Water-based inkjet ink set
The aqueous inkjet ink set addresses bleeding and fixability issues by using a pretreatment agent and specifically formulated dark and light inks to enhance dot diameter and fixability, achieving high-quality printed images on various substrates.
Patent Information
- Application Number
- JP2020163451
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-29
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Water-based inkjet inks face issues with bleeding on various substrates, slow drying times leading to color mixing in multicolor printing, and poor fixability on low-permeability substrates like resin sheets, resulting in grainy images and reduced image quality.
An aqueous inkjet ink set comprising a pretreatment agent with a surfactant having an HLB value of 10.0 or more, dark ink with a surfactant having an HLB value less than 10.0 and a specific SP value, and light ink with a higher viscosity and solvent concentration to enhance dot diameter and fixability, reducing graininess.
The ink set improves image quality by minimizing graininess and enhancing fixability on diverse substrates, including low-permeability materials, resulting in high-quality printed matter.
Smart Images

Figure 0007556730000005 
Figure 0007556730000006 
Figure 0007556730000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous inkjet ink set. [Background technology]
[0002] Inkjet recording systems are printing systems that spray highly fluid liquid ink from minute nozzles and deposit it onto a substrate to perform printing. This system has recently become increasingly popular due to its features of being able to print high-resolution, high-quality images at high speed and with little noise using relatively inexpensive equipment. Water-based inks are widely used because they can produce high-quality prints at low cost. Water-based inks have an increased drying time due to their water content, and also have the advantage of being environmentally friendly.
[0003] In an inkjet recording system, ink is applied in the form of dots on a substrate to form an image. The shape, size, spacing, etc. of the dots affect the quality of the printed image. For example, if the dot diameter is small and the distance between dots is long, a grainy appearance may be observed in the printed image. For example, there is a technique for using dark and light inks to obtain one hue, adjusting the gradation from medium density areas to high density areas, and reducing the graininess of the printed image to make it smoother.
[0004] Patent Document 1 proposes an ink set for water-based inkjet printers that uses dark and light inks, specifies the organic solvents to be blended into the dark and light inks, and further specifies the difference in viscosity between the dark and light inks to improve printability on printing media with low absorbency, such as coated paper. Patent Document 1 discloses that if the viscosity of inks differs significantly, this will result in differences in the volume of droplets ejected, which in turn will result in uneven dot diameters and problems such as a grainy appearance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-17103 A Summary of the Invention [Problem to be solved by the invention]
[0006] When a water-based ink contains a penetrating component such as a surfactant, the water-based ink spreads on various substrates, causing the printed image to bleed. Furthermore, in multi-color printing, if the water-based ink takes a long time to dry on the substrate, the colors tend to mix with each other. In addition, when using aqueous ink on a low-permeability substrate such as a resin sheet, the ink is repelled from the substrate before it dries on the substrate, which makes it difficult to fix the printed image. In addition, the aqueous ink has low affinity for resin sheets and the like, which can reduce the fixability to the substrate.
[0007] Therefore, in order to fix the water-based ink more firmly on the substrate and prevent bleeding of the printed image, there is a technique for pretreating the substrate before applying the ink. By applying a pretreatment agent to the substrate, the fixability of the ink on the substrate can be improved and bleeding of the ink can be prevented. On the other hand, the action of the pretreatment agent makes it difficult for the ink dot diameter to spread, which can cause a grainy feeling problem. Patent Document 1 targets printing media with low absorbency, such as coated paper, but does not consider using a pretreatment agent before applying ink to prevent bleeding of the printed image.
[0008] It is an object of the present invention to provide an aqueous inkjet ink set that produces high quality prints. [Means for solving the problem]
[0009] One aspect of the present invention provides a method for producing a printhead comprising the steps of: providing a printhead having an HLB value of 10.0 or more; and a light ink having an HLB value of 15.5 (cal / cm 2 ); and providing a printhead having an HLB value of 10.0 or more and a surfactant contained in the printhead having an HLB value of 10.0 or more and a difference of 2.0 or more between the HLB value of the surfactant contained in the printhead and the HLB value of the dark ink. 3 ) 1 / 2 The light ink contains the following solvents and water, and has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The light ink contains the following solvents and water, and the SP value of the light ink is 15.5 (cal / cm 3 ) 1 / 2 The concentration (mass%) of the following solvents is such that the SP value of the thick ink is 15.5 (cal / cm 3 ) 1 / 2 The concentration (mass %) of the light ink is 1.1 times or more the concentration of the following solvent, and the viscosity (mPa·s) of the light ink at 23° C. is 1.05 times or more the viscosity (mPa·s) of the dark ink. Effect of the Invention
[0010] According to one embodiment of the present invention, it is possible to provide a water-based inkjet ink set that can produce high-quality printed matter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described below using an embodiment. The following embodiment is not intended to limit the present invention.
[0012] An aqueous inkjet ink set according to one embodiment includes a pretreatment agent, and a dark ink and a light ink of the same hue. The pretreatment agent includes a surfactant having an HLB value of 10.0 or more, and water. The dark ink includes a surfactant having an HLB value of less than 10.0, the difference between the HLB value of the surfactant contained in the pretreatment agent being 2.0 or more, and an SP value of 15.5 (cal / cm 3 ) 1 / 2 The light ink contains the following solvents and water, and has an SP value of 15.5 (cal / cm3 ) 1 / 2 The following solvents and water are included in the light ink, and the SP value is 15.5 (cal / cm 3 ) 1 / 2 The concentration (mass%) of the following solvents is 15.5 (cal / cm 3 ) 1 / 2 The ink is characterized by having a concentration (mass %) of at least 1.1 times that of the solvent below, and a viscosity (mPa·s) of the light ink at 23°C of at least 1.05 times that of the dark ink. This makes it possible to obtain high-quality printed matter, and in particular to reduce graininess in the printed image, thereby improving image quality.
[0013] Hereinafter, a surfactant that is blended into a pretreatment agent and has an HLB value of 10.0 or more will be referred to as surfactant (a), a surfactant that is blended into a dark ink and has an HLB value of less than 10.0 and a difference of 2.0 or more with respect to the HLB value of the surfactant contained in the pretreatment agent will be referred to as surfactant (b), and a surfactant that is blended into a dark ink and has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The following solvent is also referred to as solvent (c1), and the SP value of the light ink is 15.5 (cal / cm 3 ) 1 / 2 The following solvents are also referred to as solvent (c2).
[0014] The aqueous inkjet ink set according to one embodiment can be used to obtain a printed matter by treating a substrate with a pretreatment agent, discharging one of the dark ink and the light ink onto the substrate, and then discharging the other of the dark ink and the light ink onto the substrate. In a preferred embodiment, the ink is discharged after applying the pretreatment agent to the substrate. As one method of forming an image, a subsequent ink is discharged onto the substrate so as to be adjacent to a dot of an ink discharged earlier, so that the colorant concentration differs between adjacent dots, and therefore the hue gradation can be adjusted. The aqueous inkjet ink set according to one embodiment has the above-mentioned characteristics, and therefore can appropriately widen the dot diameter of the dark ink on the pretreated substrate, thereby reducing the graininess of the printed image and improving the image quality of the resulting printed matter.
[0015] This mechanism is explained below, but the details of the mechanism are unknown and do not restrict the present invention. On the substrate, the light ink dots have a high concentration of low SP value solvent (c2) that can dissolve surfactant (b) with an HLB value of 10.0 or less that is blended into the dark ink, and therefore act to capture the surfactant (b) in the dark ink dots. Also, if the light ink dots spread too much on the substrate, this effect is reduced, so the viscosity of the light ink is increased to prevent the light ink dot diameter from spreading on the substrate. Furthermore, when the HLB value of the surfactant (a) in the pretreatment agent is greater than the HLB value of the surfactant (b) in the dark ink, and the difference between them is 2.0 or more, the effect of widening the diameter of dark ink dots on the substrate is manifested. This is thought to be because the dark ink dots on the substrate to which the pretreatment agent has been applied function to incorporate the surfactant (a) in the pretreatment agent. In other words, on the substrate, the dark ink dots attempt to expel the surfactant (b) in the dark ink that has an HLB value of less than 10.0, and so approach dots of light ink that are rich in solvent (c2) with a low SP value; on the substrate, the dark ink dots attempt to take in the surfactant (a) in the pretreatment agent that has been applied in advance and has an HLB value of 10.0 or more, and so the diameter of the dark ink dots becomes wider. By increasing the diameter of dots of dark ink on the substrate, the graininess of the printed image can be reduced, resulting in a high-quality print.
[0016] In one embodiment, it is preferred that the HLB value of the surfactant (a) contained in the pretreatment agent is 10.0 or more, the HLB value of the surfactant (b) contained in the dark ink is less than 10.0, and the difference between the HLB value of the surfactant (a) and the HLB value of the surfactant (b) is 2.0 or more. This difference in HLB values is also referred to as the HLB value difference (ab).
[0017] The HLB value of the surfactant (a) incorporated in the pretreatment agent is preferably 10.0 or more, more preferably 11.0 or more, and even more preferably 12.0 or more, thereby making it possible to further reduce the graininess of the printed image and obtain a printed product of higher image quality. The HLB value of the surfactant (a) blended in the pretreatment agent is not particularly limited and may be 20 or less, preferably 18.0 or less, more preferably 16.0 or less, and even more preferably 15.0 or less. This allows the surfactant to exhibit a sufficient balance of hydrophilicity and lipophilicity, enhances the affinity with the substrate to which the pretreatment agent is applied, and makes it possible to apply the pretreatment agent more uniformly to the substrate. In addition, the fixation of the ink to the substrate to which the pretreatment agent is applied can be further improved. For example, the HLB value of the surfactant (a) is preferably from 10.0 to 18.0, more preferably from 11.0 to 16.0, and even more preferably from 12.0 to 15.0.
