using molecular hydrogen as a reducing agent produce significant amounts of salt by-products and require high temperature and pressure conditions, necessitating the development of a catalytic reduction process that is efficient, safe, and environmentally friendly.
A catalyst system comprising specific metal species (Rh, Pt, Ru, Ir, Pd) supported on carriers like ZrO2, hydroxyapatite, niobium pentoxide, or hydrotalcite is used to reduce monocarboxylic, hydroxycarboxylic, or dicarboxylic acids to alcohols under mild conditions, with water as a solvent, achieving high selectivity and durability.
The method enables efficient and selective production of alcohols from carboxylic acids under mild conditions, using environmentally friendly solvents and catalysts that maintain high activity even after repeated use, reducing manufacturing costs.
Smart Images

Figure 0007555537000021 
Figure 0007555537000022 
Figure 0007555537000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an alcohol by reducing a carboxylic acid. [Background technology]
[0002] In order to reduce carbon dioxide emissions on a global scale, there is a strong demand for the development of efficient conversion reactions from biomass resources to useful chemical products. Examples of compounds derived from biomass include carboxylic acids such as succinic acid and fumaric acid. Alcohols obtained by reducing these carboxylic acids are useful as raw materials for chemical products such as plastics.
[0003] Traditionally, reducing agents such as LiAlH4 and BH3 have been used to reduce carboxylic acids to alcohols. However, the use of these reducing agents has the problem of producing a large amount of salt as a by-product after the reaction. Therefore, there is a need to develop a catalytic reduction reaction that uses molecular hydrogen as a reducing agent, which produces only water as a by-product after the reaction.
[0004] As a catalytic reduction reaction of carboxylic acid using molecular hydrogen as a reducing agent, for example, a method using a catalyst such as Ru-Ir-Re / SiO2 is known (Patent Document 1). However, in order to suppress the production of by-products and selectively obtain alcohol, it is necessary to carry out the reaction under high temperature and high pressure conditions. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-74619 A Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, an object of the present invention is to provide a method for efficiently reducing a carboxylic acid under mild conditions to selectively produce an alcohol. Another object of the present invention is to provide a method for efficiently reducing a carboxylic acid and selectively producing an alcohol using water, which is safe for the human body and environmentally friendly, as a solvent. Another object of the present invention is to provide a catalyst for use in the efficient reduction of a carboxylic acid to selectively produce an alcohol. Another object of the present invention is to provide a catalyst for use in the selective production of alcohol by efficiently reducing a carboxylic acid, which has excellent durability and can maintain high catalytic activity even after repeated use. [Means for solving the problem]
[0007] As a result of intensive research conducted by the present inventors to solve the above problems, they have found that the use of the specific catalyst described below makes it possible to rapidly reduce a monocarboxylic acid, a hydroxycarboxylic acid, or a dicarboxylic acid under mild conditions to selectively produce the corresponding alcohol. The present invention has been completed based on these findings.
[0008] That is, the present invention provides a method for producing an alcohol, which comprises reducing a carboxyl group of a substrate shown below in the presence of a catalyst shown below to produce the corresponding alcohol. Catalyst: A catalyst in which the following metal species M1 and M2 are supported on the following support (M1) Rhodium, platinum, ruthenium, iridium, or palladium (M2) Tin, vanadium, molybdenum, tungsten, or rhenium (Carrier) Zirconium oxide, hydroxyapatite, niobium pentoxide, fluoroapatite, or hydrotalcite Substrate: a carboxylic acid represented by the following formula (1a), (1b), or (1c): [ka] (In the formula, R 1 represents a hydrogen atom or a monovalent hydrocarbon group, R 2 represents a single bond or a divalent hydrocarbon group.
[0009] The present invention also provides a method for producing an alcohol, using a carboxylic acid represented by formula (1b) or (1c) as a substrate, in which, when a conversion rate of the substrate reaches 90% or more, a selectivity for an alcohol represented by formula (2) below is 70% or more and a selectivity for a lactone represented by formula (3) below is 5% or less in the total amount of reaction products. [ka] (In the formula, R 2 represents a single bond or a divalent hydrocarbon group.
[0010] The present invention also provides the method for producing an alcohol, wherein the catalyst contains, as metal species, M1 and M2, with M2 in the range of 0.05 to 1 mol per 1 mol of M1.
[0011] The present invention also provides the method for producing an alcohol, wherein the amount of the catalyst used (calculated as M1 metal) is 0.01 to 30 mol % of the substrate.
[0012] The present invention also relates to a catalyst having a specific surface area of 5 to 250 m 2 The present invention also provides a method for producing the alcohol, wherein the alcohol content is 1 / g.
[0013] The present invention also provides a method for producing the alcohol, which comprises preparing a catalyst through the following steps and using the obtained catalyst: Step 1: A support is impregnated with a solution containing metal species M2, dried, and then impregnated with a solution containing metal species M1, and dried. Step 2: Calcinate the support after the solution impregnation at 350 to 650°C.
[0014] The present invention also provides a method for producing the alcohol, comprising carrying out the reduction reaction in the presence of water.
