Method for producing AEI zeolite

JP7556210B2Active Publication Date: 2024-09-26TOSOH CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020092047
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-29
Filing Date
2020-05-27
Publication Date
2024-09-26
Estimated Expiration
2040-05-27

AI Technical Summary

Benefits of technology

【0011】 本開示により、出発原料として結晶性アルミノシリケートを使用しない従来のAEI型ゼオライトの製造方法と比べ、窒素酸化物還元触媒及びその担体として適したアルミナに対するシリカのモル比、を有するAEI型ゼオライトが、より短時間の結晶化、なおかつ、高い収率で得られ得る製造方法、又は工業的な適用が期待できるAEI型ゼオライトの製造方法、の少なくとも1つを提供すること、ができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556210000001
    Figure 0007556210000001
Patent Text Reader

Abstract

To provide at least one of a method for producing an AEI-type zeolite having a molar ratio of silica to alumina suitable as a nitrogen oxide reduction catalyst and a carrier thereof through a shorter time of crystallization in a higher yield than a conventional method for producing an AEI-type zeolite not using a crystalline aluminosilicate as a starting raw material, and a method for producing the AEI-type zeolite expected for industrial application.SOLUTION: A method for producing an AEI-type zeolite comprises a step of hydrothermally treating an amorphous composition containing an amorphous silica source, an amorphous alumina source, an alkali source and water, and then crystallizing a raw material composition obtained by mixing the amorphous composition with an organic structure-directing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing AEI zeolite. [Background technology]

[0002] AEI zeolite is a crystalline aluminosilicate that is being considered for use as a catalyst for olefin production and a selective catalytic reduction catalyst (so-called SCR catalyst). AEI zeolite is a zeolite synthesized by using Y zeolite as a starting material and subjecting the Y zeolite to structural transformation (Patent Document 1).

[0003] However, since Y-type zeolite is expensive, a method for producing AEI-type zeolite that does not use Y-type zeolite as a starting material has been investigated. To date, methods for producing AEI-type zeolite have been reported that use, as starting materials other than Y-type zeolite, crystalline aluminosilicates other than Y-type zeolite (Patent Document 2), amorphous aluminosilicates (Patent Documents 3 and 4, Non-Patent Document 1), and amorphous compounds such as silica, such as fumed silica, and aluminum hydroxide (Patent Document 5). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] U.S. Patent No. 5,958,370 [Patent Document 2] JP 2017-48105 A [Patent Document 3] JP 2017-36204 A [Patent Document 4] JP 2017-39638 A [Patent Document 5] International Publication No. 2016 / 080547 [Non-patent literature]

[0005] [Non-Patent Document 1] The 33rd Zeolite Research Symposium, A12 (2017) Summary of the Invention [Problem to be solved by the invention]

[0006] A method for producing AEI zeolite that does not use crystalline aluminosilicate as a starting material is expected to be industrially applicable. However, in the conventionally reported methods for producing AEI zeolite that use a starting material other than crystalline aluminosilicate, it is necessary to perform crystallization for a long time to increase the yield. The present disclosure aims to provide at least one of a production method that can crystallize AEI zeolite having a molar ratio of silica to alumina suitable for a nitrogen oxide reduction catalyst and its support in a shorter time and in a higher yield than conventional methods for producing AEI zeolite that do not use crystalline aluminosilicate as a starting material, or a production method for AEI zeolite that is expected to be industrially applicable. [Means for solving the problem]

[0007] The present inventors have investigated a method for producing AEI zeolite using a starting material other than crystalline aluminosilicate. As a result, they have found that AEI zeolite can be efficiently crystallized from an amorphous raw material by focusing on the relationship between the state of the raw material in the composition during crystallization and the organic structure-directing agent.

[0008] In other words, the gist of the present disclosure is as follows. [1] A method for producing an AEI zeolite, comprising: subjecting an amorphous composition containing an amorphous silica source, an amorphous alumina source, an alkali source, and water to hydrothermal treatment; and then mixing the amorphous composition with an organic structure-directing agent to obtain a raw material composition, and crystallizing the raw material composition. [2] The method for producing an AEI zeolite according to the above [1], wherein the raw material composition contains at least one of a silica source, an alumina source, an alkali source, and water. [3] The method for producing an AEI zeolite according to the above [1] or [2], wherein the molar ratio of hydroxide ions to silica in the raw material composition is 0.40 or less. [4] The method for producing AEI zeolite according to any one of [1] to [3] above, wherein the raw material composition does not contain Y zeolite.

[0009] [5] The method for producing an AEI zeolite according to any one of the above [1] to [4], wherein the amorphous composition has the following molar composition: where M is an alkali metal. SiO2 / Al2O3 ratio = 12 or more, 25 or less Na / SiO2 ratio = 0.05 or more, 0.3 or less M / SiO2 ratio = 0.05 or more, 0.4 or less OH / SiO2 ratio = 0.1 or more, 0.4 or less H2O / SiO2 ratio = 8 or more, less than 20

[0010] [6] The method according to any one of the above [1] to [5], wherein the raw material composition has the following molar composition: M is an alkali metal, and SDA is an organic structure directing agent. SiO2 / Al2O3 ratio = 20 or more, 50 or less Na / SiO2 ratio = 0.05 or more, 0.3 or less M / SiO2 ratio = 0.05 or more, 0.5 or less SDA / SiO2 ratio = 0.1 or more, 0.3 or less OH / SiO2 ratio = 0.1 or more, 0.4 or less H2O / SiO2 ratio = 8 or more, less than 20 [7] The method for producing an AEI zeolite according to any one of [1] to [6] above, wherein the fluorine content of the raw material composition is 100 ppm by mass or less. Effect of the Invention

[0011] The present disclosure makes it possible to provide at least one of the following: a production method by which an AEI zeolite having a molar ratio of silica to alumina suitable for a nitrogen oxide reduction catalyst and its support can be crystallized in a shorter time and obtained in a higher yield, as compared with conventional production methods for AEI zeolite that do not use crystalline aluminosilicate as a starting raw material; or a production method for AEI zeolite that is expected to be industrially applicable. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the method for producing AEI zeolite according to the present disclosure will be described with reference to an example of an embodiment.

