Display medium, authenticity determination method, and article including display medium

The display medium uses a first layer reflecting one circularly polarized light and a third layer reflecting the same, with a retardation layer in between, allowing authenticity verification through color differences, addressing the need for expensive viewers in existing technologies.

JP7556351B2Active Publication Date: 2024-09-26ZEON CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2021527577
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-26
Filing Date
2020-06-04
Publication Date
2024-09-26
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

Existing display media require expensive viewers with two circularly polarizing plates to determine authenticity, making it difficult for general users to verify authenticity.

Method used

A display medium comprising a first layer that reflects one circularly polarized light and transmits the opposite, a second retardation layer, and a third layer that reflects the same circularly polarized light as the first, allowing authenticity determination through color differences observed from both sides without a special viewer.

Benefits of technology

Enables authenticity verification using simple observation of color differences without specialized equipment, enhancing accessibility and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556351000012
    Figure 0007556351000012
  • Figure 0007556351000014
    Figure 0007556351000014
  • Figure 0007556351000010
    Figure 0007556351000010
Patent Text Reader

Abstract

Provided is a display medium including a first layer, a second layer, and a third layer, in which: all or part of the first layer, all or part of the second layer, and all or part of the third layer are stacked in this order in a thickness direction; the first layer can reflect circularly polarized light having a rotation direction D1, and can transmit circularly polarized light having a rotation direction D2 which is opposite the rotation direction D1; the second layer is a retardation layer; and the third layer can reflect circularly polarized light of which the rotation direction is the rotation direction D1, and can transmit circularly polarized light of which the rotation direction is the rotation direction D2.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an indication medium, a method for determining authenticity, and an article including the indication medium. [Background technology]

[0002] It is common practice to attach an identification medium that cannot be easily copied to an object to prove its authenticity. As such an identification medium, a medium using a cholesteric liquid crystal compound, which is a polymer compound, is known (Patent Document 1). Also known is an identification medium in which different information is visually recognized on the front and back (Patent Documents 2 to 6). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3652476 [Patent Document 2] JP 2017-185668 A [Patent Document 3] JP 2017-215580 A [Patent Document 4] Patent No. 5828182 [Patent Document 5] International Publication No. 2007 / 007784 (Corresponding Foreign Publication: U.S. Patent Application Publication No. 2008 / 0129036) [Patent Document 6] JP 2007-216602 A Summary of the Invention [Problem to be solved by the invention]

[0004] A material with a circularly polarized light separation function transmits one of right- and left-handed circularly polarized light and reflects part or all of the other circularly polarized light. When a display medium using such a material is observed through a right-handed circular polarizer, a different image appears when observed through a left-handed circular polarizer. Therefore, when determining the authenticity of an item equipped with such a display medium, it is common to use a viewer equipped with two circular polarizers, a right-handed circular polarizer and a left-handed circular polarizer.

[0005] Normally, authenticity determination using a display medium requires a viewer equipped with two circular polarizing plates as described above, which is costly. In addition, since it is difficult for general users to obtain a viewer, it is not easy to determine the authenticity, and in many cases, authenticity is determined by official product manufacturers, some retailers, public institutions, etc.

[0006] Therefore, there has been a demand for a display medium whose authenticity can be determined without using a special viewer; a method for determining the authenticity of a display medium; and an article containing a display medium. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by a display medium including a first layer and a third layer having a circularly polarized light separation function and a second layer that is a retardation layer, thereby completing the present invention. That is, the present invention provides the following.

[0008] [1] A composite material comprising a first layer, a second layer, and a third layer, a part or all of the first layer, a part or all of the second layer, and a part or all of the third layer are overlapped in this order in a thickness direction; the first layer is a layer capable of reflecting circularly polarized light having a rotation direction D1 and transmitting circularly polarized light having a rotation direction D2 that is opposite to the rotation direction D1, The second layer is a retardation layer, The third layer is a layer capable of reflecting circularly polarized light having a rotation direction of the rotation direction D1 and transmitting circularly polarized light having a rotation direction of the rotation direction D2. [2] The display medium according to [1], wherein the first layer is a layer having cholesteric regularity, and the third layer is a layer containing resin flakes having cholesteric regularity. [3] The display medium according to [2], wherein the first layer has a reflectance for unpolarized light of 35% or more and 50% or less in the wavelength range of 420 nm or more and 650 nm or less. [4] The display medium according to [2] or [3], wherein the resin flakes contained in the third layer have a reflectance for unpolarized light of 35% or more and 50% or less in the wavelength range of 420 nm or more and 650 nm or less. [5] The display medium according to any one of [1] to [4], wherein the second layer has a retardation Re in an in-plane direction of 40 nm or more and 1600 nm or less. [6] A step (1) of confirming that the display medium according to any one of [1] to [5] is translucent; a step (2) of irradiating the display medium with unpolarized light from the third layer side and observing the reflected light from the display medium from the third layer side to obtain color information C3 based on the third layer; a step (3) of irradiating the display medium with unpolarized light from the first layer side and observing the reflected light from the display medium from the first layer side to obtain color information C1 based on the first layer; and A step (4) of comparing the color information C3 with the color information C1 and determining that the color information C3 and the color information C1 are not identical. A method for determining authenticity, comprising: [7] An article comprising the display medium described in any one of [1] to [5]. Effect of the Invention

[0009] According to the present invention, it is possible to provide a display medium whose authenticity can be determined without using a special viewer; a method for determining the authenticity of a display medium; and an article including a display medium. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic plan view of a display medium according to one embodiment of the present invention, as viewed from its thickness direction. [Diagram 2] FIG. 2 is a cross-sectional view that diagrammatically shows a cross section taken along the X1-X1 direction in FIG. [Diagram 3] FIG. 3 is an exploded perspective view showing a schematic diagram of a display medium according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram illustrating the state of reflected light from the display medium when unpolarized light is irradiated from the third layer side. [Diagram 5] FIG. 5 is a schematic diagram illustrating the state of reflected light from the display medium when unpolarized light is irradiated from the first layer side. [Figure 6] FIG. 6 is a graph showing the measurement results of the reflectance of the cholesteric resin layer at wavelengths of 400 nm to 780 nm. [Figure 7] FIG. 7 is a side view that illustrates a schematic diagram of an apparatus for producing resin flakes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0012] In the following description, the retardation Re in the in-plane direction of the layer is a value expressed by Re=(nx-ny)×d, unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the layer (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction of the layer and perpendicular to the direction of nx. nz represents the refractive index in the thickness direction of the layer. d represents the thickness of the layer. The measurement wavelength is 560 nm, unless otherwise specified.

[0013] In the following description, unless otherwise specified, a material with positive intrinsic birefringence means a material whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto. Also, a material with negative intrinsic birefringence means a material whose refractive index in the stretching direction is smaller than that in the direction perpendicular thereto. The value of intrinsic birefringence can be calculated from the dielectric constant distribution.

[0014] In the following description, the term "(meth)acrylic" includes "acrylic", "methacrylic" and combinations thereof. In the following description, the term "(thio)epoxy" includes "epoxy", "thioepoxy", and combinations thereof. In the following description, the term "iso(thio)cyanate" includes "isocyanate", "isothiocyanate" and combinations thereof.

[0015] In the following description, "diffuse reflection" means reflection in a direction different from the direction of specular reflection.

[0016] In the following description, the term "visible light region" refers to a wavelength range of 400 nm or more and 780 nm or less.

[0017] [1. Overview of display media] A display medium according to one embodiment of the present invention includes a first layer, a second layer, and a third layer. A part or the whole of the first layer, a part or the whole of the second layer, and a part or the whole of the third layer are overlapped in this order in the thickness direction. The first layer is a layer capable of reflecting circularly polarized light having a rotation direction D1 and transmitting circularly polarized light having a rotation direction D2 that is opposite to the rotation direction D1. The second layer is a retardation layer. The third layer is a layer capable of reflecting circularly polarized light having a rotation direction of the rotation direction D1 and transmitting circularly polarized light having a rotation direction of the rotation direction D2.

[0018] Since the display medium of the present embodiment has the above-mentioned configuration, when the display medium is irradiated with non-polarized light and the reflected light is observed from the first layer side and the third layer side, the color of the first layer observed from the first layer side and the color of the third layer observed from the third layer side are different without using a special viewer. Therefore, the authenticity of the display medium can be determined without using a special viewer.

