Method for producing a positive electrode material and a method for producing a positive electrode using the same
A positive electrode material with an organic/inorganic composite modified layer addresses interfacial resistance and crack issues in solid-state batteries, enhancing conductivity and safety in lithium ion batteries.
Patent Information
- Application Number
- JP2022173478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-09
- Filing Date
- 2022-10-28
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-12-09
AI Technical Summary
High interfacial resistance and crack formation between electrodes and solid electrolytes in solid-state batteries, which degrade cycle performance and high rate discharge capability.
Development of a positive electrode material with a modified layer composed of an organic/inorganic composite material, formed by bonding an ionically conductive ceramic compound and an organic conductive compound using a coupling agent, to create a stable solid electrolyte interface (SEI) that enhances ionic and electronic conductivity.
The modified layer reduces interfacial resistance, increases high rate discharge capability, and improves safety and heat dissipation in lithium ion batteries.
Smart Images

Figure 0007556007000012 
Figure 0007556007000013 
Figure 0007556007000014
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a positive electrode material, and a method for producing a positive electrode. [Background technology]
[0002] Conventional liquid electrolyte lithium-ion batteries have a high energy storage cost per unit due to their low mass energy density and limited life span. To further improve the safety of downstream applications, the development of solid-state batteries, in which solid electrolytes are used instead of conventional liquid electrolytes, has become a goal. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Publication No. 20130149587 Summary of the Invention [Problem to be solved by the invention]
[0004] In the development of such solid-state batteries, high interfacial resistance between the electrodes and the solid electrolyte is a problem. The use of lithium-containing oxides modified with inorganic ceramic conductors is considered to be one of the solutions to the high ionic conductivity of inorganic ceramic conductors. However, cracks may easily occur between the inorganic ceramic conductors and the lithium-containing oxides, which may reduce cycle performance and high-rate discharge capability. [Means for solving the problem]
[0005] According to an embodiment of the present disclosure, the present disclosure provides a cathode material for use in a battery cathode, for example, a lithium-ion battery cathode. The cathode material may include active particles and a modified layer covering or encapsulating the active particles. According to an embodiment of the present disclosure, the modified layer may be a reaction product of a composition, which may include an ion-conducting ceramic compound, an organic conductive compound, and a coupling agent. According to an embodiment of the present disclosure, the ion-conducting ceramic compound is 50 to 84 parts by weight, the organic conductive compound is 16 to 50 parts by weight, and the total weight of the ion-conducting ceramic compound and the organic conductive compound is 100 parts by weight. According to an embodiment of the present disclosure, the coupling agent is 0.05 wt% to 10 wt% relative to the total weight of the ion-conducting ceramic compound and the organic conductive compound.
[0006] According to some embodiments of the present disclosure, the present disclosure provides a positive electrode, for example a positive electrode of a lithium ion battery. The positive electrode may include a positive electrode current collector layer and a positive electrode active layer, and the positive electrode active layer may be disposed on the positive electrode current collector layer. The positive electrode active layer may include a positive electrode material of the present disclosure, a conductive additive, and a binder.
[0007] According to some embodiments of the present disclosure, the present disclosure provides a battery, such as a lithium ion battery, which may include a positive electrode of the present disclosure, a separator, and a negative electrode, the negative electrode being separated from the positive electrode by the separator. Effect of the Invention
[0008] Compared with the positive electrode material using the modified layer made of inorganic material, the crack propagation of the modified layer is suppressed due to the design of the components of the positive electrode material of the present disclosure (made of organic / inorganic composite material). In addition, the modified layer made of organic / inorganic composite material can form a stable solid electrolyte interface (SEI), so that the positive electrode material simultaneously exhibits ionic conductivity and electronic conductivity, thereby reducing the interface resistance and enhancing the high C-rate discharge capacity. Furthermore, the heat dissipation of the active particles containing high nickel content can be reduced, and the safety of the use of lithium-ion batteries can be further improved. [Brief description of the drawings]
[0009] Detailed description will be given in the following embodiments with reference to the accompanying drawings. [Figure 1] FIG. 2 is a cross-sectional view of a cathode material according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view of a positive electrode for use in a battery according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 is a schematic diagram of a battery according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The method for manufacturing the positive electrode material and the method for manufacturing the positive electrode are described in detail in the following description. In the following detailed description, for the purpose of explanation, numerous specific details and embodiments are set forth in order to fully understand the present disclosure. The specific components and configurations described in the following detailed description are set forth in order to clearly explain the present disclosure. However, it will be apparent that the exemplary embodiments shown herein are merely used for the purpose of explanation, and the inventive concept can be embodied in various forms without being limited to these exemplary embodiments. Furthermore, in order to clearly explain the present disclosure, similar and / or corresponding symbols may be used in the figures of different embodiments to indicate similar and / or corresponding components. However, the use of similar and / or corresponding symbols in the figures of different embodiments does not imply any correlation between the different embodiments.
[0011] The present disclosure provides a method for preparing a positive electrode material, which includes dispersing an organic conductive compound and a coupling agent in a first solvent to obtain a first solution, adding an ionically conductive ceramic compound to the first solution to obtain a first mixture, heating the mixture at 50-100°C for 60-240 minutes to obtain a second solution, mixing the second solution with active particles to obtain a second mixture, stirring the second mixture at 50-100°C for 60-240 minutes to obtain a resultant, and calcining the resultant at 90-150°C for 30-360 minutes to obtain a positive electrode material.
[0012] The present disclosure provides a method for preparing a positive electrode, which includes dispersing a positive electrode material, a conductive additive, and a binder in a second solvent to obtain a positive electrode slurry, applying the positive electrode slurry to a surface of a positive electrode current collecting layer by a coating process to obtain a coating, and subjecting the coating to a drying process to obtain a positive electrode active layer.
[0013] The present disclosure provides a cathode material for use in a battery cathode, for example, a lithium-ion battery cathode. The cathode material of the present disclosure includes active particles and a modified layer covering the surface of the active particles. The modified layer is an organic / inorganic composite material, which is prepared by combining an organic conductive compound with an ion-conductive ceramic compound with a coupling agent. In some embodiments, the modified layer encapsulates the active particles. Compared with a cathode material using a modified layer made of an inorganic material, the crack propagation in the modified layer is suppressed due to the design of the components of the cathode material of the present disclosure (composed of an organic / inorganic composite material). In addition, the modified layer made of an organic / inorganic composite material can form a stable solid electrolyte interface (SEI), so that the cathode material simultaneously exhibits ionic conductivity and electronic conductivity, thereby reducing the interface resistance and enhancing the high C-rate discharge capability. Furthermore, the heat dissipation of the active particles containing a high nickel content can be reduced, and the safety of the use of the lithium-ion battery can be further improved.
