Oxidation Catalyst
A gold-supported alumina catalyst with controlled hydroxyl group mobility and peak area ratios enables low-temperature carbon monoxide oxidation and maintains activity, addressing the limitations of existing catalysts.
Patent Information
- Application Number
- JP2020163660
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Existing oxidation catalysts require high temperatures (above 100°C) for effective carbon monoxide conversion and are susceptible to moisture adsorption, limiting their use in applications requiring low-temperature operation and contact with the human body.
A gold-supported alumina catalyst with specific infrared absorption peak area ratios and hydroxyl group mobility control, allowing catalytic activity at temperatures as low as 0°C to 100°C and maintaining activity over time.
The catalyst effectively oxidizes carbon monoxide and other volatile organic compounds at low temperatures while resisting moisture adsorption, ensuring consistent performance.
Smart Images

Figure 0007556732000002 
Figure 0007556732000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an oxidation catalyst. [Background technology]
[0002] Carbon monoxide is known to be a highly lethal gas that is harmful to the human body even in small amounts. It is produced from internal combustion engines in automobiles and factories, and is also used as an industrial raw material. Various means are taken to remove it so that it is not released into the environment.
[0003] A common method for removing carbon monoxide is to oxidize carbon monoxide by complete combustion through heating. However, because high temperatures are required, catalysts that promote the oxidation reaction of carbon monoxide have been developed. For example, a gas oxidation catalyst material in which Fe-based particles are supported on γ-Al2O3 particles (Patent Document 1), an oxidation silver catalyst obtained by firing alumina having a θ phase carrying silver at 900 to 1100°C and then reducing it at 100 to 500°C (Patent Document 2), a carbon monoxide selective oxidation catalyst in which platinum and cobalt are supported on an inorganic carrier containing θ-alumina and α-alumina (Patent Document 3), and a gold catalyst in which gold fine particles are supported on the surface of a γ-alumina carrier particle (Patent Document 4) have been disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-171349 A [Patent Document 2] JP 2010-125373 A [Patent Document 3] JP 2005-342689 A [Patent Document 4] JP 2005-230699 A [Non-patent literature]
[0005] [Non-Patent Document 1] Applied Catalysis A:General volume232 issues 1-2, 159-168 (2002) Summary of the Invention [Problem to be solved by the invention]
[0006] However, the catalyst disclosed in Patent Document 1 begins to exhibit catalytic activity at a reaction temperature of 60° C., and activity increases as the temperature rises, but a reaction temperature of 280° C. is required to achieve 100% conversion. The catalysts disclosed in Patent Documents 2 and 3 have only been confirmed to have a CO conversion rate (CO purification rate) at temperatures of 100° C. or higher, and are therefore considered unsuitable for use in components used at room temperature, such as gas mask components used in close contact with the human body.
[0007] The catalyst in Patent Document 4 discloses that the rate of the carbon monoxide oxidation reaction increases with increasing temperature in the range of 50°C or higher, but it is presumed that the catalytic activity further decreases in lower temperature ranges such as room temperature. In addition, the gamma alumina used as the carrier is known to be highly hygroscopic, and there is a problem that at low temperatures below 100°C, the catalytic activity decreases over time due to the adsorption of moisture from the air (Non-Patent Document 1).
[0008] The present invention aims to provide an oxidation catalyst that can oxidize a substance to be treated, such as carbon monoxide, even at temperatures of 100°C or lower, and that is likely to maintain its catalytic activity even when the oxidation reaction is continued. [Means for solving the problem]
[0009] The gist of the present invention is as follows. [1] A carrier made of alumina and particles containing gold element supported on the carrier are included, and the infrared absorption spectrum of the carrier measured by a Fourier transform infrared spectrometer is 3727±10 cm -1 The first peak has a peak top at 3676 ± 10 cm -1 and a second peak with a peak top at 3581 ± 10 cm-1 an oxidation catalyst characterized in that, when the peaks are separated into seven or less peaks having different peak top wavelengths, including a third peak having a peak top at 100 nm, an area A of the first peak and an area B of the second peak satisfy the following formula (1): 0 [2] The oxidation catalyst according to [1], wherein the area A and the area B satisfy the following formula (2): 1.2≦B / A≦2.0 (2) [3] The specific surface area of the carrier is 20 m 2 / g or more of the oxidation catalyst described in [1] or [2]. [4] The oxidation catalyst according to any one of [1] to [3], wherein the particles further contain a precious metal element other than gold. [5] The oxidation catalyst according to any one of [1] to [4], characterized in that the amount of the particles containing gold element supported is 0.5 mass% or more and 3.0 mass% or less with respect to 100 mass% of the support. [6] An oxidation catalyst member comprising the oxidation catalyst according to any one of [1] to [5] and a substrate to which the oxidation catalyst is fixed. [7] A method for removing carbon monoxide, comprising contacting a gas to be treated containing carbon monoxide with an oxidation catalyst according to any one of [1] to [5] at a temperature of 0°C or higher and 100°C or lower in the presence of oxygen. Effect of the Invention
[0010] According to the present invention, it is possible to provide an oxidation catalyst that can oxidize a substance to be treated, such as carbon monoxide, even at temperatures of 100° C. or less, and that is likely to maintain its catalytic activity even when the oxidation reaction is continued. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the infrared absorption spectrum for Example 2 and each peak after peak separation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described.
[0013] The oxidation catalyst of this embodiment (hereinafter also simply referred to as "catalyst") contains a support made of alumina and particles containing elemental gold supported on the support. In the following description, the particles containing elemental gold are also referred to as gold particles, and the support on which the gold particles are supported is also referred to as a gold-supported support.