[0019] [1.1. Display media composition] The display medium according to this embodiment will be described in detail below with reference to the drawings. FIG. 1 is a schematic plan view of a display medium according to one embodiment of the present invention, as viewed from its thickness direction. FIG. 2 is a cross-sectional view that diagrammatically shows a cross section taken along the X1-X1 direction in FIG. FIG. 3 is an exploded perspective view showing a schematic diagram of a display medium according to one embodiment of the present invention. As shown in FIGS. 1 to 3, the display medium 100 includes a first layer 10, a second layer 20, and a third layer 30. As shown in FIGS. 1 and 2, the first layer 10 and the second layer 20 have the same shape and size when viewed in the thickness direction of the display medium 100 (in FIG. 1, the direction perpendicular to the paper surface). The second layer 20 is in contact with the surface of the first layer 10. The third layer 30 is disposed on a region A20 that is a part of the second layer 20 so as to be in contact with the surface of the second layer 20. As shown in FIGS. 2 and 3, the region A10 that is a part of the first layer 10, the region A20 that is a part of the second layer, and the region A30 that is the entire third layer are stacked in the thickness direction (in FIG. 2, the vertical direction of the paper surface) in the order of region A10-region A20-region A30. Here, overlapping in the thickness direction means that the regions A10 to A30 are in the same planar position when viewed from the thickness direction. In this embodiment, the first layer 10 and the second layer 20 have the same shape and size when viewed in the thickness direction of the display medium 100, but the first layer and the second layer may have different shapes and sizes. In another embodiment, an optional layer such as an adhesive layer or an intermediate layer having high light transmittance may be provided between the first layer and the second layer and / or between the second layer and the third layer, so long as it does not significantly impair the effects of the present invention. The optional layer is preferably a layer having high light transmittance, more preferably a layer having a total light transmittance of 80% or more, even more preferably a layer having a total light transmittance of 85% or more, and preferably a layer having a small retardation Re in the in-plane direction (for example, 0 nm or more and 5 nm or less). Specific examples of materials constituting such a layer having high light transmittance and small retardation Re include rigid polyvinyl chloride, flexible polyvinyl chloride, acrylic resin, and glass. In another embodiment, the display medium may further include a first outer layer and / or a second outer layer, so long as the effect of the present invention is not significantly impaired. The first outer layer and the second outer layer are preferably layers with high light transmittance, more preferably layers with a total light transmittance of 80% or more, and even more preferably layers with a total light transmittance of 85% or more. Specific examples of materials constituting the first outer layer and the second outer layer include hard polyvinyl chloride, soft polyvinyl chloride, acrylic resin, glass, polycarbonate (PC), and polyethylene terephthalate (PET), and may be appropriately selected depending on the application of the display medium, the required texture, durability, and mechanical strength. The first outer layer and the second outer layer may each independently be a layer with a small retardation Re in the in-plane direction (for example, 0 nm or more and 5 nm or less), and may be, for example, a layer with a retardation of 5 nm or more in the in-plane direction. The retardation Re in the in-plane direction of the first outer layer and the second outer layer may be 600 nm or less. Examples of layer configurations of the display medium further including the first outer layer and / or the second outer layer include the following. The display medium has a first outer layer, a first layer, a second layer, a third layer, and a second outer layer arranged in this order. The display medium includes a first outer layer, a first layer, a second layer, and a third layer arranged in that order. The display medium has a first layer, a second layer, a third layer, and a second outer layer arranged in this order. In this embodiment, the third layer 30 has a rectangular shape when viewed in the thickness direction of the display medium 100, but in another embodiment, the third layer 30 may have a pattern such as letters, numbers, figures, etc. when viewed in the thickness direction of the display medium 100.

[0020] [1.2. The first and third layers] The first layer and the third layer are layers that can reflect circularly polarized light having a rotation direction D1 and transmit circularly polarized light having a rotation direction D2 that is the opposite direction to the rotation direction D1. Here, the reflection may be regular reflection or diffuse reflection. Preferably, the third layer is a layer that can diffusely reflect circularly polarized light having a rotation direction D1. When the third layer is a layer that can diffusely reflect circularly polarized light having a rotation direction D1, the third layer may be provided with unevenness on its surface to diffusely reflect circularly polarized light, or, as described later, the third layer may be a layer that contains resin flakes to diffusely reflect circularly polarized light.

[0021] The rotation direction D1 of the circularly polarized light may be left or right. Therefore, both the first layer and the third layer may be layers that can reflect left-handed circularly polarized light and transmit right-handed circularly polarized light, or layers that can reflect right-handed circularly polarized light and transmit left-handed circularly polarized light. Both the first layer and the third layer may be layers capable of reflecting all of the irradiated circularly polarized light having a rotation direction D1, or may be layers capable of reflecting a portion of the circularly polarized light having a rotation direction D1. Furthermore, both the first layer and the third layer may be layers that can transmit all of the irradiated circularly polarized light having the rotation direction D2, or may be layers that can reflect a portion of the circularly polarized light having the rotation direction D2. The first layer and the third layer may be formed from the same material, or may be formed from different materials.

[0022] The first layer may be a layer having cholesteric regularity (for example, a resin layer having cholesteric regularity), and the third layer may be a layer containing resin flakes having cholesteric regularity.

[0023] The cholesteric regularity of a resin layer having cholesteric regularity means that the molecular axes are aligned in a certain direction on one plane, but the direction of the molecular axes is shifted at a slight angle on the next plane that overlaps it, and the angle is further shifted on the next plane, and so on, so that the angle of the molecular axes in the plane is shifted (twisted) as the molecules pass through the overlapping planes arranged in sequence. That is, when the molecules in the layer have cholesteric regularity, the molecules are aligned in a manner to form a layer of many molecules in the resin layer. In a certain layer A of such a layer of many molecules, the molecules are aligned so that the molecular axes are in a certain direction, and in an adjacent layer B, the molecules are aligned in a direction shifted at an angle from the direction in layer A, and in an adjacent layer C, the molecules are aligned in a direction further shifted at an angle from the direction in layer B. In this way, in a layer of many molecules, the angles of the molecular axes are continuously shifted, forming a structure in which the molecules are twisted. A structure in which the direction of the molecular axes is twisted in this way is an optically chiral structure. Hereinafter, a resin layer having cholesteric regularity is also referred to as a cholesteric resin layer.

[0024] The cholesteric resin layer usually has a circularly polarized light separation function. That is, the cholesteric resin layer has a property of transmitting one of right-handed and left-handed circularly polarized light and reflecting a part or all of the other circularly polarized light. The reflection in the cholesteric resin layer reflects the circularly polarized light while maintaining its chirality.

[0025] The wavelength at which the circularly polarized light separation function is exhibited depends on the pitch of the helical structure in the cholesteric resin layer. The pitch of the helical structure is the distance in the plane normal direction that the molecular axis direction in the helical structure gradually shifts as it progresses along the plane, and then returns to the original molecular axis direction. By changing the size of the pitch of this helical structure, it is possible to change the wavelength at which the circularly polarized light separation function is exhibited.

[0026] The cholesteric resin layer can be obtained, for example, by providing a film of a cholesteric liquid crystal composition on a suitable support for forming a resin layer, and curing the film of the cholesteric liquid crystal composition. The obtained layer can be used as a cholesteric resin layer as it is. This cholesteric resin layer is a layer made of a film of a material that can reflect one of right-handed circularly polarized light and left-handed circularly polarized light and transmit the other circularly polarized light. Therefore, the cholesteric resin layer itself can be used as the first layer.

[0027] As the cholesteric liquid crystal composition for forming the cholesteric resin layer, for example, a composition that contains a liquid crystal compound and can exhibit a cholesteric liquid crystal phase when a film is formed on a support can be used. Here, as the liquid crystal compound, a liquid crystal compound that is a polymer compound and a polymerizable liquid crystal compound can be used. In order to obtain high thermal stability, it is preferable to use a polymerizable liquid crystal compound. By polymerizing such a polymerizable liquid crystal compound in a state of exhibiting cholesteric regularity, the film of the cholesteric liquid crystal composition can be hardened, and a non-liquid crystal resin layer that is hardened while exhibiting cholesteric regularity can be obtained.

[0028] The resin flakes having cholesteric regularity are small pieces of resin having cholesteric regularity. The small pieces having cholesteric regularity can reflect one of right-handed circularly polarized light and left-handed circularly polarized light and transmit the other circularly polarized light. A layer containing an aggregate of the small pieces can scatter and reflect one of right-handed circularly polarized light and left-handed circularly polarized light and transmit the other circularly polarized light.

[0029] Even when crushed, the cholesteric resin layer can reflect one of right-handed and left-handed circularly polarized light and transmit the other circularly polarized light in at least a part of the visible light range, so it is preferable to use the crushed material as resin flakes having cholesteric regularity. When a cholesteric resin layer is used as the first layer and resin flakes are used as the material for the third layer, the resin flakes may be crushed material obtained by crushing a resin layer other than the cholesteric resin layer as the first layer. However, from the viewpoint of reducing manufacturing costs by using a standardized material, it is preferable that the resin flakes which are the material of the third layer are crushed material obtained by crushing the same cholesteric resin layer used as the first layer.

[0030] Flakes of a resin having cholesteric regularity can be produced from a cholesteric resin layer by, for example, the method for producing a peeled piece described in Japanese Patent No. 6,142,714.

[0031] Flakes of a material having no polarizing properties may be used together with flakes of a resin having cholesteric regularity. Examples of flakes having no polarizing properties include flakes of at least one type selected from carbon black, and oxides, nitrides, and oxynitrides of metals belonging to groups 3 to 11 of the fourth period of the periodic table of elements. These may be used alone or in combination of two or more types in any ratio.

[0032] When the first layer is a layer having cholesteric regularity, the first layer preferably has a reflectance for unpolarized light of 35% or more and 50% or less in the wavelength range of 420 nm or more and 650 nm or less. This enables the first layer to have good polarization separation function over a wide visible light region, that is, the wavelength range of 420 nm or more and 650 nm or less, and as a result, the color of the third layer can be made clearer when observed from the first layer side.