[0014] The cathode material of the present disclosure, the conductive additive, and the binder can be dispersed in a solvent to form a cathode slurry. The cathode slurry can be coated on a cathode current collector layer and baked to form a cathode. The cathode of the present disclosure is suitable for use as a cathode of a battery (e.g., a lithium-ion battery). The lithium-ion battery using the cathode of the present disclosure is safer, has a higher discharge capacity at high C-rates, and has a longer life.
[0015] According to an embodiment of the present disclosure, the present disclosure provides a cathode material for use in forming a battery cathode, for example, a lithium-ion battery cathode. As shown in FIG. 1, the cathode material 10 can include active particles 12 and a modified layer 14 covering or encapsulating the active particles 12. According to an embodiment of the present disclosure, the modified layer can be a reaction product of a composition. According to an embodiment of the present disclosure, the composition can include an ion-conducting ceramic compound, an organic conductive compound, and a coupling agent. According to an embodiment of the present disclosure, the ion-conducting ceramic compound can be 50 to 84 parts by weight (e.g., 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, or 80 parts by weight), the organic conductive compound can be 16 to 50 parts by weight (e.g., 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, or 45 parts by weight), and the total weight of the ion-conducting ceramic compound and the organic conductive compound is 100 parts by weight. According to embodiments of the present disclosure, the coupling agent may be 0.05 wt % to 10 wt % (e.g., 0.1 wt %, 0.2 wt %, 0.5 wt %, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt %, 6 wt %, 7 wt %, 8 wt %, or 9 wt %) based on the total weight of the ionically conductive ceramic compound and the organic conductive compound.
[0016] According to an embodiment of the present disclosure, the weight ratio of the ion-conductive ceramic compound to the organic conductive compound (or the compound derived from the organic conductive compound) in the modified layer is determined by the weight ratio of the ion-conductive ceramic compound to the organic conductive compound in the composition. According to an embodiment of the present disclosure, the weight ratio of the ion-conductive ceramic compound to the organic conductive compound (or the compound derived from the organic conductive compound) in the modified layer is about 5:1 to 3:2, for example about 4:1, about 3:1, or 2:1. If the amount of the ion-conductive ceramic compound in the modified layer is too high, the performance of the battery may be deteriorated (i.e., the energy density relative to the capacity and weight is reduced). If the amount of the ion-conductive ceramic compound in the modified layer is too low, the performance of the battery may be deteriorated due to poor ion conductivity.
[0017] According to an embodiment of the present disclosure, the addition of an organic conductive compound to the composition allows the network structure of the organic conductive compound to encapsulate the ion-conductive ceramic compound by the coupling agent, thereby avoiding the formation of cracks in the modified layer. As a result, the ion-conductive ceramic compound is prevented from peeling off from the active particles. In addition, the modified layer composed of the organic / inorganic composite material can form a stable solid electrolyte interface (SEI) on the surface of the active particles. As a result, the positive electrode material exhibits ionic conductivity and electronic conductivity at the same time, which reduces the interface resistance and enhances the high-rate discharge capacity. In addition, the heat dissipation of the active particles containing a high nickel content can be reduced, and the safety of the use of lithium-ion batteries can be further improved.
[0018] According to an embodiment of the present disclosure, the ionically conductive ceramic compound may be a doped or undoped titanium-containing phosphate, which has the structure of formula (I): Has:
[0019] Li x M y Ti z (PO4) t Formula (I)
[0020] where M can be Al, Fe, or Cr; ≦ x ≦ 3;0.1 ≦ y ≦ 3;1 ≦ z ≦ 3; and 1 ≦ t ≦3. For example, x can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, or 3; y can be 0.4, 0.8, 1, 1.2, 1.4, 1.5, 1.6, 1.7, 2, 2.5, or 3; z can be 1, 1.2, 1.4, 1.5, 1.6, 1.7, 2, 2.5, or 3; and t can be 1, 1.2, 1.4, 1.5, 1.6, 1.7, 2, 2.5, 2.9, or 3. For example, M is Al, x is 2, y is 1, z is 1, and t is 3. For example, M is Fe, x is 1.5, y is 0.8, z is 1.2, and t is 2.9. For example, M is Cr, x is 2, y is 1.2, z is 2, and t is 3.
[0021] According to an embodiment of the present disclosure, when the ion-conducting ceramic compound is a doped titanium-containing phosphate and M is Al or Fe, the doped titanium-containing phosphate is doped with an element, which is Cr, Zr, Sn, Ge, S, or a combination thereof. According to an embodiment of the present disclosure, when the ion-conducting ceramic compound is a doped titanium-containing phosphate and M is Cr, the doped titanium-containing phosphate is doped with an element, which is Zr, Sn, Ge, S, or a combination thereof. According to an embodiment of the present disclosure, the dose of the doped element is 1×10 with respect to the total atomic weight of the titanium-containing phosphate. -9 For example, when M is Al, the doped elements are Cr and S, and the dose of Cr is 0.0024 atom % and the dose of S is 0.005 atom %.
[0022] According to an embodiment of the present disclosure, the titanium-containing phosphate may be a lithium titanium-containing phosphate, such as lithium aluminum titanium phosphate, lithium iron titanium phosphate, or lithium chromium titanium phosphate. According to an embodiment of the present disclosure, the lithium titanium-containing phosphate may be a doped lithium aluminum titanium phosphate, or a doped lithium iron titanium phosphate, and the doped element may be Cr, Zr, Sn, Ge, S, or a combination thereof. According to an embodiment of the present disclosure, the lithium titanium-containing phosphate may be a doped lithium chromium titanium phosphate, and the doped element may be Zr, Sn, Ge, S, or a combination thereof.
[0023] According to embodiments of the present disclosure, the organic conductive compound can be a compound having an aniline moiety, a compound having a pyrrole moiety, a compound having a maleimide moiety, or a compound having an imino moiety.
[0024] According to an embodiment of the present disclosure, the organic conductive compound of the present disclosure may be a polymer, such as polyaniline, polyacetylene, polyphenylvinylene, poly-p-phenylene, polypyrrole, polythiophene, polyimide, maleimide compound, or a combination thereof. The weight average molecular weight of the polymer may be about 10,000 to 1,000,000, such as about 30,000 to 1,000,000, 30,000 to 900,000, 50,000 to 800,000, 80,000 to 750,000, or 100,000 to 600,000. The polydispersity index (PDI) of the polymer may be about 1.3 to 3.0, such as 1.5, 1.7, 1.9, 2.1, 2.3, 2.5, 2.7, or 2.9.
[0025] According to an embodiment of the present disclosure, the organic conductive compound may be a maleimide compound, which may be a maleimide, a bismaleimide, or a combination thereof. According to an embodiment of the present disclosure, the maleimide may have a structure represented by formula (II) or formula (III).