[0018] The HLB value of the surfactant (b) blended in the dark ink is preferably less than 10.0, more preferably 9.5 or less, and even more preferably 9.0 or less, which can reduce the graininess of the printed image and produce a higher quality print. The HLB value of the surfactant (b) to be blended in the thick ink is not particularly limited and may be 1.0 or more, preferably 2.0 or more, and more preferably 3.0 or more. This allows the surfactant to exhibit a sufficient balance of hydrophilicity and lipophilicity in the aqueous thick ink, and prevents the storage stability of the ink from decreasing. If the HLB value of the surfactant (b) is low, the solubility in water decreases, which may result in restrictions such as the need to increase the amount of solvent in the thick ink. For example, the HLB value of the surfactant (b) is preferably from 1.0 to 10.0, more preferably from 2.0 to 9.5, and even more preferably from 3.0 to 9.0. Furthermore, by including a surfactant having an HLB value within the above range in the dark ink, the affinity between the dark ink and the substrate can be increased, thereby further improving the adhesion of the dark ink to the substrate.
[0019] The difference (ab) between the HLB value of the surfactant (a) contained in the pretreatment agent and the HLB value of the surfactant (b) contained in the dark ink is preferably 2.0 or more, more preferably 3.0 or more, and even more preferably 4.0 or more. This makes it possible to further reduce the graininess of the printed image and obtain a printed product of higher image quality. Moreover, the difference (ab) between the HLB values is preferably 15.0 or less, more preferably 10.0 or less, and even more preferably 6.0 or less, which increases the solubility of each surfactant in the pretreatment agent or the concentrated ink, enabling the surfactant to better exhibit its function. For example, the difference (ab) in the HLB values is preferably from 2.0 to 15.0, more preferably from 3.0 to 10.0, and even more preferably from 4.0 to 6.0.
[0020] Here, the HLB value is one of the scales that indicate the properties of a surfactant, and is a numerical representation of the balance between hydrophilic and lipophilic groups in the molecule. The HLB value is proposed by several calculation methods, but in this specification, it is a value calculated by the Griffin method, and is calculated by the following formula (1). HLB value = 20 × (formula weight of hydrophilic part) / (molecular weight of surfactant) Equation (1)
[0021] Here, the "hydrophilic portion" refers to a hydrophilic portion contained in the molecular structure of the surfactant, and is preferably a polyoxyalkylene group, an alcohol group having 3 or less carbon atoms in the main chain relative to the hydroxyl group, or a combination thereof. When the surfactant contains multiple hydrophilic portions, the formula weight of the hydrophilic portion in the above formula (1) is the total amount of these. The polyoxyalkylene group is a polyoxyethylene group (polyethylene oxide; EO: -(CH2CH2O) n -), polyoxypropylene group (polypropylene oxide; PO: -(CH2CH2CH2O) n -) etc. Examples of the alcohol group include groups derived from methanol, ethanol, propanol, isopropanol, glycerin, polyglycerin, trimethylolpropane, pentaerythritol, sorbitol, sorbitan, sucrose (cane sugar), mannitol, glycols, etc. (for example, -CH2CH2OH for ethanol).
[0022] The "hydrophobic portion" refers to a hydrophobic portion contained in the molecular structure of a surfactant, and is preferably an aliphatic alcohol having 4 or more carbon atoms in the main chain relative to the hydroxyl group, an alkylphenol, an aliphatic hydrocarbon group derived from a fatty acid, etc., an aromatic hydrocarbon group, an organic siloxane, an alkyl halide, etc., or a combination thereof.
[0023] In one embodiment, the dark ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The following solvent (c1) is included, and the light ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The following solvent (c2) is included, and the SP value of the light ink is 15.5 (cal / cm 3 ) 1 / 2 The concentration of the following solvent (c2) is 15.5 (cal / cm 3 ) 1 / 2 It is preferable that the concentration ratio is 1.1 times or more the concentration of the following solvent (c1). This concentration ratio is also referred to as the concentration ratio (c2 / c1). The units of the concentrations of the solvents (c1) and (c2) are each % by mass.
[0024] The SP value of the dark ink is 15.5 (cal / cm 3 ) 1 / 2 The concentration of the following solvent (c1) is 15.5 (cal / cm3) in terms of the total mass of the dark ink. 3 )1 / 2 It can be expressed as the mass ratio (mass%) of the following solvent (c1). The SP value of the dark ink is 15.5 (cal / cm 3 ) 1 / 2 If two or more of the following solvents (c1) are included, the SP value of two or more of them must be 15.5 (cal / cm) based on the total mass of the dark ink. 3 ) 1 / 2 The percentage (mass%) of the total mass of the following solvent (c1) is the concentration of solvent (c1). Similarly, the SP value of the light ink is 15.5 (cal / cm 3 ) 1 / 2 The concentration of the following solvent (c2) is 15.5 (cal / cm3) in terms of the total mass of the light ink. 3 ) 1 / 2 It can be expressed as the mass ratio (mass%) of the following solvent (c2). The SP value of the light ink is 15.5 (cal / cm 3 ) 1 / 2 If two or more of the following solvents (c2) are included, the SP value of two or more of them must be 15.5 (cal / cm) based on the total mass of the light ink. 3 ) 1 / 2 The percentage (mass%) of the total mass of the following solvent (c2) is the concentration of solvent (c2).
[0025] The concentration ratio (c2 / c1) is preferably 1.1 or more, more preferably 1.12 or more, and even more preferably 1.15 or more, which can reduce the graininess of the printed image and produce a higher quality print. Furthermore, the concentration ratio (c2 / c1) is not particularly limited, and is preferably no more than 10, more preferably no more than 5, and even more preferably no more than 2. This prevents the surfactant of the dark ink from migrating excessively from the dark ink dot to the light ink dot between adjacent dark ink dots and light ink dots, and makes it possible to form a smooth image by maintaining the overall hue concentration gradient. For example, the concentration ratio (c2 / c1) is preferably 1.1 to 10 times, more preferably 1.12 to 5 times, and further preferably 1.15 to 2 times.
[0026] The dark ink and the light ink each have an SP value of 15.5 (cal / cm 3 ) 1 / 2 It is preferable that the solvent contains the following solvent, and more preferably, the SP value is 15.3 (cal / cm 3 ) 1 / 2 More preferably, the solvent has an SP value of 15.0 (cal / cm 3 ) 1 / 2 The solvent is as follows. This increases the solubility of the surfactant (b) with an HLB value of less than 10.0 in the dark ink, and improves the affinity between the ink and the substrate, the ink ejection performance, and the like. This is also true when the light ink contains a surfactant. In addition, on the substrate, the surfactant (b) in the dark ink can be moved from the dark ink dots to the light ink dots, making it possible to increase the diameter of the dark ink dots and reduce the graininess. The SP value for the dark ink and the light ink is 15.5 (cal / cm 3 ) 1 / 2 The following solvents have an SP value of 5 (cal / cm 3 ) 1 / 2 More than 10 (cal / cm3) is preferable. 1 / 2 More preferably, 12 (cal / cm 3 ) 1 / 2 This is even more preferable. In each of the dark ink and the light ink, the aqueous solvent forms a single phase, and the storage stability of the ink can be further improved. For example, the dark ink and the light ink each have an SP value of 5 to 15.5 (cal / cm 3 ) 1 / 2 is preferable, and 10 to 15.3 (cal / cm 3 ) 1 / 2 More preferably, 15.0 to 12 (cal / cm 3 ) 1 / 2 is more preferred.
[0027] Here, the SP value is the solubility parameter, and is defined as the square root of the molecular cohesive energy density. There are various calculation methods, but here we use the value calculated by the estimation method proposed by Fedor (Equation 1). [Formula 1] δ(SP value) = [ΣE coh / ΣV] 1 / 2 (1) Here, E coh indicates a constant specific to each functional group, and V indicates the molar moles (see "SP Value Basics, Applications and Calculation Methods", pp. 66-67, Johokiko Co., Ltd., published on March 31, 2005).
[0028] SP value is 15.5 (cal / cm 3 ) 1 / 2 As the following solvent, it is preferable to use a water-soluble organic solvent. It is preferable that the water-soluble organic solvent is compatible with water. As the water-soluble organic solvent, an organic compound that is liquid at room temperature and can be dissolved or mixed in water can be used, and it is preferable to use a water-soluble organic solvent that is uniformly mixed with the same volume of water at 20°C under 1 atmosphere.
[0029] SP value is 15.5 (cal / cm 3 ) 1 / 2 Specific examples of the following solvents include diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monohexyl ether, diethylene glycol monobutyl ether, diethylene glycol monoisopropyl ether, dipropylene glycol monomethyl ether, diethylene glycol monoethyl ether, ethylene glycol propyl ether, diethylene glycol monomethyl ether, ethylene glycol allyl ether, diethylene glycol benzyl ether, diethylene glycol phenyl ether, 1,2-hexanediol, N-methyl-2-pyrrolidone (NMP), 1,2-butanediol, 1,2-propanediol, 1,6-hexanediol, dipropylene glycol, 1,3-propanediol, 2-pyrrolidone, ethylene glycol, diethylene glycol, and 1,4-butanediol. These are preferably used in an amount sufficient to form a single phase together with water, and may be used alone or in combination of two or more.
[0030] In dark ink, the SP value is 15.5 (cal / cm 3 ) 1 / 2 The content of the following solvent (c1) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total amount of the dark ink. In dark ink, the SP value is 15.5 (cal / cm 3 ) 1 / 2 The content of the following solvent (c1) is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 25% by mass or less, based on the total amount of the dark ink. When the content of the solvent (c1) in the thick ink is within the above range, the concentration ratio (c2 / c1) can be appropriately adjusted, and the graininess of the printed image can be further reduced.
[0031] In light ink, the SP value is 15.5 (cal / cm 3 ) 1 / 2 The content of the following solvent (c2) is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the total amount of the light ink. In light ink, the SP value is 15.5 (cal / cm 3 ) 1 / 2 The content of the following solvent (c2) is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total amount of the light ink. When the content of the solvent (c1) in the light ink is within the above range, the concentration ratio (c2 / c1) can be appropriately adjusted, and the graininess of the printed image can be further reduced. The SP value for the dark and light inks is 15.5 (cal / cm 3 ) 1 / 2 If two or more of the following solvents are included, the SP value of two or more of them must be 15.5 (cal / cm 3 ) 1 / 2 It is preferable that the total mass of the following solvents falls within the above range.
