Lithium ion conductive material and lithium ion secondary battery

A lithium ion conductive material using cyclic carbonate and lithium amide salt at specific ratios addresses the issues of conductivity and stability, enhancing battery performance by ensuring high lithium ion conductivity and thermal stability.

JP7556371B2Active Publication Date: 2024-09-26TOYOTA JIDOSHA KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022044675
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-18
Publication Date
2024-09-26
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

Conventional lithium ion conductive materials face challenges in achieving high lithium ion conductivity and thermal stability.

Method used

A lithium ion conductive material comprising cyclic carbonate as a solvent and lithium amide salt dissolved in it, with a molar ratio of the lithium amide salt to cyclic carbonate between 0.25 and 0.33, optionally including a sulfide solid electrolyte, enhances thermal stability and lithium ion conductivity.

Benefits of technology

The material exhibits excellent lithium ion conductivity and thermal stability, while minimizing reactivity with sulfide solid electrolytes, thereby improving the performance of lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556371000001
    Figure 0007556371000001
  • Figure 0007556371000004
    Figure 0007556371000004
  • Figure 0007556371000003
    Figure 0007556371000003
Patent Text Reader

Abstract

To provide a lithium ion conductive material with excellent lithium ion conductivity and thermal stability.SOLUTION: A disclosed lithium ion conductive material contains: cyclic carbonate as a solvent; and lithium amide salt dissolved in the cyclic carbonate. The molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and less than or equal to 0.33.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a lithium ion conductive material and a lithium ion secondary battery. [Background technology]

[0002] Patent Document 1 discloses an electrolyte solution for use in a lithium ion secondary battery, the electrolyte solution containing a predetermined solvent, a lithium imide salt, and at least one of Group 1 and Group 2 elements, and the molar ratio of the lithium imide salt to the solvent is 0.8 to 2. Patent Document 2 discloses a non-aqueous electrolyte solution in which the ratio of lithium and oxygen contained in the non-aqueous electrolyte solution is within a predetermined range. Patent Document 3 discloses an electrolyte solution for use in a lithium ion secondary battery, the electrolyte solution containing a non-aqueous solvent and a lithium salt, and the amount of the non-aqueous solvent per 1 mol of the lithium salt is 3 mol or less. Patent Document 4 discloses an electrolyte solution containing a chain carbonate, an unsaturated cyclic carbonate, and a lithium salt, and the lithium salt is contained at a concentration of 1.1 to 3.8 mol / L. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-096463 A [Patent Document 2] JP 2020-053171 A [Patent Document 3] JP 2016-122657 A [Patent Document 4] International Publication No. 2017 / 179682 Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional lithium ion conducting materials have room for improvement in terms of lithium ion conductivity and thermal stability. [Means for solving the problem]

[0005] As one of the means for solving the above problems, the present application provides: A lithium ion conducting material comprising: A cyclic carbonate as a solvent; a lithium amide salt dissolved in the cyclic carbonate; The molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and is not greater than 0.33. Disclose.

[0006] In the lithium ion conductive material of the present disclosure, the cyclic carbonate may be at least one of propylene carbonate and ethylene carbonate.

[0007] In the lithium ion conductive material of the present disclosure, the lithium amide salt may be at least one of lithium bisfluorosulfonylamide and lithium bistrifluoromethanesulfonylamide.

[0008] The lithium ion conductive material of the present disclosure may include a sulfide solid electrolyte together with the cyclic carbonate and the lithium amide salt.

[0009] As one of the means for solving the above problems, the present application provides: A lithium ion secondary battery comprising a positive electrode, an electrolyte layer, and a negative electrode, At least one of the positive electrode, the electrolyte layer, and the negative electrode comprises the lithium ion conductive material of the present disclosure. Disclose. Effect of the Invention

[0010] The lithium ion conductive materials of the present disclosure have excellent lithium ion conductivity and thermal stability. [Brief description of the drawings]

[0011] [Figure 1] 1 shows a schematic configuration of a secondary battery. [Diagram 2] The results of evaluating the thermal stability of lithium ion conductive materials are shown. [Diagram 3] 1 shows the results of evaluating the lithium ion transport number of lithium ion conductive materials. [Figure 4] 1 shows the results of evaluating the lithium ion conductivity of lithium ion conductive materials. [Diagram 5] 1 shows the X-ray diffraction peaks of a sulfide solid electrolyte before and after immersion in a lithium ion conductive material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] 1. Lithium ion conductive materials The lithium ion conductive material of the present disclosure includes a cyclic carbonate as a solvent and a lithium amide salt dissolved in the cyclic carbonate, wherein the molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and less than or equal to 0.33.