[0026] [ka]
[0027] In the formula, R a is C 1-8 alkyl groups, -RNH2, -C(O)CH3, -CH2OCH3, -CH2S(O)CH3, -C6H5, -CH2(C6H5)CH3, phenylene, diphenylene, cycloaliphatics, or silane-substituted aromatic compounds; Y is H, C 1-8 Alkyl group, -S(O)-R c , -CONH2, or -C(CF3)3; R b are independently H, F, Cl, Br, HSO3, SO2, or C 1-8 R is an alkyl group; 1-8 is an alkylene group; R c is C 1-8 It is an alkyl group.
[0028] According to an embodiment of the present disclosure, C 1-8 The alkyl group may be a straight chain or branched alkyl group. For example, 1-8 The alkyl group may be methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, or an isomer thereof. 1-8 The alkylene group may be a straight chain or branched alkylene group. For example, 1-8 The alkylene groups can be methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene or isomers thereof.
[0029] According to embodiments of the present disclosure, the maleimide can be maleimide-phenylmethane, phenyl-maleimide, methylphenyl maleimide, dimethylphenyl-maleimide, ethylenemaleimide, thio-maleimid, ketone-maleimid, methylene-maleinimid, maleinimidomethylether, maleimido-ethanediol, 4-phenylether-maleimid, 4-maleimido-phenylsulfone, or combinations thereof.
[0030] According to embodiments of the present disclosure, the bismaleimide may have a structure represented by formula (IV) or formula (V).
[0031] [ka]
[0032] In the formula, R d is C 1-8 an alkylene group, -RNHR-, -C(O)CH2-, -CH2OCH2-, -C(O)-, -O-, -OO-, -S-, -SS-, -S(O)-, -CH2S(O)CH2-, -(O)S(O)-, -C6H5-, -CH2(C6H5)CH2-, -CH2(C6H5)(O)-, phenylene, diphenylene, substituted phenylene, or substituted diphenylene; R e is C 1-8 an alkylene group, -C(O)-, -C(CH3)2-, -O-, -OO-, -S-, -SS-, -(O)S(O)-, or -S(O)-; R is C 1-8 It is an alkylene group.
[0033] According to an embodiment of the present disclosure, the bismaleimide may be N,N'-bismaleimide-4,4'-diphenylmethane, [1,1'-(methylenedi-4,1-phenylene)bismaleimide], or [N,N'-(1,1'-biphenyl-4,4'-diyl)bismaleimide]. bismaleimide]), [N,N'-(4-methyl-1,3-phenylene)bismaleimide]), [1,1'-(3,3'dimethyl-1,1'-biphenyl-4,4'-diyl)bismaleimide]), N,N'-ethylenedimaleimide, [N,N'-(1,2-phenylene)dimaleimide]), [N,N'-(1,3-phenylene)dimaleimide] phenylene)dimaleimide]), N,N'-thiodimaleimide, N,N'-dithiodimaleimide, N,N'-ketonedimaleimide, N,N'-methylene-bis-maleimide, bis-maleinimidomethyl-ether, [1,2-bis-(maleimido)-1,2-ethanediol], N,N'-4,4'-diphenylether-bis-maleimid, [4,4'-bis(maleimido)-diphenylsulfone]4'-bis(maleimido)-diphenylsulfone], or a combination thereof.
[0034] According to embodiments of the present disclosure, the coupling agent may include at least one compound having the structure of formula (VI):
[0035] [ka]
[0036] In the formula, R 1 , R 2 , R 3 and R 4 are independently -OH, -OC n H 2n+1 , -C n H 2n NH2, -C n H 2n SH, -C n H 2n NCO, -C n H 2n NHCONH2, or -C n H 2n O.C.O.C.H.R. 5 and R 1 , R 2 , R 3 and R 4 At least one of the following is -C n H 2n NH2, -C n H 2n SH, -C n H 2n NCO, -C n H 2n NHCONH2, or -C n H 2n O.C.O.C.H.R. 5 n is an integer from 1 to 5; R 5 are independently hydrogen or methyl.
[0037] According to an embodiment of the present disclosure, the coupling agent may be a compound having the structure of formula (VI). For example, the coupling agent may be 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane (ATPES), 3-mercaptopropyltrimethoxysilane (MPTMS), 3-mercaptopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxy ... The silane may be 3-ureidopropyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, or a combination thereof.
[0038] According to an embodiment of the present disclosure, the active particles may be a lithium-containing oxide. For example, the lithium-containing oxide may be lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (LNCM), lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, or a combination thereof.
[0039] According to an embodiment of the present disclosure, the particle size of the active particles may be 1 μm to 20 μm. If the particle size of the active particles is too small, the dispersibility of the active particles will be insufficient. If the particle size of the active particles is too large, the conductivity of the active particles will be insufficient.
[0040] According to an embodiment of the present disclosure, the modified layer may be 0.1 wt % to 10 wt % of the total weight of the cathode material, i.e., the weight ratio of the modified layer to the total weight of the cathode material is about 0.001 to 0.1, such as about 0.002, 0.005, 0.01, 0.02, 0.05, or 0.08.
[0041] According to an embodiment of the present disclosure, the modified layer includes an organic conductive compound, and the organic conductive compound has a network structure. A chemical bond is formed between the organic conductive compound and the ion-conducting ceramic compound by using a coupling agent.
[0042] According to an embodiment of the present disclosure, a method for making a cathode material may include the following steps: First, an organic conductive compound and a coupling agent are dispersed or dissolved in a solvent to obtain a first solution. The solvent may be, for example, N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), pyrrolidone, N-dodecylpyrrolidone, γ-butyrolactone, or a combination thereof. The solid content of the first solution may be 1 wt% to 20 wt% based on the total weight of the first solution. Then, the first solution is stirred at 25-90°C for 10-120 minutes, and an ion-conductive ceramic compound is added to the solution to obtain a mixture. Here, the weight ratio of the ion-conductive ceramic compound to the organic conductive compound is about 5:1 to 3:2, and the coupling agent may be 0.05 wt% to 10 wt% (based on the total weight of the ion-conductive ceramic compound and the organic conductive compound). The mixture is then heated at 50-100° C. for 60-240 minutes to obtain a second solution. The second solution is then mixed with active particles, and the mixture is stirred at 50-100° C. for 60-240 minutes. The resultant is then baked at 90-150° C. for 30-360 minutes to obtain the cathode material of the present disclosure.
[0043] According to an embodiment of the present disclosure, the present disclosure also provides a positive electrode for use in a battery (e.g., a lithium ion battery). According to an embodiment of the present disclosure, as shown in FIG. 2, a positive electrode 20 includes a positive electrode current collecting layer 22 and a positive electrode active layer 24 disposed on the positive electrode current collecting layer 22. According to an embodiment of the present disclosure, the positive electrode active layer 24 includes the above-mentioned positive electrode material, a conductive additive, and a binder.