[0032] In one embodiment, it is preferable that the viscosity of the light ink is at least 1.05 times that of the dark ink at 23° C. Hereinafter, the viscosity of the dark ink will be referred to as v1, the viscosity of the light ink will be referred to as v2, and this viscosity ratio will be referred to as the viscosity ratio (v2 / v1). The units of the viscosity of the dark ink (v1) and the viscosity of the light ink (v2) will each be mPa s. This viscosity ratio (v2 / v1) is preferably 1.05 times or more, more preferably 1.10 times or more, and even more preferably 1.15 times or more. This makes it possible to further reduce the graininess of the printed image and obtain a printed matter of higher image quality. Specifically, by preventing the dot diameter of the light ink with higher viscosity from expanding on the substrate and allowing the surfactant (b) of the dark ink to move from the dots of the dark ink with lower viscosity to the dots of the light ink, it is possible to prevent the dot diameter of the dark ink from expanding and reduce the graininess while maintaining a certain concentration gradient. Furthermore, this viscosity ratio (v2 / v1) is not particularly limited, but is preferably 2 times or less, more preferably 1.5 times or less, and even more preferably 1.3 times or less. This prevents the viscosity difference between the two inks from becoming too large, making it easier to print the dark ink and the light ink using the same inkjet printing device. For example, the ejection performance from the inkjet nozzle can be improved for both the dark ink and the light ink. For example, the viscosity ratio (v2 / v1) is preferably from 1.05 to 2 times, more preferably from 1.10 to 1.5 times, and even more preferably from 1.15 to 1.3 times.
[0033] The viscosity of the dark ink is preferably 2 mPa·s or more, more preferably 5 mPa·s or more, even more preferably 8 mPa·s or more, and may be 9 mPa·s or more. The viscosity of the dark ink is preferably 30 mPa·s or less, more preferably 15 mPa·s or less, and even more preferably 13 mPa·s or less. When the viscosity (v1) of the dark ink is in the above range, the viscosity ratio (v2 / v1) can be appropriately adjusted, and the graininess of the printed image can be further reduced.
[0034] The viscosity of the light ink is preferably 2 mPa·s or more, more preferably 5 mPa·s or more, even more preferably 7 mPa·s or more, and may be 10 mPa·s or more. The viscosity of the light ink is preferably 30 mPa·s or less, more preferably 15 mPa·s or less, and even more preferably 15 mPa·s or less. When the viscosity (v2) of the light ink is in the above range, the viscosity ratio (v2 / v1) can be adjusted appropriately, and the graininess of the printed image can be further reduced.
[0035] Here, the viscosity of the ink is represented by the value at 23° C. and 10 Pa when the shear stress is increased from 0 Pa at a rate of 0.1 Pa / s. The ink viscosity ratio can be calculated by measuring the viscosity (v1) of the dark ink and the viscosity (v2) of the light ink according to the procedure described above, and calculating the ratio (v2 / v1).
[0036]
[0043] In an embodiment of the aqueous inkjet ink set, the pretreatment agent, the dark ink, and the light ink have the above-mentioned physical properties, thereby reducing the graininess of the printed image and providing printed matter of higher image quality.
[0037] "Pretreatment agent" The pretreatment agent will now be described. The pretreatment agent according to one embodiment includes a surfactant having an HLB value of 10.0 or more, and water. The relationship between the HLB value of the surfactant (a) contained in the pretreatment agent and the HLB value of the surfactant (a) contained in the pretreatment agent and the HLB value of the surfactant (b) contained in the dark ink is as described above.
[0038] By including a surfactant in the pretreatment agent, the affinity of the pretreatment agent to the substrate can be improved, and the pretreatment agent can be applied more uniformly onto the substrate. For example, many low-permeability substrates have a hydrophobic substrate surface in an untreated state, and therefore when an aqueous ink is applied to an untreated substrate, the wettability of the aqueous ink to the substrate is poor, resulting in non-uniform printed dots on the substrate and reduced image quality. In contrast, by using a substrate treated with a pretreatment agent containing a surfactant, the wettability of the substrate to the aqueous ink can be further improved.
[0039] The surfactant (a) has an HLB value of 10.0 or more. A nonionic surfactant can be preferably used as the surfactant (a). In addition, either a low molecular weight surfactant or a high molecular weight surfactant can be used.
[0040] Examples of nonionic surfactants include ester surfactants such as glycerin fatty acid esters and fatty acid sorbitan esters; ether surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers and polyoxypropylene alkyl ethers; ether ester surfactants such as polyoxyethylene sorbitan fatty acid esters; acetylene surfactants; silicone surfactants; and fluorine surfactants. Among these, acetylene surfactants and silicone surfactants can be preferably used. The surfactants may be used alone or in combination of two or more.
[0041] Examples of the acetylene-based surfactant include acetylene glycol-based surfactants, acetylene alcohol-based surfactants, and surfactants having an acetylene group. The acetylene glycol surfactant is a glycol having an acetylene group, preferably a glycol having a symmetrical structure with the acetylene group located in the center, and may have a structure in which ethylene oxide is added to acetylene glycol.
[0042] When acetylene glycol having ethylene oxide added thereto is used as the acetylene glycol surfactant, the number of moles of ethylene oxide added is preferably 6 or more, more preferably 8 or more, and even more preferably 10 or more.
[0043] Commercially available acetylene surfactants having an HLB value of 10.0 or more include, for example, "Olfine E1010, E1006, E1020" and "Surfynol 465, 485" (all manufactured by Nissin Chemical Industry Co., Ltd.) (all trade names).
[0044] Examples of silicone surfactants include polyether-modified silicone surfactants, alkyl / aralkyl-co-modified silicone surfactants, and acrylic silicone surfactants.
[0045] As the silicone surfactant, for example, a compound having a polyalkylene glycol chain in a polysiloxane skeleton can be used.Specifically, a compound in which at least one polyalkylene glycol chain is bonded to at least one Si element selected from the Si elements at 1st, 3rd, and 6th positions of trisiloxane can be used.In this compound, the polyalkylene glycol chain can be a polyethylene glycol chain, a polypropylene glycol chain, a polytrimethylene glycol chain, etc., but is preferably a polyethylene glycol chain.
[0046] Among them, it is preferable to use, as the silicone surfactant, heptamethyltrisiloxane having a polyethylene glycol chain with an added mole number of ethylene oxide of 7 or more. In this surfactant, the added mole number of ethylene oxide is more preferably 7 to 40, further preferably 9 to 35, and even more preferably 8 to 30. In this surfactant, the methyl group bonded to the siloxane skeleton may be substituted with another hydrophobic group such as an alkyl group having 2 or more carbon atoms. In addition, it is preferable to use, as the silicone surfactant, nonamethyltetrasiloxane having a polyethylene glycol chain with an added mole number of ethylene oxide of 9 or more. In this surfactant, the added mole number of ethylene oxide is more preferably 11 to 40, and further preferably 13 to 35. In this surfactant, the methyl group bonded to the siloxane skeleton may be substituted with another hydrophobic group, such as an alkyl group having 2 or more carbon atoms.
[0047] The surfactant (a) may also be a compound represented by the general formula "C m H 2m +1-O-(CH2CH2O) n In this general formula, it is preferable that n=1 and m=1, n=2 and m=1 to 5, n=3 and m=1 to 8, or n=4 and m=1 to 11.
[0048] The amount of the active ingredient of the surfactant (a) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.7% by mass or more, based on the total amount of the pretreatment agent. This can further reduce the graininess of the printed image and further improve the image quality. Specifically, on the substrate, the amount of the surfactant (a) in the pretreatment agent that migrates from the base pretreatment agent to the dots of the dark ink increases, further increasing the diameter of the dots of the dark ink and further reducing the graininess. In addition, the affinity between the pretreatment agent and the substrate can be further improved. The amount of the surfactant (a) in terms of active ingredient is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total amount of the pretreatment agent, which can prevent a decrease in the storage stability of the pretreatment agent. For example, the amount of the surfactant (a) in terms of active ingredient is preferably 0.1 to 10 mass %, more preferably 0.5 to 5 mass %, and even more preferably 0.7 to 1 mass %, relative to the total amount of the pretreatment agent.
[0049] The pretreatment agent may further include an aggregating agent. When the pretreatment agent includes an aggregating agent, when an aqueous ink is applied to a substrate treated with the pretreatment agent, the coloring material of the aqueous ink is agglomerated on the substrate by the aggregating agent in the pretreatment agent, thereby suppressing bleeding of the image and further improving the image quality. As the flocculant, a cationic resin, a polyvalent metal salt, an organic acid, an inorganic acid, a salt of an inorganic acid, or a combination thereof can be used.
[0050] The cationic resin may be either a cationic water-soluble resin or a cationic water-dispersible resin, or a combination of these may be used.
[0051] Examples of cationic water-soluble resins include polyethyleneimine (PEI), polyvinylamine, polyallylamine and its salts, polyvinylpyridine, cationic acrylamide copolymers, etc. More specifically, polydiallyldimethylammonium chloride, etc. can be used.
[0052] Examples of commercially available cationic water-soluble resins include the Charol series "DC-303P, DC-902P" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., the Unisense series "FCA1000L, FPA100L" manufactured by Senka Corporation, the HC Polymer series "1S, 1N, 1NS, 2, 2L" manufactured by Osaka Organic Chemical Industry Ltd., and the Himax series "Himax SC-103, SC-506, SC-700L" manufactured by Himo Corporation (all trade names).
[0053] Commercially available polyethyleneimines include, for example, the Epomin series "SP-006, SP-012, SP-018, SP-200" manufactured by Nippon Shokubai Co., Ltd.; and "Lupasol FG, Lupasol G20 Waterfree, Lupasol PR 8515" manufactured by BASF Japan Ltd. (all trade names). In addition, examples of commercially available polyallylamine products include "allylamine polymers PAA-01, PAA-03, and PAA-05, allylamine hydrochloride polymers PAA-HCL-01, PAA-HCL-03, and PAA-HCL-05, and allylamine amide sulfate polymer PAA-SA" manufactured by Nitto Boseki Co., Ltd. (all trade names).