[0013] 1.1 Solvent The lithium ion conductive material of the present disclosure includes a cyclic carbonate as a solvent. The solvent may be substantially composed of the cyclic carbonate alone, or may be a mixed solvent of the cyclic carbonate and a solvent other than the cyclic carbonate.

[0014] 1.1.1 Cyclic carbonates According to the findings of the present inventors, cyclic carbonates have a higher dielectric constant than linear carbonates and are more likely to coordinate lithium ions. In other words, in the lithium ion conductive material of the present disclosure, the cyclic carbonate is less likely to be in a free state, and as a result, the thermal stability is more likely to be increased. In particular, when a lithium amide salt is dissolved in the cyclic carbonate at a predetermined concentration, almost all of the cyclic carbonate can be solvated with lithium ions, and as a result, the thermal stability can be further improved. In addition, due to a small amount of lithium ions that are not solvated with the cyclic carbonate, the transport number of lithium ions is increased even under high viscosity, and excellent lithium ion conductivity is easily ensured.

[0015] The cyclic carbonate may have a cyclic structure as a chemical structure, be liquid at a temperature at which lithium ion conductivity is desired to be exhibited, and dissolve lithium amide salt at a predetermined concentration. Specific examples of the cyclic carbonate include propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), vinylene carbonate (VC), or derivatives thereof (e.g., halides, etc.). In particular, when the cyclic carbonate is at least one of propylene carbonate and ethylene carbonate, it is easy to ensure better lithium ion conductivity and thermal stability. The cyclic carbonate may be used alone or in combination of two or more.

[0016] 1.1.2 Solvents other than cyclic carbonates (co-solvents) The solvent constituting the lithium ion conductive material of the present disclosure may be composed of the above-mentioned cyclic carbonate, or may contain a solvent (sub-solvent) other than the cyclic carbonate in addition to the above-mentioned cyclic carbonate. Examples of the sub-solvent other than the cyclic carbonate include chain carbonates. Examples of the chain carbonate include dimethyl carbonate (DMC), diethyl carbonate (DEC) or derivatives thereof (e.g., halides, particularly those having a perfluoroalkyl group). However, chain carbonates have a lower dielectric constant than cyclic carbonates, and lithium ions tend to be less likely to be coordinated. Therefore, chain carbonates tend to be in a state where they are isolated alone in the lithium ion conductive material, are easily volatilized, and are highly reactive to the sulfide solid electrolyte described below. In this respect, in the lithium ion conductive material of the present disclosure, when the amount of the auxiliary solvent other than the cyclic carbonate is small, high thermal stability is easily ensured, and the ionic conductivity is easily improved while suppressing the reactivity with the sulfide solid electrolyte. In the lithium ion conductive material of the present disclosure, the molar ratio of the auxiliary solvent to the cyclic carbonate ([auxiliary solvent (mol)] / [cyclic carbonate (mol)]) may be 0.10 or less, 0.05 or less, or 0.03 or less. The lower limit of the molar ratio of the auxiliary solvent to the cyclic carbonate is 0.

[0017] 1.2 Lithium salts The lithium ion conductive material of the present disclosure contains a lithium salt dissolved in the above-mentioned solvent. The lithium salt may consist essentially of a lithium amide salt or may consist of a combination of a lithium amide salt and a lithium salt other than the lithium amide salt.

[0018] 1.2.1 Lithium amide salts The lithium ion conductive material of the present disclosure includes a lithium amide salt dissolved in the above-mentioned cyclic carbonate. That is, the lithium amide salt may be dissolved in the cyclic carbonate and ionized into cations and anions, or may form some association with the cyclic carbonate or the like. Here, the molar ratio of the lithium amide salt to the cyclic carbonate ([lithium amide salt (mol)] / [cyclic carbonate (mol)]) is greater than 0.25 and less than or equal to 0.33. In other words, the lithium amide salt is dissolved at a concentration of 0.25 mol to 0.33 mol per 1 mol of the cyclic carbonate.

[0019] Various amide salts can be used as the lithium amide salt. In the lithium ion conductive material of the present disclosure, it is considered that lithium ions can be coordinated to the active sites of the cyclic carbonate regardless of the type of lithium amide salt, and excellent thermal stability and lithium ion conductivity can be ensured. Specific examples of the lithium amide salt include sulfonyl amide salts such as lithium bisfluorosulfonyl amide (LiFSA, LiN(SO2F)2), lithium bistrifluoromethanesulfonyl amide (LiTFSA, Li[N(CF3SO2)2]), lithium bisperfluoroethylsulfonyl amide (Li[N(C2F5SO2)2]), lithium bisperfluorobutylsulfonyl amide (Li[N(C4F9SO2)2]), and lithium fluorosulfonyl trifluoromethanesulfonyl amide (Li[N(FSO2)(C2F5SO2)]). Alternatively, a silyl amide salt having Si instead of S may be used. In particular, when the lithium amide salt is at least one of lithium bisfluorosulfonylamide (LiFSA, LiN(SO2F)2) and lithium bistrifluoromethanesulfonylamide (LiTFSA, Li[N(CF3SO2)2]), it is easy to ensure better lithium ion conductivity and thermal stability, and furthermore, it is easy to reduce reactivity with the sulfide solid electrolyte described below. Only one type of lithium amide salt may be used alone, or two or more types may be used in combination. The term "amide salt" is a concept that also includes "imide salt".

