Cutting Tools

A cutting tool with a sintered body of alumina, zirconia, and tungsten carbide, optimized for wear and fracture resistance, addresses the inefficiencies of conventional tools by enhancing the cutting efficiency of ferrous metals through controlled composition and coating.

JP7556772B2Active Publication Date: 2024-09-26NTK CUTTING TOOLS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020209993
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-09-26
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Conventional cutting tools face challenges in wear resistance and chipping resistance when machining ferrous metals at high speed or deep cuts, necessitating improvements in cutting efficiency.

Method used

A cutting tool composed of a sintered body containing alumina, zirconia, and tungsten carbide, with specific mole fractions and peak intensity ratios, and optionally coated with materials like TiN, TiAlCrN, and AlCrN, to enhance wear and fracture resistance.

Benefits of technology

The cutting tool exhibits improved wear resistance and fracture resistance by optimizing the distribution of Zr elements at grain boundaries and controlling the peak intensity ratio, ensuring reduced reaction with iron in the workpiece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556772000006
    Figure 0007556772000006
  • Figure 0007556772000005
    Figure 0007556772000005
  • Figure 0007556772000004
    Figure 0007556772000004
Patent Text Reader

Abstract

To improve abrasion resistance and chipping resistance of a cutting tool.SOLUTION: A cutting tool 1 is a cutting tool that is composed of a sintered body containing alumina, zirconia and tungsten carbide. The sintered body 2 contains at least one metal carbide selected from Ti, Zr, Hf, V, Nb and Ta elements, and a W element is dissolved in the metal carbide. When a molar fraction of the total of W, Ti, Zr, Hf, V, Nb and Ta elements in the total carbides contained in the sintered body 2 is 100%, the molar fraction of the W element is the largest. When the sintered body 2 is measured by X-ray diffraction, strongest peak intensity of the tungsten carbide is represented by IA, and strongest peak intensity of the metal carbide is represented by IB, a value of a peak intensity ratio (IA / IB) is 1.00 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to cutting tools. [Background technology]

[0002] Conventional cutting tools have been designed to have improved fracture resistance by increasing their strength (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2014 / 002743 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, cutting tools are required to perform cutting with higher efficiency. In order to perform cutting of ferrous metals such as steel with higher efficiency, at least one of increasing the cutting speed and the depth of cut has been taken. However, when cutting ferrous metals at high speed or large depth of cut, conventional cutting tools are required to have improved wear resistance and chipping resistance. The present disclosure has been made in view of the above circumstances, and has an object to provide a cutting tool having improved wear resistance and chipping resistance even when a workpiece is an iron-based metal. The present disclosure can be realized in the following forms. [Means for solving the problem]

[0005] [1] A cutting tool made of a sintered body containing alumina, zirconia, and tungsten carbide, The sintered body contains at least one metal carbide selected from Ti, Zr, Hf, V, Nb, and Ta elements, The metal carbide contains W as a solid solution. When the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in all carbides contained in the sintered body is taken as 100%, the molar fraction of W element is the largest, The sintered body is measured by X-ray diffraction, The strongest peak intensity of the tungsten carbide is defined as IA, When the strongest peak intensity of the metal carbide is IB, A cutting tool having a peak strength ratio (IA / IB) of 1.00 or less.

[0006] [2] The cutting tool according to [1], in which Zr elements are distributed at a grain boundary, which is the interface between two alumina crystal grains, and at a grain boundary, which is the interface between an alumina crystal grain and a tungsten carbide crystal grain.

[0007] [3] The cutting tool according to [1] or [2], wherein the sintered body contains at least one selected from Co, Fe, and Ni in a total amount of 5.0 mol % or less.