[0013] The present embodiment is a method for producing an AEI zeolite, which is characterized by including a step of hydrothermally treating an amorphous composition containing an amorphous silica source, an amorphous alumina source, an alkali source, and water, and then mixing the amorphous composition with an organic structure-directing agent to obtain a raw material composition, and crystallizing the raw material composition.

[0014] The AEI zeolite obtained by the production method of this embodiment is a zeolite having an AEI structure, and in particular, is a crystalline aluminosilicate having an AEI structure.

[0015] The zeolite structure in this embodiment is a structure defined by the IZA Structure Committee, and the "AEI structure" is a structure that is an AEI type in terms of structure code. The AEI structure can be identified by comparing it with either the powder X-ray diffraction (hereinafter referred to as "XRD") pattern described in Collection of simulated XRD powder patterns for zeolites, Fifth revised edition, p. 23 (2007) or the XRD pattern described in AEI of Zeolite Framework Types on the IZA Structure Committee homepage http: / / www.iza-struture.org / databases / .

[0016] "Crystalline aluminosilicate" is a composite compound of crystalline silica and alumina having a skeletal structure consisting of a repetition of a network of aluminum (Al) and silicon (Si) via oxygen (O). In this embodiment, the terms skeletal structure, crystal structure, and crystal phase are all used interchangeably.

[0017] The AEI zeolite obtained by the production method of this embodiment is, for example, a crystalline aluminosilicate having an XRD pattern equivalent to that of SSZ-39.

[0018] In the production method of the present embodiment, an amorphous composition containing an amorphous silica source, an amorphous alumina source, an alkali source, and water is subjected to hydrothermal treatment. The hydrothermal treatment produces structural units capable of inducing AEI zeolite in the amorphous composition, which is believed to facilitate the promotion of crystallization of AEI zeolite in the subsequent step.

[0019] The amorphous alumina source is an aluminum-containing compound other than crystalline aluminosilicate, or aluminum (Al), and examples thereof include one or more selected from the group consisting of aluminum hydroxide, aluminum oxide, aluminum sulfate, aluminum chloride, aluminum nitrate, amorphous aluminosilicate, metallic aluminum, pseudoboehmite, alumina sol, and aluminum alkoxide, and is preferably one or more selected from the group consisting of aluminum hydroxide, aluminum oxide, aluminum sulfate, aluminum chloride, aluminum nitrate, amorphous aluminosilicate, alumina sol, and aluminum alkoxide. From an industrial viewpoint, the amorphous alumina source is preferably one or more selected from the group consisting of aluminum hydroxide, aluminum oxide, aluminum sulfate, aluminum chloride, and amorphous aluminosilicate, more preferably one or more selected from the group consisting of aluminum hydroxide, aluminum oxide, aluminum sulfate, aluminum chloride, and amorphous aluminosilicate, even more preferably one or more selected from the group consisting of aluminum oxide, aluminum sulfate, aluminum chloride, and amorphous aluminosilicate, and even more preferably amorphous aluminosilicate.

[0020] The amorphous silica source is a silicon-containing compound other than a crystalline aluminosilicate or silicon (Si), and examples thereof include one or more selected from the group consisting of silica sol, fumed silica, colloidal silica, precipitated silica, amorphous silicic acid, and amorphous aluminosilicate, and is preferably at least one of amorphous silicic acid and amorphous aluminosilicate.

[0021] Particularly preferred amorphous alumina sources and amorphous silica sources include amorphous aluminosilicates having a molar ratio of silica to alumina (hereinafter also referred to as the "SiO2 / Al2O3 ratio") of more than 0.7 and less than 2000 (silica content of more than 20 mass% and less than 100 mass%), 5 or more and 300 or less (silica content of 64 mass% or more and 99 mass% or less), further 10 or more and 200 or less (silica content of 78 mass% or more and 98 mass% or less), and even 10 or more and 90 or less (silica content of 78 mass% or more and 97 mass% or less). In another embodiment, the SiO2 / Al2O3 ratio in the amorphous aluminosilicate as the amorphous alumina source and the amorphous silica source is 5 or more, 10 or more, 13 or more, or 15 or more, and is less than 2000, 300 or less, 200 or less, 90 or less, 50 or less, 30 or less, or 25 or less.

[0022] In the production method of the present embodiment, the production cost is reduced by using an amorphous compound as a starting material, making it an industrially more suitable production method. Therefore, it is preferable that the amorphous composition does not contain FAU type zeolite, particularly Y type zeolite.

[0023] The alkali source is an alkali metal or a compound containing an alkali metal element, and examples of the alkali source include one or more selected from the group consisting of hydroxides, carbonates, sulfates, chlorides, bromides, and iodides of alkali metals. One or more selected from the group consisting of hydroxides, chlorides, bromides, and iodides is preferred, and hydroxide is more preferred.