[0020] As described above, the molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and less than or equal to 0.33. When the concentration of the lithium amide salt in the cyclic carbonate is within this range, the thermal stability and lithium ion conductivity are likely to be significantly improved. In addition, the reaction between the active site of the cyclic carbonate and the sulfide solid electrolyte described below is suppressed, and the deterioration of the sulfide solid electrolyte is likely to be suppressed. If the concentration of the lithium amide salt to the cyclic carbonate is too low, the thermal stability and lithium ion conductivity are difficult to improve. On the other hand, if the concentration of the lithium amide salt to the cyclic carbonate is excessive, the viscosity becomes too high, and there is a risk of the lithium ion conductivity decreasing. The molar ratio may be 0.26 or more, 0.27 or more, or 0.28 or more, and may be 0.32 or less, 0.31 or less, or 0.30 or less. The molar ratio of the lithium amide salt to the cyclic carbonate can be specified by analyzing ions, elements, etc. contained in the cyclic carbonate.

[0021] 1.2.2 Lithium salts other than lithium amide salts In the lithium ion conductive material of the present disclosure, the lithium salt dissolved in the solvent may be composed of the lithium amide salt described above, or may be a combination of the lithium amide salt described above and a lithium salt other than the lithium amide salt (other lithium salt). In any case, by dissolving the lithium amide salt in a cyclic carbonate at a predetermined concentration, excellent thermal stability and ionic conductivity are easily ensured. However, according to the knowledge of the present inventor, some lithium salts other than the lithium amide salt have reactivity with the sulfide solid electrolyte described below. For example, if the molecular weight of the anion constituting the lithium salt is too small, the charge density becomes too high (the electron donating property becomes too high), and there is a possibility that the sulfide solid electrolyte is deteriorated by depriving Li of the sulfide solid electrolyte. If the lithium amide salt is used, such a problem is unlikely to occur. In this regard, in the lithium ion conductive material of the present disclosure, it is preferable that the proportion of the lithium amide salt in the lithium salt dissolved in the solvent is high. Specifically, the proportion of the lithium amide salt in the total lithium salt (100 mol%) may be 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more.

[0022] 1.3 Optional components The lithium ion conductive material of the present disclosure may contain other components in addition to the above-mentioned cyclic carbonate and lithium amide salt. Examples of the other components include the above-mentioned auxiliary solvent and other lithium salts. The lithium ion conductive material of the present disclosure may also be a combination of a liquid material (e.g., an electrolyte) and a solid material (e.g., a solid electrolyte). The above-mentioned cyclic carbonate and lithium amide salt can be an electrolyte.

[0023] 1.3.1 Sulfide solid electrolyte The lithium ion conductive material of the present disclosure may be a combination of the above-mentioned cyclic carbonate and lithium amide salt with a sulfide solid electrolyte. That is, the lithium ion conductive material of the present disclosure may include a sulfide solid electrolyte together with the cyclic carbonate and the lithium amide salt. According to such a combination, for example, the cyclic carbonate and lithium amide salt as an electrolyte may be filled in the gaps between the sulfide solid electrolytes. That is, an ion conductive path may be formed even in the gaps of the sulfide solid electrolyte. In addition, the cyclic carbonate functions as a lubricant that improves the fluidity of the sulfide solid electrolyte, and an effect of improving the moldability of the sulfide solid electrolyte can be expected.

[0024] On the other hand, when the cyclic carbonate and lithium amide salt are combined with a sulfide solid electrolyte, it is better to suppress the reaction between the cyclic carbonate and lithium amide salt and the sulfide solid electrolyte as described above. For example, it is better to adopt an anion constituting the lithium amide salt that has low reactivity with the sulfide solid electrolyte. Specifically, when the lithium ion conductive material of the present disclosure includes the cyclic carbonate and the lithium amide salt as well as a sulfide solid electrolyte, the lithium amide salt may be at least one of lithium bisfluorosulfonylamide (LiFSA) and lithium bistrifluoromethanesulfonylamide (LiTFSA).