[0015] The present invention also provides a reduction catalyst for monocarboxylic acid, hydroxycarboxylic acid, or dicarboxylic acid, which comprises the following metal species M1 and M2 supported on the following support, and is used to reduce a carboxyl group in a substrate represented by the following formula (1a), (1b), or (1c) to obtain the corresponding alcohol. (M1) Rhodium, platinum, ruthenium, iridium, or palladium (M2) Tin, vanadium, molybdenum, tungsten, or rhenium (Carrier) Zirconium oxide, hydroxyapatite, niobium pentoxide, fluoroapatite, or hydrotalcite [ka] (In the formula, R 1 is a hydrogen atom or a monovalent hydrocarbon group, R 2 represents a single bond or a divalent hydrocarbon group. Effect of the Invention
[0016] According to the production method of the present invention, an alcohol can be efficiently and selectively produced from a monocarboxylic acid, a hydroxycarboxylic acid, or a dicarboxylic acid in one step under mild conditions. Furthermore, according to the production method of the present invention, alcohol can be produced efficiently and selectively using water as a solvent, which is safe for the human body and environmentally friendly. The alcohol thus obtained is useful as a raw material for chemical products such as plastics, etc. Therefore, the production method of the present invention is useful as a method for industrially producing alcohol.
[0017] Furthermore, the catalyst of the present invention in which M1 and M2 are supported on zirconium oxide, hydroxyapatite, niobium pentoxide, fluoroapatite, or hydrotalcite is safe for the human body and can be suitably used as a catalyst for reducing a monocarboxylic acid, a hydroxycarboxylic acid, or a dicarboxylic acid to obtain an alcohol using water, which is environmentally friendly, as a solvent.
[0018] Among the above catalysts, the catalyst having zirconium oxide as a support has particularly excellent durability and can maintain high catalytic activity even when repeatedly reused. Therefore, the catalyst having zirconium oxide as a support can be repeatedly used, and therefore the cost of alcohol production can be significantly reduced. [Brief description of the drawings]
[0019] [Figure 1] 1 shows the reaction time (h) and the yield (%) of the reaction product in the reduction reaction of Example 1. [Diagram 2] FIG. 2 shows a TEM image (a) of the catalyst (3) obtained in Preparation Example 3, and a TEM image (b) of the catalyst (4) obtained in Preparation Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] (catalyst) The method for producing an alcohol of the present invention is characterized by using at least one catalyst in which the following metal species M1 and M2 are supported on the following support. (M1) Rhodium, platinum, ruthenium, iridium, or palladium (M2) Tin, vanadium, molybdenum, tungsten, or rhenium (Carrier) Zirconium oxide, hydroxyapatite, niobium pentoxide, fluoroapatite, or hydrotalcite
[0021] As M1, one metal species selected from rhodium, platinum, ruthenium, iridium, and palladium is supported, and as M2, one metal species selected from tin, vanadium, molybdenum, tungsten, and rhenium is supported.
[0022] M1 and M2 supported on the carrier may be a simple metal, a metal salt, a metal oxide, a metal hydroxide, a metal complex, or the like.
[0023] The average particle diameter of the M1 particles supported on the carrier is, for example, 0.5 to 3.0 nm. The average particle diameter is preferably 1.0 to 2.0 nm in terms of exerting particularly excellent catalytic activity. The average particle diameter is determined by observation with a transmission electron microscope (TEM).
[0024] The amount of M1 supported (in terms of metal) is, for example, about 1 to 50% by weight, preferably 1 to 20% by weight, and particularly preferably 1 to 10% by weight, of the carrier. Even if M1 is supported in excess, the catalytic activity becomes saturated and plateaus, and no effect of promoting the reaction is obtained. On the other hand, if the amount of M1 supported is below the above range, it tends to be difficult to obtain sufficient catalytic activity.
[0025] The amount of M2 supported (metal equivalent) is, for example, about 0.01 to 20% by weight, preferably 0.01 to 10% by weight, particularly preferably 0.01 to 1% by weight, most preferably 0.05 to 0.8% by weight, and particularly preferably 0.1 to 0.6% by weight, of the carrier. If the amount of M2 supported is outside the above range, the selectivity changes, and it tends to become difficult to selectively produce an alcohol (for example, a monool when a monocarboxylic acid is used as a substrate, or a diol when a dicarboxylic acid or hydroxycarboxylic acid is used as a substrate).
[0026] The catalyst of the present invention is considered to have catalytically active sites at the interface between M1 and M2. When either M1 or M2 is in excess, the excess metal species covers the other metal species, reducing the interface and the catalytically active sites, which may decrease the catalytic activity and the alcohol yield.
[0027] Therefore, the amounts of M1 and M2 supported are preferably within a specific range, and the amount of M2 supported relative to 1 mole of M1 is preferably within a range of, for example, 0.05 to 1 mole. The upper limit of the amount of M2 supported relative to 1 mole of M1 is preferably 0.5 mole, particularly preferably 0.4 mole, most preferably 0.35 mole, and particularly preferably 0.3 mole. The lower limit of the amount of M2 supported relative to 1 mole of M1 is preferably 0.07 mole, particularly preferably 0.1 mole, most preferably 0.15 mole, and particularly preferably 0.20 mole.
[0028] In the catalyst of the present invention, the amount of the third metal species other than M1 and M2 supported is, for example, 200 mol % or less, preferably 150 mol % or less, more preferably 100 mol % or less, even more preferably 70 mol % or less, even more preferably 50 mol % or less, even more preferably 30 mol % or less, particularly preferably 10 mol % or less, most preferably 5 mol % or less, and especially preferably 1 mol % or less of the total amount of M1 and M2 supported. If the amount of the third metal species supported exceeds the above range, the effect of the present invention tends to be difficult to obtain, possibly due to a decrease in catalytic active sites.
[0029] In the present invention, M1 and M2 are used in a state of being supported on a carrier. By supporting them on a carrier, the interface area between M1 and M2 can be increased, and many catalytic active sites can be exposed.
[0030] The support includes zirconium oxide, hydroxyapatite, niobium pentoxide, fluoroapatite, and hydrotalcite.