[0033] In addition, when the third layer is a layer containing resin flakes having cholesteric regularity, the resin flakes contained in the third layer preferably have a reflectance of 35% to 50% for unpolarized light in the wavelength range of 420 nm to 650 nm. This allows the resin flakes to effectively scatter and reflect light. As a result, the color difference between the light visible when the display medium is observed from the first layer side and the light visible when the display medium is observed from the third layer side can be more easily recognized. Here, the reflectance of the cholesteric resin layer, which is the material of the resin flakes, is measured, and the measured value can be regarded as the reflectance value of the resin flakes.

[0034] Suitable examples of cholesteric resin layers having a high reflectance in the wavelength region of 420 nm or more and 650 nm or less include (i) a cholesteric resin layer in which the pitch of the helical structure is changed stepwise, and (ii) a cholesteric resin layer in which the pitch of the helical structure is changed continuously.

[0035] (i) A cholesteric resin layer in which the pitch of the helical structure is changed stepwise can be obtained by forming a plurality of cholesteric resin layers having different pitches of the helical structure. As a specific example, such a cholesteric resin layer can be produced by first preparing a plurality of cholesteric resin layers having different pitches of the helical structure, and then bonding each layer with a pressure sensitive adhesive or adhesive. Alternatively, the cholesteric resin layer can be produced by forming a certain cholesteric resin layer, and then sequentially forming other cholesteric resin layers on the cholesteric resin layer.

[0036] (ii) The cholesteric resin layer in which the pitch of the helical structure is continuously changed is not particularly limited by its manufacturing method, but a preferred example of the manufacturing method of such a cholesteric resin layer is a method in which a cholesteric liquid crystal composition containing a polymerizable liquid crystal compound for forming a cholesteric resin layer is applied onto another layer, preferably an alignment film, to obtain a layer of the liquid crystal composition, and then the layer is cured in a state in which the pitch of the helical structure is continuously changed by one or more light irradiation and / or heating treatments. This operation is called a band-widening treatment because it is an operation for expanding the reflection band of the cholesteric resin layer. By performing the band-widening treatment, a wide reflection band can be realized even in a cholesteric resin layer having a thickness as thin as 10 μm or less, and is therefore preferred. A preferred embodiment of the cholesteric liquid crystal composition to be subjected to such a band-widening treatment is the cholesteric liquid crystal composition (X) described in detail below.

[0037] The cholesteric resin layer in which the pitch of the helical structure is continuously changed may be used alone or in the form of a laminate of multiple layers. For example, a cholesteric resin layer that exhibits a circularly polarized light separation function in a part of the visible light range and a cholesteric resin layer that exhibits a circularly polarized light separation function in another range may be combined to provide a cholesteric resin layer that exhibits a circularly polarized light separation function in a wide range of the visible light range.

[0038] Thus, the cholesteric resin layer may be a resin layer consisting of only one layer, or may be a resin layer consisting of two or more layers. When the cholesteric resin layer has two or more layers, the cholesteric resin layer may have two or more cholesteric resin layers of the above (i), may have two or more cholesteric resin layers of the above (ii), or may have two or more layers by combining both of them. From the viewpoint of ease of manufacture, the number of layers constituting the cholesteric resin layer is preferably 1 to 100 layers, more preferably 1 to 20 layers. When a cholesteric resin layer having high reflectance is obtained by only one layer as a result of the above-mentioned band-widening treatment, a display medium of a preferred embodiment can be obtained even by using only that one layer.

[0039] The cholesteric liquid crystal composition (X) contains a polymerizable non-liquid crystal compound represented by the following formula (1) and a specific polymerizable liquid crystal compound. The non-liquid crystal compound represented by formula (1) and the polymerizable liquid crystal compound may each be used alone or in combination of two or more kinds in any ratio. Each of these components will be described in turn below.

[0040] R 1 -A 1 -BA 2 -R 2 (1) In formula (1), R 1 and R 2are each independently a group selected from the group consisting of a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkylene oxide group having 1 to 20 carbon atoms, a hydrogen atom, a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acrylic group, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.

[0041] The alkyl group and the alkylene oxide group may be unsubstituted or may be substituted with one or more halogen atoms. Furthermore, the halogen atom, the hydroxyl group, the carboxyl group, the (meth)acrylic group, the epoxy group, the mercapto group, the isocyanate group, the amino group, and the cyano group may be bonded to the alkyl group having 1 to 2 carbon atoms and the alkylene oxide group.

[0042] R 1 and R 2 Preferred examples of the alkyl group include a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acrylic group, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.

[0043] Also, R 1 and R 2 At least one of R is preferably a reactive group. 1 and R 2 By having a reactive group as at least one of the above, the polymerizable non-liquid crystal compound represented by the formula (1) is fixed in the cholesteric resin layer during curing, and a stronger layer can be formed. Here, examples of the reactive group include a carboxyl group, a (meth)acrylic group, an epoxy group, a mercapto group, an isocyanate group, and an amino group, and these groups may be accompanied by any intervening group.

[0044] In formula (1), A 1 and A 2each independently represents a group selected from the group consisting of a 1,4-phenylene group, a 1,4-cyclohexylene group, a cyclohexene-1,4-diyl group, a 4,4'-biphenylene group, a 4,4'-bicyclohexylene group, and a 2,6-naphthylene group. The 1,4-phenylene group, the 1,4-cyclohexylene group, the cyclohexene-1,4-diyl group, the 4,4'-biphenylene group, the 4,4'-bicyclohexylene group, and the 2,6-naphthylene group may be unsubstituted or may be substituted with one or more substituents such as a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkyl group having 1 to 10 carbon atoms, and a halogenated alkyl group. A 1 and A 2 In each of the groups, when two or more substituents are present, they may be the same or different.

[0045] A 1 and A 2 Particularly preferred examples of the aromatic ring structure include a group selected from the group consisting of a 1,4-phenylene group, a 4,4'-biphenylene group, and a 2,6-naphthylene group. These aromatic ring structures are relatively rigid compared to alicyclic structures, and have high affinity with the mesogens of the polymerizable liquid crystal compound, resulting in higher alignment uniformity.

[0046] In formula (1), B is a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH 2 -, -OCH 2 -, -CH=NN=CH-, -NHCO-, -OCOO-, -CH 2 COO- and -CH 2 OCO-. Particularly preferred values ​​for B include a single bond, -OCO-, and -CH=NN=CH-.

[0047] The compound of formula (1) preferably has chirality. The cholesteric liquid crystal composition (X) preferably contains a mixture of a plurality of optical isomers as the compound of formula (1). For example, it may contain a mixture of a plurality of enantiomers and / or diastereomers. At least one of the compounds of formula (1) preferably has a melting point within the range of 50°C to 150°C.

[0048] The compound of formula (1) preferably has a high Δn. By using a compound with a high Δn as the compound of formula (1), the Δn of the cholesteric liquid crystal composition (X) can be improved, and a cholesteric resin layer capable of reflecting circularly polarized light in a wide wavelength range can be prepared. The Δn of at least one compound of formula (1) is preferably 0.18 or more, more preferably 0.22 or more. The upper limit of Δn can be, for example, 0.50 or less.

[0049] Particularly preferred specific examples of the compound of formula (1) include the following compounds (A1) to (A10):

[0050] [ka]

[0051] In the above compound (A3), "*" represents a chiral center.

[0052] The cholesteric liquid crystal composition (X) usually contains a polymerizable liquid crystal compound having at least two reactive groups in one molecule. The polymerizable liquid crystal compound may be a compound represented by formula (2). R 3 -C 3 -D 3 -C 5 -MC 6 -D 4 -C 4 -R 4 (2)

[0053] In formula (2), R3 and R 4 are reactive groups, each independently representing a group selected from the group consisting of a (meth)acrylic group, a (thio)epoxy group, an oxetane group, a thietanyl group, an aziridinyl group, a pyrrole group, a vinyl group, an allyl group, a fumarate group, a cinnamoyl group, an oxazoline group, a mercapto group, an iso(thio)cyanate group, an amino group, a hydroxyl group, a carboxyl group, and an alkoxysilyl group. By having these reactive groups, when the cholesteric liquid crystal composition is cured, a cured product having a film strength sufficient for practical use can be obtained.

[0054] In formula (2), D 3 and D. 4 represents a group selected from the group consisting of a single bond, a linear or branched alkyl group having 1 to 20 carbon atoms, and a linear or branched alkylene oxide group having 1 to 20 carbon atoms.

[0055] In formula (2), C 3 ~C 6 is a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH 2 -, -OCH 2 -, -CH=NN=CH-, -NHCO-, -OCOO-, -CH 2 COO- and -CH 2 represents a group selected from the group consisting of OCO-.

[0056] In formula (2), M represents a mesogenic group. Specifically, M represents a mesogenic group having 2 to 4 skeletons selected from the group consisting of azomethines, azoxys, phenyls, biphenyls, terphenyls, naphthalenes, anthracenes, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles, each of which may be unsubstituted or substituted, and each of which may be -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH 2 -, -OCH 2-, -CH=NN=CH-, -NHCO-, -OCOO-, -CH 2 COO- and -CH 2 Represents a group linked by a linking group such as OCO-.