[0044] According to an embodiment of the present disclosure, a positive electrode 20 of the present disclosure for use in a battery (eg, a lithium ion battery) may comprise a positive electrode current collecting layer 22 and a positive electrode active layer 24 .
[0045] According to an embodiment of the present disclosure, in the positive electrode active layer 24, based on the total weight of the positive electrode material, the conductive additive, and the binder, the weight percentage of the positive electrode material may be about 96 wt % to 99.8 wt % (e.g., about 96.5 wt %, 97 wt %, 97.5 wt %, 98 wt %, 98.5 wt %, 99 wt %, or 99.5 wt %), and the weight percentage of the conductive additive may be about 0.1 wt % to 2 wt % (e.g., about 0.1 wt % to 2 wt %). The weight percentage of the binder may be about 0.2 wt%, 0.4 wt%, 0.6 wt%, 0.8 wt%, 1.0 wt%, 1.2 wt%, 1.4 wt%, 1.6 wt%, or 1.8 wt%, and the weight percentage of the binder may be about 0.1 wt% to 2 wt% (e.g., about 0.2 wt%, 0.4 wt%, 0.6 wt%, 0.8 wt%, 1.0 wt%, 1.2 wt%, 1.4 wt%, 1.6 wt%, or 1.8 wt%). If the amount of the conductive additive is too small, the charge and discharge performance of the battery may be poor. If the amount of the conductive additive is too large, the capacity of the battery may be reduced. If the amount of the binder is too small, the positive electrode active layer may not be formed. If the amount of the binder is too large, a hard and brittle positive electrode active layer 24 may be formed.
[0046] According to an embodiment of the present disclosure, the conductive additive may be a conductive additive used in the positive electrode of a lithium battery, such as carbon black, conductive graphite, carbon nanotubes, carbon fibers, or graphene. According to an embodiment of the present disclosure, the binder may include polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose, polyvinylidene fluoride (PVDF), styrene-butadiene copolymer, fluororubber, polyurethane, polyvinylpyrrolidone, poly(ethyl acrylate), polyvinyl chloride (PVC), polyacrylonitrile (PAN), polybutadiene, polyacrylic acid (PAA), or a combination thereof. Because the binder is added, the positive electrode active layer 24 can be disposed directly on the positive electrode current collecting layer 22, which prevents the positive electrode active layer 24 from peeling off from the positive electrode current collecting layer 22.
[0047] According to embodiments of the present disclosure, the binder used in the positive electrode may include polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose, polyvinylidene fluoride (PVDF), styrene-butadiene copolymer, fluororubber, polyurethane, polyvinylpyrrolidone, poly(ethyl acrylate), polyvinyl chloride (PVC), polyacrylonitrile (PAN), polybutadiene, polyacrylic acid (PAA), or a combination thereof.
[0048] According to embodiments of the present disclosure, the positive electrode current collecting layer 22 may include a metal foil, such as aluminum foil, carbon-coated aluminum foil, stainless steel foil, or other metal foils (eg, platinum, titanium, etc.).
[0049] According to an embodiment of the present disclosure, a method for fabricating a positive electrode may include the following steps. First, a positive electrode material, a conductive additive, and a binder are dispersed in a solvent (e.g., N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), pyrrolidone, N-dodecylpyrrolidone, γ-butyrolactone, or a combination thereof) to obtain a positive electrode slurry. The solid content of the positive electrode slurry is 40 wt% to 80 wt%. Then, a positive electrode current collecting layer is prepared. Then, the positive electrode slurry is applied to the surface of the positive electrode current collecting layer by a coating process. The coating process may be screen printing, spin coating, bar coating, blade coating, roller coating, solvent casting, or dip coating. Then, the coating is subjected to a drying process (process temperature 90 to 180° C.) to obtain a positive electrode active layer. This completes the process for fabricating a positive electrode of the present disclosure.
[0050] According to an embodiment of the present disclosure, the present disclosure also provides a battery 100, for example a lithium-ion battery, as shown in FIG. 3. The battery 100 includes the above-mentioned positive electrode 20, separator 30, and negative electrode 40, and the negative electrode 40 is separated from the positive electrode 20 by the separator 30. According to an embodiment of the present disclosure, the battery 100 may further include an electrolyte solution 50, which is disposed between the positive electrode 20 and the negative electrode 40. The positive electrode, separator, and negative electrode are stacked together and immersed in the electrolyte solution 50. That is, the battery 100 is filled with the electrolyte solution. According to some embodiments of the present disclosure, the positive electrode active layer 24 of the present disclosure is disposed between the separator 30 and the positive electrode current collecting layer 22.
[0051] According to an embodiment of the present disclosure, a battery 100 of the present disclosure may be comprised of a positive electrode 20, a separator 30, a negative electrode 40, and an electrolyte solution 50.
[0052] According to an embodiment of the present disclosure, the material of the separator 30 includes an insulating material, such as polyethylene (PE), polypropylene (PP), polytetrafluoroethylene film, polyamide film, polyvinyl chloride film, poly(vinylidene fluoride) film, polyaniline film, polyimide film, nonwoven fabric, polyethylene terephthalate, polystyrene (PS), cellulose, or a combination thereof. For example, the separator can be a PE / PP / PE multilayer composite structure. According to an embodiment of the present disclosure, the separator can have a porous structure. That is, the pores of the separator are uniformly distributed throughout the separator.
[0053] According to an embodiment of the present disclosure, the electrolyte solution 50 may include a solvent and a lithium salt (or a lithium-containing compound). According to an embodiment of the present disclosure, the solvent may be an organic solvent, such as an ester solvent, a ketone solvent, a carbonate solvent, an ether solvent, an alkane solvent, an amide solvent, or a combination thereof. According to embodiments of the present disclosure, the solvent may be 1,2-diethoxyethane, 1,2-dimethoxyethane, 1,2-dibutoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), methyl acetate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl acetate (PA), gamma-butyrolactone (GBL), ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate, butylene carbonate, dipropyl carbonate, or combinations thereof. According to an embodiment of the present disclosure, the lithium salt (or lithium-containing compound) may be LiPF6, LiClO4, lithium bis(fluorosulfonyl)imide (LiFSI), lithium oxalyl difluoroborate (LiDFOB), LiBF4, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2CF2CF3)2, LiAsF6, LiSbF6, LiAlCl4, LiGaCl4, LiNO3, LiC(SO2CF3)3, LiSCN, LiO3SCF2CF3, LiC6F5SO3, LiO2CCF3, LiSO3F, LiB(C6H5)4, LiB(C2O4)2(LiBOB), LiFePO4, Li7La3Zr2O 12 , LiLaTi2O6, Li 2.9 PO 3.3 N 0.46 , Li3PO4, Li 1.3 Al 0.3 Ti 0.7 (PO4)3, Li 3.6 S 0.6 P 0.4 O4, Li5La3Ta2O 12 , or a combination thereof.