[0024] The alkali metal (element) may be one or more selected from the group consisting of sodium, potassium, rubidium, and cesium, with at least one of sodium and potassium being preferred, and sodium being more preferred.

[0025] The alkali metal may be sodium alone, but since there is a tendency for structural units capable of deriving AEI zeolite to be easily produced, the alkali metal (element) is preferably sodium and one or more selected from the group consisting of potassium, rubidium, and cesium, and more preferably potassium and sodium.

[0026] The water may be distilled water, deionized water, or pure water, and further, water derived from other components contained in the amorphous composition, such as water-containing compounds, can also be considered as water in the amorphous composition.

[0027] The amorphous composition may not include seed crystals, whereas the amorphous composition may include a sufficiently small amount of seed crystals relative to the amorphous silica source and the amorphous alumina source, which tends to promote the formation of structural units that can lead to AEI zeolite.

[0028] Examples of seed crystals to be mixed with the amorphous composition include one or more selected from the group consisting of AEI zeolite, CHA zeolite, OFF zeolite, ERI zeolite, FER zeolite, HEU zeolite, MOR zeolite, KFI zeolite, AFX zeolite, AFT zeolite, EAB zeolite, GME zeolite, and LEV zeolite. As a preferred composition of the amorphous composition, the molar ratio of silica to alumina (SiO2 / Al2O3 ratio) is, in molar proportions, 5 to 50, 10 to 30, 10 to 29, or 15 to 25, the molar ratio of alkali metal to silica (hereinafter also referred to as "M / SiO2 ratio") is 0.1 to 0.6, 0.1 to 0.4, 0.1 to 0.3, or 0.1 to 0.2, and the ratio of hydroxide ions (OH) to silica is 0.01 to 0.02, and the ratio of silica to alumina is 0.01 to 0.02. -The molar ratio of water to silica (hereinafter also referred to as "H2O / SiO2 ratio") is, for example, 0.1 or more and 0.6 or less, 0.1 or more and 0.4 or less, 0.1 or more and 0.3 or less, or 0.1 or more and 0.2 or less, and the molar ratio of water to silica (hereinafter also referred to as "H2O / SiO2 ratio") is, for example, 3 or more and 50 or less, 5 or more and 30 or less, or 8 or more and 20 or less.

[0029] When the amorphous composition contains sodium and one or more selected from the group consisting of potassium, rubidium, and cesium, the molar ratio of one or more selected from the group consisting of potassium, rubidium, and cesium to silica (hereinafter, each of these is also referred to as the "K / SiO2 ratio", or collectively as the "(K+Rb+Cs) / SiO2 ratio") is 0 or more and 0.5 or less, preferably 0 or more and 0.3 or less, and more preferably 0 or more and 0.25 or less, and the molar ratio of sodium to silica (hereinafter, also referred to as the "Na / SiO2 ratio") is 0.01 or more and 1.0 or less, preferably 0.05 or more and 0.5 or less, and more preferably 0.1 or more and 0.3 or less.

[0030] The amorphous composition preferably does not contain quaternary ammonium cations or other organic structure directing agents, and particularly preferably does not contain organic structure directing agents that direct the AEI structure.

[0031] It is particularly preferred that the amorphous composition have the following molar composition: where M is an alkali metal (ie, the total alkali metal in the amorphous composition), preferably (Na+K).

[0032] SiO2 / Al2O3 ratio = 12 or more, 25 or less, Preferably 15 or more and 23 or less Na / SiO2 ratio = 0.05 or more, 0.3 or less, Preferably, 0.07 or more and 0.23 or less M / SiO2 ratio = 0.05 or more, 0.4 or less, Preferably, 0.1 or more and 0.3 or less OH / SiO2 ratio = 0.1 or more, 0.4 or less, Preferably, 0.1 or more and 0.3 or less H2O / SiO2 ratio = 8 or more, less than 20 Preferably 10 or more and 18 or less When the alkali metal contained in the amorphous composition is only sodium, the M / SiO2 ratio and the Na / SiO2 ratio have the same value.

[0033] The hydrothermal treatment is preferably performed by treating the amorphous composition at 100°C or higher. By treating the amorphous composition at 100°C or higher, building units capable of forming AEI zeolite in the amorphous composition are easily generated, and the building units are easily grown into composite-building units, which are three-dimensional structural units. From the viewpoint of shortening the treatment time, it is more preferable to perform the hydrothermal treatment under high temperature autogenous pressure using a sealed container. The hydrothermal treatment temperature is 100°C or higher, preferably 130°C or higher, and more preferably 160°C or higher. The hydrothermal treatment temperature does not need to be higher than necessary, and may be, for example, 230°C or lower, preferably 200°C or lower. In the hydrothermal treatment, the amorphous composition may be in either a stirred or stationary state.

[0034] The manufacturing method of this embodiment includes a step of crystallizing a raw material composition obtained by mixing the amorphous composition after the hydrothermal treatment with an organic structure directing agent (hereinafter, also referred to as a "crystallization step"). The crystallization step produces an AEI zeolite from the raw material composition. It is considered that the coexistence of the amorphous composition after the hydrothermal treatment with an organic structure directing agent (hereinafter, also referred to as an "SDA") promotes crystallization of AEI zeolite, and further AEI zeolite having a SiO2 / Al2O3 ratio suitable for a nitrogen oxide reduction catalyst or its support (for example, a SiO2 / Al2O3 ratio of 12.5 to 100, 15 to 50, 15 to 30, 16 to 25, or 18 to 23) compared to crystallizing a composition in which both coexist at the starting raw material stage.