[0008] [4] A cutting tool according to any one of [1] to [3], having a coating layer formed on the surface. Effect of the Invention

[0009] When the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in all carbides contained in the sintered body is taken as 100%, the molar fraction of W element is the largest and the peak intensity ratio (IA / IB) value is 1.00 or less, thereby providing the cutting tool with excellent wear resistance and chipping resistance. When Zr element is distributed at a grain boundary, which is the interface between two alumina crystal grains, and at a grain boundary, which is the interface between an alumina crystal grain and a tungsten carbide crystal grain, the grain boundary is strengthened, and the wear resistance and chipping resistance of the cutting tool are improved. When the steel contains at least one selected from Co, Fe, and Ni in a total amount of 5.0 mol % or less, the wear resistance and chipping resistance of the cutting tool are improved. When a coating layer is formed on the surface, the wear resistance of the cutting tool is improved. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view of an example of a cutting tool. [Diagram 2] 1 is a graph showing temperature changes during the firing process in Examples 1 to 13. [Diagram 3] 13 is a graph showing temperature changes in a firing step in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present disclosure will be described in detail below. In this specification, a description using "~" for a numerical range includes the lower limit and the upper limit unless otherwise specified. For example, the description "10 to 20" includes both the lower limit "10" and the upper limit "20". In other words, "10 to 20" has the same meaning as "10 or more and 20 or less".

[0012] 1.Cutting tool 1 The cutting tool 1 is made of a sintered body 2 containing alumina (Al2O3), zirconia (ZrO2), and tungsten carbide (WC). The sintered body 2 contains at least one metal carbide selected from the group consisting of Ti, Zr, Hf, V, Nb, and Ta elements. W element is dissolved in the metal carbide. In cutting tool 1, the molar fraction of W element is the largest when the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in all carbides contained in sintered body 2 is taken as 100%. In the cutting tool 1, the sintered body 2 is measured by X-ray diffraction, and when the strongest peak intensity of tungsten carbide is defined as IA and the strongest peak intensity of metal carbide is defined as IB, the peak intensity ratio (IA / IB) is 1.00 or less.

[0013] (1) Components contained in the sintered body and the content of each component The sintered body 2 contains alumina, zirconia, and tungsten carbide. The content of each component will be described below. The following contents are amounts when the entire sintered body 2 (cutting tool 1) is taken as 100 mol %. The alumina content is not particularly limited, but is preferably 10 mol % to 55 mol % from the viewpoints of hardness and sinterability. The content of zirconia is not particularly limited, but from the viewpoint of chipping resistance, the content of zirconia is preferably 3 mol % to 5 mol %. The content of tungsten carbide is not particularly limited, but the content of tungsten carbide in the sintered body 2 converted into carbide is preferably 20 mol % to 45 mol % from the viewpoints of hardness and sinterability.

[0014] The sintered body 2 contains at least one metal carbide selected from the group consisting of Ti (titanium), Zr (zirconium), Hf (hafnium), V (vanadium), Nb (niobium), and Ta (tantalum). In the present disclosure, the metal carbide refers to both a compound consisting of one of the above elements and carbon, and a compound consisting of two or more of the above elements and carbon. The compounds consisting of one of the above elements and carbon are titanium carbide, zirconium carbide, hafnium carbide, vanadium carbide, niobium carbide, and tantalum carbide. The compounds consisting of two or more of the above elements and carbon are titanium carbide, zirconium carbide, hafnium carbide, vanadium carbide, niobium carbide, and tantalum carbide. The compound is not particularly limited, but examples thereof include titanium tantalum carbide and titanium zirconium carbide.

[0015] Metal carbide contains dissolved W (tungsten) elements. When W elements are dissolved in metal carbide, the amount of plain tungsten carbide can be reduced according to the amount of dissolved W elements without reducing the amount of W elements in the sintered body 2. This reduces the amount of plain tungsten carbide, which is easily reactive with iron contained in the workpiece, and improves the reactivity resistance to iron. The content of the metal carbide is not particularly limited. From the viewpoint of ensuring the amount of W element in solid solution, the content of the metal carbide is preferably 30 mol % to 80 mol %, and more preferably 15 mol % to 40 mol %. The amount of W element dissolved in the metal carbide is not particularly limited as long as it satisfies the requirement of the peak intensity ratio (IA / IB) described later. A method for dissolving a predetermined amount of W element in the metal carbide will be described later.