[0057] Examples of the substituent that the mesogenic group M may have include a halogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cyano group, a nitro group, -OR 5 , -OC(=O)-R 5 , -C(=O)-OR 5 , -OC(=O)-OR 5 , -NR 5 -C(=O)-R 5 , -C(=O)-NR 5 R 7 or -OC(=O)-NR 5 R 7 Here, R 5 and R 7 R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 5 and R 7 is an alkyl group, the alkyl group may include -O-, -S-, -OC(=O)-, -C(=O)-O-, -OC(=O)-O-, -NR 6 -C(=O)-, -C(=O)-NR 6 -, -NR 6 - or -C(=O)- may be present (excluding the case where two or more adjacent -O- and -S- are present). 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0058] Examples of the substituent in the "alkyl group having 1 to 10 carbon atoms which may have a substituent" include a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkoxy group having 1 to 6 carbon atoms, an alkoxyalkoxy group having 2 to 8 carbon atoms, an alkoxyalkoxyalkoxy group having 3 to 15 carbon atoms, an alkoxycarbonyl group having 2 to 7 carbon atoms, an alkylcarbonyloxy group having 2 to 7 carbon atoms, and an alkoxycarbonyloxy group having 2 to 7 carbon atoms.

[0059] The polymerizable liquid crystal compound preferably has an asymmetric structure. Here, the asymmetric structure is defined as a structure in which, in formula (2), R 3 -C 3 -D 3 -C 5 -and-C 6 -D 4 -C 4 -R 4 By using a polymerizable liquid crystal compound having an asymmetric structure, the alignment uniformity can be further improved.

[0060] The Δn of the polymerizable liquid crystal compound is preferably 0.18 or more, more preferably 0.22 or more. When a polymerizable liquid crystal compound having a Δn value of 0.30 or more is used, the absorption end on the long wavelength side of the ultraviolet absorption spectrum may reach the visible range. However, a polymerizable liquid crystal compound having an absorption end in the visible range can also be used as long as the spectrum does not adversely affect the desired optical performance. By using a polymerizable liquid crystal compound having such a high Δn, a cholesteric resin layer having high optical performance (for example, selective reflection performance of circularly polarized light) can be obtained. The upper limit of Δn can be, for example, 0.50 or less.

[0061] Preferable specific examples of the polymerizable liquid crystal compound include the following compounds (B1) to (B9), however, the polymerizable liquid crystal compound is not limited to the following compounds.

[0062] [ka]

[0063] In the cholesteric liquid crystal composition (X), the weight ratio of (total weight of the polymerizable non-liquid crystal compounds of formula (1)) / (total weight of the polymerizable liquid crystal compounds) is preferably 0.05 or more, more preferably 0.1 or more, particularly preferably 0.15 or more, and preferably 1 or less, more preferably 0.65 or less, particularly preferably 0.45 or less. By making the weight ratio equal to or greater than the lower limit of the range, the alignment uniformity can be improved. By making the weight ratio equal to or less than the upper limit, the alignment uniformity can be improved, the stability of the liquid crystal phase can be improved, and further, the Δn of the liquid crystal composition can be increased to stably obtain the desired optical performance (for example, the property of selectively reflecting circularly polarized light). Here, the total weight refers to the weight when one type is used, and refers to the total weight when two or more types are used.

[0064] In the cholesteric liquid crystal composition (X), the molecular weight of the compound of formula (1) is preferably less than 600, and the molecular weight of the polymerizable liquid crystal compound is preferably at least 600. This allows the compound of formula (1) to enter into the gaps of the polymerizable liquid crystal compound having a larger molecular weight, thereby improving the alignment uniformity.

[0065] Cholesteric liquid crystal compositions such as the cholesteric liquid crystal composition (X) may optionally contain a crosslinking agent to improve the film strength and durability after curing. The crosslinking agent can be selected and used as appropriate from those that react simultaneously with the curing of the film of the cholesteric liquid crystal composition, promote the reaction by performing heat treatment after curing, or naturally proceed with the reaction by moisture, thereby increasing the crosslink density of the cholesteric resin layer and not deteriorating the alignment uniformity. Therefore, for example, any crosslinking agent that cures with ultraviolet light, heat, moisture, etc. can be suitably used. Examples of the crosslinking agent include polyfunctional acrylate compounds; epoxy compounds; isocyanate compounds; polyoxazoline compounds; and alkoxysilane compounds. In addition, the crosslinking agent may be used alone or in combination of two or more types at any ratio. Furthermore, a known catalyst may be used depending on the reactivity of the crosslinking agent. By using a catalyst, in addition to improving the film strength and durability of the cholesteric resin layer, productivity can be improved.

[0066] The cholesteric liquid crystal composition may contain a photoinitiator as desired. As the photoinitiator, for example, a known compound that generates a radical or an acid by ultraviolet light or visible light can be used. Specific examples of the photoinitiator include benzoin, benzyl dimethyl ketal, benzophenone, biacetyl, acetophenone, Michler's ketone, benzyl, benzyl isobutyl ether, tetramethylthiuram mono(di)sulfide, 2,2-azobisisobutyronitrile, 2,2-azobis-2,4-dimethylvaleronitrile, benzoyl peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl -1-phenyl-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-diethylthioxanthone, methylbenzoyl formate, 2,2-diethoxyacetophenone, β-ionone, β-bromostyrene, diazoaminobenzene, α-amylcinnamic aldehyde, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, p,p'-dichlorobenzophenone, p,p'-bisdiethylaminobenzophenone, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-propyl ether, benzoin n-butyl ether, diphenyl sulfide, bis(2,6-methoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide , bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, anthracenebenzophenone, α-chloroanthraquinone, diphenyl disulfide, hexachlorobutadiene, pentachlorobutadiene, octachlorobutene, 1-chloromethylnaphthalene, 1,Examples of the carbazole oxime compounds include 2-octanedione, 1-[4-(phenylthio)phenyl-2-(o-benzoyloxime)], 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(o-acetyloxime), (4-methylphenyl)[4-(2-methylpropyl)phenyl]iodonium hexafluorophosphate, 3-methyl-2-butynyltetramethylenesulfonium hexafluoroantimonate, and diphenyl-(p-phenylthiophenyl)sulfonium hexafluoroantimonate. These may be used alone or in combination of two or more in any ratio. Furthermore, if necessary, a known tertiary amine compound may be used as a photosensitizer or polymerization accelerator to control the curability.

[0067] The amount of the photoinitiator is preferably 0.03% by weight to 7% by weight in the cholesteric liquid crystal composition. By making the amount of the photoinitiator equal to or greater than the lower limit of the range, the degree of polymerization can be increased, thereby increasing the film strength of the cholesteric resin layer. By making the amount equal to or less than the upper limit, the liquid crystal material can be well aligned, thereby stabilizing the liquid crystal phase of the cholesteric liquid crystal composition.

[0068] The cholesteric liquid crystal composition may optionally contain a surfactant. For example, a surfactant that does not inhibit alignment may be appropriately selected and used. For example, a nonionic surfactant containing a siloxane or fluorinated alkyl group in the hydrophobic group portion is suitable as such a surfactant. Among them, an oligomer having two or more hydrophobic group portions in one molecule is particularly suitable. Specific examples of these surfactants include PF-151N, PF-636, PF-6320, PF-656, PF-6520, PF-3320, PF-651, and PF-652 of PolyFox from OMNOVA Co., Ltd.; FTX-209F, FTX-208G, and FTX-204D of Futergent from NEOS Co., Ltd.; and KH-40 of Surflon from Seimi Chemical Co., Ltd. The surfactant may be used alone or in combination of two or more types in any ratio.

[0069] The amount of the surfactant is preferably 0.05% by weight to 3% by weight in the cured film obtained by curing the cholesteric liquid crystal composition. By making the amount of the surfactant equal to or greater than the lower limit of the range, the alignment control force at the air interface can be increased, thereby suppressing alignment defects. In addition, by making the amount equal to or less than the upper limit, the deterioration of alignment uniformity caused by excess surfactant entering between liquid crystal molecules can be suppressed.

[0070] The cholesteric liquid crystal composition may contain a chiral agent as desired. Usually, the twist direction of the cholesteric resin layer can be appropriately selected depending on the type and structure of the chiral agent used. When the twist direction is right-handed, it can be achieved by using a chiral agent that imparts right-handedness, and when the twist direction is left-handed, it can be achieved by using a chiral agent that imparts left-handedness. Specific examples of the chiral agent include those described in JP2005-289881A, JP2004-115414A, JP2003-66214A, JP2003-313187A, JP2003-342219A, JP2000-290315A, JP6-072962A, U.S. Patent No. 6,468,444, WO98 / 00428, JP2007-176870A, etc., and are available as Paliocolor LC756 from BASF. The chiral agent may be used alone or in combination of two or more at any ratio.

[0071] The amount of the chiral agent can be set arbitrarily within a range that does not deteriorate the desired optical performance. The specific amount of the chiral agent in the cholesteric liquid crystal composition is usually 1% by weight to 60% by weight.

[0072] The cholesteric liquid crystal composition may further contain other optional components as necessary. Examples of the optional components include a solvent, a polymerization inhibitor for improving pot life, an antioxidant for improving durability, an ultraviolet absorber, and a light stabilizer. These optional components may be used alone or in combination of two or more at any ratio. The amount of these optional components may be set arbitrarily within a range that does not deteriorate the desired optical performance.

[0073] The method for producing the cholesteric liquid crystal composition is not particularly limited, and the composition can be produced by mixing the above-mentioned components.