[0014] The catalyst of this embodiment has an infrared absorption spectrum of the gold-supported carrier measured by a Fourier transform infrared spectrometer of 3727±10 cm -1 The first peak has a peak top at 3676 ± 10 cm -1 and a second peak with a peak top at 3581 ± 10 cm -1 When the spectrum is separated into seven or less peaks having different peak top wavelengths, including a third peak having a peak top at 100 nm, the area A of the first peak and the area B of the second peak satisfy the following formula (1). 0
[0015] The state of the hydroxyl groups (OH groups) present on the surface of the alumina (support) can be understood from the infrared absorption spectrum of the gold-supported support measured by a Fourier transform infrared spectrometer. The first peak (3727 ± 10 cm) obtained by peak separation of the infrared absorption spectrum -1 The second peak (3676±10cm -1 Both of these peaks (having a peak top at 1000 nm) are considered to be peaks that indicate the presence of hydroxyl groups that are chemically bonded, that is, hydroxyl groups that are chemically bonded to the alumina (carrier) itself, as opposed to hydroxyl groups that are physically adsorbed, such as adsorbed water.
[0016] By containing a gold-loaded carrier in which the area A of the first peak and the area B of the second peak satisfy the above formula (1) (hereinafter, this condition may be referred to as "this peak area condition"), the substance to be treated, such as carbon monoxide, can be oxidized even at temperatures below 100°C, and the catalytic activity is likely to be maintained even if the oxidation reaction is continued. Note that in this specification, catalytic activity refers to the activity of oxidizing the substance to be treated, such as carbon monoxide.
[0017] Here, a method for measuring the infrared absorption spectrum of a gold-loaded carrier, a method for peak separation of the infrared absorption spectrum, and a method for determining the area ratio of the separated peaks (area B of the second peak / area A of the first peak) will be specifically described.
[0018] <Infrared absorption spectrum> In this embodiment, the infrared absorption spectrum of the gold-supported carrier is measured by a Fourier transform infrared spectrometer. For example, a Fourier transform infrared spectrometer (FTIR-6000, manufactured by JASCO Corporation) capable of heating the measurement sample can be used as the Fourier transform infrared spectrometer. For example, a diffuse reflectance method can be used for the measurement by the Fourier transform infrared spectrometer. When using the diffuse reflectance method, the sample (carrier) is heated to 400°C and maintained at 400°C. The infrared absorption spectrum is measured in the range of 2000 to 4000 cm. -1 The measurement is performed at a wavelength including the range of 100 nm to 150 nm. For heating the sample, for example, a vacuum heating diffusion measuring device (DR-650 type, manufactured by JASCO Corporation) can be used. For the measurement method, a method known to those skilled in the art, such as a transmission method, a diffuse reflectance method, or an ATR method, can be applied. When pre-processing of the sample is required for the measurement, a pre-processing method known to those skilled in the art, such as a tablet method, can be used.
[0019] <Peak separation> In this embodiment, the peak separation of the infrared absorption spectrum is performed by first separating the peaks from 2000 to 4000 cm -1 For the infrared absorption spectrum in the range of -1)) is assumed to exist, and curve fitting is performed by the least squares method so that the seven peaks are separated. The seven peaks assumed to exist are at least those with a peak top of 3727 ± 10 cm -1 The first peak is located at 3676±10cm. -1 and the second peak at 3581±10 cm -1 In addition to these three fixed peaks, four variable peaks that are considered to represent hydroxyl groups observed within the above wavelength range due to physical adsorption of water from the atmosphere, etc., to alumina are specified as seven peaks assumed to exist. The peak top wavelengths of the four variable peaks are, for example, 3071 cm -1 , 3426cm -1 , 3762cm -1 and 2375 cm -1 In curve fitting (peak separation), a Gaussian function, a Lorentzian function, or a mixed function of a Gaussian function and a Lorentzian function (Gauss-Lorentz) can be used as a function representing a peak.
[0020] After the curve fitting process, the seven separated peaks (three fixed peaks and four variable peaks) obtained are superimposed to reproduce one spectrum (hereinafter also referred to as the "reproduced spectrum"), which is then compared with the spectrum before the curve fitting process (hereinafter also referred to as the "measured spectrum"). If the reproduced spectrum matches the measured spectrum, the seven separated peaks used to generate the reproduced spectrum are adopted. On the other hand, if the reproduced spectrum does not match the measured spectrum, the wavelengths (positions (cm)) of the peak tops of the four variable peaks among the seven peaks assumed to exist are used. -1 )) and perform the curve fitting process again. Here, the wavelength of the peak top for the variable peak is changed to 2000 to 4000 cm -1The reconstructed spectrum is reconstructed from the seven separated peaks after the second curve fitting process and compared with the measured spectrum. This process is repeated until the reconstructed spectrum and the measured spectrum match, and the seven separated peaks used to reconstruct the reconstructed spectrum when they match are adopted. The match between the reconstructed spectrum and the measured spectrum does not necessarily mean a perfect match, but it is sufficient if the entire spectrum roughly matches when visually inspected. The match between the reconstructed spectrum and the measured spectrum is greater when the residual sum of squares of both spectra is smaller, and this value may be used as an index to determine the match. For example, it can be determined that the reconstructed spectrum and the measured spectrum match when the residual sum of squares of both spectra is 0.01 or less.
[0021] Here, the infrared absorption spectrum (2000-4000 cm -1 If the reproduced spectrum does not match the measured spectrum even after repeating the above process, the 2000-4000 cm -1 The number of peaks assumed to be in the infrared absorption spectrum in the range is gradually decreased. At this time, the infrared absorption spectrum is assumed to include at least three fixed peaks, the first peak to the third peak, and the number of four variable peaks, the fourth peak to the seventh peak, is gradually decreased.
