Clad 2XXX Series Aerospace Products
The composite aerospace product with a 2XXX series core and 6XXX series cladding layer addresses the issues of softness and damage in 1XXX alloys by enhancing strength and formability, ensuring improved corrosion resistance and reduced surface damage.
Patent Information
- Application Number
- JP2022511388
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-22
- Filing Date
- 2020-07-27
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-07-27
AI Technical Summary
Existing 1XXX series aluminum alloys used as cladding layers in aerospace products are soft and prone to surface damage during handling and die sticking, compromising corrosion resistance and formability.
A composite aerospace product is developed with a 2XXX series core layer bonded to a 6XXX series aluminum alloy cladding layer, which provides improved hardness, formability, and corrosion resistance through optimized alloy compositions and manufacturing processes like roll bonding and homogenization.
The 6XXX series cladding layer enhances the product's strength, reduces die adhesion, and improves fatigue performance, allowing for thinner cladding layers while maintaining corrosion resistance and formability, suitable for aerospace applications.
Smart Images

Figure 0007556942000001 
Figure 0007556942000002
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of and priority to European Patent Application No. 19193108.8, entitled "CLAD2XXX-SERIES AEROSPACE PRODUCT," filed on August 22, 2019, the contents of which are incorporated herein by reference in their entirety. [Technical field]
[0002] The present invention relates to a rolled composite aerospace product comprising a 2XXX series core layer and an aluminum alloy layer bonded to at least one surface of the 2XXX series core layer. The rolled composite product is ideally suited for aerospace structural components. The present invention further relates to a method of making the rolled composite aerospace product. [Background technology]
[0003] In the aerospace industry, AA2024 series aluminum alloys and their modifications are widely used, mostly as T3-condition high-quality damage-tolerant aluminum alloys or their modifications. These aluminum alloy products have a relatively high strength to weight ratio, good fracture toughness, good fatigue properties, and adequate corrosion resistance.
[0004] For several decades already, to improve corrosion resistance, AA2024 series alloy products can be provided as composite products with a relatively thin cladding layer on one or both sides. The cladding layer is usually of higher purity to provide corrosion protection for the AA2024 core alloy. The cladding essentially comprises unalloyed aluminum. Often, general reference is made to the 1XXX series aluminum alloys, which include the 1000, 1100, 1200 and 1300 subclasses. However, in practice, the 1XXX series aluminum alloys used for the cladding layer are fairly highly pure, with a composition of Si+Fe<0.7%, Cu<0.10%, Mn<0.05%, Mg<0.05%, Zn<0.10%, Ti<0.03%, and the balance aluminum.
[0005] AA2024 series aluminum alloy clads with 1XXX series alloys can also be anodized. Anodizing increases resistance to corrosion and wear and provides better adhesion than bare metal for paint primers and adhesives. Anodized articles are applied in structural adhesive metal joints, for example in the exterior panels of wings, horizontal stabilizers, vertical stabilizers or fuselages. Further known applications include sandwich structures in which one or more (glass) fiber reinforced layers are interposed between aluminum panels or sheets using adhesive bonding, resulting in so-called fiber metal laminates. Patent document WO-2017 / 183965-A1 (Fokker) discloses a method for anodizing aluminum alloys for applying a porous anodic oxide coating in preparation for the subsequent application of adhesive bonding and / or primer layers.
[0006] A drawback of 1XXX series alloys as cladding layers is that these alloys are quite soft and sensitive to surface damage during handling of the product, and during forming operations this can result in, for example, die sticking. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] As understood hereinafter, unless otherwise indicated, the aluminum alloy and temper designations refer to the Aluminum Association designations in Aluminum Standards and Data and the Registration Records published by the Aluminum Association in 2018 and are familiar to those skilled in the art. The temper designations are also set forth in the European standard EN515.
[0008] For any description of the alloy compositions or preferred alloy compositions, all references to percentages are by weight percent unless otherwise indicated.
[0009] The terms "up to" and "up to about," as used herein, expressly include, but are not limited to, the possibility of zero weight percent of the particular alloying element to which it refers. For example, up to 0.20% Zn may include an aluminum alloy that has no Zn.
[0010] For purposes of this invention, sheet product or sheet material shall be understood as a rolled product having a thickness of 1.3 mm (0.05 inch) or more and 6.3 mm (0.25 inch) or less, and plate material or plate product shall be understood as a rolled product having a thickness of more than 6.3 mm (0.25 inch). See also Aluminum Standard and Data, the Aluminum Association, Chapter 5 Terminology, 1997.
[0011] It is an object of the present invention to provide clad rolled aerospace products which comprise 2XXX series alloys and which offer an improved balance of corrosion resistance and formability.