[0035] The SDA may be a cation that is directed toward AEI zeolite. Examples of known cations that are directed toward AEI zeolite include one or more selected from the group consisting of 1,1,3,5-tetramethylpiperidinium cation, 1,1-diethyl-2,6-dimethylpiperidinium cation, 1,1,2,6-tetramethylpiperidinium cation, 1-ethyl-1,2,6-trimethylpiperidinium cation, and 1,1,2-triethylpiperidinium cation. The 1,1,3,5-tetramethylpiperidinium cation (hereinafter referred to as "TMP") may be used. + ") and 1,1-diethyl-2,6-dimethylpiperidinium cation (hereinafter referred to as "DEDMP + " is also called. ) is preferable, and TMP + is more preferred.

[0036] It is sufficient that SDA is contained in the raw material composition in the form of a salt. Examples of the salt of SDA include one or more salts selected from the group consisting of hydroxide, chloride, bromide and iodide of SDA, and preferably one or more salts selected from the group consisting of hydroxide, chloride and bromide of SDA.

[0037] Particularly preferred examples of the salt of SDA include one or more selected from the group consisting of 1,1,3,5-tetramethylpiperidinium hydroxide, 1,1,3,5-tetramethylpiperidinium bromide, and 1,1,3,5-tetramethylpiperidinium chloride, and further includes at least one of 1,1,3,5-tetramethylpiperidinium hydroxide and 1,1,3,5-tetramethylpiperidinium bromide, and further includes 1,1,3,5-tetramethylpiperidinium hydroxide.

[0038] In order to adjust the composition of the amorphous composition and the raw material composition, such as the SiO2 / Al2O3 ratio, in the crystallization step, one or more selected from the group consisting of an alumina source, a silica source, an alkali source, and water, and SDA may be mixed with the amorphous composition after the hydrothermal treatment, and the raw material composition obtained may be crystallized. The SiO2 / Al2O3 ratio of the raw material composition is preferably larger than the SiO2 / Al2O3 ratio of the amorphous composition. It is considered that the SiO2 / Al2O3 ratio of the raw material composition is larger than that of the amorphous composition, which tends to make it difficult to finely disperse the obtained AEI type zeolite. The SiO2 / Al2O3 ratio of the raw material composition can be, for example, 1 or more, 3 or more, 5 or more, 7 or more, or 10 or more higher than the SiO2 / Al2O3 ratio of the amorphous composition.

[0039] The alumina source, silica source, alkali source, and water can be the same as the amorphous alumina source, amorphous silica source, alkali source, and water used in the amorphous composition. In the raw material composition, particularly preferred alumina sources and silica sources include amorphous aluminosilicates. The amorphous aluminosilicate preferably has a SiO2 / Al2O3 ratio of 5 or more, 10 or more, 13 or more, or 15 or more, and is less than 2000, 300 or less, 200 or less, 150 or less, 90 or less, 50 or less, 30 or less, or 25 or less. The raw material composition may contain two or more amorphous aluminosilicates having different SiO2 / Al2O3 ratios.

[0040] Since the crystallization of the AEI zeolite tends to be promoted, the raw material composition may contain a sufficiently small amount of seed crystals relative to the amorphous silica source and the amorphous alumina source.

[0041] The total mass of aluminum and silicon in the raw material composition (excluding the seed crystals) is calculated as Al2O3 and SiO2, respectively, and the raw material composition and the seed crystals are mixed so that the total mass ratio of aluminum and silicon in the seed crystals, calculated as Al2O3 and SiO2, respectively, to the total mass (hereinafter also referred to as "seed crystal content") is 0 mass% or more and 30 mass% or less, further 0.5 mass% or more and 20 mass% or less, further 1 mass% or more and 10 mass% or less, and further 0.5 mass% or more and 5 mass% or less.

[0042] The seed crystals to be mixed with the raw material composition can be exemplified by one or more selected from the group consisting of AEI zeolite, CHA zeolite, OFF zeolite, ERI zeolite, FER zeolite, HEU zeolite, MOR zeolite, KFI zeolite, AFX zeolite, AFT zeolite, EAB zeolite, GME zeolite, and LEV zeolite, preferably one or more selected from the group consisting of CHA zeolite, AEI zeolite, MOR zeolite, and FER zeolite, and preferably at least one of AEI zeolite and CHA zeolite.

[0043] The raw material composition is obtained by mixing the amorphous composition after hydrothermal treatment, SDA, and optionally a silica source, etc., by any method, preferably by mixing the amorphous composition after hydrothermal treatment, SDA, an alumina source, and a silica source, more preferably by mixing the amorphous composition after hydrothermal treatment, SDA, an alumina source, a silica source, and an alkali source. It is also preferable to obtain the raw material composition by mixing a mixture of SDA, a silica source, etc., with the amorphous composition after hydrothermal treatment, for example, by mixing SDA, and optionally an alumina source, a silica source, an alkali source, and water to obtain a mixture, and mixing the amorphous composition after hydrothermal treatment with the mixture.

[0044] Examples of preferred compositions of the raw material composition are, in terms of molar ratio, a SiO2 / Al2O3 ratio of 10 to 100, 15 to 50, 15 to 40, or 15 to 35; a molar ratio of SDA to silica (hereinafter also referred to as "SDA / SiO2 ratio") of 0.05 to 0.5, 0.10 to 0.40, 0.10 to 0.30, 0.10 to 0.20, or 0.10 to 0.16; a M / SiO2 ratio of 0.1 to 0.6, 0.1 to less than 0.3, or 0.1 to 0.25; a OH / SiO2 ratio of 0.1 to 0.5, 0.2 to 0.45, or 0.2 to 0.4; and a H2O / SiO2 ratio of 3 to 50, 5 to 50, 5 to 25, or 7 to 20.