[0025] The sulfide solid electrolyte may be any of sulfides having lithium ion conductivity. The sulfide solid electrolyte may contain at least Li and S as constituent elements. In particular, sulfide solid electrolytes containing at least Li, S, and P as constituent elements have high performance, and sulfide solid electrolytes based on a Li3PS4 skeleton and containing at least one halogen are also high in performance. Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5-GeS2, and the like. The sulfide solid electrolyte may be amorphous or crystalline. The sulfide solid electrolyte may be, for example, particulate. The sulfide solid electrolyte may be used alone or in combination of two or more kinds.

[0026] 1.3.2 Various additives The lithium ion conductive material of the present disclosure may contain various additives in addition to the above. The type of additive may be selected depending on the application of the lithium ion conductive material.

[0027] 2. Lithium-ion secondary battery The lithium ion conductive material of the present disclosure is used, for example, as an electrolyte material for a lithium ion secondary battery. Hereinafter, a lithium ion secondary battery having the lithium ion conductive material of the present disclosure will be described. As shown in FIG. 1, a lithium ion secondary battery 100 according to an embodiment has a positive electrode 10, an electrolyte layer 20, and an anode 30. Here, at least one of the positive electrode 10, the electrolyte layer 20, and the anode 30 contains the lithium ion conductive material of the present disclosure. As described above, the lithium ion conductive material of the present disclosure is excellent in thermal stability and lithium ion conductivity. In this respect, the performance of the secondary battery 100 is easily improved by including the lithium ion conductive material of the present disclosure in at least one of the positive electrode 10, the electrolyte layer 20, and the anode 30 of the secondary battery 100. In addition, in the secondary battery 100, the lithium ion conductive material of the present disclosure may be used as an electrolyte solution or in combination with a solid electrolyte (particularly a sulfide solid electrolyte). That is, the secondary battery 100 may be an electrolyte battery that does not include a solid electrolyte, or may include a solid electrolyte and a liquid.

[0028] 2.1 Positive electrode As shown in FIG. 1, a positive electrode 10 according to one embodiment may include a positive electrode active material layer 11 and a positive electrode current collector 12. In this case, the positive electrode active material layer 11 may contain the above-mentioned lithium ion conductive material.

[0029] 2.1.1 Cathode active material layer The positive electrode active material layer 11 includes a positive electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the positive electrode active material layer 11 may further include various additives. When the positive electrode active material layer 11 includes the lithium ion conductive material of the present disclosure, the positive electrode active material layer 11 includes a positive electrode active material in addition to the lithium ion conductive material, and may further include other electrolytes, conductive assistants, binders, and various additives. The content of each of the positive electrode active material, electrolyte, conductive assistant, binder, and the like in the positive electrode active material layer 11 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material may be 40% by mass or more, 50% by mass or more, or 60% by mass or more, or may be less than 100% by mass or 90% by mass or less, with the entire positive electrode active material layer 11 (total solid content) being 100% by mass. The shape of the positive electrode active material layer 11 is not particularly limited, and may be, for example, a sheet-like shape having a substantially flat surface. The thickness of the positive electrode active material layer 11 is not particularly limited and may be, for example, 0.1 μm or more, 1 μm or more, 10 μm or more, or 30 μm or more, and may be 2 mm or less, 1 mm or less, 500 μm or less, or 100 μm or less.

[0030] The positive electrode active material may be a known positive electrode active material for a secondary battery. Among known active materials, a material that exhibits a potential (charge / discharge potential) for absorbing and releasing lithium ions that is more noble than that of the negative electrode active material described below may be used as the positive electrode active material. For example, various lithium-containing composite oxides such as lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium manganese nickel cobalt oxide, and spinel-based lithium compounds may be used as the positive electrode active material. Only one type of positive electrode active material may be used alone, or two or more types may be used in combination. The positive electrode active material may be, for example, particulate, and the size is not particularly limited. The particles of the positive electrode active material may be solid particles or hollow particles. The particles of the positive electrode active material may be primary particles or secondary particles formed by agglomeration of a plurality of primary particles. The average particle size of the particles of the positive electrode active material may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less.

[0031] The surface of the positive electrode active material may be covered with a protective layer containing a lithium ion conductive oxide. That is, the positive electrode active material layer 11 may include a composite having the above-mentioned positive electrode active material and a protective layer provided on the surface thereof. This makes it easier to suppress the reaction between the positive electrode active material and a sulfide (for example, the above-mentioned sulfide solid electrolyte, etc.). Examples of the lithium ion conductive oxide include Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, Li4Ti5O 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, and Li2WO4. The coverage (area ratio) of the protective layer may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less, or 20 nm or less.

[0032] The electrolyte that can be contained in the positive electrode active material layer 11 may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination thereof.