[0031] The specific surface area of the carrier is, for example, 5 to 250 m 2 As the carrier, a carrier having a smaller specific surface area (preferably a specific surface area of 5 to 100 m 2 / g, particularly preferably 10 to 50m 2 / g) is preferred in terms of increasing the catalytic activity.
[0032] As the support, at least one selected from hydroxyapatite, niobium pentoxide, fluoroapatite, and zirconium oxide is preferable, since it can selectively and efficiently produce an alcohol (e.g., a diol when a dicarboxylic acid or a hydroxycarboxylic acid is used as a substrate) from a carboxylic acid.
[0033] As the carrier, zirconium oxide or hydroxyapatite is preferred from the viewpoint of excellent durability, and zirconium oxide is particularly preferred.
[0034] As the support, zirconium oxide is preferred because it can selectively and efficiently produce an alcohol (for example, a diol when a dicarboxylic acid or a hydroxycarboxylic acid is used as the substrate) from a carboxylic acid and has excellent durability.
[0035] As the hydroxyapatite, for example, commercially available products such as "Tricalcium Phosphate" (manufactured by Wako Pure Chemical Industries, Ltd.) can be suitably used.
[0036] The catalyst of the present invention can be suitably used as a reduction catalyst for reducing a carboxylic acid to obtain an alcohol (for example, a diol when a dicarboxylic acid or a hydroxycarboxylic acid is used as a substrate).
[0037] In addition, in the present invention, a catalyst in which M1 and M2 are supported on a carrier is used, and therefore, after completion of the reaction, the catalyst and the reaction product can be easily separated by physical separation means such as filtration, centrifugation, etc., and the catalyst separated from the reaction product and recovered can be reused as is or after being washed, dried, etc. Among the above catalysts, a catalyst supported on zirconium oxide is particularly excellent in durability and is inhibited from eluting into the reaction solution, and therefore can maintain high catalytic activity even when repeatedly reused.
[0038] As described above, in the present invention, an expensive catalyst can be repeatedly used, and therefore the production cost of alcohol can be significantly reduced.
[0039] (Catalyst Preparation Method) The catalyst of the present invention can be prepared, for example, by an impregnation method.
[0040] The impregnation method is a method in which a support is immersed in a solution (e.g., an aqueous solution) obtained by dissolving a compound containing the above-mentioned metal species (=metal compound) in a solvent (e.g., water, etc.) to impregnate the support with the metal compound, and then dried and calcined to support the metal species on the support. The amount of the metal species supported can be controlled by adjusting the concentration of the metal compound in the solution, the immersion time of the support, etc.
[0041] The catalyst can be prepared by a method of sequentially impregnating a support with a solution containing metal species M1 (a solution obtained by dissolving a compound containing metal species M1 in a solvent, hereinafter sometimes referred to as "M1-containing solution") and a solution containing metal species M2 (a solution obtained by dissolving a compound containing metal species M2 in a solvent, hereinafter sometimes referred to as "M2-containing solution") (=sequential impregnation method), or by simultaneously impregnating a support with M1-containing solution and M2-containing solution (=co-impregnation method). When preparing a catalyst by the co-impregnation method, the support is impregnated in a mixed liquid of M1-containing solution and M2-containing solution, and then dried and calcined. When preparing a catalyst by the sequential impregnation method, the support is impregnated in one of M1-containing solution and M2-containing solution, dried, and then impregnated in the other of M1-containing solution and M2-containing solution, dried, and then calcined.
[0042] For example, a catalyst in which Pt as M1 and Mo as M2 are supported on a support by co-impregnation (e.g., Pt-Mo / support) can be obtained by co-impregnation of a Pt compound (e.g., H2PtCl6, etc.) and a Mo compound [e.g., (NH4)6Mo7O 24 The support is immersed in a solution obtained by dissolving 1,4-dichloroethane (e.g., 4H2O) in water, and then the support is removed and calcined to prepare the support.
[0043] For example, a catalyst in which Pt as M1 and Mo as M2 are sequentially supported on a support in the order of Mo-Pt (e.g., Pt / Mo / support) is prepared by first immersing the support in a Mo compound [e.g., (NH4)6Mo7O 24 The specimen can be prepared by immersing the specimen in a solution obtained by dissolving Pt compound (e.g., H2PtCl6, etc.) in water, removing it from the solution and drying it, and then immersing it in a solution obtained by dissolving Pt compound (e.g., H2PtCl6, etc.) in water, and then removing it from the solution and calcining it.
[0044] The temperature when the support is immersed in the solution is, for example, about 10 to 80°C.
[0045] The time for immersing the carrier in the solution is, for example, about 1 to 30 hours, and preferably 1 to 5 hours.
[0046] In the present invention, a catalyst obtained by the sequential impregnation method, in which a support is first impregnated with an M2-containing solution, dried, then impregnated with an M1-containing solution, dried, and calcined, is particularly preferred. The catalyst obtained by the above method exhibits excellent selectivity and can produce alcohols in a high yield because M1 is not covered with M2 and the amount of M1 exposed is increased.
[0047] The calcination is carried out, for example, using a muffle furnace. The calcination temperature is, for example, 300° C. or higher and lower than 700° C. The calcination time is, for example, 1 to 5 hours. If the calcination temperature exceeds the above range, the catalytic activity tends to decrease rapidly, possibly due to aggregation of the metal species supported on the support.
[0048] The calcination temperature is preferably from 350 to 650°C, more preferably from 400 to 550°C, and particularly preferably from 450 to 550°C, in terms of increasing the catalytic activity.