[0016] (2) Requirements for the ratio of W element in carbides In the sintered body 2, the molar fraction of W element is the largest when the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in all carbides contained in the sintered body 2 is taken as 100%. In other words, the ratio of W element to metal elements in all carbides is higher than the ratios of Ti, Zr, Hf, V, Nb, and Ta elements. All carbides contained in the sintered body 2 are tungsten carbide, metal carbides, and solid solutions thereof. The ratio of the W element to the metal elements in all carbides is not particularly limited. From the viewpoint of chipping resistance, the ratio of the W element to the metal elements in all carbides is preferably 46% or more, more preferably 50% or more, and even more preferably 53% or more. From the viewpoint of reactivity resistance to iron contained in the workpiece, the ratio of the W element to the metal elements in all carbides is preferably 77% or less, more preferably 70% or less, and even more preferably 65% ​​or less. From these viewpoints, the ratio of the W element to the metal elements in all carbides is preferably 46% or more and 77% or less, more preferably 50% or more and 70% or less, and even more preferably 53% or more and 65% or less. The composition (mixture) of the raw material powder of the sintered body 2 hardly changes even after sintering, and is therefore equivalent to the composition of each sintered body 2. The ratio of W element to the metal elements in all carbides can be adjusted by appropriately changing the composition (mixture) of the raw material.

[0017] (3) Peak intensity ratio (IA / IB) requirements Here, the requirements for the peak intensity ratio (IA / IB) will be explained. The peak intensity IA represents the intensity of the peak that exhibits the highest intensity among the XRD peaks of tungsten carbide measured by an X-ray diffractometer using Cu-Kα radiation. For example, the peak height at about 2θ=35.6° is preferably used. The peak intensity IB represents the intensity of the peak that shows the highest intensity among the XRD peaks of the metal carbide measured by an X-ray diffractometer using Cu-Kα radiation. For example, the strongest peak When the metal carbide exhibiting the above formula is titanium carbide, the peak height at about 2θ=41.7° is preferably used.

[0018] The peak intensity ratio (IA / IB) is 1.00 or less. The peak intensity ratio (IA / IB) being 1.00 or less indicates that the amount of pure tungsten carbide, which easily reacts with the iron contained in the workpiece, is less than a certain amount in the total carbides. From the viewpoint of wear resistance, the value of the peak intensity ratio (IA / IB) is preferably 0.70 or less, more preferably 0.45 or less. The lower limit of the peak intensity ratio (IA / IB) is not particularly limited, but is usually 0.20, and may be a value closer to "0". The method for controlling the peak intensity ratio (IA / IB) will be described later.

[0019] (4) Distribution of Zr element In the cutting tool 1, Zr elements may be distributed in a grain boundary (hereinafter also referred to as grain boundary A) which is an interface between two alumina crystal grains and a grain boundary (hereinafter also referred to as grain boundary B) which is an interface between an alumina crystal grain and a tungsten carbide crystal grain. That is, Zr elements are preferably distributed in both grain boundary A and grain boundary B.

[0020] The presence of Zr element at grain boundary A can be confirmed as follows. The interface between two adjacent alumina crystal grains is observed with a Scanning Transmission Electron Microscope (STEM). The concentration of Zr element is measured by an Energy Dispersive X-ray Spectrometer (EDS) as it crosses this interface. If Zr element is present at the grain boundary, a peak of high Zr element concentration is observed at the interface.

[0021] The presence of Zr element at grain boundary B can be confirmed as follows. That is, the interface where an alumina crystal grain and a tungsten carbide crystal grain are adjacent is observed with a scanning transmission electron microscope. The concentration of Zr element is measured by an energy dispersive X-ray spectrometer as it crosses this interface. If Zr element is present at the grain boundary, a peak of high concentration of Zr element is observed at the interface.