[0045] When the raw material composition contains one or more elements selected from the group consisting of potassium, rubidium, and cesium, and sodium, the (K+Rb+Cs) / SiO2 ratio is, for example, 0 or more and 0.5 or less, 0 or more and 0.3 or less, 0 or more and 0.1 or less, 0 or more and 0.06 or less, more than 0 and 0.5 or less, more than 0 and 0.3 or less, more than 0 and 0.1 or less, or more than 0 and 0.06 or less, and the Na / SiO2 ratio is, for example, 0.01 or more and 1.0 or less, 0.05 or more and 0.4 or less, 0.05 or more and 0.3 or less, or 0.1 or more and 0.25 or less.

[0046] It is particularly preferred that the raw material composition has the following molar composition: where M is an alkali metal (i.e., the total alkali metals in the raw material composition), preferably (Na+K).

[0047] SiO2 / Al2O3 ratio = 20 or more, 50 or less, Preferably 25 or more and 40 or less Na / SiO2 ratio = 0.05 or more, 0.3 or less, Preferably, 0.1 or more and 0.25 or less M / SiO2 ratio = 0.05 or more, 0.5 or less, Preferably, 0.1 or more and 0.3 or less SDA / SiO2 ratio = 0.1 or more, 0.3 or less, Preferably, 0.1 or more and 0.2 or less OH / SiO2 ratio = 0.1 or more, 0.4 or less, Preferably, 0.2 or more and 0.4 or less H2O / SiO2 ratio = 8 or more, less than 20 Preferably 9 or more and 15 or less When the alkali metal contained in the raw material composition is only sodium, the M / SiO2 ratio and the Na / SiO2 ratio are equal in value.

[0048] In the crystallization step, the raw material composition is crystallized. The crystallization is preferably carried out by hydrothermal synthesis. The crystallization temperature is 100°C or higher, preferably 130°C or higher, and more preferably 160°C or higher. The crystallization temperature does not need to be higher than necessary, and may be, for example, 200°C or lower, preferably 180°C or lower. The crystallization temperature may be the same as the temperature of the hydrothermal treatment of the amorphous composition, or may be higher than the temperature of the hydrothermal treatment of the amorphous composition. In the crystallization, the raw material composition may be in either a stirred or static state. This provides a single phase of AEI zeolite, i.e., a zeolite that does not contain any crystalline material identified as having a structure other than the AEI structure in XRD measurement.

[0049] The time for the crystallization step is arbitrary, but may be 10 hours or more and 150 hours or less. In particular, in this embodiment, even if the time for the crystallization step is 100 hours or less, or even less than 80 hours, the yield of AEI zeolite (hereinafter, also simply referred to as "yield") can be 60% or more and 80% or less. Furthermore, even if the time for the crystallization step is 75 hours or less, more preferably less than 72 hours, the yield can be 50% or more and 75% or less. In order to achieve an efficient yield, the time for the crystallization step is preferably 24 hours or more and less than 80 hours, or even more preferably 48 hours or more and 75 hours or less. The time for the crystallization step is the total time for the hydrothermal treatment of the amorphous composition and the crystallization of the raw material composition, in other words, the time until the crystallization of the AEI zeolite is completed and the crystallinity of the AEI structure becomes constant.

[0050] In the crystallization step, the time for hydrothermal treatment of the amorphous composition and the time for crystallization of the raw material composition are arbitrary, and the hydrothermal treatment of the amorphous composition may be performed until the composition of the amorphous composition becomes stable, for example, for 5 hours or more. The time for crystallization of the raw material composition may be the time required for crystallization of the AEI zeolite. For example, the ratio of the time for hydrothermal treatment of the amorphous composition to the time for crystallization of the raw material composition in the crystallization step may be 1:9 to 7:3.

[0051] In this embodiment, the yield is calculated from the following formula.

[0052] Yield (mass%) = W Cry / W Raw ×100 W in the above formula Cry and W Raw are the total masses of Al in terms of Al2O3 and Si in terms of SiO2 in the AEI zeolite and the raw material composition, respectively.

[0053] In order to facilitate the application of manufacturing equipment made of general-purpose materials, the amorphous composition and raw material composition preferably do not contain fluorine (F) and phosphorus (P). The amorphous composition and raw material composition preferably have a fluorine content and phosphorus content of 100 mass ppm or less, more preferably 10 mass ppm or less, and even more preferably below the measurement limit, in a general composition analysis such as ICP measurement.

[0054] The amorphous composition after hydrothermal treatment may be mixed with SDA either intermittently or continuously, or the amorphous composition may be mixed with SDA or the like successively. For example, the amorphous composition after hydrothermal treatment may be cooled, and then the amorphous composition and SDA or the like are mixed to prepare a raw material composition, which is then reheated and crystallized. On the other hand, by mixing SDA or the like with the amorphous composition using a pressure pump or the like, the amorphous composition after hydrothermal treatment may be mixed with SDA without cooling the amorphous composition, and the raw material composition may be continuously crystallized.

[0055] The manufacturing method of this embodiment may include at least one of a washing step, a drying step, an SDA removal step, and an ion exchange step.

[0056] In the washing step, the AEI zeolite and the liquid phase are separated into a solid-liquid separation by a known method, and the AEI zeolite obtained as a solid phase may be washed with pure water.