[0049] After the calcination, a reduction treatment may be further carried out. The reducing agent used in the reduction treatment may be, for example, hydrogen (H2).
[0050] The reduction treatment temperature and time are, for example, 0 to 600° C. (preferably 100 to 200° C.) and about 0.5 to 5 hours (preferably 0.5 to 2 hours).
[0051] The catalyst obtained by the above-mentioned preparation method may then be subjected to a washing treatment (washing with water, an organic solvent, etc.), a drying treatment (drying by vacuum drying, etc.), and the like.
[0052] (substrate) In the present invention, a monocarboxylic acid represented by the following formula (1a), a hydroxycarboxylic acid represented by the following formula (1b), or a dicarboxylic acid represented by the following formula (1c) is used as a substrate. [ka]
[0053] In the above formula, R 1 is a hydrogen atom or a monovalent hydrocarbon group, R 2 represents a single bond or a divalent hydrocarbon group.
[0054] R 1 The monovalent hydrocarbon group in the above formula includes a monovalent aliphatic hydrocarbon group, a monovalent alicyclic hydrocarbon group, a monovalent aromatic hydrocarbon group, and a monovalent group formed by bonding two or more groups selected from these.
[0055] Examples of the monovalent aliphatic hydrocarbon group include linear or branched alkyl groups having 1 to 10 carbon atoms (preferably 1 to 5 carbon atoms), such as methyl, ethyl, propyl, isopropyl, butyl, pentyl, octyl, 2-ethylhexyl, and decyl groups; and linear or branched alkenyl groups having 2 to 10 carbon atoms (preferably 2 to 5 carbon atoms), such as vinyl, allyl, propenyl, 1-butenyl, 2-butenyl, 1-pentenyl, and 2-pentenyl groups.
[0056] Examples of the monovalent alicyclic hydrocarbon group include cycloalkyl groups having 3 to 10 carbon atoms (preferably 3 to 6 carbon atoms), such as cyclopentyl, cyclohexyl, and cycloheptyl groups; and cycloalkenyl groups having 3 to 10 carbon atoms (preferably 3 to 6 carbon atoms), such as cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclohexenyl, and cyclooctenyl groups.
[0057] Examples of the monovalent aromatic hydrocarbon group include aryl groups having 6 to 20 carbon atoms, such as phenyl, biphenyl, naphthyl, binaphthyl, and anthracenyl groups.
[0058] Examples of the monovalent group formed by bonding two or more groups selected from the above-mentioned hydrocarbon groups include cyclohexylmethyl and benzyl groups.
[0059] R 2 The divalent hydrocarbon group in the above formula includes a divalent aliphatic hydrocarbon group, a divalent alicyclic hydrocarbon group, a divalent aromatic hydrocarbon group, and a divalent group formed by bonding two or more groups selected from these.
[0060] Examples of the divalent aliphatic hydrocarbon group include linear or branched alkylene groups having 1 to 10 carbon atoms (preferably 1 to 5 carbon atoms), such as methylene, methylmethylene, dimethylmethylene, ethylene, propylene, and trimethylene groups; and linear or branched alkenylene groups having 2 to 10 carbon atoms (preferably 2 to 5 carbon atoms), such as vinylene, 1-methylvinylene, propenylene, 1-butenylene, 2-butenylene, 1-pentenylene, and 2-pentenylene groups.
[0061] Examples of the divalent alicyclic hydrocarbon group include cycloalkylene groups having 3 to 10 carbon atoms (preferably having 3 to 6 carbon atoms), such as cyclopentylene, cyclohexylene (e.g., 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene), and cycloheptylene groups; and cycloakenylene groups having 3 to 10 carbon atoms (preferably having 3 to 6 carbon atoms), such as cyclopropenylene, cyclobutenylene, cyclopentenylene, cyclohexenylene, and cyclooctenylene groups.
[0062] Examples of the divalent aromatic hydrocarbon group include arylene groups having 6 to 20 carbon atoms, such as phenylene (for example, o-phenylene, m-phenylene, p-phenylene), biphenylene, naphthylene, binaphthylene, and anthracenylene groups.
[0063] Examples of divalent groups formed by bonding two or more groups selected from the above-mentioned hydrocarbon groups include cyclohexylenebis(methylene) [e.g., 1,2-cyclohexylenebis(methylene), 1,3-cyclohexylenebis(methylene), 1,4-cyclohexylenebis(methylene)], phenylenebis(methylene) (e.g., 1,2-phenylenebis(methylene), 1,3-phenylenebis(methylene), 1,4-phenylenebis(methylene)), and the like.
[0064] The monovalent hydrocarbon group and the divalent hydrocarbon group may have one or more substituents. Examples of the substituents include, for example, C 1-5 Alkoxy group, C 6-10 Aryloxy group, C 7-11 Aralkyloxy group, oxo group, halogen atom, haloC 1-5 Examples of such groups include alkyl groups.
[0065] [Alcohol production method] The method for producing an alcohol of the present invention is characterized in that a carboxyl group of a substrate is reduced (preferably reduced or hydrogenated with molecular hydrogen) in the presence of the above catalyst to produce the corresponding alcohol.