[0054] According to embodiments of the present disclosure, the negative electrode 40 may include a negative electrode current collecting layer 42 and a negative electrode active layer 44 disposed on the negative electrode current collecting layer 42, the negative electrode active layer 44 including a negative electrode material. In some embodiments, the negative electrode active layer further includes a binder, where the weight percentage of the negative electrode material may be about 98 wt % to 99.9 wt % (e.g., about 98.5 wt %, 99 wt %, or 99.5 wt %) and the weight percentage of the binder may be about 0.1 wt % to 2 wt % (e.g., about 0.2 wt %, 0.4 wt %, 0.6 wt %, 0.8 wt %, 1.0 wt %, 1.2 wt %, 1.4 wt %, 1.6 wt %, or 1.8 wt %) based on the total weight of the negative electrode material and the binder. According to an embodiment of the present disclosure, the binder used in the negative electrode may include polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose, polyvinylidene fluoride (PVDF), styrene-butadiene copolymer, fluororubber, polyurethane, polyvinylpyrrolidone, poly(ethyl acrylate), polyvinyl chloride (PVC), polyacrylonitrile (PAN), polybutadiene, polyacrylic acid (PAA), or a combination thereof. According to an embodiment of the present disclosure, the negative electrode current collecting layer may be a metal foil, such as copper foil, nickel foil, or aluminum foil.
[0055] According to some embodiments of the present disclosure, the anode active layer 44 is disposed between the separator 30 and the anode current collecting layer 42. According to embodiments of the present disclosure, the anode material includes a carbonaceous material, lithium, a transition metal oxide, a lithium-containing compound, a silicon-containing compound, or a combination thereof. According to embodiments of the present disclosure, the carbonaceous material may include mesocarbon microbeads (MCMB), vapor grown carbon fibers (VGCF), carbon nanotubes (CNTs), graphene, coke, graphite, carbon black, acetylene black, carbon fibers, or a combination thereof. According to embodiments of the present disclosure, the lithium-containing compounds may include LiAl, LiMg, LiZn, Li3Bi, Li3Cd, Li3Sb, Li4Si, Li 4.4 Pb, Li 4.4 Sn, LiC6, Li3FeN2, Li 2.6 Co0.4 N, or Li 2.6 Cu 0.4 According to an embodiment of the present disclosure, the silicon-containing compound may include silicon oxide, carbon-modified silicon oxide, silicon carbide, a pure-silicon material, or a combination thereof. According to an embodiment of the present disclosure, the transition metal oxide may include Li4Ti5O 12 , or TiNb2O7.
[0056] In the following, exemplary embodiments will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily understand. The concept of the present invention is not limited to the exemplary embodiments shown herein, but may be embodied in various forms. For clarity, the description of well-known parts will be omitted, and similar reference numerals will refer to similar components throughout. EXAMPLES
[0057] Example 1: Polyaniline (PANI) (commercially available from Chanmol Biotech Co., Ltd. under the trade name CM-PAD9901) was dispersed or dissolved in N-methylpyrrolidone (NMP) to obtain a polyaniline solution. The solid content of this polyaniline solution was 5 wt% (i.e., the weight ratio of PANI to NMP was 5:95). Then, 3-aminopropyltriethoxysilane (ATPES) (which serves as a coupling agent) was added to the polyaniline solution. The weight ratio of ATPES to PANI was 1:100. Then, the resulting solution was uniformly stirred at 25°C for 60 minutes, and then lithium aluminum titanium phosphate (LATP) (commercially available from NEI under the trade name Nanoyte® LATP) (the molar ratio of Li / Al / Ti / PO4 was 2 / 1 / 1 / 3) was added to the solution to obtain a mixture. The weight ratio of LATP to PANI was 2:1. Then, the mixture was stirred at 70°C for 180 minutes to obtain a slurry (1).
[0058] Example 2: TIFF0007556007000004.tif39115 was dispersed or dissolved in N-methylpyrrolidone (NMP) to obtain a maleimide solution. The solid content of the maleimide solution was 5 wt% (i.e., the weight ratio of maleimide to NMP was 5:95). Then, 3-aminopropyltriethoxysilane (ATPES) (which serves as a coupling agent) was added to the maleimide solution. The weight ratio of ATPES to maleimide was 0.2:100. Then, the resulting solution was stirred uniformly at 25°C for 60 minutes, and then lithium aluminum titanium phosphate (LATP) (commercially available from NEI under the trade name Nanoyte® LATP) (the molar ratio of Li / Al / Ti / PO4 was 2 / 1 / 1 / 3) was added to the solution to obtain a mixture. The weight ratio of LATP to maleimide was 3:2. Then, the mixture was stirred at 70°C for 180 minutes to obtain a slurry (2).
[0059] Example 3: Polyaniline (PANI) (commercially available from Chanmol Biotech Co., Ltd. under the trade name CM-PAD9901) (purity 99.2%) was dispersed or dissolved in N-methylpyrrolidone (NMP) to obtain a polyaniline solution. The solid content of the polyaniline solution was 5 wt% (i.e., the weight ratio of PANI to NMP was 5:95). Then, 3-aminopropyltriethoxysilane (ATPES) (which serves as a coupling agent) was added to the polyaniline solution. The weight ratio of ATPES to PANI was 2:100. Then, the resulting solution was stirred uniformly at 25°C for 60 minutes, and then lithium aluminum titanium phosphate (LATP) (commercially available from NEI under the trade name Nanoyte® LATP) (molar ratio of Li / Al / Ti / PO4 was 2 / 1 / 1 / 3) was added to the solution to obtain a mixture. The weight ratio of LATP to PANI was 4:1. The mixture was then stirred at 70° C. for 180 minutes to obtain a slurry (3).
[0060] Example 4: TIFF0007556007000005.tif39115 was dispersed or dissolved in N-methylpyrrolidone (NMP) to obtain a maleimide solution. The solid content of the maleimide solution was 5 wt% (i.e., the weight ratio of maleimide to NMP was 5:95). Then, 3-mercaptopropyltrimethoxysilane (MPTMS) (which serves as a coupling agent) was added to the maleimide solution. The weight ratio of MPTMS to maleimide was 0.2:100. Then, the obtained solution was uniformly stirred at 25°C for 60 minutes, and then lithium aluminum titanium phosphate (LATP) (commercially available from NEI under the trade name Nanoyte® LATP) (the molar ratio of Li / Al / Ti / PO4 was 2 / 1 / 1 / 3) was added to the solution to obtain a mixture. The weight ratio of LATP to maleimide was 3:2. Then, the mixture was stirred at 70°C for 180 minutes to obtain a slurry (4).