[0022] More specifically, if the reproduced spectrum does not match the measured spectrum even after repeating the above process assuming that the infrared absorption spectrum has seven peaks, the agreement between the reproduced spectrum and the measured spectrum is confirmed by assuming that the infrared absorption spectrum has six peaks. The six peaks assumed to exist include at least three fixed peaks, the first peak to the third peak, and in addition, three variable peaks, the fourth peak to the sixth peak, are specified. If the reproduced spectrum does not match the measured spectrum, the wavelengths (positions (cm)) of the peak tops of the three variable peaks are checked. -1)) is changed, peak separation is performed again, and the coincidence between the reproduced spectrum and the measured spectrum is judged. Note that the method of peak separation and the coincidence between the reproduced spectrum and the measured spectrum are the same as those described above, so detailed explanations are omitted.
[0023] Infrared absorption spectrum (2000-4000cm -1 If the reproduced spectrum does not match the measured spectrum even after repeating the above-mentioned process assuming that there are six peaks in the range of 1 to 3, the above-mentioned process of decreasing the number of variable peaks is repeated until the number of peaks assumed to exist is reduced to three (three fixed peaks, the first peak to the third peak), and the separated peak whose reproduced spectrum matches the measured spectrum until then is used.
[0024] In addition, 3581±10cm -1 The third peak, which has a peak top at , is also considered to be a peak indicating the presence of hydroxyl groups chemically bonded to alumina, and in this curve fitting, in addition to the first to third fixed peaks indicating hydroxyl groups chemically bonded to alumina, the presence of the fourth to seventh variable peaks due to physical adsorption of water is assumed. Peak separation is preferably performed after background correction by the Shirley method in order to more accurately grasp the state of the OH groups on the alumina (support) surface.
[0025] <Peak area ratio> In this embodiment, the area ratio of the separated peaks (area B of the second peak / area A of the first peak) is 2000 to 4000 cm -1 Within this range, the areas of the first peak and the second peak are determined, and the area B of the second peak is divided by the area A of the first peak. The method for determining the areas of the first peak and the second peak is not particularly limited, and the areas can be determined by a known method.
[0026] To produce a gold-loaded support (alumina) that satisfies this peak area condition, an aluminum source such as aluminum oxide sol, aluminum oxide hydrate, or aluminum hydroxide (hereinafter, also simply referred to as "aluminum source") can be used. For the aluminum oxide sol, which is the aluminum source, aluminum oxide having an amorphous or crystalline structure can be used, and for the aluminum oxide hydrate, which is the aluminum source, boehmite can also be used. The concentration of aluminum oxide in the aluminum oxide sol is not particularly limited, and can be, for example, 5 wt% to 25 wt%.
[0027] The support according to this embodiment can be produced by calcining the aluminum source described above in air. The calcination conditions vary depending on the type of aluminum source. When an amorphous aluminum oxide sol is used, the calcination conditions can be 800 to 1300 ° C for 1 hour to 12 hours, and when a crystalline aluminum oxide sol is used, the calcination conditions can be 600 to 1200 ° C for 1 hour to 12 hours. When aluminum hydroxide or boehmite is used as the aluminum source, the calcination conditions can be 600 to 1400 ° C for 1 hour to 12 hours. In particular, when boehmite is used, it is preferable to calcinate at a temperature of 700 ° C to 1100 ° C for 1 hour to 12 hours, since it is easy to obtain a support that satisfies the formula (2) described later. If the calcination conditions do not satisfy the above conditions, it is difficult to obtain a gold-supported support that satisfies this peak area condition.
[0028] When an aluminum oxide sol is used as the aluminum source, the primary particle diameter of the colloidal particles (colloidal particles made of aluminum oxide) constituting the sol is preferably 5 to 1000 nm, more preferably 500 to 800 nm, in terms of average particle diameter, in order to further enhance the catalytic activity. In addition, the form of the aluminum source other than the aluminum oxide sol is not limited, but is preferably in the form of particles in order to further enhance the catalytic activity, more preferably particles with an average particle diameter of 5 to 1000 nm, and most preferably particles with an average particle diameter of 500 to 800 nm. The aforementioned average particle diameter of the aluminum source refers to the volume average diameter.
[0029] The reason why a catalyst using a gold-supported carrier that satisfies this peak area condition can exhibit catalytic activity even at low temperatures below 100 °C and furthermore, the catalytic activity is likely to be maintained even if the oxidation reaction is continued is not clear, but the first peak (3727 ± 10 cm -1 The second peak (3676±10cm -1 As mentioned above, the peaks B / A (having a peak top at 1.0001 Hz) are considered to be peaks indicating hydroxyl groups chemically bonded to the alumina itself. The area ratio of the peaks having peak tops at different infrared absorption wavelengths, that is, the ratio of the intensities of the different vibration modes of the hydroxyl groups, is considered to indicate the mobility of the hydroxyl groups, and it is presumed that when B / A is 2.0 or less, the mobility of the hydroxyl groups is restricted, making it difficult for water in the air to be adsorbed, and therefore the approach of the target substance such as carbon monoxide to the gold particles (particles containing gold element) is not hindered, and the above-mentioned function can be expressed.
[0030] In the gold-loaded carrier of this embodiment, it is sufficient that the area A of the first peak and the area B of the second peak satisfy the above formula (1). However, from the viewpoint of further enhancing the catalytic activity and making it easier to maintain the catalytic activity, it is more preferable that they satisfy the following formula (2). 1.2≦B / A≦2.0 (2)
[0031] The crystal type of the alumina used for the carrier is not particularly limited as long as it satisfies the above formula (1), but α-type, γ-type, δ-type, and θ-type are preferable because they have high activity, and γ-type, δ-type, and θ-type are particularly preferable because they have even higher activity. The crystal type may not be a single type, but may be a mixed crystal of two or more crystal types, and may contain an amorphous portion.
[0032] The specific surface area of the support is 20m2, which can further increase the catalytic activity. 2 / g or more, and 20 to 500m 2 / g, and the specific surface area is preferably 100 to 300 m 2 / g, and the specific surface area is preferably 150 to 300 m 2 The specific surface area according to this embodiment can be calculated by performing a pretreatment at 300° C. for 2 hours, measuring the nitrogen adsorption at liquid nitrogen temperature (−196° C.), and using an automatic specific surface area measuring device according to the BET method.
