Cutting Tools
The cutting tool with a hexagonal composite carbide structure at the grain boundary and a coating layer addresses chipping and fracture resistance issues, enhancing performance in high-speed cutting operations.
Patent Information
- Application Number
- JP2020196843
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Cutting tools face challenges in chipping resistance and fracture resistance, particularly when used in high-speed cutting operations on hardened steel.
A cutting tool composed of a ceramic sintered body containing tungsten carbide, alumina, and zirconia, with a composite carbide of tungsten and cobalt having a hexagonal crystal structure, and a coating layer, where the composite carbide is present at the grain boundary between tungsten carbide crystal particles, and the X-ray diffraction intensity ratio of the composite carbide is within specific ranges.
The cutting tool exhibits improved chipping resistance and fracture resistance, with the hexagonal composite carbide structure enhancing toughness and the coating layer increasing wear resistance.
Smart Images

Figure 0007556765000003 
Figure 0007556765000002 
Figure 0007556765000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to cutting tools. [Background technology]
[0002] An alumina-tungsten carbide-zirconia ceramic composition is known (see Patent Document 1). In the alumina-tungsten carbide-zirconia ceramic composition, zirconium is distributed in the first grain boundary where an alumina crystal grain and a tungsten carbide crystal grain are adjacent to each other, and in the second grain boundary where two alumina crystal grains are adjacent to each other, improving the bonding strength between the crystal grains at each grain boundary. Therefore, the alumina-tungsten carbide-zirconia ceramic composition has excellent mechanical properties and can be used for cutting tools for heat-resistant alloys, which require high impact resistance and heat resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2015 / 019391 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, cutting tools have been required to withstand ever-increasing efficiency in cutting processes. However, conventional cutting tools have room for improvement in terms of chipping resistance and fracture resistance when used for, for example, machining hardened steel, which requires increased cutting speeds and high loads. The present disclosure has been made in view of the above circumstances, and has an object to provide a cutting tool having improved chipping resistance and fracture resistance. The present disclosure can be realized in the following aspects. [Means for solving the problem]
[0005] [1] A cutting tool made of a ceramic sintered body containing tungsten carbide, alumina, and zirconia, The ceramic sintered body contains a composite carbide of tungsten and cobalt, The composite carbide can have a hexagonal crystal structure, The X-ray diffraction pattern obtained by measuring the ceramic sintered body by X-ray diffraction is A cutting tool showing a diffraction pattern in the case where the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal.
[0006] [2] The cutting tool according to [1], wherein the composite carbide is present at a grain boundary, which is an interface between two adjacent tungsten carbide crystal grains.
[0007] [3] The cutting tool according to [1] or [2], wherein the ceramic sintered body is measured by X-ray diffraction, and when the X-ray diffraction intensity of the (002) plane of tungsten carbide is taken as 100, the X-ray diffraction intensity of the composite carbide of tungsten and cobalt is 9.0 or more and 24.5 or less.
[0008] [4] A cutting tool comprising a base made of cemented carbide and the ceramic sintered body according to any one of [1] to [3] joined to the base via a brazing material, the cutting tool having a coating layer formed on the surface. Effect of the Invention
[0009] When the X-ray diffraction pattern obtained by measuring the ceramic sintered body by X-ray diffraction shows a diffraction pattern in which the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal, the chipping resistance and fracture resistance of the cutting tool are improved. When composite carbides are present at the grain boundary, which is the interface between two adjacent tungsten carbide crystal grains, the chipping resistance and fracture resistance of the cutting tool are further improved. When the ceramic sintered body is measured by X-ray diffraction, and the X-ray diffraction intensity of the (002) plane of tungsten carbide is taken as 100, if the X-ray diffraction intensity of the composite carbide of tungsten and cobalt is 9.0 or more and 24.5 or less, the chipping resistance and fracture resistance of the cutting tool are further improved. When a coating layer is formed on the surface, the wear resistance of the cutting tool is improved. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a perspective view of an example of a cutting tool. [Diagram 2] 1 is an X-ray diffraction pattern of an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following is a more detailed explanation. In this specification, when a numerical range is described using "to", the range includes the lower limit and the upper limit unless otherwise specified. For example, the description "10 to 20" includes both the lower limit "10" and the upper limit "20". In other words, "10 to 20" has the same meaning as "10 or more and 20 or less".