[0074] The cholesteric resin layer can be obtained, for example, by subjecting the surface of a support made of a film such as a transparent resin to treatments such as corona discharge treatment and rubbing treatment as necessary, further providing an alignment film as necessary, further providing a film of a cholesteric liquid crystal composition on this surface, and further performing an alignment treatment and / or curing treatment as necessary.

[0075] The cholesteric liquid crystal composition can be applied onto the support or the alignment film by a known method such as extrusion coating, direct gravure coating, reverse gravure coating, die coating, or bar coating.

[0076] The alignment treatment can be carried out, for example, by heating the film of the cholesteric liquid crystal composition for 0.5 to 10 minutes at 50° C. to 150° C. By carrying out the alignment treatment, the cholesteric liquid crystal composition in the film can be well aligned.

[0077] The curing treatment can be carried out by combining one or more light irradiation and heating treatments. The heating conditions may be, for example, a temperature of preferably 40° C. or higher, more preferably 50° C. or higher, and preferably 200° C. or lower, more preferably 140° C. or lower, for a time of preferably 1 second or more, more preferably 5 seconds or more, and preferably 3 minutes or less, more preferably 120 seconds or less. The light used for the light irradiation includes not only visible light but also ultraviolet light and other electromagnetic waves. The light irradiation can be carried out, for example, by irradiating light having a wavelength of 200 nm to 500 nm for 0.01 seconds to 3 minutes.

[0078] Here, 0.01 mJ / cm 2 ~50mJ / cm 2 By repeatedly irradiating the film with weak ultraviolet light and heating several times, it is possible to obtain a circularly polarized light separation function with a wide reflection band, in which the pitch of the helical structure is continuously and greatly changed. 2 ~10,000mJ / cm 2 A cholesteric resin layer can be obtained by irradiating the liquid crystal compound with relatively strong ultraviolet light such as 1000 nm to completely polymerize the liquid crystal compound. The above-mentioned expansion of the reflection band and irradiation with strong ultraviolet light may be performed in air, or a part or all of the steps may be performed in an atmosphere with a controlled oxygen concentration (for example, a nitrogen atmosphere).

[0079] The process of applying and curing the cholesteric liquid crystal composition onto another layer such as an alignment film is not limited to one time, and the application and curing may be repeated several times to form two or more cholesteric resin layers. However, by using a cholesteric liquid crystal composition such as the cholesteric liquid crystal composition (X), a cholesteric resin layer containing a well-aligned polymerizable liquid crystal compound with a Δn of 0.18 or more and having a thickness of 5 μm or more can be easily formed by applying and curing the cholesteric liquid crystal composition only once.

[0080] The cholesteric resin layer thus obtained can be used as it is together with the support and the alignment film as the first layer, or, if necessary, the support and the like can be peeled off and only the cholesteric resin layer can be transferred and used as the first layer.

[0081] [1.3. Second Layer] The second layer is a retardation layer. The retardation layer is a layer that can change the polarization state of the light incident on the layer. The retardation layer may be uniaxial or biaxial. Examples of the retardation layer include a so-called positive A plate having the characteristics of nx>ny≒nz; a so-called negative A plate having the characteristics of nz≒nx>ny; a so-called positive C plate having the characteristics of nz>nx≒ny; a so-called negative C plate having the characteristics of nx≒ny>nz; a so-called positive B plate having the characteristics of nz>nx>ny; a so-called negative B plate having the characteristics of nx>ny>nz; and a so-called Z plate having the characteristics of nx>nz>ny. Among these, the positive A plate or the negative A plate is preferable since it is easy to manufacture and easily exhibits an in-plane retardation.

[0082] Examples of the retardation layer include a stretched film obtained by stretching a resin film formed from a thermoplastic resin, and a liquid crystal cured film obtained by aligning a liquid crystal composition containing a polymerizable liquid crystal compound in a predetermined direction and then curing the composition while maintaining the alignment.

[0083] The material for the stretched film may be any of the following: a material with positive intrinsic birefringence; a material with negative intrinsic birefringence; and a material in which a material with positive intrinsic birefringence and a material with negative intrinsic birefringence are combined in any ratio. An appropriate material may be selected depending on the desired characteristics of the retardation layer.

[0084] Specific examples of materials for forming the stretched film include polyolefin resins such as polyethylene resin and polypropylene resin; resins containing polymers containing an alicyclic structure such as norbornene-based resins; vinyl aromatic compound polymer resins such as polystyrene; cellulose-based resins such as triacetyl cellulose resin; polyimide resins; polyamideimide resins; polyamide resins; polyetherimide resins; polyetheretherketone resins; polyetherketone resins; polyketone sulfide resins; polyethersulfone resins; polysulfone resins; polyphenylene sulfide resins; polyphenylene oxide resins; polyethylene terephthalate resins; polybutylene terephthalate resins; polyethylene naphthalate resins; polyacetal resins; polycarbonate resins; polyarylate resins; (meth)acrylic resins; polyvinyl alcohol resins; (meth)acrylic acid ester-vinyl aromatic compound copolymer resins; isobutene / N-methylmaleimide copolymer resins; styrene / acrylonitrile copolymer resins; combinations of these resins; and the like.

[0085] The resin forming the stretched film is preferably a resin containing a polymer containing an alicyclic structure. Hereinafter, the polymer containing an alicyclic structure may be appropriately referred to as an "alicyclic structure-containing polymer". The alicyclic structure-containing polymer is a polymer containing an alicyclic structure in the repeating unit. Examples of the alicyclic structure-containing polymer include a polymer that can be obtained by a polymerization reaction using a cyclic olefin as a monomer; and a hydrogenated product thereof. In addition, as the alicyclic structure-containing polymer, both a polymer containing an alicyclic structure in the main chain and a polymer containing an alicyclic structure in the side chain can be used. Among them, the alicyclic structure-containing polymer preferably contains an alicyclic structure in the main chain. Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure, and from the viewpoint of thermal stability, a cycloalkane structure is preferable.

[0086] Examples of the polymer containing an alicyclic structure include (1) norbornene-based polymers, (2) monocyclic olefin polymers, (3) cyclic conjugated diene polymers, (4) vinyl alicyclic hydrocarbon polymers, and (5) hydrogenated versions of these. Among these, norbornene-based polymers and hydrogenated versions thereof are more preferred from the viewpoints of transparency and moldability.

[0087] Examples of norbornene-based polymers include ring-opening polymers of norbornene-based monomers, ring-opening copolymers of norbornene-based monomers and other monomers copolymerizable by ring-opening, and hydrogenated products thereof; addition polymers of norbornene-based monomers, addition copolymers of norbornene-based monomers and other monomers copolymerizable by ring-opening, etc. Among these, from the viewpoint of transparency, hydrogenated ring-opening polymers of norbornene-based monomers are particularly preferred.

[0088] As the resin containing the alicyclic structure-containing polymer, various products are commercially available, and one having the desired properties can be appropriately selected and used. Examples of such commercially available products include the product groups under the trade names "ZEONOR" (manufactured by Zeon Corporation), "Arton" (manufactured by JSR Corporation), "Apel" (manufactured by Mitsui Chemicals, Inc.), and "TOPAS" (manufactured by Polyplastics Co., Ltd.).

[0089] Using these resins as materials, a resin film can be obtained by a method such as cast molding, extrusion molding, or inflation molding, and the resin film can be stretched to obtain a stretched film as a retardation layer.

[0090] The second layer has a retardation Re in the in-plane direction of preferably 40 nm or more, more preferably 300 nm or more, and preferably 1600 nm or less, more preferably 1250 nm or less. When the retardation Re in the in-plane direction of the second layer is equal to or greater than the lower limit, the second layer gives a large phase difference to incident light and emits it, thereby making it possible to increase the color difference between the light recognized when the display medium is observed from the first layer side and the light recognized when the display medium is observed from the third layer side. By setting the retardation Re of the second layer in the in-plane direction to the upper limit or less, the reflectance of the display medium for non-polarized light can be set to a value that does not have many maxima and minima in the visible light range. When the reflection spectrum does not have many maxima and minima, the color of the reflected light can be recognized more accurately with the naked eye. As a result, the color difference between the light recognized when observed from the first layer side and the light recognized when observed from the third layer side can be more easily distinguished with the naked eye.

[0091] The in-plane retardations Re of the second layer at wavelengths of 400 nm, 560 nm, and 650 nm are Re(400), Re(560), and Re(650), respectively. The value of Re(400) / Re(560) is preferably 0.8 or more, more preferably 1.0 or more, and the upper limit can be, for example, 1.3 or less. The value of Re(650) / Re(560) is preferably 1.1 or less, more preferably 1.000 or less, and the lower limit can be, for example, 0.8 or more. In the second layer, when the value of Re(400) / Re(560) and / or the value of Re(650) / Re(560) are within the above range, the second layer can impart significantly different phase differences to light of different wavelengths, thereby making it possible to increase the color difference between the light recognized when the display medium is observed from the first layer side and the light recognized when the display medium is observed from the third layer side.