[0033] The support may have pores, and the pores are preferably mesopores (pores with a pore size of 1 nm or more and 100 nm or less), because this can further enhance the catalytic activity. A plurality of pores may be formed in the support. From the viewpoint of further enhancing the catalytic activity, the pore volume is preferably 0.1 cm or less. 3 / g or more, and 0.2 cm 3 The upper limit of the pore volume is not particularly limited, but is, for example, 0.7 cm 3 / g or less.
[0034] Here, mesopores can be identified by obtaining the pore diameter value by the BET method. The pore volume can be calculated by the BJH method (EP Barrett, LG Joyner, PH Halenda: J. Am. Chem. Soc., 73, 373 (1951)), which determines the pore diameter from the desorption isotherm, which is the relationship between the relative pressure when the adsorbate is desorbed and the amount of adsorption, and indicates the average volume of the pores formed in the support.
[0035] The carrier supports particles containing gold elements. The supported particles only need to contain gold elements, and catalytic activity is high, so gold elements are preferably zero-valent, i.e., gold in a metallic state, but gold particles may contain oxidized gold in addition to zero-valent gold. In addition, to enhance catalytic activity, precious metal elements other than gold, such as silver, platinum, palladium, and rhodium, may be included. The form in which precious metal elements other than gold are included is not particularly limited, and it is sufficient that the gold element and the precious metal element other than gold are included in the same particle, and they may be completely compatible with each other or partially mixed. A plurality of gold particles may be supported on the carrier. The particle size of the gold particles is preferably 5 nm or less in average particle size, and more preferably 0.1 to 3 nm, in order to further enhance catalytic activity.
[0036] The particle size of the gold particles in this embodiment is the diameter of the gold particles that can be measured from an image photograph taken with a transmission electron microscope (TEM), and the average particle size of the gold particles is the arithmetic average of the diameters of all gold particles when the catalyst contains 200 or fewer gold particles, and is the arithmetic average of the diameters of at least 200 gold particles when the catalyst contains more than 200 gold particles.
[0037] In order to further enhance catalytic activity, the amount of gold particles supported in this embodiment is preferably 0.1% by mass or more and 15.0% by mass or less, more preferably 0.5% by mass or more and 12.0% by mass or less, and most preferably 0.5% by mass or more and 3.0% by mass or less, relative to 100% by mass of the support.
[0038] In the catalyst according to the present embodiment, the gold particles may be supported on the surface of the support. In addition, as described above, there may be cases where pores are formed inside the support, in which case the gold particles may be supported on the surface of the support within the pores.
[0039] In addition, in the catalyst of this embodiment, in addition to the gold particles, co-catalyst particles composed of metal elements other than gold may be supported on the carrier. The co-catalyst particles may be supported on the carrier in a state separated from the gold particles, or may be supported on the carrier in a state fixed to the gold particles. When the gold particles are used alone or when the gold particles and the co-catalyst particles are fixed, the gold particles can be within the above-mentioned size range (average particle size is 5 nm or less). Metal particles that can be used in the co-catalyst particles include metal particles such as noble metals and their oxides, such as Pd and Ir, or base metals and their oxides. Two or more kinds of metal particles of these noble metals and their oxides, and base metals and their oxides may be supported on the carrier.
[0040] In order to make the catalyst less susceptible to the effects of moisture, the catalyst may be made hydrophobic, or a moisture absorbent or a desiccant may be added.
[0041] The catalyst of the present embodiment is particularly useful as an oxidation catalyst for carbon monoxide, but can also be used as an oxidation catalyst for other substances. Examples of substances that can be oxidized include substances that volatilize from materials such as automobile interior materials, building materials and interior materials for housings, and housings and components for home appliances, and substances that volatilize from organic solvents such as paints, adhesives, and cleaning agents. Specifically, hydrocarbons such as methane, ethane, propane, butane, ethylene, propylene, isoprene, benzene, xylene, toluene, ethylbenzene, styrene, α-farnesene, and β-farnesene, methanol, ethanol, propan-1-ol, butan-1-ol, pentan-1-ol, hexane-1-ol, heptan-1-ol, octan-1-ol, trans-2-hexenol, cis-2-hexenol, trans-3-hexenol, cis-2-hexenol, cis-3 ... -Hexenol, cis-3-hexenol, linalool, benzyl alcohol, and other alcohols, formaldehyde, acetaldehyde, propionaldehyde, butanal, pentanal, nonanal, benzaldehyde, hexanal, trans-2-hexenal, cis-2-hexanal, trans-2-octenal, trans-2-nonenal, cis-2-nonenal, trans,cis-2,6-nonadienal, trans,cis-2,Aldehydes such as 4-decadienal, ketones such as acetone, ethyl methyl ketone, diethyl ketone, methyl isobutyl ketone, cyclohexanone, and acetophenone, methyl formate, ethyl acetate, pentyl acetate, isopentyl acetate, octyl acetate, hexyl acetate, benzyl acetate, methyl butyrate, ethyl butyrate, pentyl butyrate, methyl salicylate, ethyl caproate, pentyl valerate, ethyl 2-methylpropanoate, ethyl butanoate, methyl 2-methylbutanoate, ethyl 2-methylbutanoate, ethyl 3-methylbutanoate, methyl 3-hydroxybutanoate, methyl hexanoate, ethyl hexanoate, hexyl hexanoate, methyl 3-hydroxyhexanoate, octyl hexanoate, ethyl octanoate, and ethyl octanoate. Examples of the esters include esters such as methacrylate, methacrylate crosspolymer ...
[0042] Next, the supporting step of supporting particles containing elemental gold on a support will be described.