[0012] 1.Cutting tools The cutting tool is composed of a ceramic sintered body containing tungsten carbide (WC), alumina (Al2O3), and zirconia (ZrO2). The ceramic sintered body contains a composite carbide ((W,Co)C) of tungsten (W) and cobalt (Co). The above composite carbide can have a hexagonal crystal structure. The X-ray diffraction pattern obtained by measuring the ceramic sintered body by X-ray diffraction shows a diffraction pattern when the crystal structure of the above composite carbide in the ceramic sintered body is only hexagonal. Hereinafter, the "composite carbide of tungsten and cobalt" will also be referred to simply as "composite carbide".
[0013] (1) Sintered ceramics The ceramic sintered body contains a composite carbide of tungsten and cobalt. The composite carbide can have a hexagonal crystal structure. Such composite carbides include those with the formula W9Co3C4, W 10 Co3C4 and W 10 Co3C 3.4 The composite carbide may be one that can form a crystal structure other than a hexagonal crystal structure, or one that cannot form a crystal structure other than a hexagonal crystal structure.
[0014] The X-ray diffraction pattern obtained by measuring the ceramic sintered body by X-ray diffraction shows a diffraction pattern when the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal. Hexagonal composite carbides are tough and hard. Therefore, by including hexagonal composite carbides, the toughness of the ceramic sintered body is improved, and the chipping resistance and defect resistance of the cutting tool are improved. Furthermore, a ceramic sintered body that does not include composite carbides other than hexagonal carbides can maximize the proportion of hexagonal crystals in the entire composite carbide, and can satisfactorily obtain the above effects.
[0015] Figure 2 shows the X-ray diffraction pattern obtained by measuring a ceramic sintered body containing a composite carbide represented by W9Co3C4 using X-ray diffraction with a 2θ / θ focusing optical system and Cu-Kα radiation. The vertical axis represents the X-ray diffraction intensity, and the horizontal axis represents the diffraction angle 2θ (°). When the composition formula of the composite carbide is W9Co3C4, if both of the following conditions 1 and 2 are satisfied, it is determined that the composite carbide in the ceramic sintered body exhibits a diffraction pattern in which the crystal structure is only hexagonal. Condition 1: The diffraction pattern has a diffraction peak in the 2θ range of 41.0° to 42.0°. Condition 2: The diffraction pattern has no diffraction peaks in the 2θ range of 45.0° to 46.0°. Note that "having no diffraction peaks" means that the peak intensity is below the detection limit. The presence of the diffraction peak of condition 1 means that at least one of hexagonal composite carbides and cubic composite carbides is present. When both hexagonal composite carbides and cubic composite carbides are present, the two peaks overlap, resulting in a somewhat broader pattern than when only one of them is present. The absence of the diffraction peak of condition 2 means that no cubic composite carbide is present. The diffraction pattern shown in FIG. 2 has a diffraction peak marked with a black circle in the range of 41.0° to 42.0°, which is derived from a hexagonal composite carbide (see the lower left diagram). In other words, condition 1 is satisfied. The diffraction pattern shown in FIG. 2 does not have a diffraction peak derived from a cubic composite carbide in the range of 45.0° to 46.0° (see the lower right diagram). In other words, condition 2 is satisfied. This X-ray diffraction pattern, which satisfies conditions 1 and 2, shows a diffraction pattern when the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal.
[0016] The composition formula of the composite carbide is W 10 Co3C4 and W 10 Co3C 3.4 Even in this case, the diffraction pattern when the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal is almost the same as when the composition formula of the composite carbide is expressed as W9Co3C4. Therefore, when both conditions 1 and 2 are satisfied, it is judged that the diffraction pattern shown is the one when the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal. Incidentally, the mechanism by which composite carbides with a hexagonal crystal structure are formed is not clear; however, by keeping the temperature approximately constant within a specific temperature range during the heating up to a specified firing temperature, which is commonly used, it is possible to form only hexagonal composite carbides.
[0017] (2) Existence of complex carbides on grain boundaries The composite carbide is preferably present at a grain boundary, which is an interface between at least two adjacent tungsten carbide crystal grains. The presence of the composite carbide at the grain boundary improves the bonding strength between the tungsten carbide crystal grains, and further improves the chipping resistance and fracture resistance of the cutting tool.