[0033] The solid electrolyte may be any known solid electrolyte for secondary batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes are excellent in ion conductivity and heat resistance. In addition to the above-mentioned sulfide solid electrolyte, examples of inorganic solid electrolytes include lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X Examples of oxide solid electrolytes include (PO4)3, Li-SiO-based glass, and Li-Al-SO-based glass. In particular, sulfide solid electrolytes, particularly sulfide solid electrolytes containing at least Li, S, and P as constituent elements, have high performance, and sulfide solid electrolytes based on a Li3PS4 framework and containing at least one type of halogen also have high performance. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be, for example, particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination.

[0034] The electrolytic solution may contain, for example, lithium ions as carrier ions. The electrolytic solution may be, for example, a non-aqueous electrolytic solution. For example, the electrolytic solution may be a carbonate-based solvent in which a lithium salt is dissolved at a predetermined concentration. Specifically, as described above, the electrolytic solution may be a cyclic carbonate in which a lithium amide salt is dissolved at a predetermined concentration.

[0035] Examples of the conductive assistant that may be included in the positive electrode active material layer 11 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0036] Examples of binders that can be included in the positive electrode active material layer 11 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, polyacrylic acid-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0037] 2.1.2 Positive electrode current collector As shown in FIG. 1, the positive electrode 10 may include a positive electrode collector 12 in contact with the positive electrode active material layer 11. The positive electrode collector 12 may be any of those commonly used as a positive electrode collector for a battery. The positive electrode collector 12 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The positive electrode collector 12 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 12 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 12 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 12 may contain Al. The positive electrode collector 12 may have some kind of coating layer on its surface for the purpose of adjusting resistance, or the like. The positive electrode current collector 12 may be a metal foil or a substrate plated or vapor-deposited with the above metal. When the positive electrode current collector 12 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the positive electrode current collector 12 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0038] In addition to the above configuration, the positive electrode 10 may have a general configuration as a positive electrode of a secondary battery. For example, a tab, a terminal, etc. The positive electrode 10 can be manufactured by applying a known method. For example, the positive electrode active material layer 11 can be easily formed by forming a positive electrode mixture containing the above various components in a dry or wet manner. The positive electrode active material layer 11 may be formed together with the positive electrode current collector 12, or may be formed separately from the positive electrode current collector 12.

[0039] 2.2 Electrolyte layer The electrolyte layer 20 includes at least an electrolyte. The electrolyte layer 20 may include a solid electrolyte, an electrolyte solution, or may further include a binder or the like. When the electrolyte layer 20 includes the lithium ion conductive material of the present disclosure, the electrolyte layer 20 may further include other electrolytes, binders, and various additives in addition to the lithium ion conductive material. In this case, the content of the electrolyte and binders in the electrolyte layer 20 is not particularly limited. Alternatively, the electrolyte layer 20 may include the lithium ion conductive material of the present disclosure as an electrolyte solution, and may have a separator or the like for holding the electrolyte solution and preventing contact between the positive electrode active material layer 11 and the negative electrode active material layer 31. The thickness of the electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0040] The electrolyte contained in the electrolyte layer 20 may be appropriately selected from the electrolytes (electrolytic solution and / or sulfide solid electrolyte) constituting the lithium ion conductive material of the present disclosure and the electrolytes exemplified as those that may be contained in the positive electrode active material layer. The binder that may be contained in the electrolyte layer 20 may also be appropriately selected from the binders exemplified as those that may be contained in the positive electrode active material layer. Each of the electrolytes and binders may be used alone or in combination of two or more kinds. The separator may be any separator that is commonly used in lithium ion secondary batteries, and examples of the separator include those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multilayer structure. Examples of the multilayer structure separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0041] 2.3 Negative electrode As shown in FIG. 1, an anode 30 according to one embodiment may include an anode active material layer 31 and an anode current collector 32. In this case, the anode active material layer 31 may contain the above-mentioned lithium ion conductive material.

[0042] 2.3.1 Negative electrode active material layer The negative electrode active material layer 31 includes a negative electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. Furthermore, the negative electrode active material layer 31 may further include various additives. When the negative electrode active material layer 31 includes the lithium ion conductive material of the present disclosure, the negative electrode active material layer 31 includes a negative electrode active material in addition to the lithium ion conductive material, and may further include other electrolytes, conductive assistants, binders, and various additives. The content of each of the negative electrode active material, electrolyte, conductive assistant, binder, and the like in the negative electrode active material layer 31 may be appropriately determined according to the intended battery performance. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, or may be less than 100 mass% or 90 mass% or less, with the entire negative electrode active material layer 31 (total solid content) being 100 mass%. The shape of the negative electrode active material layer 31 is not particularly limited, and may be, for example, a sheet-like shape having a substantially flat surface. The thickness of the negative electrode active material layer 31 is not particularly limited and may be, for example, 0.1 μm or more, 1 μm or more, 10 μm or more, or 30 μm or more, and may be 2 mm or less, 1 mm or less, 500 μm or less, or 100 μm or less.