[0022] In the sintered body 2 as one embodiment, the Zr element distributed in the grain boundaries A and B can improve the bonding strength between the crystal grains at each of the grain boundaries A and B. This improves the mechanical properties of the alumina-tungsten carbide-zirconia ceramic composition, and as a result, the wear resistance and chipping resistance thereof can be improved.

[0023] In order to distribute the Zr element to the grain boundaries A and B, each component may be thoroughly dispersed by a method such as ball mill grinding during the manufacture of the sintered body 2. For example, if fine zirconia powder or a zirconium salt solution is used as the zirconia raw material, the zirconium element is effectively distributed to the grain boundaries. In addition, it is also effective to use a dispersion mixing process in which only the zirconia raw material is first ground, or to use zirconia as the grinding media. In addition, the movement (diffusion) of Zr elements can be promoted by optimizing the heating rate and holding time during firing.

[0024] (5) Other ingredients The sintered body 2 may contain at least one selected from Co, Fe, and Ni in a total amount of 5.0 mol % or less. The sintered body 2 contains Co, Fe, and Ni, which improves the wear resistance and chipping resistance. Although the reason is unclear, it is speculated that the bonding strength between metal carbide crystal particles can be improved by metals such as Co, Fe, and Ni being precipitated in layers at the grain boundaries between metal carbide crystal particles. On the other hand, if the total content of Co, Fe, and Ni is more than 5.0 mol%, there will be more metal phases that are easily softened at high temperatures as phases other than the grain boundaries, which may reduce the wear resistance. The sintered body 2 as one embodiment contains at least one selected from Co, Fe, and Ni in a total amount of 5.0 mol % or less, thereby ensuring wear resistance and improving fracture resistance.

[0025] (6) Covering layer The cutting tool 1 may have a coating layer formed on its surface. The coating layer is preferably made of at least one carbide, nitride, oxide, carbonitride, carbonate, oxynitride, or oxycarbonitride selected from the group consisting of titanium (Ti), zirconium (Zr), silicon (Si), chromium (Cr), and aluminum (Al). Specifically, TiN, Ti AlN, TiAlCrN, and AlCrN are preferred. When the coating layer is formed, the surface hardness of the cutting tool 1 increases, and the progress of wear caused by reaction and adhesion with the work material is suppressed. As a result, the wear resistance of the cutting tool 1 is improved. The coating layer may be a single layer or multiple layers, and the total thickness is: Although there are no particular limitations, it is usually 0.5 μm to 15 μm.

[0026] 2. Control of peak intensity ratio (IA / IB) (manufacturing method of cutting tool 1) The peak intensity ratio (IA / IB) can be controlled by adjusting the amount of W element dissolved in the metal carbide in the process of manufacturing the cutting tool 1. The cutting tool 1 is manufactured through a raw material powder preparation process, a compounding process, a mixing process, a drying and granulating process, and a firing process. The amount of W element dissolved in the metal carbide can be adjusted, for example, by using a solid solution raw material in which W element is dissolved in the metal carbide as the raw material powder in the blending process of the raw material powder, and by controlling the heating conditions of hot pressing, spark plasma sintering (SPS), etc. in the firing process of the raw material powder. This will be explained in more detail below.

[0027] (1) Preparation and mixing of raw powder The solid solution raw material used in the raw material powder blending step can be prepared as follows. First, at least one metal powder selected from Ti, Zr, Hf, V, Nb, and Ta elements, W element powder, and C element powder are mixed and pulverized in a ball mill or the like. The resulting mixed powder is heated and carbonized. For cooling after carbonization, rapid cooling faster than the normal furnace cooling speed is preferable.

[0028] When preparing a solid solution raw material, a homogeneous solid solution raw material can be obtained by using a metal powder and a powder of W element as the starting raw material for the carbide. This is because the metal element and W element can be mixed homogeneously, and the combustion reaction accompanying the carbonization reaction of the metal element and W element promotes the solid solution reaction. In addition, rapid cooling after carbonization can suppress the separation of WC. In general, the lower the temperature, the less the amount of W element that dissolves in other metal carbides. Therefore, by rapidly cooling to shorten the time it takes for WC separation to occur, the separation of WC can be suppressed compared to cooling at the normal furnace cooling rate.