[0018] The presence of composite carbides at grain boundaries, which are the interfaces between two adjacent tungsten carbide crystal grains, can be confirmed as follows: Any surface of a ceramic sintered body is observed with a STEM (Scanning Transmission Electron Microscope), and the grain boundaries, which are the interfaces between two adjacent tungsten carbide crystal grains, are measured by EDS (Energy Dispersive X-ray Spectroscopy) line analysis. Five such grain boundaries are arbitrarily selected, and the above measurements are performed. If composite carbides are observed at all of the locations, it is determined that composite carbides exist at the grain boundaries, which are the interfaces between two adjacent tungsten carbide crystal grains. The presence or absence of composite carbides at the grain boundary, which is the interface between two adjacent tungsten carbide crystal grains, can be controlled by adjusting the amount of composite carbides relative to tungsten carbide.
[0019] (3) X-ray diffraction intensity ratio of composite carbides When the ceramic sintered body is measured by X-ray diffraction, the X-ray diffraction intensity IB of the composite carbide of tungsten and cobalt is preferably 9.0 or more and 24.5 or less, where the X-ray diffraction intensity IA of the (002) plane of tungsten carbide is taken as 100. As the X-ray diffraction intensity IA of the (002) plane of tungsten carbide, for example, the peak height in the vicinity of 2θ=65.0° to 66.0° is suitably used. When the composition formula is W9Co3C4, the X-ray diffraction intensity IB of the composite carbide is suitably determined by the higher peak height of either the peak near 2θ=41.0° to 42.0° or the peak near 2θ=42.1° to 43.0°.
[0020] That is, the X-ray diffraction intensity IB of the composite carbide of tungsten and cobalt is expressed by the peak intensity ratio of the following formula (1) when the X-ray diffraction intensity IA of the (002) plane of tungsten carbide is taken as 100. This peak intensity ratio is an index of the content of the composite carbide. Peak intensity ratio = IB / IA × 100 Equation (1) The peak intensity ratio is preferably 9.0 or more, more preferably 10.5 or more. In this way, the content of the composite carbide is sufficient. On the other hand, the peak intensity ratio is preferably 24.5 or less, more preferably 21.0 or less. If the content of the composite carbide is too large, the composite carbide exists in a particulate form, and the starting point of softening at high temperatures is likely to occur. If the value of the peak intensity ratio is within the above range, the effect obtained by the composite carbide can be maximized, and the chipping resistance and fracture resistance of the cutting tool are further improved.
[0021] (4) Ratio of components constituting ceramic sintered body The contents of tungsten carbide (WC), alumina (Al2O3), zirconia (ZrO2), and composite carbide of tungsten (W) and cobalt (Co) ((W,Co)C) constituting the ceramic sintered body are not particularly limited, but it is preferable that the content of tungsten carbide is 21 volume % or more and 39 volume % or less, the content of zirconia is 0.50 volume % or more and 0.90 volume % or less, the content of cobalt is 0.01 volume % or more and 0.15 volume % or less, and alumina accounts for the remainder. The above content is the amount when the total volume of the ceramic sintered body is taken as 100 volume %. The content of each component in the ceramic sintered body can be calculated by determining the mass % of each element by X-ray fluorescence analysis or the like and converting it to volume %. Tungsten carbide, alumina, and zirconia are calculated in compound terms. Cobalt is calculated assuming it exists as a simple substance. The cobalt content is rounded off to two decimal places and is expressed to two decimal places.
[0022] The ceramic sintered body may contain impurities. The impurities are substances that are unintentionally mixed in during the manufacturing process, and examples of such impurities include at least one of iron (Fe), chromium (Cr), and nickel (Ni). The amount of impurities may be an amount (e.g., 0.1 mass% or less) that does not substantially reduce the properties of tungsten carbide (bending strength, thermal conductivity, etc.).
[0023] By setting the content of each component within a preferred range, the chipping resistance and fracture resistance can be further improved. The reason for this is presumed to be as follows. By setting the content of each component within a preferred range, a good balance is achieved between tungsten carbide, which has excellent hardness, and alumina, which has excellent resistance to reaction with the work material. In addition, the effect of two tungsten carbide crystal particles being firmly bonded to each other by the composite carbide, and the effect of alumina crystal particles and tungsten carbide crystal particles, and two alumina crystal particles being firmly bonded to each other by zirconium, can be maximized. This is believed to improve the chipping resistance and fracture resistance of the cutting tool.
[0024] The method of adding cobalt is not particularly limited. Cobalt powder may be added directly to the raw material. Cobalt may be used as abrasion powder obtained by, for example, dry rubbing with carbide balls containing cobalt and ethanol alone. Although the exact reason is not clear, the use of abrasion powder is expected to have a high effect on chipping resistance and chipping resistance.