[0054] Examples of cationic water-dispersible resins include urethane resins, (meth)acrylic resins, styrene / (meth)acrylic resins, polyester resins, olefin resins, vinyl chloride resins, vinyl acetate resins, melamine resins, amide resins, ethylene-vinyl chloride copolymer resins, styrene-maleic anhydride copolymer resins, vinyl acetate-(meth)acrylic copolymer resins, vinyl acetate-ethylene copolymer resins, and composite resins thereof. These resins may be given a positive surface charge by introducing a cationic functional group into them or by surface-treating them with a cationic dispersant. Representative examples of cationic functional groups include primary, secondary, or tertiary amino groups, pyridine groups, imidazole groups, benzimidazole groups, triazole groups, benzotriazole groups, pyrazole groups, or benzopyrazole groups. Examples of cationic dispersants include primary, secondary, tertiary, or quaternary amino group-containing acrylic polymers, polyethyleneimines, cationic polyvinyl alcohol resins, and cationic water-soluble hyperbranched polyesteramide resins. Here, the term "(meth)acrylic resin" refers to an acrylic resin, a methacrylic resin, or a copolymer thereof.
[0055] Examples of commercially available cationic water-dispersible resins include "PRINTRITE DP375" manufactured by Lubrizol, "PP-17" manufactured by Meisei Chemical Industry Co., Ltd., "Polysol AP-1350, AP-1370, AE-803, AM-3400" manufactured by Showa Denko K.K., "Boncoat SFC-55" manufactured by DIC Corporation, "Aquatex AC-3100" manufactured by Japan Coating Resins Co., Ltd., "Hydran CP7610, CP7050" manufactured by DIC Corporation, "Superflex 620, 650" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and "Mowinyl 7820" manufactured by Nippon Synthetic Chemical Industry Co., Ltd. (all trade names). These may be used alone or in combination of two or more. When a cationic resin is used, the content of the cationic resin (active ingredient) is preferably from 1 to 50 mass %, and more preferably from 3 to 20 mass %, based on the total amount of the pretreatment agent.
[0056] Examples of polyvalent metal salts include halides, nitrates, sulfates, acetates, fatty acid salts, lactates, etc. of divalent or higher metals such as Mg, Ca, Al, Zn, Ba, etc. Specific examples include calcium nitrate, magnesium nitrate, copper nitrate, calcium acetate, magnesium acetate, calcium chloride, barium sulfate, aluminum sulfate, etc. These may be used alone or in combination of two or more. When a polyvalent metal salt is used, the content of the polyvalent metal salt is preferably 0.1 to 10 mass % based on the total amount of the pretreatment agent.
[0057] Examples of organic acids include formic acid, acetic acid, oxalic acid, polyacrylic acid, acetic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, ascorbic acid, succinic acid, glutaric acid, fumaric acid, citric acid, tartaric acid, phthalic acid, 4-methylphthalic acid, lactic acid, pyrrolidone carboxylic acid, pyrone carboxylic acid, pyrrole carboxylic acid, furan carboxylic acid, pyridine carboxylic acid, coumaric acid, thiophene carboxylic acid, nicotinic acid, etc. These may be used alone or in combination of two or more. When an organic acid is used, the organic acid is preferably used in an amount of 1 to 30 mass % based on the total amount of the pretreatment agent.
[0058] Examples of inorganic acids that can be used include phosphorous acid, hypophosphorous acid, pyrophosphoric acid, metaphosphoric acid, polyphosphoric acid, and salts thereof. These may be used alone or in combination of two or more. When an inorganic acid is used, the amount of the inorganic acid is preferably 1 to 30 mass % based on the total amount of the pretreatment agent.
[0059] The total amount of the flocculant containing the cationic resin, polyvalent metal salt, organic acid, and inorganic acid is preferably from 1 to 50 mass %, and more preferably from 3 to 20 mass %, based on the total amount of the pretreatment agent.
[0060] The pretreatment agent may further contain a binder resin. The binder resin may be any of cationic resin, anionic resin, amphoteric resin, and nonionic resin, but cationic resin, amphoteric resin, and nonionic resin are preferably used. By using the cationic resin as the above-mentioned flocculant, it is also possible to obtain the effect of the binder resin. Examples of amphoteric resins and nonionic resins include "Boncoat 40-418EF (amphoteric)" manufactured by DIC Corporation, and "Superflex 500M (nonionic) and E-2000 (nonionic)" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (all trade names). These can be used in combination with the cationic resins described above as flocculants, and therefore can be used preferably. The binder resin (active ingredient) is preferably 0.5 to 20.0% by mass based on the total amount of the pretreatment agent.
[0061] The pretreatment agent preferably contains water as an aqueous solvent, and the main solvent may be water. The water is not particularly limited, but it is preferable that the water contains as few ionic components as possible. In particular, from the viewpoint of storage stability of the ink, it is preferable that the content of polyvalent metal ions such as calcium is small. As the water, for example, ion-exchanged water, distilled water, ultrapure water, etc. may be used. Water may be the balance of the various components, but is preferably contained in an amount of 20% to 90% by mass, and more preferably 50% to 80% by mass, based on the total amount of the pretreatment agent.
[0062] The pretreatment agent may contain a water-soluble organic solvent from the viewpoints of viscosity adjustment and moisturizing effect. The pretreatment agent may contain a water-soluble organic solvent having an SP value of 15.5 (cal / cm 3 ) 1 / 2 The following solvents may be included: 3 ) 1 / 2 The details of the following solvents are as described above. The SP value is 15.5 (cal / cm 3 ) 1 / 2 The amount of the following solvent is preferably from 1 to 50 mass % and may be from 10 to 30 mass % based on the total amount of the pretreatment agent. The pretreatment agent may contain other water-soluble organic solvents such as glycerin, etc. From the viewpoints of viscosity adjustment and moisturizing effect, the other water-soluble organic solvents may be contained in an amount of 1% by mass to 30% by mass, and more preferably 10% by mass to 20% by mass, based on the total amount of the pretreatment agent.
[0063] Furthermore, in addition to the above components, the pretreatment agent may optionally contain a wetting agent (moisturizing agent), a surface tension adjuster (penetrating agent), an antifoaming agent, a fixing agent, an antioxidant, a preservative, a pH adjuster, and the like. The method for preparing the pretreatment agent is not particularly limited, and the pretreatment agent can be prepared by mixing the respective components. For example, the pretreatment agent can be obtained by adding and mixing all the components of the pretreatment agent at once or in portions.
[0064] "Dark ink and light ink" The dark ink and the light ink will be described below. An aqueous inkjet ink set according to an embodiment may include a dark ink and a light ink that are the same hue. The dark ink and the light ink contain color materials of the same hue at different concentrations, and can be provided as inks of the same hue but different concentrations. The dark ink and the light ink preferably contain color materials of the same component, but may contain color materials of different components as long as they are of the same hue. In more detail, the dark ink and the light ink preferably contain color materials of the same hue and different concentrations of color materials of the same component. For example, the light ink is preferably of the same color as the dark ink in the KCMY color system, and contains color materials whose mass is one-third or less of the mass of the color materials in the dark ink.
[0065] In addition, the dark ink and the light ink can be used to print images successively on a substrate using the same printing device. In contrast to the dark ink, the light ink is sometimes called gray ink, light cyan, light magenta, light cyan, light magenta, etc.
[0066] The dark ink is made of a surfactant (b) whose HLB value is less than 10.0 and whose difference with the HLB value of the surfactant contained in the pretreatment agent is 2.0 or more, and whose SP value is 15.5 (cal / cm 3 ) 1 / 2 The following solvents (c1) and water may be included. The relationship between the HLB value of the surfactant (b) contained in the dark ink, the HLB value of the surfactant (a) contained in the pretreatment agent, and the HLB value of the surfactant (b) contained in the dark ink is as described above.
[0067] The surfactant (b) has an HLB value of less than 10.0. A nonionic surfactant can be preferably used as the surfactant (b). In addition, either a low molecular weight surfactant or a high molecular weight surfactant can be used.
[0068] Examples of nonionic surfactants include ester surfactants such as glycerin fatty acid esters and fatty acid sorbitan esters; ether surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers and polyoxypropylene alkyl ethers; ether ester surfactants such as polyoxyethylene sorbitan fatty acid esters; acetylene surfactants; silicone surfactants; and fluorine surfactants. Among these, acetylene surfactants and silicone surfactants can be preferably used. Although it is preferable to use one surfactant alone, two or more surfactants may be used in combination.
[0069] Examples of the acetylene-based surfactant include acetylene glycol-based surfactants, acetylene alcohol-based surfactants, and surfactants having an acetylene group. The acetylene glycol surfactant is a glycol having an acetylene group, preferably a glycol having a symmetrical structure with the acetylene group located in the center, and may have a structure in which ethylene oxide is added to acetylene glycol.
[0070] When acetylene glycol having ethylene oxide added thereto is used as the acetylene glycol surfactant, the number of moles of ethylene oxide added is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less. Commercially available acetylene surfactants having an HLB value of less than 10.0 include, for example, "Olfine E1004" and "Surfynol 420, 440, 104" (all manufactured by Nissin Chemical Industry Co., Ltd.) (all trade names).
[0071] Examples of silicone surfactants include polyether-modified silicone surfactants, alkyl / aralkyl-co-modified silicone surfactants, and acrylic silicone surfactants.
[0072] As the silicone surfactant, for example, a compound having a polyalkylene glycol chain in a polysiloxane skeleton can be used.Specifically, a compound in which at least one polyalkylene glycol chain is bonded to at least one Si element selected from the Si elements at 1st, 3rd, and 6th positions of trisiloxane can be used.In this compound, the polyalkylene glycol chain can be a polyethylene glycol chain, a polypropylene glycol chain, a polytrimethylene glycol chain, etc., but is preferably a polyethylene glycol chain.