[0057] The drying step removes moisture physically adsorbed on the AEI zeolite. Drying conditions are arbitrary, and examples of drying methods include leaving the AEI zeolite in the air at 50° C. or higher and 150° C. or lower for 2 hours or longer or drying with a spray dryer.

[0058] The SDA removal step removes SDA contained in the AEI zeolite. Examples of the method for removing SDA include one or more methods selected from the group consisting of a liquid phase treatment with an acidic aqueous solution, an exchange treatment with a resin, a pyrolysis treatment, and a calcination treatment. From the viewpoint of production efficiency, the SDA removal step is preferably at least one of a pyrolysis treatment and a calcination treatment.

[0059] The ion exchange process converts the AEI zeolite into any cation type. For example, the cation type is ammonium (NH4 + In the case of converting the cation type to a proton (H + ) type, ammonium (NH4 + ) type AEI zeolite is calcined in air.

[0060] Examples of the AEI zeolite obtained by the production method of this embodiment (hereinafter also referred to as "AEI zeolite of this embodiment") include AEI zeolites that satisfy at least one of the following: a SiO2 / Al2O3 ratio of 12.2 to 100, preferably 14 to 50, and more preferably 15 to 30; an average crystal size of 0.3 μm to 5.0 μm, preferably 0.4 μm to 3.0 μm, and more preferably 0.5 μm to 3.0 μm; and an acid amount of 0.5 mmol / g to 3 mmol / g, and preferably 1 mmol / g to 2 mmol / g.

[0061] In this embodiment, the "crystal size" refers to the particle size of a primary particle, which is the diameter of an independent particle of the smallest unit observed by an electron microscope. The "average crystal size" refers to the arithmetic mean of the crystal sizes of 30 or more (preferably 50±15) primary particles observed by an electron microscope. Therefore, the secondary particle size and average secondary particle size, which are the diameters of secondary particles formed by agglomeration of a plurality of primary particles, are different from the crystal size and average crystal size. The shape of the primary particles may be at least one of the group consisting of a cubic crystal shape, a tetragonal crystal shape, and a twin crystal shape formed by combining a cubic crystal shape or a tetragonal crystal shape.

[0062] The "acid amount" can be determined by subjecting proton-type AEI zeolite from which organic matter has been removed to an ammonia TPD measurement.

[0063] The AEI zeolite of the present embodiment has high heat resistance and exhibits little decrease in crystallinity before and after exposure to a hydrothermal atmosphere, and preferably exhibits little decrease in crystallinity before and after exposure to a hydrothermal atmosphere compared to conventional AEI zeolite obtained using Y zeolite as a raw material. The degree of decrease in crystallinity due to exposure to a hydrothermal atmosphere can be indexed by the ratio of the crystallinity after exposure to a hydrothermal atmosphere to the crystallinity before exposure to a hydrothermal atmosphere (hereinafter also referred to as "crystallization maintenance rate"). This can be determined by comparing the intensities of XRD peaks before and after exposure to a hydrothermal atmosphere.

[0064] The AEI zeolite of the present embodiment can be used as a catalyst carrier or an adsorbent. Furthermore, by modifying the AEI zeolite of the present embodiment with at least one of copper and iron, it is expected to be used as a catalyst, and further as a nitrogen oxide reduction catalyst. EXAMPLES

[0065] The manufacturing method of this embodiment will be described below with reference to examples, but this embodiment is not limited to these examples.

[0066] (Identification of crystalline phase) XRD measurements of the samples were performed using a general X-ray diffraction device (Ultima IV, manufactured by Rigaku Corporation). The radiation source used was CuKα radiation (λ = 1.5405 Å), and the measurement range was 2θ from 3° to 43°. The obtained XRD pattern was compared with the XRD patterns in Table 1 of Patent Document 1 to identify the structure of the sample. (composition analysis) A sample solution was prepared by dissolving the sample in a mixed aqueous solution of hydrofluoric acid and nitric acid. The sample solution was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) using a general ICP device (device name: OPTIMA5300DV, manufactured by PerkinElmer). The SiO2 / Al2O3 ratio of the sample was calculated from the measured values ​​of Si and Al. (Crystallization maintenance rate) The AEI zeolite sample before and after hydrothermal durability treatment was subjected to XRD measurement in the same manner as for identifying the crystal structure. The obtained XRD pattern was subjected to background removal processing and peak search processing, and the peak intensities of the XRD peaks corresponding to 2θ=16.9±0.2° and 17.2±0.2° were summed up to determine the crystallinity of the AEI zeolite sample. The following formula is used: Crystallinity maintenance rate (%)=(Crystallization degree after hydrothermal durability treatment) ÷ (Degree of crystallinity before hydrothermal durability treatment) × 100 The crystallization retention rate was calculated using the formula:

[0067] Example 1 Pure water, sodium hydroxide, potassium hydroxide, and amorphous aluminosilicate with a SiO2 / Al2O3 ratio of 19 were mixed to obtain a composition having the following molar composition, which was designated as an amorphous composition. The M / SiO2 ratio in the following molar composition indicates the (Na+K) / SiO2 ratio in the amorphous composition. SiO2 / Al2O3 ratio =19 Na / SiO2 ratio =0.12 (K / SiO2 ratio =0.08) M / SiO2 ratio =0.20 H2O / SiO2 ratio =16 OH / SiO2 ratio =0.20