[0043] The method of supporting gold particles on the alumina carrier is to immerse the carrier in a solution or colloidal solution of a gold compound (hereinafter, these are also simply referred to as "gold compound solution") and bring the gold compound solution into contact with the surface of the carrier (when pores are formed in the carrier, the surface of the carrier and the surface inside the pores). When an alloy of gold element and base metal constituting the gold particles is to be supported, a solution in which a salt of a base metal is further dissolved in addition to the gold compound may be used as the gold compound solution. Thereafter, a calcination treatment and, if necessary, a reduction treatment are further performed to form gold particles on the surface of the carrier (when mesopores are formed in the carrier, the surface of the carrier and the surface inside the mesopores), thereby fixing the gold particles to the carrier. This process makes it possible to obtain the catalyst according to this embodiment.
[0044] The method of supporting gold particles on a carrier will be described in more detail. First, the gold compound solution is heated to 20 to 90°C, preferably 50 to 70°C, and while stirring, the pH is adjusted to 3 to 10, preferably 5 to 8, using an alkaline solution. Next, the carrier is put into the gold compound solution, and the gold compound solution is allowed to penetrate into the carrier. At this time, if necessary, if the carrier has pores, a reduced pressure degassing treatment may be further performed. If pores are formed in the carrier, the gold compound solution also penetrates into the pores by the reduced pressure degassing treatment. Then, the gold particles can be supported on the carrier by heating and calcining at 200 to 600°C for 1 to 6 hours. If the supporting process satisfies the above-mentioned conditions, it becomes easier to obtain a gold-supported carrier that satisfies the peak area condition.
[0045] In addition, gold particles can be supported on a carrier by carrying out a known reduction operation such as a hydrogen reduction method in which the carrier is permeated with a gold compound solution as described above, followed by a calcination treatment at 200 to 600 ° C and a treatment of exposing the carrier to a hydrogen stream at 100 to 300 ° C, or a liquid phase reduction method in which the carrier is immersed in a sodium borohydride solution. The specific conditions of the reduction operation are not particularly limited as long as the gold-supported carrier satisfies the peak area condition. Depending on the type of compound contained in the gold compound solution, gold particles can be supported on a carrier only by a heating and calcination treatment at 200 to 600 ° C without carrying out the known reduction operation described above. In addition, when mesopores are formed in the carrier, the reduction of the gold compound contained in the gold compound solution is limited to a part, and gold oxide particles may coexist with the gold particles in the mesopores.
[0046] Examples of gold compounds include HAuCl4·4H2O, NH4AuCl4, KAuCl4·nH2O, KAu(CN)4, Na2AuCl4, KAuBr4·2H2O, and NaAuBr4. The concentration of the gold compound in the gold compound solution is not particularly limited, but is preferably 1×10 -2 ~1×10 -5 It is preferable to prepare the solution in mol / L because the resulting gold particles are less likely to aggregate.
[0047] The base metal salt that can be contained in the gold compound solution is not particularly limited as long as it is a compound that can dissolve in the solution and does not cause precipitation when coexisting with the gold compound, and examples thereof include halide salts such as chlorides and bromides of base metals, nitrates, carbonates, bicarbonates, and carboxylates. The concentration of the base metal salt is not particularly limited, but is preferably 1×10 -2 ~1×10 -5 It is preferable to prepare the solution in mol / L because the resulting gold particles are less likely to aggregate.
[0048] Alternatively, gold particles may be supported on a carrier by a colloidal method using a gold colloid solution, which will be described below.
[0049] In the gold particle supporting step, the carrier is preferably a gold particle having a specific surface area of 20 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 A gold colloid solution containing gold particles (including surface-modified gold particles) having a particle size of 5 nm or less, preferably 0.5 to 3 nm, can be used. If the specific surface area is outside the above range or if the gold particles have a particle size exceeding 5 nm, it becomes difficult for the gold particles to be supported on the carrier.
[0050] In the colloidal method using a gold colloidal solution, the gold particles can be supported by immersing the carrier in the gold colloidal solution, then filtering and calcining the carrier. Specifically, for example, the carrier is immersed in the gold colloidal solution, and the pH of the gold colloidal solution is adjusted to 8 to 11 using sodium hydroxide or the like while stirring and mixing for 30 minutes to 2 hours. Next, 50 to 200 parts by mass of sodium borohydride is added to 100 parts by mass of gold particles in the colloidal solution. The carrier is filtered out from the colloidal solution, washed, dried at 60 to 100°C, and then calcined in air at 200 to 500°C for 2 to 10 hours to support the gold particles on the surface of the carrier (on the surface of the carrier and the surface inside the mesopores, if the carrier has mesopores). If the supporting step satisfies the above-mentioned conditions, it becomes easier to obtain a gold-supported carrier that satisfies the peak area condition. This treatment makes it possible to obtain a carrier on which gold particles are supported. If mesopores are formed in the support, it is desirable to subject the gold colloid solution in which the support is immersed to a reduced pressure degassing treatment, as this will promote the penetration of the gold colloid solution into the mesopores of the support.
[0051] A gold colloid solution can be formed by dissolving a gold compound that forms a colloid in water in water. Examples of gold compounds that can be used in this case include tetrachloroauric acid, HAuCl4, and Au(en)2Cl3 (en: ethylenediamine group). When tetrachloroauric acid is used, a toluene solution of tetrachloroauric acid and a toluene solution of tetraoctylammonium bromide can be added to water in the presence of sodium borohydride to obtain a gold colloid solution. When HAuCl4 is used, a toluene solution of tetraoctylammonium bromide can be added to water together with HAuCl4 in the presence of sodium borohydride to obtain a gold colloid solution. In addition, Au(en)2Cl3 can be directly added to water to obtain a gold colloid solution. Note that sodium borohydride is added when supporting gold particles on a carrier as described above, and the gold colloid solution can also be prepared without adding it during colloid formation.