[0073] Among them, it is preferable to use, as the silicone surfactant, heptamethyltrisiloxane having a polyethylene glycol chain with an added mole number of ethylene oxide of 0 to 6, more preferably 1 to 4. In this surfactant, the methyl group bonded to the siloxane skeleton may be substituted with another hydrophobic group such as an alkyl group having 2 or more carbon atoms. Furthermore, it is preferable to use, as the silicone surfactant, nonamethyltetrasiloxane having a polyethylene glycol chain in which the number of moles of ethylene oxide added is 0 to 8, more preferably 1 to 6. In this surfactant, the methyl group bonded to the siloxane skeleton may be substituted with another hydrophobic group, such as an alkyl group having 2 or more carbon atoms.
[0074] The surfactant (b) may also be a compound represented by the general formula "C m H 2m+1 -O-(CH2CH2O) n In this general formula, it is preferable that n=1 and m=2 or more, n=2 and m=6 or more, n=3 and m=9 or more, or n=4 and m=12 or more.
[0075] The active ingredient amount of the surfactant (b) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.7% by mass or more, based on the total amount of the dark ink. This can further reduce the graininess of the printed image and further improve the image quality. Specifically, on the substrate, the amount of surfactant (b) in the dark ink that moves from the dark ink dots to the light ink dots increases, widening the dot diameter of the dark ink and further reducing the graininess. In addition, the affinity with the substrate can be further improved. The amount of the active ingredient of the surfactant (b) is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total amount of the dark ink, which can prevent a decrease in the storage stability of the dark ink. For example, the active ingredient amount of the surfactant (b) is preferably 0.1 to 10 mass %, more preferably 0.5 to 5 mass %, and even more preferably 0.7 to 1 mass %, relative to the total amount of the dark ink.
[0076] The concentrated ink preferably contains water as an aqueous solvent, and may be mainly made of water. When the pigment dispersion described below contains water as a solvent, the water in the pigment dispersion is calculated as a part of the water in the ink when preparing the ink. The water is not particularly limited, but it is preferable that the water contains as few ionic components as possible. In particular, from the viewpoint of storage stability of the ink, it is preferable that the content of polyvalent metal ions such as calcium is small. As the water, for example, ion-exchanged water, distilled water, ultrapure water, etc. may be used. From the viewpoint of adjusting the ink viscosity, the water content is preferably 20% by mass to 90% by mass, and more preferably 30% by mass to 80% by mass, based on the total amount of the dark ink.
[0077] The dark ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The solvent (c1) may be the following: This solvent (c1) is preferably compatible with water. The SP value of the solvent (c1) contained in the dark ink and the relationship between the solvent (c1) contained in the dark ink and the solvent (c2) contained in the light ink are as described above. 3 ) 1 / 2 The following solvents are as described above.
[0078] The dark ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 In addition to the following solvent (c1), other water-soluble organic solvents may be included, such as glycerin. From the viewpoint of viscosity adjustment and moisturizing effect, the other water-soluble organic solvent may be contained in an amount of 1% by mass to 30% by mass, and more preferably 10% by mass to 20% by mass, based on the total amount of the dark ink.
[0079] The dark ink may include a pigment, a dye, or a combination thereof as a colorant. From the viewpoint of weather resistance and color development of the image, a pigment can be preferably used as the coloring material.
[0080] The pigment may be preferably incorporated into the ink as a pigment dispersion. The pigment dispersion may be any one in which the pigment can be dispersed in a solvent and in which the pigment is in a dispersed state in the ink. For example, a pigment dispersed in water using a pigment dispersant, a self-dispersing pigment dispersed in water, or a microencapsulated pigment in which the pigment is coated with a resin dispersed in water may be used.
[0081] Examples of the pigment that can be used include organic pigments such as azo pigments, phthalocyanine pigments, polycyclic pigments, and dye lake pigments, and inorganic pigments such as carbon black and metal oxides. Examples of the azo pigment include soluble azo lake pigments, insoluble azo pigments, and condensed azo pigments. Examples of phthalocyanine pigments include metal phthalocyanine pigments such as copper phthalocyanine pigments, and metal-free phthalocyanine pigments. Examples of polycyclic pigments include quinacridone pigments, perylene pigments, perinone pigments, isoindoline pigments, isoindolinone pigments, dioxazine pigments, thioindigo pigments, anthraquinone pigments, quinophthalone pigments, metal complex pigments, and diketopyrrolopyrrole (DPP). Examples of carbon black include furnace carbon black, lamp black, acetylene black, and channel black. Examples of metal oxides include titanium oxide and zinc oxide. The average particle size of these pigments is preferably 50 to 500 nm, and more preferably 50 to 200 nm. From the viewpoint of color development, the average particle size of these pigments is preferably 50 nm or more, and from the viewpoint of ejection stability, the average particle size of these pigments is preferably 500 nm or less.
[0082] In order to stably disperse the pigment in the ink, a pigment dispersant such as a polymer dispersant or a surfactant can be preferably used. Examples of commercially available polymer dispersants include the TEGO Disperse series (TEGO Disperse 740W, 750W, 755W, 757W, 760W) manufactured by EVONIK, the Solsperse series (Solsperse 20000, 27000, 41000, 41090, 43000, 44000, 46000) manufactured by Lubrizol Japan Co., Ltd., the Joncryl series (Joncryl 57, 60, 62, 63, 71, 501) manufactured by Johnson Polymer, the DISPERBYK-102, 185, 190, 193, 199) manufactured by BYK, and polyvinylpyrrolidone (K-30, K-90) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (all trade names).
[0083] As the surfactant-type dispersant, a non-ionic surfactant can be preferably used, taking into consideration the dispersion stability of the pigment in the ink and the influence of ionic properties from the pretreatment agent. Commercially available surfactant-type dispersants include, for example, nonionic surfactants such as the Emulgen series manufactured by Kao Corporation, including "Emulgen A-60, A-90, A-500, B-40, L-40, and 420" (all trade names).
[0084] These pigment dispersants may be used alone or in combination of two or more. When a pigment dispersant is used, the amount of pigment dispersant added varies depending on the type of pigment dispersant and is not particularly limited. For example, the pigment dispersant can be added in an amount of 0.005 to 0.5 parts by mass of the active ingredient per 1 part by mass of pigment.
[0085] A self-dispersing pigment may be blended as a coloring material. A self-dispersing pigment is a pigment in which a hydrophilic functional group has been introduced to the surface of the pigment by chemical or physical treatment. The hydrophilic functional group introduced to the self-dispersing pigment is preferably ionic, and by charging the pigment surface anionically or cationic, the pigment particles can be stably dispersed in water by electrostatic repulsion. As the anionic functional group, a sulfonic acid group, a carboxy group, a carbonyl group, a hydroxyl group, a phosphonic acid group, etc. are preferred. As the cationic functional group, a quaternary ammonium group, a quaternary phosphonium group, etc. are preferred.
[0086] These hydrophilic functional groups may be bonded directly to the pigment surface or via other atomic groups. Examples of the other atomic groups include, but are not limited to, alkylene groups, phenylene groups, naphthylene groups, etc. Methods for treating the pigment surface include diazotization treatment, sulfonation treatment, hypochlorous acid treatment, humic acid treatment, vacuum plasma treatment, etc.
[0087] As the self-dispersing pigment, for example, CAB-O-JET series "CAB-O-JET200, 300, 250C, 260M, 270" manufactured by Cabot Corporation, and "BONJET BLACK CW-1, CW-2, CW-4" manufactured by Orient Chemical Industries Co., Ltd. can be preferably used (all are product names).
[0088] A pigment dispersion in which the pigment is previously dispersed with a pigment dispersant may be used. Commercially available pigment dispersions dispersed with a pigment dispersant include, for example, the HOSTAJET series manufactured by Clariant and the FUJI SP series manufactured by Fuji Pigment Co., Ltd. (both are trade names). A pigment dispersion dispersed with the above-mentioned pigment dispersant may be used. A microencapsulated pigment in which the pigment is coated with a resin may also be used.
[0089] A dye may be blended as a coloring material. As the dye, those generally used in the technical field of printing can be used, and are not particularly limited. Specific examples include basic dyes, acid dyes, direct dyes, soluble vat dyes, acid mordant dyes, mordant dyes, reactive dyes, vat dyes, and sulfur dyes. Of these, those that are water-soluble and those that become water-soluble by reduction or the like can be preferably used. More specific examples include azo dyes, rhodamine dyes, methine dyes, azomethine dyes, xanthene dyes, quinone dyes, triphenylmethane dyes, diphenylmethane dyes, and methylene blue.
[0090] The above coloring materials can be used alone or in combination of two or more. The coloring material preferably contains 0.1% by mass to 25% by mass, more preferably 1% by mass to 20% by mass, and even more preferably 3% by mass to 15% by mass, in terms of the amount of active ingredients relative to the total amount of ink.
[0091] The dark ink may further contain a water-soluble resin, a water-dispersible resin, or a combination thereof, which can further improve the fixation of the colorant to the substrate. The water-soluble resin and the water-dispersible resin may be any of cationic resin, anionic resin, amphoteric resin, and nonionic resin, respectively. Since many coloring materials suitable for aqueous inks have anionic surface charges, particularly when dispersed in water, anionic resins, amphoteric resins, and nonionic resins can be preferably used in consideration of the stability of the coloring materials in water, and more preferably anionic resins. In a configuration in which the color material of the aqueous ink is stabilized by the anionic resin, by containing a cationic aggregating agent in the pretreatment agent, when the aqueous ink is applied to a substrate that has been treated with the pretreatment agent, the color material of the aqueous ink is agglomerated on the substrate by the cationic aggregating agent in the pretreatment agent, thereby suppressing bleeding of the image and further improving image quality. The water-soluble resin and the water-dispersible resin are preferably resins that form a transparent coating film on the substrate, thereby making it possible to reduce the effect on the color development of the water-based ink.
[0092] Examples of the water-soluble resin include polyvinyl alcohol, polyacrylic acid, neutralized polyacrylic acid, acrylic acid / maleic acid copolymer, acrylic acid / sulfonic acid copolymer, and styrene / maleic acid copolymer. In addition, anionic water-soluble resins obtained by introducing an anionic functional group into these resins can be used. These can be used alone or in combination of two or more.