[0043] As the negative electrode active material, various materials having a potential (charge / discharge potential) for absorbing and releasing lithium ions that is lower than that of the positive electrode active material can be used. For example, silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like can be used. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be a general shape as a negative electrode active material for a secondary battery. For example, the negative electrode active material may be in a particulate form. The negative electrode active material particles may be primary particles, or may be secondary particles in which a plurality of primary particles are aggregated. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material may be in the form of a sheet (foil or film) such as lithium foil, etc. In other words, the negative electrode active material layer 31 may be made of a sheet of the negative electrode active material.

[0044] Examples of the electrolyte that can be contained in the negative electrode active material layer 31 include the above-mentioned solid electrolyte, electrolytic solution, or a combination thereof. Examples of the conductive assistant that can be contained in the negative electrode active material layer 31 include the above-mentioned carbon material and metal material. The binder that can be contained in the negative electrode active material layer 31 may be appropriately selected from, for example, those exemplified as the binder that can be contained in the above-mentioned positive electrode active material layer 11. Only one type of electrolyte or binder may be used alone, or two or more types may be used in combination.

[0045] 2.3.2 Negative electrode current collector As shown in FIG. 1, the negative electrode 30 may include a negative electrode current collector 32 in contact with the negative electrode active material layer 31. The negative electrode current collector 32 may be any of those commonly used as a negative electrode current collector for a battery. The negative electrode current collector 32 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The negative electrode current collector 32 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, a metal foil is excellent in terms of ease of handling. The negative electrode current collector 32 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 32 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 32 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 32 may have some kind of coating layer on its surface for the purpose of adjusting the resistance or the like. The negative electrode current collector 32 may be a metal foil or a base material on which the above metal is plated or vapor-deposited. When the negative electrode current collector 32 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 32 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0046] In addition to the above configuration, the negative electrode 30 may have a general configuration as a negative electrode of a secondary battery. For example, a tab, a terminal, etc. The negative electrode 30 can be manufactured by applying a known method. For example, the negative electrode active material layer 31 can be easily formed by forming a negative electrode mixture containing the above various components in a dry or wet manner. The negative electrode active material layer 31 may be formed together with the negative electrode current collector 32, or may be formed separately from the negative electrode current collector 32.

[0047] 2.4 Other matters The lithium ion secondary battery 100 may have the above-mentioned components housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. A plurality of secondary batteries 100 may be electrically connected and stacked in any manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The secondary battery 100 may also have other obvious components such as necessary terminals. The shape of the secondary battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, or the like.

[0048] The lithium ion secondary battery 100 can be manufactured by applying a known method. For example, it can be manufactured as follows. However, the manufacturing method of the secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding. (1) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used, and N-methylpyrrolidone (NMP) can also be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, which serves as a positive electrode. (2) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used, and N-methylpyrrolidone (NMP) can also be used. The negative electrode layer slurry is then applied to the surface of a negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, forming a negative electrode. (3) The layers are laminated so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of a battery containing electrolyte, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3). EXAMPLES

[0049] The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0050] 1. Preparation of Lithium-ion Conductive Material 1.1 Example 1 A lithium ion conductive material for evaluation was obtained by weighing, mixing, and stirring each component so that the molar ratio of propylene carbonate (PC, Kishida Chemical Co., Ltd.) as the solvent and lithium bisfluorosulfonylamide (LiFSA, Kishida Chemical Co., Ltd.) as the lithium salt was 0.33 (PC:LiFSA = 3:1).

[0051] 1.2 Example 2 Each component was weighed, mixed and stirred so that the molar ratio of LiFSA to PC was 0.29 (PC:LiFSA=3.5:1), thereby obtaining a lithium ion conductive material for evaluation.

[0052] 1.3 Example 3 Each component was weighed, mixed and stirred so that the molar ratio of LiFSA to PC was 0.26 (PC:LiFSA=3.8:1), thereby obtaining a lithium ion conductive material for evaluation.

[0053] 1.4 Example 4 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 1, except that lithium bistrifluoromethanesulfonylamide (LiTFSA, manufactured by Kishida Chemical Co., Ltd.) was used instead of LiFSA.

[0054] 1.5 Example 5 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 2, except that LiTFSA was used instead of LiFSA.

[0055] 1.6 Example 6 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 3, except that LiTFSA was used instead of LiFSA.

[0056] 1.7 Example 7 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 1, except that a mixed solvent of PC and ethylene carbonate (EC, manufactured by Kishida Chemical Co., Ltd.) (mixed so that the molar ratio of PC and EC was PC:EC = 1:2) was used instead of a solvent containing PC alone.

[0057] 1.8 Comparative Example 1 Each component was weighed, mixed and stirred so that the molar ratio of LiFSA to PC was 0.08 (PC:LiFSA=11.8:1), thereby obtaining a lithium ion conductive material for evaluation.