[0029] The amount of the obtained solid solution raw material is not particularly limited, but is preferably 30 mol % to 80 mol %, and more preferably 15 mol % to 40 mol %, when the entire raw materials of the sintered body 2 are taken as 100 mol %.

[0030] (2) Firing process Conventionally, when manufacturing the sintered body 2, a sintering process has been adopted in which sintering is performed at a predetermined sintering temperature under a predetermined press pressure, and the temperature is decreased from the sintering temperature at a predetermined temperature decrease rate. The predetermined temperature decrease rate is usually 2.5°C / min to 5.0°C / min. In contrast, by increasing the temperature decrease rate from the sintering temperature, it is possible to suppress separation of WC from the metal carbide in which the W element is dissolved. In order to ensure the amount of W element dissolved in the metal carbide, the temperature decrease rate from the sintering temperature is preferably 15°C / min or more, and more preferably 20°C / min or more.

[0031] 3. Possible reasons for superior wear resistance and fracture resistance Here, the reason why it is believed that the cutting tool 1 of the present disclosure has excellent wear resistance and fracture resistance will be described. Generally, tungsten carbide has a tendency to react with iron. Therefore, in order to improve the reactivity between a sintered body containing tungsten carbide and the iron contained in the workpiece, the amount of tungsten carbide in the sintered body can be reduced. However, this reduces the amount of W element in the sintered body, resulting in insufficient mechanical strength of the sintered body. A cutting tool made of such a sintered body has excellent wear resistance but poor chipping resistance. In contrast, the sintered body 2 of the present embodiment has improved reactivity resistance to iron contained in the work material, since the W element is dissolved in the metal carbide, compared with a configuration in which the W element is not dissolved in the metal carbide. Accordingly, it is considered that the cutting tool 1 has excellent chipping resistance and improved wear resistance. The sintered body 2 of the present embodiment satisfies the above-mentioned requirement regarding the ratio of W element in the carbide, and therefore the W element is sufficiently secured. Therefore, it is considered that the sintered body 2 has excellent mechanical strength, and the cutting tool 1 has excellent chipping resistance. Furthermore, the sintered body 2 of this embodiment also satisfies the requirement of the peak intensity ratio (IA / IB). Since the value of the peak intensity ratio (IA / IB) is 1.00 or less, the amount of simple tungsten carbide that easily reacts with iron in the work material can be reduced. As a result, the reactivity resistance of the sintered body 2 to iron contained in the work material is improved, and the wear resistance of the cutting tool 1 is improved. Thus, the sintered body 2, which satisfies the above-mentioned requirements regarding the proportion of W element in the carbide and also satisfies the requirements for the peak intensity ratio (IA / IB), can be subjected to the treatment without reducing the amount of W element. Since it is possible to improve the resistance to reactivity with iron contained in the cutting material, it has excellent wear resistance and chipping resistance. EXAMPLES

[0032] In the following experiments, sintered bodies of Examples 1 to 13 and Comparative Examples 1 to 4 were produced, and these ceramic sintered bodies were processed into cutting tools of Examples 1 to 13 and Comparative Examples 1 to 4.

[0033] 1. Preparation of sintered body (1) Preparation of raw powder The raw material powders are as follows: (Ti,W)C powder, (Zr,W)C powder, (V,W)C powder, (Nb,W)C powder, (Ta,W)C powder, and (Ti,Ta,W)C powder are solid solution raw material powders. Al2O3 powder: average particle size 0.3μm ZrO2 powder: average particle size 0.3μm, partially stabilized with 3mol% Y2O3 WC powder: average particle size 0.5μm (Ti,W)C powder: average particle size 0.7μm (Zr,W)C powder: average particle size 0.7μm (V,W)C powder: average particle size 0.7μm (Nb,W)C powder: average particle size 0.7μm (Ta,W)C powder: average particle size 0.7μm (Ti,Ta,W)C powder: average particle size 0.7μm TiC powder: average particle size 0.7μm