[0012] This and other objects, as well as further advantages, are met or exceeded by the present invention which provides a rolled composite aerospace product comprising a 2XXX series core layer, the core layer having two faces, and a 6XXX series aluminum alloy clad layer bonded to at least one surface of the 2XXX series core layer, wherein the 6XXX series aluminum alloy is comprised, by weight percent, of: Si 0.3%~1.0%, Mg 0.3%~1.1%, Mn 0.04%~1.0%, Fe 0.03%~0.4%, Cu max 0.10%, Cr max 0.25% V max 0.2%, Zr 0.2% max. Zn max 0.5% Ti max 0.15%, Incidental impurities include <0.05% each, <0.15% total, and the balance aluminum.
[0013] The 6XXX series alloys have very good forming properties, especially bendability and tensile formability, so that rolled composite aerospace products can be formed in forming operations requiring high deformation degrees. The forming properties are comparable to those of some automotive sheet aluminum alloys. Die sticking of the clad layer to the forming die is significantly reduced or even avoided due to the increased hardness of the clad layer compared to the 1XXX series clad layers. The 6XXX series alloys have very good surface quality after forming into a shaped product. The absence of surface cracks avoids the entrapment of any forming lubricant into the surface. The absence of surface cracks also significantly increases the fatigue performance of the rolled composite aerospace products. Also, the very good resistance to pitting improves fatigue performance, since fatigue is commonly caused by pitting initiation sites. The 6XXX series alloys have significantly higher strength than the 1XXX series alloys, resulting in a harder surface and a corresponding reduction in surface damage, such as scratches, during product handling. The 6XXX series alloys are significantly stronger than the 1XXX series alloys such that the overall strength of the composite aerospace product is increased compared to 1XXX series alloys of the same clad layer thickness. This also allows the design of rolled composite aerospace products with thinner clad layers while providing weight savings and still providing the required good corrosion resistance and improved forming properties. The 6XXX series alloys are extremely well anodizable such that subsequent application of adhesive bond and / or primer layers is problem-free.
[0014] In one embodiment, the 6XXX series aluminum alloy clad layer achieves a hardness of at least 55HB in the T4 temper. In one embodiment, the 6XXX series aluminum alloy clad layer achieves a hardness of at least 60HB, and preferably at least 65HB in the T4 temper.
[0015] In one embodiment, the 6XXX series aluminum alloy clad layer is bonded to the core layer by roll bonding, preferably by hot rolling, to achieve the required metallurgical bond between the layers. Such roll bonding process is highly economical and results in a highly efficient composite product exhibiting the desired properties. When performing such roll bonding process to produce a rolled composite product according to the present invention, it is preferred that both the core layer and the 6XXX series aluminum alloy clad layer(s) undergo thickness reduction during roll bonding. Typically, prior to rolling, and particularly prior to hot rolling, the rolled surfaces of both the core layer and the clad layer(s) are stripped to remove segregation areas close to the as-cast surface of the rolled ingot and to increase the flatness of the product.
[0016] Preferably, the cast ingot or slab of 2XXX alloy core layer is homogenized before hot rolling, and / or it may be preheated and hot rolled immediately thereafter. Homogenization and / or preheating of 2XXX series alloys before hot rolling is usually carried out at a temperature in the range of 400°C to 505°C. Segregation of alloying elements in the as-cast material is reduced and soluble elements are dissolved. If the treatment is carried out below about 400°C, the resulting homogenization effect is insufficient. If the temperature exceeds about 505°C, eutectic melting may occur resulting in unwanted pore formation. The preferred duration of this heat treatment is between 2 and 30 hours. Longer times are usually not detrimental. Homogenization is usually carried out at a temperature above about 480°C. Typical preheat temperatures are in the range of about 430°C to 460°C with soak times in the range of up to about 15 hours. Homogenization can be carried out in one or several stages of increasing temperature to avoid incipient melting.
[0017] In one embodiment of the present invention, the cast ingot or slab forming the 6XXX series aluminum alloy clad liner is homogenized to a thinner gauge prior to hot rolling to a thinner gauge to form a suitable clad liner for rolling together with the 2XXX series alloy core alloy to the desired gauge. The rolled surface of the 6XXX series alloy ingot or slab may be stripped to remove segregation areas close to the as-cast surface of the rolled ingot and increase the flatness of the product. Homogenization results in a finer, more homogenous grain structure resulting in increased formability of the alloy layer in the final rolled composite aerospace product. It dissolves most of the coarse phases and completes the transformation from beta to alpha-AlFeSi which improves the anodization behavior of the 6XXX series alloy. The homogenization heat treatment is preferably performed at a temperature of at least 480°C for at least about 0.5 hours, preferably in the range of about 1-30 hours, typically about 6-20 hours. Preferably, the homogenization temperature is in the range of about 500° C. to 590° C., preferably in the range of 510° C. to 580° C. In one embodiment, homogenization is carried out at a temperature of up to 570° C. As is well known in the art, homogenization can be carried out in one or several stages of increasing temperature to avoid premature melting.