[0025] (5) Manufacturing method of cutting tools There is no particular limitation on the method for producing the cutting tool. An example of the method for producing the cutting tool will be described below. Here, an example in which cobalt is contained will be described.
[0026] (5.1) Raw materials The following raw material powders are used as raw materials. Alumina powder (Al2O3 powder) ·Tungsten carbide powder (WC powder) · Zirconia powder (ZrO2 powder) Cobalt powder (Co powder)
[0027] (5.2) Preparation of mixed dry powder Prepare alumina powder, tungsten carbide powder, zirconia powder, and cobalt powder. Weigh out the raw powders in a predetermined ratio, put them into a ball mill together with a solvent and a dispersant, and mix and grind them to obtain a slurry. The obtained slurry is degassed in a hot water bath to remove the solvent from the slurry. The powders are then sieved to produce a mixed powder.
[0028] (5.3) Firing The obtained mixed dry powder is put into a carbon jig and hot-pressed at a predetermined temperature. Conventionally, when manufacturing a ceramic sintered body, a firing process (for convenience, referred to as the main firing process here) in which firing is performed at a predetermined firing temperature under a predetermined pressing pressure has been adopted. In contrast, a pre-firing process is provided prior to the main firing process in which the temperature is kept approximately constant in a specific temperature range during the heating up to the predetermined firing temperature, thereby controlling the crystal structure of the composite carbide. For example, the pre-firing process is preferably performed in a temperature range of 1000°C to 1200°C and for a pressurizing time of 10 minutes to 60 minutes. The pressure in the pre-firing process may be the same as that in the main firing process.
[0029] (6) Covering layer The cutting tool may have a coating layer formed on its surface. When the coating layer is formed, the surface hardness of the cutting tool increases and the progression of wear caused by reaction and adhesion with the workpiece is suppressed. As a result, the wear resistance of the cutting tool is improved. The components of the coating layer are not particularly limited. The coating layer is preferably formed of at least one compound selected from carbides, nitrides, oxides, carbonitrides, carbonates, oxynitrides, and carbonitrides of titanium, zirconium, chromium, and aluminum. The at least one compound selected from carbides, nitrides, oxides, carbonitrides, carbonates, oxynitrides, and carbonitrides of titanium, zirconium, chromium, and aluminum is not particularly limited, but suitable examples include TiN, TiAlN, and TiAlVN. The coating layer may be a single layer or multiple layers. The thickness is not particularly limited. From the viewpoint of abrasion resistance, the thickness of the coating layer is preferably 0.02 μm or more and 30 μm or less.
[0030] (7) Use of cutting tools The cutting tool can be applied to various cutting tools known in the art. Suitable examples of the cutting tool include an indexable tip tip (cutting insert, throw-away tip) for turning or milling, and an end mill. The cutting tool is a cutting tool in a broad sense, and refers to all tools for turning, milling, etc.
[0031] 2.Cutting tools 10 As shown in Fig. 1, the cutting tool 10 includes a base 11 made of cemented carbide and a ceramic sintered body 1 joined to the base 11 via a brazing material. A coating layer is formed on the surface of the cutting tool 10. The coating layer is preferably formed on at least the surface of the ceramic sintered body 1. The composition of the cemented carbide is not particularly limited. For example, the cemented carbide may preferably include a cemented carbide containing tungsten carbide crystal grains (hereinafter, also referred to as "tungsten carbide (WC)-based cemented carbide"). For example, the tungsten carbide-based cemented carbide may preferably include a WC-Ni-Cr-based cemented carbide, a WC-Co-based cemented carbide, and a WC-Co-Cr-based cemented carbide. The components of the brazing material are not particularly limited. The brazing material is composed of, for example, an active metal and one or more ductile metals. Examples of the active metal include titanium (Ti), zirconium (Zr), and hafnium (Hf). Examples of the ductile metal include gold (Au), silver (Ag), copper (Cu), and nickel (Ni). Examples of the brazing material include Au-Ni-Ti alloys.