[0061] Example 5: Polypyrrole (PPy) (available from Sigma-Aldrich under the trade name 577030) was dispersed or dissolved in N-methylpyrrolidone (NMP) to obtain a polypyrrole solution. The solid content of the polypyrrole solution was 5 wt% (i.e., the weight ratio of PPy to NMP was 5:95). Then, 3-aminopropyltriethoxysilane (ATPES) (which serves as a coupling agent) was added to the polypyrrole solution. The weight ratio of ATPES to PPy was 1:100. Then, the resulting solution was uniformly stirred at 25°C for 60 minutes, and then lithium aluminum titanium phosphate (LATP) (available from NEI under the trade name Nanoyte® LATP) (the molar ratio of Li / Al / Ti / PO4 was 2 / 1 / 1 / 3) was added to the solution to obtain a mixture. The weight ratio of LATP to PPy was 3:2. Then, the mixture was stirred at 100°C for 150 minutes to obtain a slurry (5).
[0062] Example 6: TIFF0007556007000006.tif39115 and polyaniline (PANI) (commercially available from Chanmol Biotech Co., Ltd. under the trade name CM-PAD9901) were dispersed or dissolved in N-methylpyrrolidone (NMP) to obtain a solution. The weight ratio of polyaniline to maleimide was 1:4. The solid content of the solution was 5 wt% (i.e., the ratio of the total weight of maleimide and polyaniline to the weight of NMP was 5:95). Then, 3-aminopropyltriethoxysilane (ATPES) (which serves as a coupling agent) was added to the solution. The ratio of the weight of APTES to the total weight of maleimide and polyaniline was 0.1:100. The resulting solution was then stirred at 90° C. for 60 minutes, and then lithium aluminum titanium phosphate (LATP) (commercially available from NEI under the trade name Nanoyte® LATP) (Li / Al / Ti / PO4 molar ratio of 2 / 1 / 1 / 3) was added to the solution to obtain a mixture. The ratio of the weight of LATP to the total weight of maleimide and polyaniline was 1:1. The mixture was then stirred at 70° C. for 180 minutes to obtain a slurry (6).
[0063] The amounts of starting materials and slurries (1) to (6) are shown in Table 1:
[0064] [Table 1]
[0065] Example 1 The slurry (1) of Preparation Example 1 (solid content: 1 part by weight) and 96.83 parts by weight of lithium nickel cobalt manganese oxide (LiNi i Mn j Co kO2, i: 0.83-0.85; j: 0.4-0.5; and k: 0.11-0.12) (commercially available from Ningbo Ronbay New Energy Technology Co., Ltd. under the trade name NMC811-S85E) were mixed and stirred at 60 °C for 120 minutes to obtain modified lithium nickel cobalt manganese oxide (solid content 97.83 parts by weight). Then, 0.99 parts by weight of conductive carbon (commercially available from TimCal Co. under the trade name super-p), carbon nanotube solution (carbon nanotubes dissolved in NMP) (solid content 2.2%, solid content 0.3 parts by weight), and 1.39 parts by weight of binder (commercially available from Solvay SA under the trade name PVDF5130) were mixed with the modified lithium nickel cobalt manganese oxide. After stirring uniformly, a lithium ion battery positive electrode slurry was obtained.
[0066] The lithium-ion battery cathode slurry was then applied to an aluminum foil (which would become the cathode current collector layer) (12 μm thick, commercially available from An Chuan Enterprise Co., Ltd.). After drying, a cathode with an cathode active layer was obtained. Then, an anode (the anode active layer was a mixture of SiO / C (silicon oxide and carbon) (commercially available under the trade name KYX-2 from Kaijin New Energy Technology Co., Ltd.), and the anode current collector layer was a copper foil (commercially available under the trade name BFR-F from Chang Chun Group)) and a separator (commercially available under the trade name Celgard 2320 from Asahi Kasei) were prepared. The anode, separator, and cathode were then arranged in order and sealed in a jelly roll (size 65 mm (height) × 55 mm (width) × 65 mm (length)). An electrolyte solution (containing LiPF6 salt and a solvent, the solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) (the volume ratio of EC to DEC is 1:1, and the concentration of LiPF6 is 1.1M) was injected into the jelly roll to obtain a battery. Then, the battery was tested. The results are shown in Table 2.
[0067] Example 2 A battery was obtained by carrying out Example 2 in the same manner as Example 1, except that the slurry (1) of Preparation Example 1 was replaced with the slurry (2) of Preparation Example 2. The battery was then tested. The results are shown in Table 2.
[0068] Example 3 A battery was obtained by carrying out Example 3 in the same manner as Example 1, except that the slurry (1) of Preparation Example 1 was replaced with the slurry (3) of Preparation Example 3 and the solid content of the slurry was increased from 1 part by weight to 1.5 parts by weight. The battery was then tested. The results are shown in Table 2.
[0069] Example 4 A battery was obtained by carrying out Example 4 in the same manner as Example 1, except that the slurry (1) of Preparation Example 1 was replaced with the slurry (4) of Preparation Example 4. The battery was then tested. The results are shown in Table 2.
[0070] Example 5 A battery was obtained by carrying out Example 5 in the same manner as Example 1, except that the slurry (1) of Preparation Example 1 was replaced with the slurry (5) of Preparation Example 5. The battery was then tested. The results are shown in Table 2.
[0071] [Table 2]
[0072] Here, the sheet resistance of the positive electrode was measured by four-probe resistivity measurement; the adhesion of the electrode was measured by a tensile tester; the battery resistance was measured by battery internal resistance measurement; the discharge capacity and discharge rate were measured by a battery charge / discharge system; and the heat release of the battery was measured by a differential scanning calorimeter.
[0073] Example 6 A battery was obtained by carrying out Example 6 in the same manner as Example 1, except that the slurry (1) of Preparation Example 1 was replaced with the slurry (6) of Preparation Example 6. The battery was then tested. The results are shown in Table 3.
[0074] Example 7 A battery was obtained by carrying out Example 7 in the same manner as Example 1, except that the solid content of the slurry (1) was increased from 1 part by weight to 5 parts by weight. Then, the battery was tested. The results are shown in Table 3.
[0075] Example 8 A battery was obtained by carrying out Example 8 in the same manner as Example 3, except that the solid content of the slurry (3) was reduced from 1 part by weight to 0.5 parts by weight. Then, the battery was tested. The results are shown in Table 3.
[0076] Example 9 A battery was obtained by carrying out Example 9 in the same manner as Example 6, except that the solid content of the slurry (6) was increased from 1 part by weight to 5 parts by weight. Then, the battery was tested. The results are shown in Table 3.