[0034] Of the above, Al2O3 powder, ZrO2 powder, and WC powder were used as commercially available raw materials. Solid solution raw materials such as (Ti,W)C powder were prepared using the following procedure. First, Ti powder, Zr powder, V powder, Nb powder, Ta powder, and W powder with an average particle size of 1.0 μm and C powder (carbon black) with an average particle size of 0.3 μm were mixed to the composition (mol%) shown in Table 1. Carbide balls and ethanol were placed in a SUS pot, and the mixed powder was then added. Next, the SUS pot was rotated for 48 hours to grind and mix the powder.

[0035] [Table 1]

[0036] The resulting mixed slurry was dried in a vibration dryer to obtain a mixed powder. The resulting mixed powder was placed in a carbon mold and carbonized at 2,000°C in an Ar atmosphere. The temperature was reduced from 2,000°C by rapid cooling. Powder X-ray diffraction analysis of the resulting powder confirmed that the W element was a solid solution raw material in which the W element was dissolved in the carbides of the other elements. (2)Blending process The prepared raw material powders were mixed (blended) to obtain the composition (mol %) shown in Table 2. In addition, in Table 3, "Use of solid solution raw materials" means that "solid solution raw materials were used as raw materials."

[0037] [Table 2]

[0038] (3) Mixing, drying and granulation process The cemented carbide balls and ethanol were placed in a stainless steel pot, and the mixed raw powder was then placed in the pot. The stainless steel pot was then rotated for 72 hours to pulverize and mix the materials. The resulting mixed slurry was dried in a vibration dryer to obtain a mixed powder. The above steps ((1) to (3)) are common to all of the ceramic sintered bodies of the Examples and Comparative Examples.

[0039] (4) Firing process (4-1) Ceramic sintered bodies of Examples 1 to 13 and Comparative Examples 1, 2, and 4 The ceramic sintered bodies of Examples 1 to 13 and Comparative Examples 1, 2, and 4 were obtained by hot-press firing using the following method. That is, the dry mixed powder was put into a carbon jig and sintered under the conditions of the sintering temperature, the press pressure of 30 MPa, and the atmosphere of Ar of 3 atmospheres in Table 3. When the temperature was lowered from the sintering temperature, it was rapidly cooled. A typical temperature change during this hot press firing is shown in Figure 2. Figure 2 shows the state in which the temperature is lowered at 20°C / min after being held at the firing temperature (1500°C) for a specified time. In this manner, the ceramic sintered bodies of Examples 1 to 13 and Comparative Examples 1, 2, and 4 were obtained. In Table 3, "Quick cooling during firing" means "Quick cooling was performed when the temperature was lowered from the firing temperature." Also, "No" means "Quick cooling was not performed when the temperature was lowered from the firing temperature."

[0040] [Table 3]

[0041] (4-2) Ceramic sintered body of Comparative Example 3 The ceramic sintered body of Comparative Example 3 was dried and granulated in the same manner as the ceramic sintered bodies of Examples 1 to 13 and Comparative Examples 1, 2, and 4, but was not cooled rapidly from the firing temperature but at a normal rate. The temperature change during this hot press firing is shown in Figure 3. After firing, uniaxial pressure of 1550°C and 800 MPa is applied. Figure 3 shows the state in which the temperature is lowered at 2.5°C / min after being held at the firing temperature (1525°C) for a specified time. In this manner, the ceramic sintered body of Comparative Example 3 was obtained.