[0032] The cutting tool 10 can be applied to various cutting tools known in the art. Suitable examples of such cutting tools include cutting tools for turning or milling, end mills, and reamers. The cutting tool 10 is a cutting tool in a broad sense, and refers to all tools used for turning, milling, and the like. EXAMPLES
[0033] In the following experiments, the ceramic sintered bodies of Examples 1 to 10 and Comparative Examples 1 to 4 were produced, and the ceramic sintered bodies were processed to produce the cutting tools of Examples 1 to 10 and Comparative Examples 1 to 4.
[0034] 1. Preparation of sintered ceramics (1) Raw materials The following raw material powders were used: Alumina powder (Al2O3 powder): average particle size 0.5μm Tungsten carbide powder (WC powder): average particle size 0.5 μm Zirconia powder (ZrO2 powder): average particle size 0.5μm Cobalt powder (Co powder): average particle size 0.5 μm
[0035] (2) Preparation of mixed dry powder Alumina powder, tungsten carbide powder, zirconia powder, and cobalt powder were prepared. Each raw material powder was weighed out to the ratio shown in Table 1, and was put into a ball mill together with a solvent and a dispersant to obtain a slurry by mixing and grinding. Ethanol or the like was used as the solvent. Florene G-700 (manufactured by Kyoeisha Chemical Co., Ltd.), SN Dispersant 9228 (manufactured by San Nopco Ltd.), Marialim AKM-0531 (manufactured by NOF Corporation), or the like was used as the dispersant. The obtained slurry was deaerated while being heated in a hot water bath to remove the solvent from the slurry. The powder was then passed through a sieve to produce a mixed powder. The steps (1) and (2) described above are common to all of the ceramic sintered bodies of the Examples and Comparative Examples.
[0036] (3) Firing (3-1) Ceramic sintered bodies of Examples 1 to 10 and Comparative Example 1 The ceramic sintered bodies of Examples 1 to 10 and Comparative Example 1 were obtained by hot press firing in the following manner. That is, the obtained mixed dry powder was put into a carbon jig and hot-pressed and fired at the firing temperature shown in Table 1 to produce a ceramic sintered body. The firing time was 45 minutes to 1.5 hours, the pressure was 20 MPa to 40 MPa, and the atmospheric gas was argon (Ar). The mixed dry powder was held at the holding temperature shown in Table 1, the pressure was 20 MPa to 40 MPa, and the atmospheric gas was argon (Ar), for 10 minutes to 60 minutes during the heating period before reaching the firing temperature. In this manner, the ceramic sintered bodies of Examples 1 to 10 and Comparative Example 1 were obtained. (3-2) Ceramic sintered bodies of Comparative Examples 2 to 4 For the ceramic sintered bodies of Comparative Examples 2 to 4, conventional hot press sintering was used, in which no holding was performed in a specific temperature range during heating before reaching the firing temperature. In addition, "no holding" in the "holding temperature" column in Table 1 means "no holding in a specific temperature range during heating before reaching the firing temperature." In this manner, the ceramic sintered bodies of Comparative Examples 2 to 4 were obtained.
[0037] [Table 1]
[0038] 2. XRD analysis (X-ray diffraction analysis) (1)Measurement method The ceramic sintered body was measured by X-ray diffraction using Cu-Kα radiation with a 2θ / θ focusing optical system to obtain an X-ray diffraction pattern. The measurement conditions were as follows: X-ray Diffraction Equipment Rigaku Corporation X-ray Diffraction System RINT-TTR III X-ray diffraction conditions Output: 45kV, 200mA Scan speed: 2° / min Step width: 0.02° 2θ measurement range: 20°~80°
[0039] (2) X-ray diffraction pattern When the X-ray diffraction patterns of the ceramic sintered bodies of Examples 1 to 10 were analyzed, it was found that they satisfied the conditions 1 and 2 described in the embodiment. That is, the ceramic sintered bodies of Examples 1 to 10 showed diffraction patterns in which the crystal structure of the composite carbide in the ceramic sintered body was only hexagonal. The ceramic sintered body of Comparative Example 1 does not contain cobalt in the raw material, that is, the ceramic sintered body does not have a composite carbide formed therein. In the ceramic sintered body of Comparative Example 1, no diffraction peak derived from the composite carbide in the ceramic sintered body was confirmed. The ceramic sintered bodies of Comparative Examples 2 to 4 are ceramic sintered bodies that were not held in a specific temperature range during heating before reaching the firing temperature. When the X-ray diffraction patterns of the ceramic sintered bodies of Comparative Examples 2 to 4 were analyzed, they satisfied condition 1 described in the embodiment, but did not satisfy condition 2. That is, the ceramic sintered bodies of Comparative Examples 2 to 4 showed diffraction patterns in which the crystal structure of the composite carbide in the ceramic sintered body was only cubic. In the "Crystal Structure" column of Table 1, "Hexagonal" indicates that the crystalline structure of the composite carbide in the ceramic sintered body is only hexagonal, and "Cubic" indicates that the crystalline structure of the composite carbide in the ceramic sintered body is only cubic. In Comparative Example 1, no diffraction peak derived from the composite carbide was detected, and thus it is indicated as "-".