[0068] The amorphous composition was filled into a sealed container and hydrothermally treated at 180°C while stirring, and then the hydrothermally treated amorphous composition was mixed with 1,1,3,5-tetramethylpiperidinium hydroxide (hereinafter also referred to as "TMPOH"), pure water, sodium hydroxide, potassium hydroxide, an amorphous aluminosilicate with a SiO2 / Al2O3 ratio of 20, and an amorphous aluminosilicate with a SiO2 / Al2O3 ratio of 90 to obtain a raw material composition having the following molar composition. The M / SiO2 ratio in the following molar composition indicates the (Na+K) / SiO2 in the raw material composition. SiO2 / Al2O3 ratio =30 Na / SiO2 ratio =0.20 (K / SiO2 ratio =0.04) M / SiO2 ratio =0.24 TMP + / SiO2 ratio =0.13 H2O / SiO2 ratio =12.7 OH / SiO2 ratio =0.37

[0069] After mixing the raw material composition with CHA-type zeolite so that the seed crystal content was 0.9% by mass, the raw material composition was filled into a sealed container and hydrothermally synthesized at 170° C. while stirring. The time required for the crystallization step in this example was 70 hours.

[0070] After the hydrothermal synthesis, the obtained crystallized product was collected by solid-liquid separation, washed with pure water, and dried in air at 110°C. The crystallized product was AEI zeolite with a SiO2 / Al2O3 ratio of 21, and did not contain any crystallized products other than AEI zeolite. The yield was 71% by mass, and the average crystal diameter was 0.55 μm.

[0071] Example 2 The raw material composition was crystallized, washed, and dried in the same manner as in Example 1, except that TMPOH and the like were mixed with the same amorphous composition as in Example 1 so that the raw material composition had the following molar composition. The M / SiO2 ratio in the following molar composition indicates the (Na+K) / SiO2 ratio in the raw material composition. SiO2 / Al2O3 ratio =30 Na / SiO2 ratio =0.21 (K / SiO2 ratio =0.04) M / SiO2 ratio =0.25 TMP + / SiO2 ratio =0.13 H2O / SiO2 ratio =12.7 OH / SiO2 ratio =0.38

[0072] The time required for the crystallization step in this example was 70 hours, and the obtained product was AEI zeolite with a SiO2 / Al2O3 ratio of 20, and did not contain any crystallized products other than AEI zeolite. The yield was 69% by mass.

[0073] Example 3 The raw material composition was crystallized, washed, and dried in the same manner as in Example 1, except that TMPOH and the like were mixed with the same amorphous composition as in Example 1 so that the raw material composition had the following molar composition. The M / SiO2 ratio in the following molar composition indicates the (Na+K) / SiO2 ratio in the raw material composition. SiO2 / Al2O3 ratio =30 Na / SiO2 ratio =0.20 K / SiO2 ratio =0.04 M / SiO2 ratio =0.24 TMP + / SiO2 ratio =0.14 H2O / SiO2 ratio =12.9 OH / SiO2 ratio =0.38

[0074] The time required for the crystallization step in this example was 70 hours, and the obtained product was AEI zeolite with a SiO2 / Al2O3 ratio of 20, and did not contain any crystallized products other than AEI zeolite. The yield was 69% by mass.

[0075] Example 4 The amorphous composition was crystallized in the same manner as in Example 1, except that the composition of the amorphous composition was as follows and a seed crystal was used. SiO2 / Al2O3 ratio =20 Na / SiO2 ratio =0.18 (K / SiO2 ratio =0.01) M / SiO2 ratio =0.19 H2O / SiO2 ratio =12 OH / SiO2 ratio =0.19

[0076] The amorphous composition after crystallization was used to obtain a raw material composition having the following composition. SiO2 / Al2O3 ratio =26 Na / SiO2 ratio =0.22 (K / SiO2 ratio =0.01) M / SiO2 ratio =0.23 TMP + / SiO2 ratio =0.13 H2O / SiO2 ratio =11 OH / SiO2 ratio =0.36

[0077] After the seed crystal content was adjusted to 12.9% by mass, the raw material composition was filled into a sealed container and hydrothermally synthesized at 170°C while stirring. The time required for the crystallization step in this example was 60 hours. The obtained product was AEI zeolite with a SiO2 / Al2O3 ratio of 17, and did not contain any crystallized products other than AEI zeolite. The yield was 65% by mass.

[0078] Comparative Example 1 Referring to the examples of U.S. Patent No. 5,958,370, AEI zeolite was produced using Y zeolite as a starting material. That is, pure water, sodium hydroxide, sodium silicate aqueous solution, Y zeolite with a SiO2 / Al2O3 ratio of 6, and 1,1-diethyl-cis-2,6-dimethylpiperidinium hydroxide (hereinafter also referred to as "DEDMPOH") were mixed to obtain a raw material composition having the following composition. SiO2 / Al2O3 ratio =50 Na / SiO2 ratio =0.56 DEDMPOH / SiO2 ratio =0.16 H2O / SiO2 ratio =44.8 OH / SiO2 ratio =0.72

[0079] The content of zeolite in the raw material composition was 13.9% by mass. The raw material composition was filled in a sealed container and subjected to hydrothermal synthesis at 135°C for 168 hours while stirring. The obtained product was AEI type zeolite with a SiO2 / Al2O3 ratio of 19, and the yield was 40% by mass.