[0093] Examples of the water-dispersible resin include ethylene-vinyl chloride copolymer resin, (meth)acrylic resin, styrene-maleic anhydride copolymer resin, urethane resin, vinyl acetate-(meth)acrylic copolymer resin, vinyl acetate-ethylene copolymer resin, etc. These can be used alone or in combination of two or more. The water-dispersible resin can be added to the ink as an oil-in-water (O / W) type resin emulsion.
[0094] As the water-dispersible resin, it is preferable to use anionic resin particles whose resin particle surface is negatively charged and negatively charged. This is a resin that can be dispersed in particulate form without dissolving in water to form an oil-in-water (O / W) type resin emulsion. As in the case of a self-emulsifying resin, the anionic functional group of the resin may be present on the resin particle surface, or the resin may be surface-treated by attaching an anionic dispersant to the resin particle surface. The anionic functional group is typically a carboxy group, a sulfo group, or the like, and the anionic dispersant is an anionic surfactant, or the like. The resin that serves as the skeleton is as described above.
[0095] As the water-dispersible resin, from the viewpoints of adhesion to the substrate, stability in the ink, and the like, it is preferable to use a urethane resin emulsion, a (meth)acrylic resin emulsion, a resin emulsion of a (meth)acrylic resin copolymer, or a combination thereof. Commercially available examples of urethane resin emulsions include "Superflex 460, 420, 470, 460S," "Superflex 740, 860," and "Superflex 870" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; "NeoRez R-9660, R-2170," and "NeoRez R-986, R-9603" manufactured by DSM; and "Takelac WS-5100" manufactured by Mitsui Chemicals, Inc. (all product names).
[0096] Commercially available (meth)acrylic resin emulsions and (meth)acrylic resin copolymer resin emulsions include, for example, "Mowinyl 966A, 6963, 6960, 6969D" manufactured by Nippon Synthetic Chemical Industry Co., Ltd.; "Joncryl 7100, PDX-7370, PDX-7341" manufactured by BASF; "Boncoat EC-905EF, 5400EF, CG-8400" manufactured by DIC Corporation; and "NeoCryl A-1125" manufactured by DSM (all of which are product names).
[0097] The total amount (active components) of the water-soluble resin and the water-dispersible resin is preferably 0.5 to 10, and more preferably 1 to 5, parts by mass per part of the coloring material. The total amount (active components) of the water-soluble resin and the water-dispersible resin is preferably 1 to 20% by mass, and more preferably 3 to 10% by mass, based on the total amount of the dark ink.
[0098] The thick ink may further contain a binder resin. The binder resin can be blended to fix the solid content of the colorant and the like more firmly on the substrate and to increase the strength of the coating film. The binder resin may be any of cationic resin, anionic resin, amphoteric resin, and nonionic resin. Since many colorants suitable for aqueous inks have anionic surface charges, particularly when dispersed in water, the binder resin can be preferably anionic or nonionic resin, taking into consideration the stability of the colorant in water. It is also possible to obtain the effect of the binder resin by using the water-soluble resin and the water-dispersible resin as the resin components described above. The binder resin (active ingredient) is preferably 1 to 20% by mass based on the total amount of the dark ink.
[0099] In addition to the above components, the thick ink may optionally contain a wetting agent (moisturizing agent), a surface tension adjuster (penetrating agent), an antifoaming agent, a fixing agent, a pH adjuster, an antioxidant, a preservative, etc. The method for producing a dark ink is not particularly limited, but the desired ink can be obtained by appropriately mixing each component. For example, when a pigment dispersion is used as a coloring material, the ink can be obtained by mixing the pigment dispersion with a solution in which a water-soluble organic solvent and additives are appropriately added to water. The obtained composition may also be filtered using a filter or the like.
[0100] The light ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The following solvents (c2) and water may be included.
[0101] The light ink preferably contains water as an aqueous solvent, and may be mainly made of water. When the pigment dispersion described below contains water as a solvent, the water in the pigment dispersion is calculated as a part of the water in the ink when preparing the ink. The water is not particularly limited, but it is preferable that the water contains as few ionic components as possible. In particular, from the viewpoint of storage stability of the ink, it is preferable that the content of polyvalent metal ions such as calcium is small. As the water, for example, ion-exchanged water, distilled water, ultrapure water, etc. may be used. From the viewpoint of adjusting the ink viscosity, the water content is preferably 20% by mass to 90% by mass, and more preferably 30% by mass to 80% by mass, based on the total amount of the light ink.
[0102] The light ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 The solvent (c2) may be the following: This solvent (c2) is preferably compatible with water. The relationship between the SP value of the solvent (c2) contained in the light ink and the solvent (c1) contained in the dark ink and the solvent (c2) contained in the light ink is as described above. 3 ) 1 / 2 The following solvents are as described above.
[0103] The light ink has an SP value of 15.5 (cal / cm 3 ) 1 / 2 In addition to the following solvent (c1), other water-soluble organic solvents may be included, such as glycerin. From the viewpoint of viscosity adjustment and moisturizing effect, the other water-soluble organic solvent may be contained in an amount of 1% by mass to 30% by mass, and more preferably 10% by mass to 20% by mass, based on the total amount of the light ink.
[0104] The light ink may further include a surfactant. The surfactant blended in the dark ink and the surfactant blended in the light ink may be the same, or may be partially or completely different. When printing dark ink and light ink using the same inkjet printing device, it is preferable that the physical properties of both inks are similar, so it is preferable that the surfactant blended in the dark ink and the light ink are the same, partially the same, or have similar HLB values. The surfactant that can be blended in the light ink preferably has an HLB value of 1.0 to 20, more preferably 2.0 to 15, and even more preferably 3.0 or more and less than 10.0.
[0105] The surfactant that can be blended in the light ink may be any of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Of these, nonionic surfactants are preferred from the viewpoint of preventing foaming of the pretreatment agent. In addition, any of low molecular weight surfactants and polymeric surfactants may be used.
[0106] Examples of nonionic surfactants include ester surfactants such as glycerin fatty acid esters and fatty acid sorbitan esters; ether surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers and polyoxypropylene alkyl ethers; ether ester surfactants such as polyoxyethylene sorbitan fatty acid esters; acetylene surfactants; silicone surfactants; and fluorine surfactants. Among these, acetylene surfactants and silicone surfactants can be preferably used. Although it is preferable to use one surfactant alone, two or more surfactants may be used in combination.
[0107] Examples of the acetylene-based surfactant include acetylene glycol-based surfactants, acetylene alcohol-based surfactants, and surfactants having an acetylene group. Examples of silicone surfactants include polyether-modified silicone surfactants, alkyl / aralkyl-co-modified silicone surfactants, and acrylic silicone surfactants.
[0108] Specifically, the surfactant for the light ink can be appropriately selected from the surfactant (a) that can be blended in the pretreatment agent and the surfactant (b) that can be blended in the dark ink. Also, an ionic surfactant that can be blended in the normal ink can be used as the surfactant for the light ink.
[0109] When a surfactant is blended into the light ink, the surfactant in the light ink preferably contains an active ingredient amount of 0.1 mass % or more relative to the total mass of the light ink, more preferably 0.5 mass % or more, and even more preferably 0.7 mass % or more. The amount of active ingredients of the surfactant in the light ink is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total amount of the light ink. For example, the surfactant in the light ink preferably has an active ingredient content of 0.1 to 10 mass %, more preferably 0.5 to 5 mass %, and even more preferably 0.7 to 1 mass %, relative to the total amount of the light ink. By using the surfactant within the above range, it is possible to prevent a decrease in storage stability in a light ink while further improving the affinity with the base material.
[0110] The light ink may contain a pigment, a dye, or a combination thereof as a coloring material. In terms of the weather resistance and print density of the image, a pigment can be preferably used as the coloring material. The pigment is preferably blended into the ink as a pigment dispersion. The coloring material of the light ink is preferably a coloring material having the same hue as that of the dark ink. The coloring material of the light ink may be the same component as that of the dark ink or may be a different component, but is preferably the same component. The coloring material of the light ink may be the same as that of the dark ink described above.
[0111] The mass ratio (colorant concentration 2 / colorant concentration 1) of the mass ratio of the colorant to the total amount of the dark ink (colorant concentration 1) to the mass ratio of the colorant to the total amount of the light ink (colorant concentration 2) is preferably 1 or less or less than 1, more preferably 0.5 or less, even more preferably 0.35 or less, and may be 0.3 or less. Moreover, this mass ratio (colorant concentration 2 / colorant concentration 1) is preferably 0.05 or more, and more preferably 0.1 or more. In the light ink, the coloring material preferably has an active ingredient content of 0.1% to 10% by mass, more preferably 0.3% to 5% by mass, and even more preferably 0.5% to 3% by mass, relative to the total amount of the light ink.
[0112] The light ink may further contain a water-soluble resin, a water-dispersible resin, or a combination thereof, which can further improve the fixation of the colorant to the substrate. In the light ink, the water-soluble resin, the water-dispersible resin, or a combination thereof may be the same as that described for the dark ink. These components may be the same between the dark ink and the light ink, or may be partially or entirely different components, but it is preferable that they are the same components. By using the same resin components between the dark ink and the light ink, it is possible to form a resin film more uniformly on the substrate, and the fixation of the coloring material can be further improved.
[0113] The total amount (active components) of the water-soluble resin and the water-dispersible resin is preferably 0.5 to 15, and more preferably 1 to 10, parts by mass per part of the coloring material. The total amount (active components) of the water-soluble resin and the water-dispersible resin is preferably 1 to 20% by mass, and more preferably 3 to 10% by mass, based on the total amount of the light ink.
[0114] The light ink may further contain a binder resin, which may be the same as that described above for the dark ink.
[0115] In addition to the above components, the light ink may optionally contain a wetting agent (moisturizing agent), a surface tension adjuster (penetrating agent), an antifoaming agent, a fixing agent, a pH adjuster, an antioxidant, a preservative, etc. The method for preparing the light ink is not particularly limited, and the light ink can be prepared in the same manner as the dark ink described above.