[0040] (3) X-ray diffraction intensity ratio of composite carbides The X-ray diffraction intensity IA of the (002) plane of tungsten carbide and the X-ray diffraction intensity IB of the composite carbide were measured. Each X-ray diffraction intensity IA and IB was determined as the peak height at the following 2θ values. X-ray diffraction intensity IA: Peak height at 2θ = 65.0° to 66.0° X-ray diffraction intensity IB: the height of the higher peak between the peak in the vicinity of 2θ=41.0° to 42.0° and the peak in the vicinity of 2θ=42.1° to 43.0° For each ceramic sintered body, the X-ray diffraction intensities IA and IB were obtained, and the peak intensity ratio (IB / IA×100) was calculated.
[0041] The calculated peak intensity ratios are shown in Table 1. In Comparative Example 1, no diffraction peak derived from the composite carbide was detected, and therefore the peak intensity ratio was not calculated. Of the ceramic sintered bodies of Examples 1 to 10, the ceramic sintered bodies of Examples 2, 4 to 7, and 9 had a value of IB / IA×100 of 9.0 or more and 24.5 or less.
[0042] 3. Existence of complex carbides on grain boundaries (1)Measurement method The surface of the ceramic sintered body was observed by STEM, and the grain boundaries, which are the interfaces where two tungsten carbide crystal grains are adjacent, were measured by EDS line analysis. Five such grain boundaries were randomly selected, and it was confirmed whether composite carbides were observed. If composite carbides were observed at any of the five selected grain boundaries, it was determined that "composite carbides exist at the grain boundaries, which are the interfaces where two tungsten carbide crystal grains are adjacent," and if composite carbides were not observed at at least one of the five selected grain boundaries, it was determined that "composite carbides do not exist at the grain boundaries, which are the interfaces where two tungsten carbide crystal grains are adjacent."
[0043] (2) Measurement results The measurement results are shown in the "Grain boundary presence of composite carbides" column in Table 1. In the "Grain boundary presence of composite carbides" column, "present" indicates that "composite carbides are present at the grain boundary, which is the interface between two adjacent tungsten carbide crystal grains," and "absent" indicates that "composite carbides are not present at the grain boundary, which is the interface between two adjacent tungsten carbide crystal grains." Of the ceramic sintered bodies of Examples 1 to 10, in the ceramic sintered bodies of Examples 1 to 4, 6, 7, and 9, it was observed that composite carbides were present at the crystal grain boundaries, which are the interfaces between two adjacent tungsten carbide crystal grains.
[0044] 4.Cutting test (1) Test method Cutting tools were produced from the ceramic sintered bodies of Examples 1 to 10 and Comparative Examples 1 to 4. Using each cutting tool, a cutting test was carried out to evaluate chipping resistance and fracture resistance. The test conditions were as follows. ·Tool shape: TNGA160408Z01225 ·Work material: High hardness material (SCM415) ·Cutting speed: 300m / min Depth of cut: 0.1mm Feed rate: 0.2mm / rev. ·Cutting environment: DRY
[0045] (2) Test results The test results are shown in Table 1 and will be discussed below. The cutting tools of Examples 1 to 10 satisfy the following first requirement. In contrast, the cutting tools of Comparative Examples 1 to 4 do not satisfy the first requirement. The cutting tools of Examples 1 to 10 did not suffer chipping at the cutting edge even after machining for 2 km. Furthermore, the cutting tools of Examples 1 to 10 did not suffer chipping at the cutting edge even after machining for 3 km. The cutting tools of Comparative Examples 1 to 4 suffered chipping at the cutting edge after machining for a maximum of 1.5 km. Furthermore, the cutting tools of Comparative Examples 1 to 4 suffered chipping and could not machine for a maximum of 3 km. Thus, the cutting tools of Examples 1 to 10 had higher chipping resistance and fracture resistance than the cutting tools of Comparative Examples 1 to 4. [First requirement]: The X-ray diffraction pattern obtained by measuring the ceramic sintered body by X-ray diffraction shows a diffraction pattern in which the crystal structure of the composite carbide in the ceramic sintered body is only hexagonal.