[0092] [1.4. Effects of display media] Next, the function of the display medium will be described below. Fig. 4 is a schematic diagram illustrating the state of reflected light from the display medium when non-polarized light is irradiated from the third layer side, and Fig. 5 is a schematic diagram illustrating the state of reflected light from the display medium when non-polarized light is irradiated from the first layer side. 4, when unpolarized light A1 is irradiated from the third layer 30 side of the display medium 100, the third layer 30 reflects circularly polarized light A1R having a rotation direction D1, and a color corresponding to the selective reflection band of the third layer 30 is visible. The third layer 30 transmits circularly polarized light B1 having a rotation direction D2, and the circularly polarized light B1 passes through the second layer 20 and the first layer 10 and is absorbed by the absorption layer 200.

[0093] As shown in FIG. 5, when unpolarized light A2 is irradiated onto the first layer 10 side of the display medium 100, the first layer 10 transmits circularly polarized light A3L having a rotation direction D2. The circularly polarized light A3L has a phase difference and its polarization state is changed by the retardation layer, the second layer 20. As a result, the second layer 20 transmits the circularly polarized light A4RL including the circularly polarized light having the rotation direction D1 and the circularly polarized light having the rotation direction D2. The third layer 30 reflects the circularly polarized light A5R having the rotation direction D1 out of the circularly polarized light A4RL and transmits the circularly polarized light B2 having the rotation direction D2. The circularly polarized light B2 is absorbed by the absorption layer 200. Typically, in the circularly polarized light A4RL, the ratio of the circularly polarized light having the rotation direction D1 to the circularly polarized light having the rotation direction D2 varies depending on the wavelength, and therefore the intensity of the circularly polarized light A5R varies depending on the wavelength. The circularly polarized light A5R is incident on the second layer 20, where a phase difference is imparted to change the polarization state of the light. As a result, the second layer 20 transmits circularly polarized light A6RL, which includes circularly polarized light having a rotation direction D1 and circularly polarized light having a rotation direction D2. The first layer 10 transmits the circularly polarized light A7L having the rotation direction D2 out of the circularly polarized light A6RL. Usually, in the circularly polarized light A6RL, the ratio of the circularly polarized light having the rotation direction D1 to the circularly polarized light having the rotation direction D2 varies depending on the wavelength, so that the intensity of the circularly polarized light A7L varies depending on the wavelength. Therefore, the color of the circularly polarized light A7L is different from that of the circularly polarized light A1R that is not transmitted through the second layer 20. In this way, the color of reflected light A1R of display medium 100 when non-polarized light is irradiated from the third layer 30 side of display medium 100 is different from the color of reflected light A7L of display medium 100 when non-polarized light A2 is irradiated from the first layer 10 side of display medium 100.

[0094] When the first layer 10 is a layer having cholesteric regularity and the third layer 30 is a layer containing resin flakes having cholesteric regularity, the following effect is further added to the display medium. When non-polarized light A1 is applied from the third layer 30 side, the third layer 30 scatters and reflects the circularly polarized light A1 with a rotation direction D1 among the non-polarized light A1, and the circularly polarized light A1R reflected by the third layer 30 is visually recognized as scattered light. When non-polarized light A2 is applied from the first layer 10 side, the circularly polarized light A7L emitted by the first layer 10 is visually recognized as scattered light. Scattered light is easily distinguished from regular reflected light. In addition, the reflected light from the area of ​​the display medium 100 where the third layer 30 does not overlap in the thickness direction is regular reflected light. Therefore, the shape of the third layer 30 can be more easily recognized when the shape is observed by applying non-polarized light from the third layer 30 side or when the shape is observed by applying non-polarized light from the first layer 10 side.

[0095] [1.5. Use of display media] Due to the effect of the display medium, the displayed colors are different on the front and back of the display medium. Therefore, the display medium functions as an identification medium for identifying authenticity, and it is possible to determine whether the display medium is authentic or not. The method for determining the authenticity of the display medium will be described in further detail below. Furthermore, the display medium can be suitably used as, for example, cards such as business cards, printed matter for display, decorative items, etc., by taking advantage of its ability to display different colors on the front and back.

[0096] [2. How to determine the authenticity of display media] Based on the function of the display medium, the authenticity of the display medium can be determined in the following manner. A method for determining authenticity of a display medium according to an embodiment of the present invention includes the steps of: A step (1) of confirming that the display medium is semi-transparent; a step (2) of irradiating the display medium with unpolarized light from the third layer side and observing the reflected light from the display medium from the third layer side to obtain color information C3 based on the third layer; a step (3) of irradiating the display medium with unpolarized light from the first layer side and observing the reflected light from the display medium from the first layer side to obtain color information C1 based on the first layer; and A step (4) of comparing the color information C3 with the color information C1 and determining that the color information C3 and the color information C1 are not identical. Includes. Step (1) may be carried out before or after steps (2) to (4). Step (3) may be carried out after step (2), or step (2) may be carried out after step (3). Step (4) is usually carried out after steps (2) and (3).

[0097] [2.1. Process (1)] In step (1), it is confirmed that the display medium is translucent. Here, translucency means that the display medium has a transmittance of 30% or more when non-polarized light is incident on the display medium. If the display medium is not translucent, it is determined that the display medium is made of a material that does not have a circularly polarized light separation function and is not genuine.

[0098] [2.2. Process (2)] In step (2), the display medium is irradiated with non-polarized light from the third layer side, and the reflected light of the display medium is observed from the third layer side to obtain color information C3 from the third layer. Examples of the color information C3 include lightness, hue, and saturation. The color information C3 may be obtained qualitatively by naked eye or quantitatively by a colorimeter or the like. In order to observe only the reflected light from the display medium, step (2) is usually performed by placing the display medium on an object that has a high light absorption rate, such as black paper.

[0099] [2.3. Process (3)] In step (3), the display medium is irradiated with non-polarized light from the first layer side, and the reflected light from the display medium is observed from the first layer side to obtain color information C1 from the first layer. Examples of color information C1 include the same information as the examples of color information C3. As with color information C3, color information C1 may be obtained qualitatively by naked eye or quantitatively by a colorimeter or the like. In order to observe only the reflected light from the display medium, step (3) is usually performed by placing the display medium on an object that has a high light absorption rate. In step (3), the color information C1 from the first layer means color information about the region where the first layer overlaps with the second layer and the third layer in the thickness direction.

[0100] [2.4. Process (4)] In step (4), the color information C3 is compared with the color information C1, and it is determined that the color information C3 and the color information C1 are not identical. If it is confirmed in step (1) that the display medium is translucent, and it is determined in step (4) that the color information C3 and the color information C1 are not identical, the display medium can be determined to be authentic.

[0101] The color information C3 and C1 are, for example, in the color space CIE 1976 L * a * b * in a * value and b * In this case, the determination that the color information C3 and the color information C1 are not the same can be made by, for example, determining the coordinates of the color observed from the first layer side (a * 1 ,b * 1 ) and the color coordinates observed from the third layer side (a * 3 ,b * 3 ) and the distance (difference Δ (1-3) ) is equal to or greater than a predetermined value. (1-3) is preferably 20 or more, and more preferably 40 or more, it can be determined that the color information C3 and the color information C1 are not identical.

[0102] From the viewpoint of determining the authenticity of a display medium without requiring a special viewer, it is preferable that the determination be made by comparing qualitative color information C3 obtained by naked eye with qualitative color information C1 obtained by naked eye.

[0103] [3. Products including display media] The display medium can be attached to an object in any form, such as a certificate, a tag, etc., to form an article containing the display medium. An example of an object to which the display medium can be attached is an object whose authenticity is to be identified. EXAMPLES

[0104] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.

[0105] In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature and pressure unless otherwise specified.

[0106] (Measurement of average particle size) The average particle size of the resin flakes was measured by the following method. First, several sieves with different mesh sizes are used to measure the proportion of resin flakes passing through the sieves with those mesh sizes. Then, the particle size distribution of the resin flakes is expressed as an integrated weight percentage based on the size of the mesh size and the proportion of resin flakes passing through the sieves with those mesh sizes. In this particle size distribution, the particle size at which the integrated value of the weight is 50% is defined as the average particle size.

[0107] (chromaticity) Regarding the identification medium as a display medium, the difference Δ between the chromaticity of the reflected light from the portion of the first layer overlapping the third layer in the thickness direction (i.e., the portion of the character pattern "GENUINE") observed from the first layer side and the chromaticity of the reflected light from the third layer (the portion of the character pattern "GENUINE") observed from the third layer side (1-3)was calculated in the following way. First, using a spectrophotometer ("UV-VIS550" manufactured by JASCO Corporation), reflectance 1 of the "GENUINE" character pattern was measured from the first layer side in the wavelength range of 400 nm or more and 780 nm or less, and reflectance 3 of the "GENUINE" character pattern was measured from the third layer side. Using the color calculation software provided with the spectrophotometer, the reflected light color space CIE 1976 L was calculated based on reflectance 1 or reflectance 3, with D65 as the reflected light source. * a * b * in a * value and b * The value was calculated. Based on the reflectance 1 observed from the first layer side, the reflected light from the part of the first layer overlapping the third layer in the thickness direction (the part of the character pattern "GENUINE") is * value and b * The value was calculated and the obtained a * value and b * The values ​​are a * 1 and b * 1 It was decided. Similarly, based on the reflectance 3 observed from the third layer side, the reflected light from the third layer (the part of the character pattern "GENUINE") is a * value and b * The value was calculated and the obtained a * value and b * The values ​​are a * 3 and b * 3 It was decided. The obtained a * 1 , b * 1 , a * 3 , and b * 3 Based on the following formula, the difference Δ (1-3) asked for. Δ (1-3) =√{(a * 1 -a *3 ) 2 +(b * 1 -b * 3 ) 2}

[0108] (Layer thickness) The measurement was performed using a digital micrometer (manufactured by Mitutoyo Corporation).