[0042] 2. W element ratio (1) Calculation method After mirror polishing the cut surface at any position of the sintered body, EPMA images with a field of view of 25 μm were obtained at five different points on the cut surface using an electron probe microanalyzer (EPMA). The EPMA images were analyzed to calculate the average value of the molar fractions of W, Ti, Zr, Hf, V, Nb, and Ta elements in the sintered body at the five points. The molar fraction of W element was calculated by taking the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements contained in the sintered body as 100%. In addition, a composition analysis was performed by XRD analysis separately, and the calcined samples of the examples and comparative examples were It was confirmed that the composition of the sintered body did not change before and after the treatment. (2) Calculation results Table 3 shows the proportion of W element in the examples and comparative examples. The molar fraction of W element was 50% or more in all of Examples 1 to 13 and Comparative Examples 1 to 3. The molar fraction of W element in Examples 1 to 13 and Comparative Examples 1 to 3 was the largest when the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in the carbide contained in the sintered body was taken as 100%, and satisfied the requirement for the ratio of W element in the carbide. The molar fraction of W element in Comparative Example 4 was 45.0%. When the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in the carbide contained in the sintered body was taken as 100%, the molar fraction of W element in Comparative Example 4 was less than the molar fraction of Ti element (55%), and did not satisfy the requirement regarding the ratio of W element in the carbide. In the composition of Comparative Example 4, the molar fraction of Ti element is larger than the molar fraction of W element in the carbide by adding the same amount of TiC powder raw material instead of the WC powder raw material in Example 3. The preparation method of Comparative Example 4 is the same as that of the Example.

[0043] 3. XRD analysis (X-ray diffraction analysis) (1)Measurement method The obtained sintered body was processed into a columnar body of 12 mm x 12 mm x 4 mm, and one of the 12 mm x 12 mm faces was polished to a mirror finish. The mirror surface was evaluated as follows. X-ray diffraction measurements were performed on each ceramic sintered body to measure the strongest peak intensity IA of tungsten carbide and the strongest peak intensity IB of metal carbide. Each peak intensity IA and IB is the height of the peak observed near the following 2θ values. Peak intensity IA: 2θ=35.6° Peak intensity IB: When the metal carbide showing the strongest peak is TiC, 2θ=41.7°, When the metal carbide showing the strongest peak is ZrC, 2θ=33.0°, When the metal carbide showing the strongest peak is VC, 2θ=37.4°, When the metal carbide showing the strongest peak is NbC, 2θ=34.8°, When the metal carbide showing the strongest peak is TaC, 2θ=35.0°, When the metal carbide showing the strongest peak is TiTaC, 2θ=35.3° For each sintered body, the peak intensities IA and IB were determined, and the peak intensity ratio IA / IB was calculated. The peak intensity of each surface was measured under the following conditions. X-ray Diffraction Equipment Rigaku Corporation X-ray Diffraction System RINT-TTR III X-ray diffraction conditions Monochromator: Used Target: Cu Tube current: 300mA Tube voltage: 50kV Scan speed: 2 degrees / min Sampling width 0.02 degrees

[0044] (2) Measurement results Table 3 shows the peak intensity ratios IA / IB in the examples and comparative examples. The peak intensity ratios IA / IB in Examples 1 to 13 were all 1.00 or less. The peak intensity ratio IA / IB of Comparative Example 1 was equal to or greater than 2 and greater than 1.00. The preparation method of Comparative Example 1 was the same as that of the Examples, but the composition of Comparative Example 1 did not contain any metal carbide other than WC in the carbide. The peak intensity ratio IA / IB of Comparative Example 2 was 1.44, which was larger than 1.00. The production method of Comparative Example 2 was the same as that of the Examples, but the composition of Comparative Example 2 had a larger amount of WC powder raw material blended than Examples 1-13. The peak intensity ratio IA / IB of Comparative Example 3 was 1.20, which was larger than 1.00. The composition of Comparative Example 3 was the same as that of Example 3, but in the production method of Comparative Example 3, rapid cooling was not performed when the temperature was lowered from the firing temperature.

[0045] 4. Fabrication of Cutting Tools The sintered bodies of Examples 1 to 13 and Comparative Examples 1 to 4 were machined into a tool shape (SEKN42). Since each sintered body was machined into a cutting tool after sintering, the composition of the cutting tool was the same as the composition of the raw material powder.