[0046] Next, the cutting tools of Examples 1 to 10 will be compared. The cutting tools of Examples 2, 4, 6, and 9 all satisfied the following requirements 2, 3, and 4 in addition to the first requirement. The cutting tools of Examples 2, 4, 6, and 9 showed the best chipping resistance, with no chipping even after machining for 3 km. Therefore, it was confirmed that chipping resistance is further improved by satisfying the second, third, and fourth requirements in addition to the first requirement. The cutting tool of Example 1, which satisfied the first and second requirements, exhibited better chipping resistance than the cutting tool of Example 10, which satisfied only the first requirement. The cutting tool of Example 5, which satisfied the first and third requirements, exhibited better chipping resistance than the cutting tool of Example 10, which satisfied only the first requirement. The cutting tool of Example 8, which satisfied the first and fourth requirements, exhibited better chipping resistance than the cutting tool of Example 10, which satisfied only the first requirement. [Second requirement]: Composite carbides are present at the grain boundary, which is the interface between two adjacent tungsten carbide crystal grains. [Third requirement]: The ceramic sintered body is measured by X-ray diffraction. When the X-ray diffraction intensity of the (002) plane of tungsten carbide is taken as 100, the X-ray diffraction intensity of the composite carbide of tungsten and cobalt is 9.0 or more and 24.5 or less. [Fourth requirement]: In the ceramic sintered body, tungsten carbide is 21 volume % or more and 39 volume % or less, cobalt is 0.01 volume % or more and 0.15 volume % or less, zirconia is 0.50 volume % or more and 0.90 volume % or less, and alumina accounts for the remainder. Note that, as explained in the embodiment, each volume % is expressed in terms of compound for tungsten carbide, alumina, and zirconia, and is calculated assuming that cobalt exists as a simple substance. Table 1 shows the composition (mixture) of the raw material powder of the ceramic sintered body as described above, but this composition is equivalent to the composition of each ceramic sintered body converted into a compound.
[0047] The cutting tool of Comparative Example 1, which did not contain composite carbide, experienced chipping at the cutting edge during machining, resulting in breakage. The cutting tool of Comparative Example 2 satisfied the second and third requirements, but chipping occurred at the cutting edge during machining, resulting in breakage. The cutting tool of Comparative Example 3 satisfied the fourth requirement, but chipping occurred at the cutting edge during machining, resulting in breakage. The cutting tool of Comparative Example 4 satisfied the third and fourth requirements, but chipping occurred at the cutting edge during machining, resulting in breakage.
[0048] From the above results, it was confirmed that a cutting tool that satisfies the first requirement has good chipping resistance and fracture resistance.
[0049] The present invention is not limited to the above-described embodiments, and various modifications and variations are possible within the scope of the claims of the present invention. [Explanation of symbols]
[0050] 1. Sintered ceramics 10...Cutting tools 11 ... Pedestal
Claims
1. A cutting tool made of a ceramic sintered body containing tungsten carbide, alumina, and zirconia, The ceramic sintered body contains a composite carbide of tungsten and cobalt, The composite carbide can have a hexagonal crystal structure, The X-ray diffraction pattern obtained by measuring the ceramic sintered body by X-ray diffraction shows a diffraction pattern in the case where the crystal structure of the composite carbide in the ceramic sintered body is only a hexagonal crystal, The ceramic sintered body is measured by X-ray diffraction, and when the X-ray diffraction intensity of the (002) plane of tungsten carbide is taken as 100, the X-ray diffraction intensity of the composite carbide of tungsten and cobalt is 9.0 or more and 24.5 or less.
2. 2. The cutting tool according to claim 1, wherein the composite carbide is present at a grain boundary, which is an interface between two adjacent tungsten carbide crystal grains.
3. 3. A cutting tool comprising a base made of cemented carbide and the ceramic sintered body according to claim 1 or 2 joined to the base via a brazing material, the cutting tool having a coating layer formed on the surface thereof.
Citation Information
Patent Citations
Ceramic member and cutting tool
JP2016113320A
Sintered ceramic bodies and applications thereof
US20170334788A1
Sintered ceramic body
WO2014002743A1
Ceramic composition and cutting tool
WO2015019391A1