[0116] "Method of manufacturing printed matter" An example of a method for producing a printed matter will be described below. The method for producing a printed matter can include, for example, printing a substrate with an aqueous inkjet ink set. The aqueous inkjet ink set can be any of the aqueous inkjet ink sets described above. For example, a method for producing a printed product can include treating a substrate with a pretreatment agent and forming an image on the substrate with a dark ink and a light ink.
[0117] The method of treating the substrate with the pretreatment agent may be, for example, by uniformly applying the pretreatment agent to the substrate surface using a brush, roller, bar coater, air knife coater, spray, or the like, or by printing the pretreatment agent in the image area by a printing method such as inkjet printing, gravure printing, or flexographic printing. The application area may be the entire substrate surface, or the pretreatment agent may be selectively applied only to the image area. Alternatively, the pretreatment agent may be applied only to a portion where a certain amount or more of ink is applied per unit area, such as a solid image portion. When the pretreatment agent is to be applied uniformly to a large area of a substrate, application by spraying is preferred. Furthermore, when the pretreatment liquid is applied to the substrate in accordance with the image area to be printed, printing by inkjet printing is preferred.
[0118] The pretreatment agent does not need to be dried in a drying step, and the printing step can be carried out subsequently. If necessary, the pretreatment agent may be dried by heating at a temperature of 25°C to 120°C before the printing step. The heating time is preferably 1 minute to 120 minutes, more preferably 10 minutes to 60 minutes, depending on the type and amount of volatile matter in the pretreatment agent. In addition, when the pretreatment agent contains a resin component, the resin can be melted or softened on the substrate by carrying out a heat treatment after applying the pretreatment agent, and the pretreatment agent layer can be more firmly fixed to the substrate.
[0119] The amount of pretreatment agent applied to the substrate is 0.5 to 200 g / m2 (effective ingredient amount) per unit area of the coating region. 2 is preferable, and 1 to 50 g / m 2 is more preferred.
[0120] A method for forming an image on a substrate using a dark ink and a light ink can be performed by applying one of the dark ink and the light ink to the substrate, and then applying the other of the dark ink and the light ink to the substrate. In an aqueous inkjet ink set according to one embodiment, the pretreatment agent, the dark ink, and the light ink have the above-mentioned physical properties, so that the spread of the dark ink dots can be appropriately adjusted regardless of the order in which the dark ink and the light ink are applied, thereby further improving the image quality of the printed matter. In a preferred embodiment, the pretreatment agent, the light ink, and the dark ink can be applied to the substrate in that order.
[0121] The printing method of the dark ink and the light ink on the substrate can be performed by inkjet printing, which can easily and freely form an image on demand without contacting the substrate. The inkjet printing device may be of any type, such as a piezoelectric type, an electrostatic type, or a thermal type, and ejects ink from an inkjet head based on a digital signal, causing the ejected ink droplets to adhere to a substrate.
[0122] For example, a dark ink and a light ink can be printed using a line head type inkjet printing device. Using an inkjet printing device in which a plurality of inkjet heads in a line shape intersecting the transport direction of the substrate are arranged in the transport direction of the substrate, a light ink is loaded into the line head on the upstream side with respect to the transport direction of the substrate, and a dark ink is loaded into the line head on the downstream side, and an image can be formed by ejecting the light ink from the line head on the upstream side and then ejecting the dark ink from the line head on the downstream side in one transport of the substrate. The order of the dark ink and the light ink may be reversed.
[0123] Also, the dark ink and the light ink can be printed using a serial head type inkjet printing device. Using a printing device that is movable in a direction intersecting the transport direction of the substrate and has an inkjet head with multiple nozzle rows arranged along the moving direction, one of the multiple nozzle rows is loaded with light ink and the other is loaded with dark ink, and while transporting the substrate, the inkjet head is moved back and forth while ejecting the light ink and then the dark ink, thereby forming an image. The order of the dark ink and the light ink may be reversed. In both the line head type and the serial head type, by discharging the subsequent ink so as to be adjacent to the dot of the ink discharged earlier on the substrate, the color material concentration differs between the adjacent dots, so that the hue gradation can be adjusted. In this case, by using the dark ink and the light ink according to one embodiment, the graininess of the printed image can be reduced, and a high-quality image can be obtained.
[0124] The obtained printed matter is preferably subjected to a heat treatment to remove volatile matter. The heat treatment temperature is preferably 25° C. to 150° C., more preferably 50° C. to 120° C. The heat treatment time is preferably 1 minute to 24 hours, more preferably 10 minutes to 200 minutes, depending on the type and amount of volatile matter in the ink, the coating thickness, etc. Furthermore, when the ink contains a resin component, the resin component in the ink can be melted or softened by heat treating the resulting decorated article to form a uniform resin film, thereby further increasing the strength of the ink image layer.
[0125] The aqueous inkjet ink set according to an embodiment can be applied to both permeable and low-permeable substrates, and in particular, when printing with aqueous inks on a low-permeable substrate that has been treated with a pretreatment agent, graininess in the printed image can be more effectively prevented.
[0126] A low-permeability substrate is one in which liquid does not penetrate into the substrate, specifically, one in which most of the liquid in the ink remains on the surface of the substrate. Examples of low-permeability substrates include metal substrates such as metal plates of aluminum, iron, copper, titanium, tin, chromium, cadmium, and alloys (e.g., stainless steel, steel, etc.); glass substrates such as plate glass such as borosilicate glass, quartz glass, and soda-lime glass; resin substrates such as resin sheets such as PET films, OHT sheets, polyester sheets, and polypropylene sheets, and acrylic plates; and ceramic substrates such as molded bodies of alumina, zirconia, steatite, and silicon nitride. These substrates may have a plating layer, a metal oxide layer, a resin layer, etc. formed thereon, or may have been surface-treated using a surfactant, corona treatment, etc. The aqueous inkjet ink set according to an embodiment can exert its effect even when it is used to treat an untreated substrate.
[0127] Examples of permeable substrates include printing paper such as plain paper, coated paper, and special paper, cloth, porous building materials for humidity control, sound absorption, heat insulation, and the like, wood, concrete, etc. By using the aqueous inkjet ink set according to one embodiment for permeable substrates such as cloth, porous building materials, and wood, which are prone to ink penetration into the substrate to the inside and image bleeding, the spread of dots can be suppressed and image quality can be improved more effectively. EXAMPLES
[0128] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. In the following description, unless otherwise specified, "%" indicates "% by mass." Tables 1 to 4 show the formulations of the pretreatment agents, dark cyan inks, and light cyan inks of the Examples and Comparative Examples, and the evaluation results of the printed matter. In each table, when a solvent or the like is contained in each component, the blending ratio of the active ingredient is shown, and the solvent or the like is treated as being contained in the remaining water. In each table, the unit of the active ingredient amount shown in parentheses is % by mass, and the unit of the SP value is (cal / cm 3 ) 1 / 2 It is.
[0129] <Preparation of pretreatment agent> According to the formulation of the pretreatment agent shown in each table, each component was mixed in the corresponding ratio to obtain a pretreatment liquid. The water content was adjusted so that the total amount of the pretreatment agent was 100 mass %.
[0130] <Preparation of dark and light inks> The components were mixed according to the pretreatment formulation shown in each table, and then filtered through a membrane filter with a pore size of 3 μm to obtain a dark cyan ink and a light cyan ink. The dark ink and the light ink were adjusted to have different image densities, mainly by varying the concentration of the cyan self-dispersing pigment. The water content was adjusted so that the total amount of the ink was 100% by mass.
[0131] The components used are as follows: (Activator) Acetylenic surfactant (1); HLB 8.8: "Olfine E1004" manufactured by Nissin Chemical Industry Co., Ltd., active ingredient amount 100% by mass. Acetylenic surfactant (2); HLB 13.2: "Olfine E1010" manufactured by Nissin Chemical Industry Co., Ltd., active ingredient amount 100% by mass. Acetylenic surfactant (3); HLB 4.0: "Surfynol 420" manufactured by Nissin Chemical Industry Co., Ltd., active ingredient amount 100% by mass. Acetylenic surfactant (4); HLB 10.8: "Olfine E1006" manufactured by Nissin Chemical Industry Co., Ltd., active ingredient amount 100% by mass. Silicone surfactant (1); HLB 12.2: Synthesized according to the following procedure. Active ingredient amount 100% by mass. Silicone surfactant (2); HLB 2.7: Synthesized according to the following procedure. Active ingredient amount 100% by mass. Silicone surfactant (3); HLB 7.7: Synthesized according to the following procedure. Active ingredient amount 100% by mass.
[0132] (Pretreatment component) Flocculant; Water-soluble cationic resin: Himax SC-700L, active ingredient amount 30%. Flocculant; polyvalent metal salt: calcium chloride anhydrous, purity 95%, manufactured by Yoneyama Pharmaceutical Co., Ltd. Binder: Cationic resin emulsion: Ester-based urethane, "Superflex 620" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., active ingredient amount 30%, particle size 0.02 μm. Binder: Cationic resin emulsion: acrylic acid ester / methacrylic acid ester copolymer emulsion, "Movinyl 7820" manufactured by Japan Coating Resin Co., Ltd., active ingredient amount 45%, particle size 0.4 μm. Diethylene glycol: Water-soluble organic solvent, SP value 15.0 (cal / cm 3 ) 1 / 2 .
[0133] (Ink components) Glycerin: Water-soluble organic solvent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., SP value 16.4 (cal / cm 3 ) 1 / 2 . Diethylene glycol: Water-soluble organic solvent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., SP value 15.0 (cal / cm 3 ) 1 / 2 . 1,3-Propanediol: Water-soluble organic solvent, manufactured by Tokyo Chemical Industry Co., Ltd., SP value 13.7 (cal / cm 3 ) 1 / 2 . 1,2-Hexanediol: Water-soluble organic solvent, manufactured by Tokyo Chemical Industry Co., Ltd., SP value 11.8 (cal / cm 3 ) 1 / 2 . Urethane resin emulsion: aromatic isocyanate-based, ether-based urethane, anion resin emulsion, "Superflex 870" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., particle size 30 nm, active ingredient content 30%. Acrylic resin emulsion: "NeoCryl A-1125" manufactured by DSM Coating Resins, LLC., anionic resin emulsion, active ingredient content 19.5%. Cyan pigment dispersion: Cabot Corporation's "CAB-0-JET-250C", self-dispersing pigment, active ingredient amount 10% by mass.