[0077] [Table 3]
[0078] Comparative Example 1 Standard lithium-ion battery cathode slurry (97.3% NMC811(LiNi i Mn j Co kO2, i: 0.83-0.85; j: 0.4-0.5; and k: 0.11-0.12) (commercially available from Ningbo Ronbay New Energy Technology Co., Ltd. under the trade name NMC811-S85E), 1% Super-P (conductive carbon powder) (commercially available from TimCal Co.), and 1.4% PVDF-5130, 0.3% carbon nanotubes (commercially available from OCSiAl under the trade name TUBALL® BATT NMP 0.4% PVDF SOLVAY SOLEF® 5130)) were applied onto an aluminum foil (to be the positive electrode current collecting layer) (12 μm thick, commercially available from An Chuan Enterprise Co., Ltd.). After drying, a positive electrode having a positive electrode active layer was obtained. Then, a negative electrode was prepared. The negative electrode active layer was SiO / C (commercially available under the trade name KYX-2 from Kaijin New Energy Technology Co., Ltd.), and the negative electrode current collecting layer was copper foil (commercially available under the trade name BFR-F from Chang Chun Group). A separator (commercially available under the trade name Celgard 2320) was prepared. Then, the negative electrode, the separator, and the positive electrode were arranged in order and sealed in a jelly roll (size 65 mm (height) × 55 mm (width) × 65 mm (length)). An electrolyte solution (containing LiPF6 and a solvent, the solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio of EC to DEC is 1:1, and the concentration of LiPF6 is 1.1 M) was injected into the jelly roll to obtain a battery. Then, the battery was tested. The results are shown in Table 4.
[0079] Comparative Example 2 Standard lithium-ion battery cathode slurry (97.3% NMC811(LiNi i Mn j Co kO2, i: 0.83-0.85; j: 0.4-0.5; and k: 0.11-0.12) (commercially available from Ningbo Ronbay New Energy Technology Co., Ltd. under the trade name NMC811-S85E), 1% Super-P (conductive carbon powder) (commercially available from TimCal Co.), 1.4% PVDF-5130, and 0.3% carbon nanotubes (commercially available from OCSiAl under the trade name TUBALL™ BATT NMP 0.4% PVDF SOLVAY SOLEF™ 5130)) were applied onto an aluminum foil (to be the positive electrode current collecting layer) (12 μm thick, commercially available from An Chuan Enterprise Co., Ltd.). After drying, a positive electrode having a positive electrode active layer was obtained. Then, a negative electrode was prepared. The negative electrode active layer was SiO / C (commercially available under the trade name KYX-2 from Kaijin New Energy Technology Co., Ltd.), and the negative electrode current collecting layer was copper foil (commercially available under the trade name BFR-F from Chang Chun Group). A separator (commercially available under the trade name Celgard 2320) was prepared. Then, the negative electrode, separator, and positive electrode were arranged in order and sealed in a jelly roll (size 65 mm (height) × 55 mm (width) × 65 mm (length)). An electrolyte solution (containing LiPF6 and a solvent, the solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio of EC to DEC is 1:1, and the concentration of LiPF6 is 1.1 M) was injected into the jelly roll. Then, the battery was tested. The results are shown in Table 4.
[0080] Comparative Example 3 Standard lithium-ion battery cathode slurry (97.3% NMC811(LiNi i Mn j Co kO2, i: 0.83-0.85; j: 0.4-0.5; and k: 0.11-0.12) (commercially available from Ningbo Ronbay New Energy Technology Co., Ltd. under the trade name NMC811-S85E), 1% Super-P (conductive carbon powder) (commercially available from TimCal Co.), 1.4% PVDF-5130, and 0.3% carbon nanotubes (commercially available from OCSiAl under the trade name TUBALL™ BATT NMP 0.4% PVDF SOLVAY SOLEF™ 5130)) were applied onto an aluminum foil (to be the positive electrode current collecting layer) (12 μm thick, commercially available from An Chuan Enterprise Co., Ltd.). After drying, a positive electrode having a positive electrode active layer was obtained. Then, a negative electrode was prepared. The negative electrode active layer was SiO / C (commercially available under the trade name KYX-2 from Kaijin New Energy Technology Co., Ltd.), and the negative electrode current collecting layer was copper foil (commercially available under the trade name BFR-F from Chang Chun Group). A separator (commercially available under the trade name Celgard 2320) was prepared. Then, the negative electrode, separator, and positive electrode were arranged in order and sealed in a jelly roll (size 65 mm (height) × 55 mm (width) × 65 mm (length)). An electrolyte solution (containing LiPF6 and a solvent, the solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio of EC to DEC is 1:1, and the concentration of LiPF6 is 1.1 M) was injected into the jelly roll. Then, the battery was tested. The results are shown in Table 4.
[0081] Comparative Example 4 Standard lithium-ion battery cathode slurry (97.3% NMC811(LiNi i Mn j Co kO2, i: 0.83-0.85; j: 0.4-0.5; and k: 0.11-0.12) (commercially available from Ningbo Ronbay New Energy Technology Co., Ltd. under the trade name NMC811-S85E), 1% Super-P (conductive carbon powder) (commercially available from TimCal Co.), 1.4% PVDF-5130, and 0.3% carbon nanotubes (commercially available from OCSiAl under the trade name TUBALL™ BATT NMP 0.4% PVDF SOLVAY SOLEF™ 5130)) were applied onto an aluminum foil (to be the positive electrode current collecting layer) (12 μm thick, commercially available from An Chuan Enterprise Co., Ltd.). After drying, a positive electrode having a positive electrode active layer was obtained. Then, a negative electrode was prepared. The negative electrode active layer was SiO / C (commercially available under the trade name KYX-2 from Kaijin New Energy Technology Co., Ltd.), and the negative electrode current collecting layer was copper foil (commercially available under the trade name BFR-F from Chang Chun Group). A separator (commercially available under the trade name Celgard 2320) was prepared. Then, the negative electrode, separator, and positive electrode were arranged in order and sealed in a jelly roll (size 65 mm (height) × 55 mm (width) × 65 mm (length)). An electrolyte solution (containing LiPF6 and a solvent, the solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio of EC to DEC is 1:1, and the concentration of LiPF6 is 1.1 M) was injected into the jelly roll. Then, the battery was tested. The results are shown in Table 4.