[0046] 5.Cutting test (1) Abrasion resistance test Cutting tests were carried out using each cutting tool under the following test conditions: ·Work material: Alloy steel SCM440 ·Cutting speed: 400m / min Depth of cut: 2.0mm Cutting width: 50mm Feed rate: 0.2mm / tooth ·Cutting environment: Dry Evaluation: The cutting distance (m) when the flank wear reached 0.3 mm was used for evaluation. (2) Fracture resistance test Cutting tests were carried out using each cutting tool under the following test conditions: ·Work material: Alloy steel SCM440 ·Cutting speed: 200m / min Depth of cut: 2.0mm~5.0mm Cutting width: 50mm Feed rate: 0.2mm / tooth ·Cutting environment: Dry Evaluation: The cutting depth was increased by 0.25 mm from 2.0 mm, and 0.5 m was machined each time the cutting depth was increased. The cutting depth at which defects occurred was used for evaluation. (3) Test results The results of the wear resistance test and the fracture resistance test in the examples and comparative examples are shown in Table 3. The cutting tools of Examples 1 to 13 exhibited good wear resistance and fracture resistance. The cutting tools of Comparative Examples 1 to 3, which satisfy the requirements regarding the ratio of elements but have a peak intensity ratio IA / IB greater than 1.00, have the same chipping resistance as the cutting tools of Examples 1 to 13, but have lower wear resistance. This is thought to be because the inclusion of a large amount of W element ensures mechanical strength, while the sintered body contains a large amount of simple WC, which makes it easy for the reaction with the iron of the workpiece to proceed. In addition, the cutting tool of Comparative Example 4, which has a peak intensity ratio IA / IB less than 1.00 but does not satisfy the requirements regarding the ratio of W element in the carbide, has the same wear resistance as the cutting tools of Examples 1 to 13, but has lower chipping resistance. This is thought to be because the sintered body contains a small amount of simple WC, which makes it difficult for the reaction with the iron of the workpiece to proceed, while the W element is insufficient, and mechanical strength is not ensured. From the above results, it was confirmed that the wear resistance and fracture resistance are improved by satisfying the requirements regarding the proportion of W element in the carbide and also the requirements regarding the peak intensity ratio (IA / IB).

[0047] The present disclosure is not limited to the above-described embodiments, and various modifications and variations are possible within the scope of the claims of the present disclosure. [Explanation of symbols]

[0048] 1...Cutting tools 2. Sintered body

Claims

1. A cutting tool made of a sintered body containing alumina, zirconia, and tungsten carbide, The sintered body contains at least one metal carbide selected from Ti, Zr, Hf, V, Nb, and Ta elements, The metal carbide contains W as a solid solution, When the total molar fraction of W, Ti, Zr, Hf, V, Nb, and Ta elements in all carbides contained in the sintered body is taken as 100%, the molar fraction of W element is the largest, The sintered body is measured by X-ray diffraction, The strongest peak intensity of the tungsten carbide is defined as IA, When the strongest peak intensity of the metal carbide is IB, The peak intensity ratio (IA / IB) is 1.00 or less, The sintered body comprises at least one element selected from the group consisting of Co, Fe, and Ni, in a total content of 5.0 mol % or less.

2. 2. The cutting tool according to claim 1, wherein Zr elements are distributed at a grain boundary which is an interface between two alumina crystal grains and at a grain boundary which is an interface between an alumina crystal grain and a tungsten carbide crystal grain.

3. 3. The cutting tool according to claim 1, further comprising a coating layer formed on the surface of the cutting tool.

Citation Information

Patent Citations

  • Surface coated cermet member for cutting tool

    JP1985149775A

  • Ti BASED CERMET, ITS PRODUCTION METHOD AND CUTTING TOOL

    JP2005272877A

  • Alumina-based ceramic sintered compact, cutting insert and cutting tool

    JP2010235351A

  • Ceramic member and cutting tool

    JP2016113320A

  • Sintered ceramic bodies and applications thereof

    US20170334789A1