[0058] 1.9 Comparative Example 2 Each component was weighed, mixed and stirred so that the molar ratio of LiFSA to PC was 0.25 (PC:LiFSA=4:1), thereby obtaining a lithium ion conductive material for evaluation.

[0059] 1.10 Comparative Example 3 A lithium ion conductive material for evaluation was obtained in the same manner as in Comparative Example 1, except that LiTFSA was used instead of LiFSA.

[0060] 1.11 Comparative Example 4 A lithium ion conductive material for evaluation was obtained in the same manner as in Comparative Example 2, except that LiTFSA was used instead of LiFSA.

[0061] 1.12 Comparative Example 5 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 1, except that dimethyl carbonate (DMC, manufactured by Kishida Chemical Co., Ltd.) was used instead of PC.

[0062] 1.13 Comparative Example 6 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 1, except that a mixed solvent of DMC and EC (mixed so that the molar ratio of DMC and EC was DMC:EC=1:2) was used instead of a single solvent of PC. In the lithium ion conductive material of Comparative Example 6, the molar ratio of LiFSA to EC was 0.50 (EC:LiFSA=2:1).

[0063] 1.14 Comparative Example 7 A lithium ion conductive material for evaluation was obtained in the same manner as in Example 1, except that lithium hexafluorophosphate (LiPF6, Kishida Chemical Co., Ltd.) was used instead of LiFSA.

[0064] 1.15 Comparative Example 8 The solvent, tetraglyme (G4, Kishida Chemical Co., Ltd.), was weighed out, mixed, and stirred so that the molar ratio of LiTFSA to tetraglyme was 1.25 (G4:LiTFSA=8:10), thereby obtaining a lithium ion conductive material for evaluation.

[0065] 2. Evaluation method for lithium ion conductive materials 2.1 Evaluation of heat resistance A TG-DTA test was performed on each lithium ion conductive material at a heating rate of 10°C / min. The temperature at which the liquid component volatilized and the weight loss of 0.5 wt% (T -0.5wt% The higher the temperature, the better the heat resistance (thermal stability). The results are shown in Figure 2.

[0066] 2.2 Ionic conductivity and lithium ion transport number (tLi + ) Evaluation In a two-electrode target cell with a fixed electrode distance using Li metal as the electrode, the ionic conductivity was measured by the complex impedance method at 25°C, and the lithium ion transport number was calculated by the Bruce method (Bruce et al. Solid State Ionics 28-30, 1987, 918-922), which combines DC polarization and impedance methods. The results for the lithium ion transport number are shown in Figure 3.

[0067] 2.3 Evaluation of lithium ion conductivity The lithium ion conductivity was evaluated by multiplying the lithium ion transport number obtained by the electrochemical method described above by the ionic conductivity. The results are shown in Figure 4.

[0068] 2.4 Reactivity evaluation with sulfide solid electrolyte A sulfide solid electrolyte with a composition of 75(75Li2S 25P2S5) 10LiI 15LiBr (units of mol%) was immersed in each lithium ion conductive material for two months, and X-ray diffraction measurements were performed on the sulfide solid electrolyte before and after immersion to confirm the change in the X-ray diffraction spectrum. The results are shown in Figure 5.

[0069] 3. Evaluation results of lithium ion conductive materials 3.1 Heat resistance The results shown in FIG. 2 reveal the following. When the molar ratio of the lithium salt to the solvent is less than 0.1 as in Comparative Example 1, the heat resistance is the same as when no lithium salt is included. In other words, the effect of improving heat resistance by dissolving the lithium salt in the solvent is not observed. Also, when the molar ratio is 0.25 as in Comparative Examples 2 and 4, the heat resistance is slightly improved. Furthermore, when the molar ratio exceeds 0.25 as in Examples 1 and 4, the heat resistance is significantly improved.

[0070] 3.2 Lithium ion conductivity 3.2.1 Lithium ion transport number The results shown in Fig. 3 reveal the following. Compared with the case where the molar ratio of the lithium salt to the solvent is 0.25 or less as in Comparative Examples 1 to 4, when the molar ratio exceeds 0.25 as in Examples 1 to 6, the lithium ion transport number is significantly higher. On the other hand, as far as the present inventors have confirmed, when the molar ratio of the lithium salt to the solvent is excessive, the viscosity becomes too high (for example, it becomes solid at room temperature), and the lithium ion conductivity is likely to decrease. When the molar ratio of the lithium salt to the solvent is greater than 0.25 and equal to or less than 0.33 as in Examples 1 to 6, such a problem does not occur.