[0018] The rolled composite aerospace product is gauge reduced to the final gauge by hot rolling and optionally subsequent cold rolling as is customary in the art. After the rolled composite product is rolled to the final gauge, the product is typically solution heat treated (SHT) at a temperature in the range of about 450°C to 505°C for a time sufficient for the solution effect to approach equilibrium, with typical soak times in the range of 5 to 120 minutes. Preferably, the solution heat treatment (SHT) is at a temperature in the range of 475°C to 500°C, for example about 495°C. The solution heat treatment is typically performed in a batch or continuous furnace. The preferred soak times at the indicated temperatures are in the range of about 5 to 35 minutes. However, with clad products, caution should be exercised against excessively long soak times, since too much copper, especially from the 2XXX core layer, may diffuse into the 6XXX series aluminum alloy clad layer(s), which may have a detrimental effect on the corrosion protection provided by said layer(s). After the solution heat treatment (SHT), it is important to cool the rolled composite product to a temperature below 175°C, preferably below 100°C, more preferably to ambient temperature quickly enough to prevent or minimize uncontrollable precipitation of secondary phases, e.g., Al2CuMg and Al2Cu in the 2XXX core alloy. On the other hand, the cooling rate should not be too high to allow sufficient flatness and low levels of residual stress in the rolled composite product. A suitable cooling rate can be achieved by the use of water, e.g., water immersion or water jet. Solution heat treatment in this temperature range results in a crystallized microstructure of the 6XXX series alloy layer. With the 6XXX series aluminum alloys used according to the present invention, the proportion of unmelted coarse Mg2Si and Si particles is minimized after applying the SHT, especially at 475°C to 500°C, e.g., about 495°C, which has a positive effect on the strength, formability, and corrosion resistance of the 6XXX series aluminum alloy clad layer. Microstructural evolution at ambient (room) temperature takes the 6XXX series aluminum alloy layer from the W (as-quenched) to the T4 temper. In this temper, the 6XXX series aluminum alloy clad layer provides improved formability compared to the non-recrystallized condition.
[0019] The composite product may be further cold worked, for example by stretching in the range of 0.5-8% of its original length, to relieve residual stresses and improve the flatness of the product. Preferably, the stretching is in the range of 0.5%-6%, more preferably 0.5%-4%, and most preferably 0.5%-3%.
[0020] After cooling, the rolled composite aerospace product is typically naturally aged at ambient temperature, alternatively, the composite aerospace product may also be artificially aged.
[0021] The 6XXX series aluminum alloy layer(s) are typically much thinner than the core, with each 6XXX series aluminum alloy layer constituting 1%-20% of the total thickness of the composite. More preferably, the 6XXX series aluminum alloy layer(s) constituting about 1%-10% of the total thickness of the composite.
[0022] In one embodiment, a 6XXX series aluminum alloy layer is bonded onto one surface or face of a 2XXX series core layer.
[0023] In one embodiment, a 6XXX series aluminum alloy layer is bonded onto both surfaces or faces of a 2XXX series core layer, thereby forming the outer surface of the rolled composite aerospace product.
[0024] In one embodiment, the rolled composite aerospace product has a total thickness of at least 0.8 mm.
[0025] In one embodiment, the rolled composite aerospace product has a total thickness of at most 2 inches, preferably at most 1 inch, and most preferably at most 12 mm.
[0026] In one embodiment the rolled composite aerospace product is a plate product.
[0027] In one embodiment, the rolled composite aerospace product is a sheet product.
[0028] The 6XXX series aluminum alloy cladding layer is derived from an aluminum alloy having a composition, by weight, of 0.3%-1.0% Si, 0.3%-1.1% Mg, 0.04%-1.0% Mn, 0.03%-0.4% Fe, 0.10% max Cu, 0.25% max Cr, 0.2% max V, 0.2% max Zr, 0.5% max Zn, 0.15% max Ti, with incidental impurities each <0.05% and total <0.15%, and the balance being aluminum.
[0029] Si and Mg are the most important alloying elements in the 6XXX series alloys, providing the necessary levels of strength and formability, especially tensile formability, for aluminum. The Si content should be in the range of 0.3%-1.0%. The preferred lower limit of the Si content is 0.40%. The preferred upper limit of the Si content is 0.9%, more preferably 0.75%. The Mg content should be in the range of 0.3%-1.1%. The preferred lower limit of the Mg content is 0.40%, more preferably 0.45%. The preferred upper limit of the Mg content is 0.90%, more preferably 0.80%. These Si and Mg ranges, together with the other alloying elements, provide yield strengths in the range of about 110-125 MPa after about one month of natural aging after SHT and rapid cooling, which only gradually increase further with longer natural aging, resulting in a very stable set of strength levels in the T4 temper. Preferably, the 6XXX series alloys have Si in excess of Mg to provide improved aging kinetics and formation of a refined Mg2Si precipitate structure, which results in high strength levels upon aging, both after artificial aging, especially during solution heat treatment at 475°C-500°C, and during the first month of natural aging after rapid cooling.