[0052] The catalyst of this embodiment can be used, for example, in a member or gas purification device having a function of removing carbon monoxide, and can be used by contacting a gas to be treated containing carbon monoxide in the presence of oxygen. Examples of such members or devices include exhaust gas purification devices for internal combustion engines, air purification devices installed in air conditioning facilities, air purifiers installed in offices and smoking rooms, and protective equipment such as gas masks. Such members or devices may be provided with a function for setting a usage environment in which the catalyst operates favorably, such as a catalyst heating mechanism or a blower mechanism for sending a gas to be treated to the catalyst.
[0053] Here, the shape of the catalyst of this embodiment is not particularly limited, but as described above, the contact area with the substance to be treated (e.g., carbon monoxide) is large and the decomposition reaction of the substance to be treated is easily promoted, so that a shape such as a powder, a particle, or a pellet is preferable. The catalyst can also be formed on a substrate and used. The substrate to which the catalyst is fixed can be used as an oxidation catalyst member that oxidizes the substance to be treated, and can be used as a member constituting the above-mentioned exhaust gas purification device, air purification device, air purifier, protective equipment, etc. The shape of the substrate is also not particularly limited, but a substrate such as a honeycomb shape or a fibrous shape is preferable. If the substrate has a fibrous or honeycomb shape, air permeability is obtained, so that the oxidation catalyst member can be used as an oxidation catalyst filter, and the pressure loss during ventilation of the gas to be treated is reduced, which is preferable.
[0054] Since the substrate may be heated to high temperatures during production or use of the catalyst according to the present embodiment, it is preferable that the substrate is made of a material having heat resistance capable of withstanding the heating temperature. Specifically, the substrate material is preferably a metal material, ceramics, glass, carbon fiber, silicon carbide fiber, or the like, and more preferably a metal, a metal oxide, or glass.
[0055] Examples of metal materials that can be used for the substrate include high-melting-point metals such as tungsten, molybdenum, tantalum, niobium, TZM (Titanium Zirconium Molybdenum), and W-Re (tungsten-rhenium), precious metals such as silver and ruthenium, and alloys or oxides thereof, special metals such as titanium, nickel, zirconium, chromium, Inconel, and Hastelloy, and general-purpose metals such as aluminum, copper, stainless steel, zinc, magnesium, and iron, and alloys containing these general-purpose metals or oxides of these general-purpose metals. Also, members on which a coating of the above-mentioned metals, alloys, or oxides is formed by various plating methods, vacuum deposition, CVD, sputtering, or the like may be used as the metal material.
[0056] Furthermore, examples of ceramics used in the substrate include ceramics such as earthenware, pottery, stoneware, and porcelain, cement, gypsum, enamel, and fine ceramics. The ceramics may have an elemental, oxide, hydroxide, carbide, carbonate, nitride, halide, and phosphate composition, or may be a composite of these.
[0057] Further examples of the ceramics used for the substrate include barium titanate, lead zirconate titanate, ferrite, alumina, forsterite, zirconia, zircon, mullite, steatite, cordierite, aluminum nitride, silicon nitride, silicon carbide, new carbon, and the like, as well as ceramics such as high-strength ceramics, functional ceramics, superconducting ceramics, nonlinear optical ceramics, antibacterial ceramics, biodegradable ceramics, and bioceramics.
[0058] Furthermore, examples of glasses that can be used as the substrate include soda-lime glass, potash glass, crystal glass, quartz glass, chalcogenide glass, uranium glass, water glass, polarized glass, tempered glass, laminated glass, heat-resistant glass, borosilicate glass, bulletproof glass, glass fiber, dichroic, goldstone (brown goldstone, sand goldstone, purple goldstone), glass ceramics, low-melting point glass, metallic glass, new glass, and sapphire.
[0059] In addition, other cements such as ordinary Portland cement, early strength Portland cement, extra early strength Portland cement, moderate heat Portland cement, low heat Portland cement, sulfate-resistant Portland cement, and mixed cements such as blast furnace cement, silica cement, and fly ash cement, which are Portland cement to which blast furnace slag, fly ash, and siliceous admixtures have been added, can also be used for the base material.
[0060] Other examples of the substrate that can be used include titania, zirconia, alumina, ceria (cerium oxide), zeolite, apatite, silica, activated carbon, diatomaceous earth, etc. Furthermore, the substrate can also be made of metal oxides such as chromium, manganese, cobalt, nickel, and tin.
[0061] When the catalyst of this embodiment is formed on a substrate, for example, a catalyst formed on a substrate can be produced by fixing alumina as a carrier to the substrate, and then carrying out a process of supporting particles containing gold element on the carrier.
[0062] In the step of fixing the carrier to the substrate, for example, when an aluminum oxide sol is used as the aluminum source, the substrate is immersed in the aluminum oxide sol to cause the aluminum oxide sol to adhere to the substrate surface, and then the aluminum oxide sol on the substrate is fired under the firing conditions described above, thereby fixing the carrier to the substrate surface.
[0063] The catalyst of the present embodiment is used by contacting a gas to be treated containing a substance to be treated with the catalyst in the presence of oxygen. In the presence of oxygen, the gas to be treated comes into contact with the catalyst, and the substance to be treated in the gas to be treated is oxidized and decomposed. The source of the gas to be treated is not particularly limited, and examples thereof include internal combustion engines such as automobiles and boilers, and by-product gases generated from secondary batteries.
[0064] The concentration of the substance to be treated in the gas to be treated is not particularly limited, but when the substance to be treated is carbon monoxide, the carbon monoxide is preferably 5 ppm or more and 5% or less by volume relative to the gas to be treated from the viewpoint of increasing the decomposition rate. The gas to be treated may contain other components such as nitrogen, argon, etc. in addition to the substance to be treated (e.g., carbon monoxide) and oxygen.