[0082] Comparative Example 5 Standard lithium-ion battery cathode slurry (97.3% NMC811(LiNi i Mn j Co kO2, i: 0.83-0.85; j: 0.4-0.5; and k: 0.11-0.12) (commercially available from Ningbo Ronbay New Energy Technology Co., Ltd. under the trade name NMC811-S85E), 1% Super-P (conductive carbon powder) (commercially available from TimCal Co.), 1.4% PVDF-5130, and 0.3% carbon nanotubes (commercially available from OCSiAl under the trade name TUBALL™ BATT NMP 0.4% PVDF SOLVAY SOLEF™ 5130)) were applied onto an aluminum foil (to be the positive electrode current collecting layer) (12 μm thick, commercially available from An Chuan Enterprise Co., Ltd.). After drying, a positive electrode having a positive electrode active layer was obtained. Then, a negative electrode was prepared. The negative electrode active layer was SiO / C (commercially available under the trade name KYX-2 from Kaijin New Energy Technology Co., Ltd.), and the negative electrode current collecting layer was copper foil (commercially available under the trade name BFR-F from Chang Chun Group). A separator (commercially available under the trade name Celgard 2320) was prepared. Then, the negative electrode, separator, and positive electrode were arranged in order and sealed in a jelly roll (size 65 mm (height) × 55 mm (width) × 65 mm (length)). An electrolyte solution (containing LiPF6 and a solvent, the solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio of EC to DEC is 1:1, and the concentration of LiPF6 is 1.1 M) was injected into the jelly roll. Then, the battery was tested. The results are shown in Table 4.
[0083] [Table 4]
[0084] As shown in Tables 2 to 4, when the positive electrode of a lithium ion battery is made of the positive electrode material of the present disclosure, the sheet resistance of the positive electrode of the lithium ion battery and the adhesion of the electrode can be improved. Furthermore, the resistance and heat dissipation of the battery are reduced, and the high-rate discharge capacity is improved.
[0085] It will be apparent that various modifications and variations can be made to the methods and materials disclosed. It is intended that the specification and examples be considered as exemplary only, with the true scope of the disclosure being indicated by the following claims and their equivalents. [Explanation of symbols]
[0086] 10…Positive electrode material 12…Active particles 13...Modification layer 20...Positive electrode 22...Positive electrode current collecting layer 24...Cathode active layer 30…Separator 40...Negative electrode 42...Negative electrode current collecting layer 44...Negative electrode active layer 50...Electrolyte solution 100...battery
Claims
1. Dispersing an organic conductive compound and a coupling agent in a first solvent to obtain a first solution; adding an ion-conductive ceramic compound to the first solution to obtain a first mixture, wherein the first mixture consists solely of the organic conductive compound, the coupling agent, the first solvent, and the ion-conductive ceramic compound; heating the mixture at 50-100°C for 60-240 minutes to obtain a second solution; mixing the second solution with the active particles to obtain a second mixture; The second mixture is stirred at 50-100°C for 60-240 minutes to obtain a resultant product. and calcining the resultant at 90 to 150°C for 30 to 360 minutes to obtain a positive electrode material.
2. 2. The method of claim 1, wherein the weight ratio of the ion-conducting ceramic compound to the organic conductive compound is 5:1 to 3:
2.
3. 10. The method of claim 1, wherein the coupling agent is 0.05 wt% to 10 wt% based on the total weight of the ion-conducting ceramic compound and the organic conductive compound.
4. 2. The method of claim 1, wherein the ion-conducting ceramic compound is a doped or undoped titanium-containing phosphate, the titanium-containing phosphate having the structure of formula (I): Li x M y Ti z (PO 4 ) t Formula (I) wherein M is Al, Fe, or Cr; 0.1≦x≦3; 0.1≦y≦3; 1≦z≦3; and 1≦t≦3.
5. 5. The method of claim 4, wherein the ion-conducting ceramic compound is the doped titanium-containing phosphate, and M is Al or Fe, and the doped element is Cr, Zr, Sn, Ge, S, or a combination thereof.
6. 5. The method of claim 4, wherein the ion-conducting ceramic compound is the doped titanium-containing phosphate, and M is Cr, and the doped element is Zr, Sn, Ge, S, or a combination thereof.
7. 5. The method of claim 4, wherein the titanium-containing phosphate is lithium aluminum titanium phosphate, lithium iron titanium phosphate, or lithium chromium titanium phosphate.
8. The method of claim 1 , wherein the organic conductive compound is a compound having an aniline moiety, a pyrrole moiety, a maleimide moiety, or an imino moiety.
9. 2. The method of claim 1, wherein the organic conductive compound is polyaniline, polyacetylene, polyphenylvinylene, poly-p-phenylene, polypyrrole, polythiophene, polyimide, maleimide compound, or a combination thereof.
10. 10. The method of claim 1, wherein the coupling agent comprises at least one compound having the structure of formula (VI): 【Chemistry 3】 (In the formula, R 1 , R 2 , R 3 and R 4 are independently -OH, -OC n H 2n+1 , -C n H 2n NH 2 , -C n H 2n SH or -C n H 2n OCOCHC HR 5 and R 1 , R 2 , R 3 and R 4 At least one of the following is -C n H 2n NH 2 , -C n H 2n SH, -C n H 2n NCO, -C n H 2n NHCONH 2 , or -C n H 2n OCOCHCH R 5 n is independently an integer from 1 to 5; R 5 are independently hydrogen or a methyl group.)
11. The coupling agent is a compound having a structure of formula (VI), and the coupling agent is selected from the group consisting of 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane (ATPES), 3-mercaptopropyltrimethoxysilane (MPTMS), 3-mercaptopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 11. The method of claim 10, wherein the silane is 3-ureidopropyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, or a combination thereof.
12. 2. The method of claim 1, wherein the active particles are a lithium-containing oxide, and the lithium-containing oxide is lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (LNCM), lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, or a combination thereof.
13. Dispersing a positive electrode material, a conductive additive, and a binder in a second solvent to obtain a positive electrode slurry, wherein the positive electrode material is prepared by the method of any one of claims 1 to 12; The positive electrode slurry is applied to the surface of the positive electrode current collecting layer in a coating step to obtain a coating film; and The method for producing a positive electrode includes subjecting the coating to a drying step to obtain a positive electrode active layer.
14. 14. The method of claim 13, wherein the conductive additive comprises carbon black, conductive graphite, carbon nanotubes, carbon fiber, or graphene.
15. 14. The method of claim 13, wherein in the positive electrode active layer, based on the total weight of the positive electrode material, the conductive additive, and the binder, the weight percentage of the positive electrode material is 96 wt % to 99.8 wt %, the weight percentage of the conductive additive is 0.1 wt % to 2 wt %, and the weight percentage of the binder is 0.1 wt % to 2 wt %.
Citation Information
Patent Citations
Mixed polymer-coated core-shell composite positive electrode material, preparation method thereof and application in lithium ion battery
CN107706377A
Lithium ion secondary battery
JP2007242303A
Electrode active material for secondary battery and electrode for secondary battery
JP2015069878A
Battery electrode paste composition
JP2016146322A
Lithium ion battery additive, electrode slurry composition, and lithium ion battery
JP2017117792A