[0071] 3.2.2 Lithium ion conductivity The results shown in Fig. 4 reveal the following. Usually, as the concentration of lithium salt in a solvent increases, there is concern that the viscosity will increase and the ion conductivity will decrease. In contrast, in Examples 1 to 6, even if the viscosity increases, high lithium ion conductivity is easily ensured due to the increase in the lithium ion transport number.

[0072] As described above, the lithium ion conductive materials (Examples 1 to 6) in which the molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and is 0.33 or less can be said to have a better balance between heat resistance and lithium ion conductivity than the lithium ion conductive materials (Comparative Examples 1 to 4) in which the molar ratio is 0.25 or less. As far as the inventors have confirmed, when a large amount of a solvent other than the cyclic carbonate (e.g., a chain carbonate) is present, the amount of the cyclic carbonate is relatively small, as in Comparative Example 6, and as a result, the concentration of the Li salt relative to the cyclic carbonate becomes relatively excessive, the heat resistance of the lithium ion conductive material tends to decrease.

[0073] 3.3 Reactivity with sulfide solid electrolytes The results shown in FIG. 5 reveal the following. In FIG. 5, for Examples 1, 4, and 7, the X-ray diffraction peak patterns of the sulfide solid electrolyte after immersion in the lithium ion conductive material are substantially the same as those of the sulfide solid electrolyte (Reference Example) before immersion. In contrast, for Comparative Examples 5 to 8, the X-ray diffraction peak patterns of the sulfide solid electrolyte after immersion in the lithium ion conductive material are significantly different from those of the sulfide solid electrolyte (Reference Example) before immersion. From this, it can be said that the reactivity between the lithium ion conductive material and the sulfide solid electrolyte changes depending on the type and polarity of the solvent constituting the lithium ion conductive material, the type of anion of the lithium salt, and the like. For example, in the case of Comparative Example 5 where a chain carbonate is used as a solvent instead of a cyclic carbonate, or in the case of Comparative Example 6 where a large amount of a chain carbonate is used together with a cyclic carbonate as a solvent (resulting in an excessive molar ratio of lithium salt to cyclic carbonate), the chain carbonate is likely to be present in a free state, and the active site of the chain carbonate reacts with the sulfide solid electrolyte, which is considered to have altered and deteriorated the sulfide solid electrolyte. The same is true in the case of Comparative Example 8 where G4 is used as a solvent. In addition, in the case of Comparative Example 7 where LiPF6 is used as a lithium salt instead of a lithium amide salt, the PF6 anion reacts with the sulfide solid electrolyte, which is considered to have altered and deteriorated the sulfide solid electrolyte.

[0074] 4. Summary From the above results, it can be said that the lithium ion conductive materials having the following configurations (1) and (2) have excellent thermal stability and lithium ion conductivity. (1) A solution comprising a cyclic carbonate as a solvent and a lithium amide salt dissolved in the cyclic carbonate. (2) The molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and not greater than 0.33.

[0075] The lithium ion conductive material having the above configurations (1) and (2) may contain a sulfide solid electrolyte together with the cyclic carbonate and the lithium amide salt. In particular, the lithium ion conductive material having the following configuration (3) can suppress the deterioration of the sulfide solid electrolyte in addition to the above effects. (3) The lithium amide salt is at least one of lithium bisfluorosulfonylamide and lithium bistrifluoromethanesulfonylamide. [Explanation of symbols]

[0076] 10 positive electrode 11 Cathode active material layer 12 Positive electrode current collector 20 Electrolyte layer 30 negative electrode 31 Negative electrode active material layer 32 Negative electrode current collector 100 Lithium-ion secondary battery

Claims

1. A lithium ion conducting material comprising: A cyclic carbonate as a solvent; a lithium amide salt dissolved in the cyclic carbonate; a molar ratio of the lithium amide salt to the cyclic carbonate is greater than 0.25 and less than or equal to 0.33; the lithium amide salt is at least one of lithium bisfluorosulfonylamide and lithium bistrifluoromethanesulfonylamide; The cyclic carbonate and the lithium amide salt are combined with a sulfide solid electrolyte. Lithium ion conducting material.

2. 2. The lithium ion conductive material according to claim 1 , The cyclic carbonate is at least one of propylene carbonate and ethylene carbonate. Lithium ion conducting material.

3. A lithium ion secondary battery comprising a positive electrode, an electrolyte layer, and a negative electrode, At least one of the positive electrode, the electrolyte layer and the negative electrode comprises the lithium ion conductive material according to claim 1 or 2. Lithium-ion secondary battery.

Citation Information

Patent Citations

  • Lithium secondary battery electrolyte, and secondary battery including the same

    JP2016122657A

  • Lithium ion secondary battery

    JP2017147184A

  • Electrolyte solution for lithium ion secondary battery and lithium ion secondary battery

    JP2019096463A

  • Electrode for lithium ion battery and lithium ion battery

    JP2020009750A