[0065] The method and conditions for contacting the gas to be treated with the catalyst are not particularly limited and are affected by the environment in which the gas is used, but from the viewpoint of increasing the decomposition rate, it is preferable to contact the gas to be treated with the catalyst at a space velocity of 10,000 mL / g / hr or more and 5,000,000 mL / g / hr or less. The space velocity is expressed as the speed at which the volume of the gas to be treated that is multiples of the volume of the catalyst contacts (passes) the catalyst per unit time, and is the value obtained by dividing the flow rate (volume) of the gas to be treated per unit time by the volume of the catalyst. The contact of the gas to be treated with the catalyst may be carried out under atmospheric pressure, or under reduced pressure or pressurized atmosphere.
[0066] The temperature at which the gas to be treated is contacted with the catalyst is not particularly limited, but is preferably 0°C or higher since the catalytic activity is high. The catalyst of this embodiment exhibits catalytic activity even at temperatures below 0°C, but below 0°C, moisture adsorbed on the catalyst may be adsorbed, inhibiting contact between the catalyst and the substance to be treated (e.g., carbon monoxide), thereby inhibiting the catalytic activity. In addition, unlike conventional catalysts that cannot oxidize the substance to be treated (e.g., carbon monoxide) unless the gas to be treated is contacted at a high temperature exceeding 100°C, the catalyst of this embodiment can oxidize the substance to be treated (e.g., carbon monoxide) even at temperatures below 100°C, and can further oxidize the substance to be treated even at temperatures below 25°C.
[0067] The temperature at which the gas to be treated is brought into contact with the catalyst can be adjusted by heating or cooling the catalyst, or by heating or cooling the gas to be treated. It may also be adjusted by heating or cooling both the catalyst and the gas to be treated. For example, by setting the catalyst at 0°C or higher and 100°C or lower, or by setting the temperature of the gas to be treated at 0°C or higher and 100°C or lower, the gas to be treated can be brought into contact with the catalyst at a temperature of 0°C or higher and 100°C or lower. EXAMPLES
[0068] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to these examples.
[0069] [Example 1] 100 ml of amorphous aluminum oxide sol (Taki Chemical Co., Ltd., Al-L7) with an aluminum oxide concentration of 7 wt% and a primary particle size of 5 to 10 nm was heated from room temperature to 1100°C over a period of 4 hours, and then calcined at 1100°C for 4 hours to obtain an alumina carrier.
[0070] 250 ml of a 2.94 mmol / L aqueous solution of chloroauric acid, adjusted to pH 7 with an aqueous solution of sodium hydroxide, was heated to 70° C., and 1 g of the obtained alumina carrier was added and stirred. The alumina carrier was then filtered off and calcined at 350° C. for 2 hours to obtain the catalyst of Example 1. The amount of gold supported on the catalyst was measured with an atomic absorption spectrometer.
[0071] [Example 2] The catalyst of Example 2 was obtained under the same conditions as in Example 1, except that the amorphous aluminum oxide sol (Al-L7) used in Example 1 was replaced with 100 ml of a γ-type aluminum oxide sol (Al-C20, manufactured by Taki Chemical Industry Co., Ltd.) having an aluminum oxide concentration of 20 wt% and a primary particle size of 15 to 20 nm, and the calcination temperature was changed from 1100°C to 700°C.
[0072] [Example 3] A catalyst of Example 3 was obtained under the same conditions as in Example 1, except that 10 g of boehmite powder (manufactured by Taimei Chemical Industry Co., Ltd., C06) was used instead of the amorphous aluminum oxide sol (Al-L7) used in Example 1.
[0073] [Comparative Example 1] A catalyst of Comparative Example 1 was obtained under the same conditions as in Example 1, except that the calcination temperature was changed from 1100°C to 700°C.
[0074] For the obtained catalysts (gold-supported carriers) of Examples 1 to 3 and Comparative Example 1, the infrared absorption spectrum of the carrier was obtained under the following conditions, and peak separation was performed to determine the ratio (B / A) of the area B of the second fixed peak to the area A of the first fixed peak. In addition, the crystal type of the alumina contained in the catalysts of the examples and comparative example was identified by X-ray diffraction measurement (X-ray source: Cu-Kα, X-ray output: 40 kV, 30 mA, scan speed: 2.0 deg / min, step width: 0.02 deg, scan axis: 2θ / θ, scan range: 5.0 to 90.0 deg). Furthermore, the following CO removal test was performed using the catalysts of Examples 1 to 3 and Comparative Example 1.
[0075] (Infrared absorption spectrum) Infrared absorption spectrum was measured in a state heated to 400℃ using a full vacuum Fourier transform infrared spectrophotometer (JASCO FT / IR-6700FV) and a vacuum heating diffusion measuring device (JASCO DR-650). The measurement sample was placed in the sample chamber of the device without dilution, and measurements were performed by the diffuse reflectance method using CaF2 powder as a reference. The resolution was 4cm -1 The number of integrations was set to 64. The sample chamber was purged with nitrogen gas, and the interferometer and the inside of the cell were evacuated during the measurement.
[0076] <Peak separation and peak area> For the obtained spectrum, 4000 cm -1 From 2000cm -1 The number of separated peaks was set to seven, and the peak tops of the three fixed peaks were 3727 cm -1 , 3676cm -1 and 3581 cm -1 The peak tops of the other four variable peaks are fixed at 3071 cm -1 , 3426cm -1 , 3762cm -1 and 2375 cm -1The curve fitting process was performed using a curve fitting program built into the measurement device, according to the principle described in the instruction manual for the all-vacuum Fourier transform infrared spectrophotometer. If the reproduced spectrum obtained by superimposing the seven separated peaks did not match the actually measured spectrum before the curve fitting process, the wavelengths (positions (cm)) of the peak tops of the four variable peaks that were provisionally set were used. -1 )) to 4000 cm -1 From 2000cm -1 The wavelength (position (cm) of the peak top of the provisionally set variable peak was changed within the range and the curve fitting process was performed again. -1 By repeatedly changing the temperature, seven separated peaks were identified. -1 If the reproduced spectrum does not match the measured spectrum even after repeating the above process, the 2000-4000 cm -1 The number of peaks assumed to be in the infrared absorption spectrum in the range was gradually reduced. Here, the number of variable peaks was reduced by four, from the fourth peak to the seventh peak, so that the peaks assumed to exist included at least the first to third peaks. Here, the agreement between the reproduced spectrum and the measured spectrum was determined when the residual sum of squares of both spectra was 0.01 or less.