[0134] The HLB value of a surfactant is a value calculated from the molecular structure of the surfactant using the following formula (1) according to the Griffin method. HLB value = 20 × (formula weight of hydrophilic part) / (molecular weight of surfactant) Equation (1) The SP value of the solvent is a value based on the estimation method proposed by Fedor. The ink viscosity was measured at 23° C. using an Anton Paar “Rheometer MCR302.” Specifically, the viscosity value at 10 Pa was determined when the shear stress was increased from 0 Pa at a rate of 0.1 Pa / s.
[0135] <Preparation of Silicone-Based Surfactant (1)> To obtain the compound represented by the following chemical formula (1), the following components were placed in a flask together with an ARP platinum catalyst, and the mixture was heated and stirred at 70°C under a nitrogen atmosphere for 5 hours to react. The product was filtered, and the toluene was removed under reduced pressure. The resulting compound was used as silicone surfactant (1). Hydroxypolyethoxy(10) allyl ether (98%) 20.7% by mass; 9.3% by weight of methylbis(trimethylsilyloxy)silane; Toluene: 70.0% by mass.
[0136] <Preparation of Silicone Surfactant (2)> To obtain the compound represented by the following chemical formula (2), the following components were placed in a flask together with an ARP platinum catalyst, and the mixture was heated and stirred at 70°C under a nitrogen atmosphere for 5 hours to react. The product was filtered, and the toluene was removed under reduced pressure. The resulting compound was used as silicone surfactant (2). Ethylene glycol monoallyl ether 9.4% by weight; 20.6% by mass of methylbis(trimethylsilyloxy)silane; Toluene 70.0% by mass.
[0137] <Preparation of Silicone Surfactant (3)> To obtain the compound represented by the following chemical formula (3), the following components were placed in a flask together with an ARP platinum catalyst, and the mixture was heated and stirred at 70°C under a nitrogen atmosphere for 5 hours to react. The product was filtered, and the toluene was removed under reduced pressure. The resulting compound was used as silicone surfactant (3). 2-[2-[2-(2-prop-2-enoxyethoxy)ethoxy]ethoxy]ethanol 15.4% by mass; 14.6% by mass of methylbis(trimethylsilyloxy)silane; Toluene 70.0% by mass.
[0138] [ka]
[0139] [ka]
[0140] The components used are as follows: Hydroxypolyethoxy (10) allyl ether (98%): Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Methylbis(trimethylsilyloxy)silane: manufactured by Tokyo Chemical Industry Co., Ltd. Ethylene glycol monoallyl ether: manufactured by Tokyo Chemical Industry Co., Ltd. 2-[2-[2-(2-prop-2-enoxyethoxy)ethoxy]ethoxy]ethanol Manufactured by Aurora Fine Chemicals. ARP platinum: Fujifilm Wako Pure Chemical Industries, Ltd. Toluene: Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0141] <Evaluation method> The substrate used was a PET film. The pretreatment agent was sprayed onto the PET film. The amount of the active ingredient applied was 20 g / m 2 After the pretreatment agent was applied, the PET film was heat-treated at 90° C. for 20 minutes. A 600 x 600 dpi grayscale (dark cyan to light cyan) image was formed on the pretreated PET film using ANAJET's "mPower mP5i / SOLD" to obtain a print. Printing was performed by loading light ink and dark ink into adjacent nozzle rows of a serial head type inkjet head, and ejecting the light ink and dark ink in that order onto the substrate while the inkjet head was moved back and forth in a direction perpendicular to the substrate transport direction. A solid image was formed by printing the light ink and dark ink so that dots of the ink were adjacent to each other on the substrate, and the light ink and dark ink were each printed at 600 x 600 dpi. The resulting print was heat treated at 100° C. for 120 minutes.
[0142] For the printed matter of each of the Examples and Comparative Examples, the printed surface was visually observed using a magnifying glass and evaluated according to the following criteria. A: The graininess doesn't bother me. B: There is a slight graininess. C: The graininess is noticeable.
[0143] [Table 1]
[0144] [Table 2]
[0145] [Table 3]
[0146] [Table 4]
[0147] As shown in each table, the graininess was reduced in the prints of each example, and good image quality was obtained. Examples 1 to 7 are examples in which the surfactant composition is changed between the dark ink and the light ink. Examples 1 to 7 show that when the difference between the HLB value of the surfactant (a) in the pretreatment agent and the HLB value of the surfactant (b) in the dark ink is equal to or greater than a predetermined value, the graininess of the printed matter is reduced. It can be seen from Examples 1 to 4 that when the content of the surfactant (b) in the dark ink is 0.7% by mass or more, the graininess of the printed matter is further reduced. In Examples 5 and 7, the surfactant in the light ink was changed, and the graininess of the printed matter was reduced. Example 6 is an example in which the HLB value of the surfactant (b) in the dark ink is smaller, and the graininess of the printed matter was reduced.
[0148] Examples 8 to 11 are examples in which the composition of the solvent in the dark ink and the light ink is changed. From Examples 8 and 9, it can be seen that when the viscosity ratio (v2 / v1) of the dark ink to the light ink is equal to or greater than a predetermined value, the graininess of the printed matter is reduced. From Example 10, the SP value was 15.5 (cal / cm 3 ) 1 / 2 It can be seen that the graininess of the printed matter is reduced when the concentration ratio (c2 / c1) of the following solvents is equal to or greater than a predetermined value. From Example 11, the SP value was 15.5 (cal / cm 3 ) 1 / 2 It can be seen that the graininess of printed matter is reduced regardless of the type of solvent used.
[0149] Examples 12 to 14 are examples in which the composition of the pretreatment agent was changed. Example 12 is an example in which a silicone-based surfactant was used as the surfactant (a) in the pretreatment agent, and the graininess of the printed matter was reduced. It can be seen from Examples 13 and 14 that the graininess of printed matter is reduced regardless of the type of flocculant and binder in the pretreatment agent.
[0150] Examples 15 to 19 are examples in which the surfactant composition is changed between the dark ink and the light ink. In Examples 15 and 16, the dark ink contained a small amount of surfactant (b), but the graininess of the printed matter was reduced. Examples 17 to 19 are examples in which a silicone surfactant was used as the surfactant (b) in the dark ink, and the graininess of the printed matter was reduced.
[0151] Comparative Example 1 is an example in which the viscosity ratio (v2 / v1) of the dark ink to the light ink is small, and graininess was observed in the printed matter. In Comparative Example 2, the SP value was 15.5 (cal / cm 3 ) 1 / 2 The following is an example where the concentration ratio (c2 / c1) of the solvents is small, and graininess was observed in the printed matter. Comparative Example 3 is an example in which the HLB value of the surfactant in the dark ink was large, and graininess was observed in the printed matter. Comparative Examples 4 and 5 are examples in which the HLB value of the surfactant in the pretreatment agent was small and the difference between the surfactant in the pretreatment agent and the surfactant (b) in the dark ink was small, and graininess was observed in the printed matter. Comparative Example 6 is an example in which the pretreatment agent was not applied to the substrate, and the dark ink and the light ink were not fixed to the substrate, and the image was not formed well.
Claims
1. A pretreatment agent and a dark ink and a light ink having the same hue are provided, the pretreatment agent contains a nonionic surfactant having an HLB value of 10.0 or more, and water in an amount of 50 mass% or more based on the total amount of the pretreatment agent, The dark ink contains a nonionic surfactant having an HLB value of less than 10.0, the difference between the HLB value of the nonionic surfactant contained in the pretreatment agent being 2.0 or more, and an SP value of 15.5 (cal / cm 3 ) 1/2 The following water-soluble organic solvents and water are included: The light ink has an SP value of 15.5 (cal / cm 3 ) 1/2 The following water-soluble organic solvents and water are included: The SP value of the light ink is 15.5 (cal / cm 3 ) 1/2 The concentration (mass%) of the water-soluble organic solvents listed below is such that the SP value of the thick ink is 15.5 (cal / cm 3 ) 1/2 The concentration (mass%) of the water-soluble organic solvent is 1.1 times or more: The aqueous inkjet ink set, wherein the viscosity (mPa·s) of the light ink at 23° C. is 1.05 times or more the viscosity (mPa·s) of the dark ink.
2. 2. The aqueous inkjet ink set according to claim 1, wherein a nonionic surfactant contained in the dark ink has an HLB value of less than 10.0 and a difference in HLB value between the HLB value of the nonionic surfactant contained in the pretreatment agent and the HLB value of the nonionic surfactant is 2.0 or more, and the content of the nonionic surfactant is 0.7% by mass or more relative to the total amount of the dark ink.
3. The aqueous inkjet ink set according to claim 1 , wherein the nonionic surfactant contained in the pretreatment agent and having an HLB value of 10.0 or greater includes at least one of an acetylene-based surfactant and a silicone-based surfactant.
4. 4. The aqueous inkjet ink set according to claim 1, wherein the nonionic surfactant contained in the dark ink has an HLB value of less than 10.0 and has an HLB value that differs by 2.0 or more from the HLB value of the nonionic surfactant contained in the pretreatment agent.
5. The aqueous inkjet ink set according to claim 1 , wherein the light ink further comprises a surfactant.
6. The SP value is 15.5 (cal / cm 3 ) 1/2 The aqueous inkjet ink set according to any one of claims 1 to 5, wherein the water-soluble organic solvent comprises one or more selected from the group consisting of diethylene glycol, 1,3-propanediol, and 1,2-hexanediol.
Citation Information
Patent Citations
Ink set for inkjet recording, recording unit, inkjet recording apparatus and inkjet recording method
JP2003176431A
Ink set and recording device
JP2014237742A
Aqueous inkjet ink set
JP2016017103A
Reaction liquid and inkjet recording method
JP2018053124A
Pretreatment liquid, ink set, and printed matter production method
JP2018114751A