[0066] In the method for producing an alcohol of the present invention, an alcohol can be obtained according to the substrate used. For example, when a monocarboxylic acid represented by the following formula (1a) is used as a substrate, a monool represented by the following formula (4) is obtained. When a hydroxycarboxylic acid represented by the following formula (1b) or a dicarboxylic acid represented by the following formula (1c) is used as a substrate, a diol represented by the following formula (2) is obtained. [ka] (In the formula, R 1 , R 2 is the same as above)
[0067] More specifically, when a dicarboxylic acid represented by formula (1c) is used as a substrate, the two carboxyl groups of the dicarboxylic acid represented by formula (1c) are reduced simultaneously or sequentially to give a hydroxycarboxylic acid represented by formula (1b) via the hydroxycarboxylic acid represented by formula (1c) and then a diol represented by formula (2)[1][2]. In addition, some of the hydroxycarboxylic acids represented by formula (1b) obtained via [1] undergo intramolecular dehydration condensation to form lactones represented by formula (3) [3], and the lactones are further reduced to open the cyclic ester group, thereby forming diols represented by formula (2) [4]. [ka]
[0068] The amount of the catalyst used (calculated as the M1 metal contained in the catalyst) is, for example, about 0.01 to 30 mol %, preferably 0.1 to 10 mol %, particularly preferably 0.5 to 5 mol %, and most preferably 1 to 5 mol % of the substrate.
[0069] The amount of the catalyst used (calculated as the M2 metal contained in the catalyst) is, for example, about 0.01 to 10 mol %, preferably 0.05 to 5 mol %, and particularly preferably 0.1 to 2 mol %, of the substrate.
[0070] When the catalyst is used in the above range, the substrate can be efficiently reduced under mild conditions to selectively produce an alcohol. When the amount of the catalyst used is less than the above range, the yield of the alcohol tends to decrease.
[0071] Hydrogen used in the reduction reaction (or hydrogenation reaction) is supplied, for example, by a method of carrying out the reaction under a hydrogen atmosphere or a method of bubbling hydrogen gas.
[0072] In the present invention, since the above catalyst is used, the reduction of the carboxyl group or cyclic ester group of the substrate can proceed rapidly under mild conditions, and the hydrogen pressure during the reduction reaction is, for example, 10 MPa or less, preferably 8 MPa or less, and particularly preferably 5 MPa or less (e.g., 1 to 5 MPa).
[0073] The reaction temperature for the reduction reaction varies depending on the catalyst used, but is, for example, 50 to 200°C, preferably 100 to 180°C, particularly preferably 120 to 160°C, and most preferably 120 to 150°C.
[0074] In particular, a catalyst supported by zirconium oxide (particularly a catalyst in which metal species are supported in the order M2-M1 by a sequential impregnation method on zirconium oxide as a support) has high catalytic activity, and therefore when this is used as a catalyst, the reaction temperature of the reduction reaction can be lowered, for example, to 70 to 100°C (particularly, to 80 to 95°C).
[0075] The reaction time for the reduction reaction is, for example, about 1 to 36 hours, preferably 5 to 30 hours, and particularly preferably 5 to 20 hours.
[0076] The reduction reaction can be carried out by any method such as a batch method, a semi-batch method, or a continuous method.
[0077] The reduction reaction is preferably carried out in a liquid phase. That is, the reduction reaction in the present invention is preferably a liquid phase reaction. Since monocarboxylic acids, dicarboxylic acids, and hydroxycarboxylic acids have high boiling points, if the reduction reaction is carried out in a gas phase, the reaction product tends to decompose and the yield of alcohol tends to decrease.
[0078] When the reaction is carried out in a liquid phase, examples of the solvent include water, alcohol solvents such as methanol, ethanol, 2-propanol, and 1-butanol, ether solvents such as 1,4-dioxane, THF, 1,2-dimethoxyethane, and diethyl ether, hydrocarbon solvents such as toluene, hexane, and dodecane, and halogenated hydrocarbon solvents such as 1,2-dichloroethane and dichloromethane. These can be used alone or in combination of two or more.
[0079] In the present invention, water is preferred because it is safe for the human body and environmentally friendly. That is, the reduction reaction in the present invention is preferably carried out in the presence of water. In addition, in the present invention, when the lactone represented by formula (3) produced by the reaction [3] above is reduced in the presence of water, the ester ring-opening reaction [4] above proceeds to produce the diol represented by formula (2). Therefore, in the present invention, when a carboxylic acid represented by formula (1b) or (1c) is used as a substrate, it is particularly preferred to carry out the reduction reaction in the presence of water, since the diol represented by formula (2) can be obtained in high yield.
[0080] The amount of water used in the total amount of the solvent is, for example, preferably 1% by weight or more, more preferably 5% by weight or more, more preferably 10% by weight or more, even more preferably 30% by weight or more, even more preferably 50% by weight or more, particularly preferably 70% by weight or more, most preferably 80% by weight or more, and particularly preferably 90% by weight or more. Therefore, the amount of a solvent other than water (for example, an organic solvent, particularly an ether-based organic solvent such as THF) used in the total amount of the solvent is, for example, preferably 90% by weight or less, more preferably 80% by weight or less, more preferably 70% by weight or less, even more preferably 50% by weight or less, even more preferably 30% by weight or less, even more preferably 20% by weight or less, particularly preferably 10% by weight or less, most preferably 5% by weight or less, and particularly preferably 1% by weight or less.
[0081] When the reaction is carried out in a batch system, the amount of the solvent used is preferably in the range such that the initial concentration of the substrate is, for example, about 0.01 to 10% by weight.
[0082] In the present invention, since the above catalyst is used, the reduction reaction of the substrate can be rapidly carried out even if one or more selected from acids such as hydrochloric acid, sulfuric acid, phosphoric acid, and acetic acid, and bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, and potassium hydrogen carbonate are not present in the reaction system. In addition, in the present invention, the above acids and bases may be used, but the amount of these used (the total amount when two or more types are contained) is preferably less than 0.001 mol per mol of the substrate, and it is particularly preferable that they are not used substantially. If the above acids and bases are present in the reaction system in excess of the above ranges, a neutralization treatment is required in the post-treatment, but the neutralization treatment produces salts as by-products, and removing the by-product salts causes loss of the product. In addition, the above acids and bases are corrosive, so the material of the reactor used is limited.