[0077] FIG. 1 shows the infrared absorption spectrum (upper spectrum) of Example 2 and the peaks after peak separation (lower spectrum). -1 The area A of the first fixed peak having a peak top at 3676 cm -1 The area B of the second fixed peak having a peak top at was calculated using the value calculated simultaneously with the curve fitting process, and the area ratio of these peaks (area B of the second fixed peak / area A of the first fixed peak) was calculated.
[0078] (CO removal test) Carbon monoxide (CO) was used to evaluate the CO oxidation reaction of each catalyst of the examples and comparative examples. Specifically, a test device was prepared in which 50 mg of each catalyst of the examples and comparative examples was installed in a flow path to achieve a predetermined flow path width and height. The gas to be treated was prepared by mixing air so that the carbon monoxide concentration was 200 ppm, and the gas to be treated with a constant CO concentration was supplied to the flow path while controlling the flow rate to 0.5 L / min (space velocity: 600,000 mL / g / hr) with a mass flow controller, and the CO concentration of the gas to be treated that had permeated the catalyst was measured when a predetermined time had elapsed since the start of the test, thereby performing a CO removal test. The flow path used in this test was an open type flow path in which the gas to be treated that had permeated the catalyst was discharged to the outside, and the gas to be treated with the above-mentioned carbon monoxide concentration was continuously supplied at the above-mentioned flow rate. The temperature of the gas to be treated was adjusted to 20±2°C, and the humidity was adjusted to 50±5%.
[0079] The treated gas before and after treatment with the test device was analyzed using a gas chromatograph (Agilent 7820A GC system, manufactured by Agilent Technologies, Inc.).
[0080] Using the above-mentioned gas chromatograph, the CO concentration in the gas being treated that was being supplied to the test device (hereinafter also referred to as the "initial CO concentration") and the CO concentration in the gas being treated that had permeated the catalyst a certain time after the start of the test (10 minutes, 2 hours, and 4 hours) (hereinafter also referred to as the "post-reaction CO concentration") were measured, and the CO removal rate was calculated using the following formula. The results are shown in Table 1. CO removal rate (%) = {(initial CO concentration - CO concentration after reaction) / initial CO concentration} x 100
[0081] The fact that the CO in the treated gas was oxidized to CO2 was confirmed by detecting by gas chromatography that the amount of CO2 in the treated gas after the treatment was increased compared to the amount in the treated gas before the treatment.
[0082] [Table 1]
[0083] As can be seen from the above results, the CO removal rates of the catalysts of Examples 1 to 3 are higher than that of the catalyst of Comparative Example 1 after both 10 minutes and 2 hours, and the CO removal performance of the catalyst of this example is superior. In addition, the catalysts of Examples 1 to 3 have a smaller difference in CO removal rate after 10 minutes and 2 hours compared to the catalyst of Comparative Example 1, and it is understood that the catalytic activity is easily maintained even if the oxidation reaction is continued. In particular, Examples 2 and 3, in which B / A is 1.2 or more, have a higher CO removal rate after 10 minutes, 2 hours, and 4 hours than Example 1, and the difference in the CO removal rate after 10 minutes and 4 hours is smaller. From these results, it can be seen that Examples 2 and 3 have a higher catalyst and can suppress the decrease in catalytic activity more effectively compared to Example 1.
Claims
1. The catalyst comprises a support made of alumina and particles containing elemental gold supported on the support, The infrared absorption spectrum of the carrier measured by a Fourier transform infrared spectrometer is 3727±10 cm -1 The first peak having a peak top at 3676±10 cm -1 and a second peak having a peak top at 3581 ± 10 cm -1 1. An oxidation catalyst characterized in that, when the peaks are separated into seven or less peaks having different peak top wavelengths, including a third peak having a peak top at a wavelength of 100 nm, an area A of the first peak and an area B of the second peak satisfy the following formula (1): 0<B / A≦2.0...(1)
2. 2. The oxidation catalyst according to claim 1, wherein the area A and the area B satisfy the following formula (2): 1.2≦B / A≦2.0 (2)
3. 3. The oxidation catalyst according to claim 1, wherein the particles further contain a noble metal element other than gold.
4. 4. The oxidation catalyst according to claim 1, wherein the amount of the particles containing elemental gold supported is 0.5% by mass or more and 3.0% by mass or less with respect to 100% by mass of the support.
5. An oxidation catalyst according to any one of claims 1 to 4; A substrate on which the oxidation catalyst is fixed; An oxidation catalyst member comprising:
6. 5. A method for removing carbon monoxide, comprising contacting a gas to be treated containing carbon monoxide with the oxidation catalyst according to claim 1 at a temperature of 0° C. or higher and 100° C. or lower in the presence of oxygen.
Citation Information
Patent Citations
Production method for gold catalyst and its usage
JP2005230699A
Carbon monoxide selective oxidation catalyst and its production method
JP2005342689A
Silver catalyst for oxidation
JP2010125373A
Catalyst-carrying electrode and gas treatment device prepared therewith
JP2016193428A
Hydrogenation treatment catalyst for hydrocarbon oil, method for producing the same, and hydrogenation treatment method