[0109] (In-plane retardation Re) For the retardation layer as the second layer, the retardation Re in the in-plane direction at wavelengths of 400 nm, 560 nm, and 650 nm was measured with a retardation meter ("Axoscan" manufactured by AXOMETRICS). From the measured retardation Re in the in-plane direction, the values ​​of Re(400) / Re(560) and Re(650) / Re(560) were calculated. Here, the retardations Re in the in-plane direction at wavelengths of 400 nm, 560 nm, and 650 nm are defined as Re(400), Re(560), and Re(650), respectively.

[0110] [Production Example A1] Production of layer having cholesteric regularity (Preparation of Liquid Crystal Composition L1) The components were mixed according to the composition shown in the table below to prepare a photocurable liquid crystal composition L1.

[0111] [Table 1]

[0112] The components used in preparing liquid crystal composition L1 are as follows.

[0113] The photopolymerizable liquid crystal compound 1 is a compound having a structure represented by the following formula (B5). [ka]

[0114] The photopolymerizable non-liquid crystal compound is a compound having a structure represented by the following formula (A10). [ka]

[0115] As the chiral agent, "LC756" manufactured by BASF was used. The photoinitiator used was "Irgacure OXE02" manufactured by Ciba Japan. The surfactant used was "Ftergent 209F" manufactured by Neos Corporation.

[0116] (Manufacturing long multi-layered films) A long polyethylene terephthalate (PET) film with an isotropic in-plane refractive index (Toyobo Co., Ltd. "PET film A4100"; thickness 100 μm) was prepared as the base film. This base film was attached to the unwinding section of a film transport device, and the following operations were performed while transporting the base film in the longitudinal direction. First, a rubbing treatment was performed in the longitudinal direction parallel to the transport direction. Next, the prepared liquid crystal composition L1 was applied to the rubbed surface using a die coater. As a result, a film of the uncured liquid crystal composition was formed on one side of the base film.

[0117] Next, the uncured liquid crystal composition film is subjected to an alignment treatment by heating at 120°C for 4 minutes, and then subjected to a dipping treatment of 800 mJ / cm2 in a nitrogen atmosphere. 2 The liquid crystal composition film was completely cured by irradiating it with ultraviolet light of 1000 nm to obtain a multilayer film having a layer with cholesteric regularity (cholesteric resin layer) having a thickness shown in Table 2 on one side of a long PET film.

[0118] The liquid crystal composition L1 containing the chiral agent is cured under the conditions shown in Table 2 while maintaining cholesteric regularity, to obtain a layer having cholesteric regularity.

[0119] [Table 2]

[0120] (Measurement of reflectance of layer with cholesteric order) The PET film was peeled off from the multilayer film containing the obtained cholesteric resin layer to obtain a single-layer film of the cholesteric resin layer. Non-polarized light (wavelength 400 nm to 780 nm) was incident on the obtained cholesteric resin layer, and the reflectance was measured using an ultraviolet-visible spectrophotometer (UV-Vis 550, manufactured by JASCO Corporation). Fig. 6 is a graph showing the measurement results of the reflectance of the cholesteric resin layer in the wavelength range of 400 nm to 780 nm. As shown in Fig. 6, it is found that the cholesteric resin layer has a reflectance of 35% or more and 50% or less in the wavelength range of 420 nm or more and 650 nm or less.

[0121] [Production Example B1] Production of paint containing resin flakes having cholesteric regularity (Manufacturing of resin flakes) Using the multilayer film obtained in Production Example A1, resin flakes having cholesteric regularity were produced. The apparatus used to produce resin flakes is shown in Fig. 7. Fig. 7 is a side view that illustrates the apparatus for producing resin flakes.

[0122] As shown in Fig. 7, a manufacturing apparatus 400 was prepared that included a film delivery section 420, a peeling section 430, and a film recovery section 440. The peeling section 430 included a bar 434 having a corner 435 provided at an acute angle, and a nozzle 436 capable of spraying air that was provided immediately downstream of the corner 435. In this case, the angle of the corner 435 of the bar 434 was set so that the multilayer film 410 could be folded back at an angle θ (45°). The corner had a chamfered structure with R = 0.2 mm to 0.3 mm.

[0123] Multilayer film 410 was attached to film delivery section 420 in a direction that allowed multilayer film 410 to be folded back at corner portion 435 of bar 434 with cholesteric resin layer 411 facing outward relative to PET film 412, which was the support. Then, multilayer film 410 was delivered from film delivery section 420 in a state in which tension was applied to multilayer film 410 in the transport direction by film recovery section 440. At this time, the magnitude of tension applied to multilayer film 410 was set to 80 N / m. Air was sprayed from nozzle 436 at a pressure of 0.5 MPa.

[0124] Multilayer film 410 was folded back at corners 435 of bar 434, forming many cracks. Then, cholesteric resin layer 411 with the cracks formed therein was peeled off and blown away by air jetted from nozzle 436, and peeled piece 411A was obtained. The obtained peeled piece 411A was collected by a collector.

[0125] The peeled pieces of the collected cholesteric resin layer were pulverized using a stone mill grinder (West Micro Powder MPW-G008) to obtain resin flakes. The average particle size of the obtained resin flakes was 50 μm.

[0126] The reflectance of the resin flakes for unpolarized light is the same as the reflectance measured for the cholesteric resin layer that is the raw material for the resin flakes. Therefore, the reflectance of the resin flakes for unpolarized light is 35% to 50% in the wavelength range of 420 nm to 650 nm, as shown in FIG.

[0127] (Paint manufacturing) The resulting resin flakes were used as a pigment to produce a paint in the following manner. Coating material 1 was prepared by mixing 100 parts by weight of screen ink ("No. 2500 Medium" manufactured by Jujo Chemical Co., Ltd.) as a binder solution, 10 parts by weight of a dedicated diluent for the screen ink (Tetoron standard solvent), and 15 parts by weight of the above-mentioned flakes.

[0128] [Manufacturing example B2] Paint 2 was produced in the same manner as in Production Example B1 (production of paint) except for the following changes. Instead of resin flakes, metallic aluminum flakes (Seiko Advance's "Silver Pigment 606H") were used.

[0129] [Manufacturing Example B3] A pigment containing metallic aluminum (Seiko Advance Corporation's "Half Mirror Z Silver R1") was diluted with a solvent (Seiko Advance Corporation's "T-477") to produce paint 3. The dilution ratio was appropriately adjusted so that a semi-transparent aluminum layer with a total light transmittance of 50% was obtained from paint 3.

[0130] [Production Example C1] Production of Retardation Layer Pellets of a cycloolefin resin (ZEONOR 1215, manufactured by Zeon Corporation) were prepared. The pellets were fed to a single-screw extruder (manufactured by OCS Corporation) and extruded to obtain an extruded film having a thickness of 200 μm.

[0131] The obtained extruded film (length 150 mm × width 50 mm) was stretched in the length direction using a thermostatic tensile tester (manufactured by Instron) to obtain a retardation layer 1 having an in-plane retardation Re shown in Table 3. The stretching temperature was 125°C, the chuck distance of the tensile tester was 50 mm, and the stretching speed was 100 mm / min. The stretching ratio was as shown in Table 3.

[0132] [Manufacturing example C2~C22] Except for changing the stretching ratio as shown in Table 3, the same procedures as in Production Example C1 were carried out to obtain retardation layers 2 to 22.

[0133] Table 3 shows the stretching ratios, in-plane retardation Re, layer thicknesses, and birefringence Δn, values ​​of Re(400) / Re(560), and values ​​of Re(650) / Re(560) of the retardation layers 1 to 22.

[0134] [Table 3]

[0135] [Example 1] (1-1. Manufacturing of laminated bodies) The cholesteric resin layer of the multilayer film obtained in Production Example A1 was laminated to the retardation layer 1 using a sheet-shaped adhesive. As the adhesive, Nitto Denko Corporation's "Transparent Adhesive Tape LUCIACS CS9621T" (thickness 25 μm, visible light transmittance: 90% or more, in-plane retardation Re: 3 nm or less) was used. Next, the PET film was peeled off from the multilayer film laminated with the retardation layer to obtain a multilayer body 1 having a layer structure of (cholesteric resin layer) / (adhesive layer) / (retardation layer).

[0136] (1-2. Manufacturing of identification media as display media) The retardation layer of the obtained laminate 1 was screen-printed using paint 1. A 100 mesh per inch plate capable of printing the character pattern "GENUINE" was used as the screen printing plate. Next, the laminate 1 was placed on a hot plate set at 40°C and heated for 10 minutes to dry the paint. As a result, an identification medium 1 was obtained as a display medium, including a portion in which the (cholesteric resin layer) / (adhesive layer) / (retardation layer) / (layer of dried paint 1) were overlapped in this order in the thickness direction. In this identification medium, the "cholesteric resin layer" corresponds to the first layer, the "retardation layer" corresponds to the second layer, and the "layer of dried paint 1" corresponds to the third layer. Paint 1 includes resin flakes produced from the cholesteric resin layer. The resin flakes can reflect circularly polarized light in the same rotation direction as the circularly polarized light that the cholesteric resin layer can reflect, and can transmit circularly polarized light in the same rotation direction as the circularly polarized light that the cholesteric resin layer can transmit. Therefore, the dried layer of paint 1 can reflect circularly polarized light of the same rotation direction as the circularly polarized light that the cholesteric resin layer can reflect, and can transmit circularly polarized light of the same rotation direction as the circularly polarized light that the cholesteric resin layer can transmit.