[0083] After completion of the reaction, the reaction product can be separated and purified by a separation means such as filtration, concentration, distillation, extraction, crystallization, recrystallization, column chromatography, or a combination of these.
[0084] In the alcohol production method of the present invention, the substrate can be efficiently converted even under mild conditions. The conversion rate of the substrate 30 hours (preferably 20 hours) after the start of the reaction is, for example, 80% or more, preferably 90% or more, and particularly preferably 95% or more.
[0085] When a carboxylic acid represented by formula (1b) or (1c) is used as a substrate, the above catalyst can rapidly reduce the carboxyl group of the carboxylic acid, thereby suppressing the progress of an intramolecular dehydration condensation reaction to produce a lactone as a by-product, and by reducing the by-product lactone, the corresponding alcohol can be selectively produced in a high yield.
[0086] Therefore, when a carboxylic acid represented by formula (1b) or (1c) is used as a substrate and the conversion rate of the substrate reaches 90% or more, the selectivity of the alcohol represented by formula (2) in the total amount of reaction products is, for example, 70% or more, preferably 80% or more, more preferably 85% or more, and particularly preferably 90% or more. The selectivity of the lactone represented by formula (3) is, for example, 5% or less, preferably 3% or less, and particularly preferably 1% or less. [ka] (In the formula, R 2 represents a single bond or a divalent hydrocarbon group.
[0087] Therefore, according to the method for producing an alcohol of the present invention, an alcohol can be selectively produced in a high yield by a simple one-step method using water as a solvent, which is safe for the human body and environmentally friendly. In particular, when a carboxylic acid represented by formula (1b) or (1c) is used as a substrate, the by-production of lactone is suppressed, and a diol can be selectively produced in a high yield. EXAMPLES
[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0089] Preparation Example 1 (Catalyst preparation: co-impregnation method) 0.0898g of HPtCl6 and (NH)MoO 24 1 g of hydroxyapatite (HAP, product name "tricalcium phosphate", manufactured by Wako Pure Chemical Industries, Ltd.) was immersed for 4 hours at room temperature (25°C) in a solution obtained by dissolving 0.088 g of 4H2O in 50 mL of water. After immersion, the hydroxyapatite was taken out of the solution, and water was distilled off under reduced pressure using a rotary evaporator. This resulted in a powder. The obtained powder was then calcined in an air atmosphere in a muffle furnace at 500°C for 3 hours to obtain catalyst (1) [Pt-Mo / HAP, Pt loading: 4 wt%, Mo loading: 0.485 wt%, Mo / Pt (molar ratio) = 0.25].
[0090] Preparation Example 2 (Catalyst preparation: co-impregnation method) A catalyst (2) [Pt-Mo / FAP, Pt loading: 4 wt%, Mo loading: 0.485 wt%, Mo / Pt (molar ratio) = 0.25] was obtained in the same manner as in Preparation Example 1, except that fluoroapatite (FAP, product name "Fluoroapatite", manufactured by Taihei Chemical Industry Co., Ltd.) was used instead of hydroxyapatite.
[0091] Preparation Example 3 (Catalyst preparation: co-impregnation method) Instead of hydroxyapatite, zirconium oxide (ZrO2, specific surface area: 22.1 m 2 Catalyst (3) [Pt-Mo / JRC-ZRO-8, Pt loading: 4 wt%, Mo loading: 0.5 wt%, Mo / Pt (molar ratio) = 0.25, average particle size of supported Pt particles: 1.5 nm, standard deviation (δ): 0.4 nm] was obtained in the same manner as in Preparation Example 1, except that a catalyst having a molecular weight of 1.0 kg / g and a catalyst temperature of 100° C. and a molecular weight of 1.0 kg / g, the Catalysis Society reference catalyst "JRC-ZRO-8" was used. A TEM image of the obtained catalyst (3) is shown in FIG. 2.
[0092] Preparation Example 4 (Catalyst preparation: co-impregnation method) Instead of hydroxyapatite, zirconium oxide (ZrO2, specific surface area: 100.5 m 2 Catalyst (4) [Pt-Mo / JRC-ZRO-7, Pt loading: 4 wt%, Mo loading: 0.5 wt%, Mo / Pt (molar ratio) = 0.25, average particle size of supported Pt particles: 0.8 nm, standard deviation (δ): 0.2 nm] was obtained in the same manner as in Preparation Example 1, except that the catalyst (4) was used instead of the catalyst (1) (Pt-Mo / JRC-ZRO-7, Pt loading: 4 wt%, Mo loading: 0.5 wt%, Mo / Pt (molar ratio) = 0.25, average particle size of supported Pt particles: 0.8 nm, standard deviation (δ): 0.2 nm). A TEM image of the obtained catalyst (4) is shown in Figure 2.
[0093] Preparation Example 5 (Catalyst preparation: sequential impregnation method) 1 g of "JRC-ZRO-8" was immersed in a Pt solution obtained by dissolving 0.0898 g of HPtCl6 in 50 mL of water for 4 hours at room temperature (25°C). After immersion, the zirconium oxide was removed from the Pt solution and dried at 110°C. After drying, the zirconium oxide was dissolved in water. 24 The catalyst was immersed in a Mo solution prepared by dissolving 0.088 g of 4H2O in 50 mL of water for 4 hours at room temperature (25°C). After immersion, the zirconium oxide was removed from the Mo solution, dried at 110°C, and then calcined in an air atmosphere in a muffle furnace at 500°C for 3 hours to obtain catalyst (5) [Mo / Pt / JRC-ZRO-8, Pt loading: 4 wt%, Mo loading: 0.5 wt%, Mo / Pt (molar ratio) = 0.25].