[0080] Comparative Example 2 AEI zeolite was produced by a method according to Example 29 of Patent Document 5. That is, pure water, potassium hydroxide, TMPOH, Al(OH)3, and Snowtex 40 were mixed to obtain a raw material composition having the following composition. SiO2 / Al2O3 ratio =15 K / SiO2 ratio =0.30 TMP + / SiO2 ratio =0.15 H2O / SiO2 ratio =15 OH / SiO2 ratio =0.45

[0081] After mixing 5% by mass of AEI zeolite with the raw material composition, this was filled into a sealed container and subjected to hydrothermal synthesis at 175°C for 48 hours while stirring. The yield was 68% by mass, and the obtained product was AEI zeolite with a SiO2 / Al2O3 ratio of 9.7.

[0082] Comparative Example 3 Pure water, sodium hydroxide, potassium hydroxide, amorphous aluminosilicate with a SiO2 / Al2O3 ratio of 27, and TMPOH were mixed to obtain a raw material composition having the following composition. SiO2 / Al2O3 ratio =27 Na / SiO2 ratio =0.13 K / SiO2 ratio =0.03 M / SiO2 ratio =(Na+K) / SiO2 ratio =0.16 TMP + / SiO2 ratio =0.20 H2O / SiO2 ratio =9.8 OH / SiO2 ratio =0.36

[0083] After mixing 4.3% by mass of AEI zeolite into the raw material composition, the raw material composition was filled into a sealed container and subjected to hydrothermal synthesis at 170°C for 168 hours while stirring. The obtained product was AEI zeolite with a SiO2 / Al2O3 ratio of 18. The yield was 69% by mass.

[0084] Comparative Example 4 The hydrothermal synthesis was carried out in the same manner as in Comparative Example 1, except that the hydrothermal synthesis time was changed to 75 hours.

[0085] The product obtained was only amorphous, and no AEI zeolite was obtained.

[0086] From Comparative Examples 3 and 4, it was confirmed that when a starting material containing SDA was used, crystallization took a long time.

[0087] Measurement example The AEI zeolite obtained in Example 3 was calcined in air at 600° C. for 2 hours to exchange the AEI zeolite into a proton type. The exchanged AEI zeolite was subjected to a hydrothermal durability treatment under the following conditions, and the crystallization retention rate was measured.

[0088] Processing temperature: 900℃ Processing time: 4 hours Treatment atmosphere: Moisture-containing air (10% by volume water, 90% by volume air) Heating rate: 20℃ / min Heating atmosphere: From room temperature to 200℃ under air flow. Above 200℃, under humid air flow For comparison, AEI zeolite produced by structural transformation of Y zeolite (hereinafter also referred to as "comparative sample") was subjected to hydrothermal durability treatment in the same manner, and the crystallization retention rate was measured.

[0089] The crystallization retention rate results are shown in Table 1.

[0090] [Table 1]

[0091] From Table 1, it was confirmed that the AEI zeolite obtained by the production method of this embodiment has a high crystallization maintenance rate after hydrothermal durability treatment, and the crystals are more stable than AEI zeolite obtained by conversion of Y zeolite. Furthermore, it was confirmed that the AEI zeolite obtained by the production method of this embodiment has very high durability, as no change in crystallinity was observed before and after hydrothermal durability treatment at 900°C for 4 hours.

Claims

1. An amorphous composition comprising an amorphous silica source, an amorphous alumina source, an alkali source, and water, and having the following molar composition: SiO 2 / Al 2 O 3 ratio = 12 or more, 25 or less Na / SiO 2 ratio = 0.05 or more, 0.3 or less M / SiO 2 ratio = 0.05 or more, 0.4 or less OH / SiO 2 ratio = 0.1 or more, 0.4 or less H2O / SiO2 ratio = 8 or more and less than 20 (wherein the M / SiO 2 ratio indicates (Na+K) / SiO 2 in the amorphous composition). and then mixing the amorphous composition after the hydrothermal treatment with an organic structure directing agent to obtain a raw material composition having the following molar composition: SiO 2 / Al 2 O 3 ratio = 20 or more, 50 or less Na / SiO 2 ratio = 0.05 or more, 0.3 or less M / SiO 2 ratio = 0.05 or more, 0.5 or less SDA / SiO 2 ratio = 0.1 or more, 0.3 or less OH / SiO 2 ratio = 0.1 or more, 0.4 or less H2O / SiO2 ratio = 8 or more and less than 20 (Note that the M / SiO 2 ratio indicates (Na+K) / SiO 2 in the raw material composition.) A method for producing AEI zeolite, comprising:

2. The method for producing AEI zeolite according to claim 1, wherein the raw material composition contains at least one of a silica source, an alumina source, an alkali source, and water.

3. The method for producing AEI zeolite according to claim 1 or 2, wherein the molar ratio of hydroxide ions to silica in the raw material composition is 0.40 or less.

4. The method for producing AEI zeolite according to any one of claims 1 to 3, wherein the raw material composition does not contain Y zeolite.

5. A method for producing AEI type zeolite described in any one of claims 1 to 4, wherein the duration of the crystallization process is 10 hours or more and 150 hours or less.

6. A method for producing AEI type zeolite described in any one of claims 1 to 5, wherein the average crystal diameter of the AEI type zeolite is 0.3 μm or more and 5.0 μm or less.

7. The method for producing AEI zeolite according to any one of claims 1 to 6, wherein the raw material composition has a fluorine content of 100 ppm by mass or less.

Citation Information

Patent Citations

  • Method for producing AEI type zeolite

    JP2017036204A

  • Manufacturing method of AEI type zeolite

    JP2017039638A

  • Method for producing AE type i zeolite

    JP2017048105A

  • AEI zeolite and manufacturing method and application thereof

    JP2017081809A

  • Aluminosilicate AEI zeolite preparation

    US20170128921A1