[0137] [Examples 2 to 22] Identification media 2 to 22 were obtained as display media in the same manner as in Example 1, except for the following changes. In (1-1. Production of laminate), laminates 2 to 22 were obtained by using the retardation layers 2 to 22 obtained in Production Examples C2 to C22 in place of the retardation layer 1 in the production of (1-1. Production of laminate). In (1-2. Production of discrimination medium as display medium), the laminated body 1 was replaced with the laminated body 2 to 22 to obtain discrimination media 2 to 22. Each of the identification media 2 to 22 includes a portion in which a (cholesteric resin layer) / (adhesive layer) / (retardation layer) / (layer of dried paint 1) are layered in this order in the thickness direction. In the identification media 2 to 22, the "cholesteric resin layer" corresponds to the first layer, the "retardation layer" corresponds to the second layer, and the "layer of dried paint 1" corresponds to the third layer.

[0138] [Comparative Examples 1 to 3] Identification media C1 to C3 as display media were obtained in the same manner as in Example 1, except for the following changes. In (1-1. Production of laminate), the retardation layer 4, 13, or 21 obtained in Production Example C4, C13, or C21 was used instead of the retardation layer 1 to obtain laminates C1 to C3. In (1-2. Production of discrimination medium as display medium), the laminated bodies C1 to C3 were used instead of the laminated body 1, and the paint 2 produced in Production Example B2 was used instead of the paint 1 to obtain discrimination media C1 to C3.

[0139] Each of the discrimination media C1 to C3 includes a portion in which a cholesteric resin layer / adhesive layer / retardation layer / layer of dried paint 2 are layered in this order in the thickness direction.

[0140] [Comparative Example 4] (C4-1. Manufacturing of laminated bodies) One side of the retardation layer 4 obtained in Production Example C4 was screen-printed using the paint 3. A 100 mesh per inch plate was used as the screen printing plate. The retardation layer 4 was then placed on a hot plate set at 40°C and heated for 10 minutes to dry the paint. As a result, a translucent aluminum layer with a total light transmittance of 50% was formed on one side of the retardation layer 4, and a laminate C4 having a structure of (dried paint 3 layer (aluminum layer)) / (retardation layer) was obtained.

[0141] (C4-2. Manufacturing of identification media as display media) Identification medium C4 was obtained in the same manner as in Example 1 (1-2. Production of identification medium as display medium) except that laminate C4 was used instead of laminate 1. Identification medium C4 includes a portion in which (aluminum layer) / (retardation layer) / (layer of dried paint 1) are layered in this order in the thickness direction.

[0142] [Comparative Examples 5 and 6] Identification media C5 and C6 as display media were obtained in the same manner as in Comparative Example 4, except for the following changes. In (C4-1. Production of laminate), the retardation layer 13 or 21 was used instead of the retardation layer 4 to obtain the laminate C5 or C6. In (C4-2. Production of identification medium as display medium), the laminate C5 or C6 was used instead of the laminate C4 to obtain the identification medium C5 or C6.

[0143] [Comparative Example 7] The retardation layer of the laminate C4 obtained in Comparative Example 4 (C4-1. Manufacturing of laminate) was screen-printed using paint 2. A 100 mesh per inch plate capable of printing the character pattern "GENUINE" was used as the screen printing plate. Next, the laminate C4 was placed on a hot plate set at 40°C and heated for 10 minutes to dry the paint. This resulted in the identification medium C7 as a display medium, which includes a portion where (aluminum layer) / (retardation layer) / (layer of dried paint 2) are overlapped in this order in the thickness direction.

[0144] [Comparative Examples 8 and 9] Identification media C8 and C9 as display media were obtained in the same manner as in Comparative Example 7, except for the following changes. Instead of the laminate C4, the laminate C5 or C6 obtained in Comparative Examples 5 or 6 was used to obtain a discrimination medium C8 or C9.

[0145] [Reference example R1] The PET film was peeled off from the multilayer film obtained in Production Example A1 to obtain a cholesteric resin layer as a single layer film. One side of the obtained cholesteric resin layer was screen printed using paint 1. A 100 mesh per inch screen capable of printing the character pattern "GENUINE" was used as the screen printing plate. The cholesteric resin layer was then placed on a hot plate set at 40°C and heated for 10 minutes to dry the paint. This resulted in the identification medium R1 as a display medium, which includes a portion where the (cholesteric resin layer) / (dried paint 1 layer) overlap in this order in the thickness direction.

[0146] The layer structures and evaluation results of the Examples, Comparative Examples, and Reference Examples are shown in the table below. In the table below, the abbreviations have the following meanings. CLC sheet: Cholesteric resin layer CLC flake: A layer of paint 1 containing resin flakes made from cholesteric resin layers. Al Flake: 2 layers of paint containing flakes of metallic aluminum Al sheet: A semi-transparent aluminum layer formed from paint 3

[0147] [Table 4]

[0148] [Table 5]

[0149] From the above results, the following can be seen: The discrimination media (display media) according to Examples 1 to 22 have a Δ (1-3) is 20 or more, and it can be judged by the naked eye that there is a difference between the chromaticity observed from the third layer side and the chromaticity observed from the first layer side. Therefore, the identification medium (display medium) according to Examples 1 to 22 can be judged to be a genuine medium without requiring a special viewer. The identification media (display media) according to Comparative Examples 1 to 3, in which the third layer is a layer containing metallic aluminum flakes and does not have a circularly polarized light separation function; the identification media (display media) according to Comparative Examples 4 to 6, in which the first layer is a semi-transparent aluminum layer and does not have a circularly polarized light separation function; and the identification media (display media) according to Comparative Examples 7 to 9, in which both the third layer and the first layer are layers that do not have a circularly polarized light separation function, have a significantly lower Δ (1-3) The value of is small, less than 20, and it cannot be determined by the naked eye that there is a difference between the chromaticity observed from the third layer side and the chromaticity observed from the first layer side. Therefore, the discrimination media (display media) according to Comparative Examples 1 to 9 cannot be determined to be genuine media. [Explanation of symbols]

[0150] 10...First layer 20...Second layer 30...Third layer 100...Display medium (identification medium) 400...Manufacturing equipment 410...Multi-layer film 411...Cholesteric resin layer 412...Support (PET film) 411A…Peeled piece 420...Film sending section 430…Peeled part 434…Bar 435...Corner part 436…Nozzle 440…Film recovery section A10…area A20…area A30…area

Claims

1. a first layer, a second layer, and a third layer; a part or all of the first layer, a part or all of the second layer, and a part or all of the third layer are overlapped in this order in a thickness direction; the first layer is a layer that reflects circularly polarized light having a rotation direction D1 and transmits circularly polarized light having a rotation direction D2 that is opposite to the rotation direction D1, The second layer is a retardation layer, the third layer is a layer that reflects circularly polarized light having a rotation direction of the rotation direction D1 and transmits circularly polarized light having a rotation direction of the rotation direction D2, the first layer is a layer having cholesteric regularity, the third layer is a layer containing resin flakes having cholesteric regularity, The second layer is Re(560) is 300 nm or more and 1250 nm or less, Re(400) / Re(560) is 1.0 or more, Re(650) / Re(560) is 1.000 or less, Here, Re(400) represents the in-plane retardation Re of the second layer at a wavelength of 400 nm, Re(560) represents the in-plane retardation Re of the second layer at a wavelength of 560 nm, and Re(650) represents the in-plane retardation Re of the second layer at a wavelength of 650 nm.

2. The display medium according to claim 1 , wherein the first layer is a cured film of a cholesteric liquid crystal composition.

3. 3. The display medium according to claim 1, wherein the first layer has a reflectance of 35% to 50% for unpolarized light in a wavelength range of 420 nm to 650 nm.

4. The display medium according to any one of claims 1 to 3, wherein the resin flakes contained in the third layer have a reflectance for unpolarized light of 35% to 50% in the wavelength range of 420 nm to 650 nm.

5. A step (1) of confirming that the display medium according to any one of claims 1 to 4 is semi-transparent; a step (2) of irradiating the display medium with unpolarized light from the third layer side and observing the reflected light from the display medium from the third layer side to obtain color information C3 based on the third layer; A step (3) of irradiating the display medium with unpolarized light from the first layer side and observing the reflected light from the display medium from the first layer side to obtain color information C1 based on the first layer; and A step (4) of comparing the color information C3 with the color information C1 and determining that the color information C3 and the color information C1 are not identical. A method for determining authenticity, comprising:

6. An article comprising the display medium according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Storage battery

    JP1983028182A

  • Forgery preventive material and method for discriminating forgery

    JP2000255200A

  • Object identification medium and identification method

    JP2004338257A

  • Thread-like printed matter and forgery preventive paper

    JP2007216602A

  • Optical element, polarizing plate, retardation plate, lighting system and liquid crystal display device

    JP2008197223A