[0094] Preparation Example 6 (Catalyst preparation: sequential impregnation method) A catalyst (6) [Pt / Mo / JRC-ZRO-8, Pt loading: 4 wt%, Mo loading: 0.5 wt%, Mo / Pt (molar ratio) = 0.25] was obtained in the same manner as in Preparation Example 5, except that the carrier was first immersed in the Mo solution and then in the Pt solution, instead of first immersed in the Pt solution and then in the Mo solution.
[0095] Preparation Example 7 (Catalyst preparation: co-impregnation method) A catalyst (7) [Pt-Mo / Nb2O5, Pt loading: 4 wt%, Mo loading: 0.485 wt%, Mo / Pt (molar ratio) = 0.25] was obtained in the same manner as in Preparation Example 1, except that niobium pentoxide (Nb2O5, manufactured by Wako Pure Chemical Industries, Ltd.) was used instead of hydroxyapatite.
[0096] Preparation Example 8 (Catalyst preparation: sequential impregnation method) A catalyst (8) [Pt / Mo / JRC-ZRO-8, Pt loading: 4 wt%, Mo loading: 0.5 wt%, Mo / Pt (molar ratio) = 0.25] was obtained in the same manner as in Preparation Example 6, except that the calcination temperature was changed to 300°C.
[0097] Preparation Example 9 (Catalyst preparation: sequential impregnation method) A catalyst (9) [Pt / Mo / JRC-ZRO-8, Pt loading: 4 wt%, Mo / Pt (molar ratio) = 0.13] was obtained in the same manner as in Preparation Example 6 except for changing the Mo solution concentration.
[0098] Preparation Example 10 (Catalyst preparation: sequential impregnation method) A catalyst (10) [Pt / Mo / JRC-ZRO-8, Pt loading: 4 wt%, Mo / Pt (molar ratio) = 0.19] was obtained in the same manner as in Preparation Example 6 except for changing the Mo solution concentration.
[0099] Preparation Example 11 (Catalyst preparation: sequential impregnation method) A catalyst (11) [Pt / Mo / JRC-ZRO-8, Pt loading: 4 wt%, Mo / Pt (molar ratio) = 0.31] was obtained in the same manner as in Preparation Example 6 except for changing the Mo solution concentration.
[0100] Comparative Preparation Example 1 (Catalyst preparation: sequential impregnation method) A catalyst (12) [Pt / JRC-ZRO-8, Pt loading: 4 wt %, Mo loading: 0] was obtained in the same manner as in Preparation Example 6, except that the immersion in the Mo solution was not performed.
[0101] Example 1 (This is a reference example) In an autoclave equipped with a Teflon (registered trademark) inner cylinder, 1 mmol of succinic acid as a substrate, 100 mg of catalyst (1) [2 mol% Pt, 0.5 mol% Mo (metal equivalent) of the substrate], and 3 mL of water were charged, and the reaction was carried out at 130°C for 12 hours under a hydrogen pressure of 5 MPa to obtain a reaction product. The conversion rate (conv. [%]) of the substrate was measured using HPLC, and the yield (yield [%]) of each reaction product was measured using a gas chromatograph mass spectrometer (GC-MS). The results are shown in Figure 1.
[0102] [ka]
[0103] Example 2 (This is a reference example) The same procedure as in Example 1 was repeated except that the reaction conditions were changed as follows. Hydrogen pressure: 8MPa Water: 100mL Reaction time: 31 hours
[0104] Example 3 (This is a reference example) The same procedure as in Example 1 was repeated, except that the catalyst (1) was replaced by the catalyst (2).
[0105] Example 4 The same procedure as in Example 1 was repeated, except that the catalyst (1) was replaced by the catalyst (3).
[0106] Example 5 (This is a reference example) The same procedure as in Example 1 was repeated, except that the catalyst (1) was replaced by the catalyst (7).
[0107] Comparative Examples 1 to 9 The same procedure as in Example 1 was repeated, except that the catalyst shown in Table 1 was used instead of the catalyst (1).
[0108] The results are summarized in the table below. [Table 1]
[0109] Examples 6 to 10 (This is a reference example) The same procedure as in Example 1 was carried out except that the substrate and reaction time were changed as shown in the table below.
[0110] The results are summarized in the table below. [Table 2]
[0111] Examples 11 and 12 (This is a reference example) The same procedure as in Example 1 was carried out except that the substrate, reaction time, and reaction temperature were changed as shown in the table below.
[0112] The results are summarized in the table below. [Table 3]
[0113] Example 13 (This is a reference example) The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), a catalyst (1) reuse 1 was used, which was obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 1, washing it with water, and drying it.
[0114] Example 14 (This is a reference example) The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), catalyst (1) reuse 2 was used, which was obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 13, washing it with water, and drying it.
[0115] Example 15 (This is a reference example) The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), catalyst (1) reuse 3 obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 14, washing it with water, and drying it was used.
[0116] Example 16 (This is a reference example) The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), the catalyst (2) reuse 1 obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 3, washing it with water, and drying it was used.
[0117] Example 17 The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), a catalyst (3) was used, which was obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 4, washing it with water, and drying it.
[0118] Example 18 The same procedure as in Example 1 was repeated except that, instead of catalyst (1), catalyst (3) reuse 2 was used, which was obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 17, washing it with water, and drying it.
[0119] Example 19 The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), the catalyst (3) was used, which was obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 18, washing it with water, and drying it.
[0120] Example 20 (This is a reference example) The same procedure as in Example 1 was carried out except that, instead of the catalyst (1), a catalyst (7) reuse 1 was used, which was obtained by taking out the catalyst contained in the reaction product after the completion of the reaction in Example 5, washing it with water, and drying it.
[0121] The results are summarized in the table below. It can be seen from the table below that the catalyst using zirconium oxide as the carrier has excellent durability and its activity does not decrease even when it is reused twice or more.
[0122] [Table 4]
[0123] Examples 21 and 22 (Example 22 is a reference example) The same procedure as in Example 1 was carried out except that the catalysts shown in the table below were used and the reaction temperature was changed to 110° C. The results are summarized in the table below. It can be seen from the table below that the smaller the specific surface area of zirconium oxide, the higher the catalytic activity.
[0124] [ka] [Table 5]
[0125] Examples 23 to 25 The same procedure as in Example 1 was repeated except that the catalysts shown in the table below (catalysts obtained in Preparation Examples 3, 5, or 6) were used, and the reaction temperature was changed to 110° C. and the reaction time to 3 hours. The results are summarized in the table below. From the table below, it can be seen that the catalyst obtained by loading M1 and M2 in the order of M2-M1 by the sequential impregnation method has higher activity than the catalyst obtained by the co-impregnation method and the catalyst obtained by loading M1-M2 in the order of M1-M2 even by the sequential impregnation method.
[0126] [Table 6]
[0127] Example 26, 2 7 The same procedure as in Example 1 was repeated except that the catalysts shown in the table below (catalysts obtained in Preparation Examples 6 or 8) were used, and the reaction temperature was changed to 80° C. and the reaction time to 12 hours. The results are summarized in the table below.
[0128] [Table 7]
[0129] Examples 28 to 33, Comparative Example 10 The same procedure as in Example 1 was repeated, except that the catalysts shown in the table below (the catalysts obtained in Preparation Examples 6, 9, 10, 11, or Comparative Preparation Example 1) were used and the reaction was carried out at the temperatures shown in the table below. The results are summarized in the table below.
[0130] [Table 8]
Claims
1. A method for producing an alcohol, comprising reducing a carboxyl group of a substrate shown below in the presence of a catalyst shown below to produce the corresponding alcohol. Catalyst: The following metal species M 1 and M. 2 A catalyst comprising the above supported on the following carrier: (M 1 )platinum (M 2 )molybdenum (Support) Zirconium oxide with a specific surface area of 10 to 50 m 2 / g Substrate: a carboxylic acid represented by the following formula (1a), (1b), or (1c) [Formula 1] (In the formula, R 1 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkenyl group having 2 to 5 carbon atoms; R 2 represents a single bond, a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylene group, a trimethylene group, a vinylene group, a 1-methylvinylene group, a methylideneethylene group, a propenylene group, a 1-butenylene group, a 2-butenylene group, a 1,3-butadienylene group, a 1-pentenylene group, or a 2-pentenylene group.
2. 2. The method for producing an alcohol according to claim 1, wherein a carboxylic acid represented by formula (1b) or (1c) is used as a substrate, and when a conversion rate of the substrate reaches 90% or more, a selectivity of an alcohol represented by formula (2) below is 70% or more and a selectivity of a lactone represented by formula (3) below is 5% or less in a total amount of reaction products. [chemical 2] (In the formula, R 2 represents a single bond, a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylene group, a trimethylene group, a vinylene group, a 1-methylvinylene group, a methylideneethylene group, a propenylene group, a 1-butenylene group, a 2-butenylene group, a 1,3-butadienylene group, a 1-pentenylene group, or a 2-pentenylene group.
3. The catalyst is a metal species M 1 and M. 2 A, M 1 M per mole 2 The method for producing an alcohol according to claim 1 or 2, wherein the amount of
4. Amount of catalyst used (M 1 The method for producing an alcohol according to any one of claims 1 to 3, wherein the amount of the aryl group (calculated as metal) is 0.01 to 30 mol % of the substrate.
5. The method for producing an alcohol according to any one of claims 1 to 3, wherein the reduction reaction is carried out in the presence of water.
6. The metal species is as follows: 1 and M. 2 The catalyst for reducing a monocarboxylic acid, a hydroxycarboxylic acid, or a dicarboxylic acid is supported on the following carrier and is used for reducing a carboxyl group of a substrate represented by the following formula (1a), (1b), or (1c) to obtain the corresponding alcohol. (M 1 )platinum (M 2 )molybdenum (Support) Zirconium oxide with a specific surface area of 10 to 50 m 2 / g [C3] (In the formula, R 1 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkenyl group having 2 to 5 carbon atoms; R 2 represents a single bond, a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylene group, a trimethylene group, a vinylene group, a 1-methylvinylene group, a methylideneethylene group, a propenylene group, a 1-butenylene group, a 2-butenylene group, a 1,3-butadienylene group, a 1-pentenylene group, or a 2-pentenylene group.
Citation Information
Patent Citations
Hydrogenation catalysts prepared by high surface area sol-gel route
JP2002536164A
Improved catalyst and method for producing alcohols by hydrogenation over this catalyst
JP2006505399A
Method for producing alcohol compound
JP2015074619A
Production of 1,6-hexanediol from adipic acid
JP2016532704A