[0030] Mn is also an important alloying element in the 6XXX series alloys used in the clad layer(s) and should be in the range of 0.04% to 1.0%. The preferred lower limit of the Mn content is 0.20%, preferably 0.25%. The preferred upper limit of the Mn content is 0.90%, preferably 0.80%. In one embodiment, the upper limit of the Mn content is 0.7%. Mn enhances the strength of the aluminum alloy in the T4 or T6 temper after solution heat treatment and rapid cooling. Mn contributes to maintaining a small grain size of the clad layer(s), improving the surface appearance after forming operations and reducing surface cracks. The presence of Mn promotes the conversion of the beta-AlFeSi phase (Al5FeSi) to alpha-AlFeSi (Al8Fe2Si) and stabilizes the alpha-AlFeSi phase, thus improving the anodization quality of the outer surface of the 6XXX series layer. The presence of Mn also advantageously increases the corrosion potential of the 6XXX series aluminum alloys, and the amount of Mn added can be adjusted to reduce and optimize the corrosion potential difference between the core alloy and the clad layer(s) accordingly, thereby improving the corrosion resistance of rolled composite aerospace products.
[0031] In an embodiment of the 6XXX series aluminum alloy, the Cu content is max 0.10%, preferably max 0.05%, more preferably max 0.03% to enhance corrosion resistance.
[0032] Fe is an effective element for strength improvement and grain refinement. Fe contents below 0.03% may not be effective enough, while Fe contents above 0.4% may generate multiple coarse intermetallic compounds, especially when a large amount of Mn is present, which may reduce the tensile formability and corrosion resistance of the aluminum alloy. As a result, the Fe content is in the range of 0.03%-0.4%, preferably 0.1%-0.3%. In one embodiment, the Fe content is less than 0.25%. In a preferred embodiment, the ratio Fe / Mn is less than 1.8 to provide a balance between good corrosion resistance and good anodizing quality.
[0033] Cr can be added up to 0.25% to increase the strength and refine the grains of the aluminum alloy. Preferably, it is present at a maximum of 0.20%, more preferably at a maximum of 0.15%. In one embodiment, Cr is one of the inevitable impurities.
[0034] Zn can be present up to 0.5%, preferably up to 0.25%, without departing from the advantages of the present invention. In one embodiment, Zn is one of the inevitable impurities.
[0035] V can be added up to 0.2%, preferably up to 0.1%, without departing from the advantages of the present invention. In a preferred embodiment, V is one of the inevitable impurities, preferably up to 0.02%, more preferably up to 0.01%, so as to prevent complete recrystallization of the rolled material after solution heat treatment and rapid cooling. Moreover, it can form intermetallic particles that are harmful to the aluminum alloy.
[0036] Zr can be added up to 0.2%, preferably up to 0.1%, without departing from the advantages of the present invention. In a preferred embodiment, Zr is one of the inevitable impurities, preferably up to 0.02%, more preferably up to 0.01%, so as to prevent complete recrystallization of the rolled material after solution heat treatment and rapid cooling. Moreover, it may form intermetallic particles that are harmful to the aluminum alloy.
[0037] Grain refiners such as Ti, TiB2, Ti-C, etc. are typically added with a total Ti content of up to 0.15%, preferably up to 0.10%, more preferably 0.005% to 0.05%.
[0038] The balance consists of aluminum and incidental impurities, each <0.05%, total <0.15%.
[0039] In one embodiment, the 6XXX series layer is derived from an aluminum alloy having, by weight, 0.3%-1.0% Si, 0.3%-1.1% Mg, 0.04%-1.0% Mn, 0.03%-0.4% Fe, max 0.10% Cu, max 0.25% Cr, max 0.2% V, max 0.2% Zr, max 0.5% Zn, max 0.1% Ti, incidental impurities each <0.05%, total <0.15%, and balance Aluminum, with the preferred narrower composition ranges as described and claimed herein.
[0040] In one embodiment, the composition of the 6XXX series aluminum alloy clad layer is adjusted or set to have a natural-state corrosion value (vs. standard calomel electrode (SCE), also referred to as "corrosion potential") of -710 mV or less (e.g., -750 mV) to provide optimal corrosion protection for the 2XXX series core alloy, as measured on solution heat treated and quenched material in a solution of 53 g / L NaCl + 3 g / L H2O2 at 25°C using a 0.1 N calomel electrode. In a preferred embodiment, the corrosion potential of the 6XXX series aluminum alloy clad layer is in the range of -730 mV to -810 mV, as measured after SHT and quenching, thus when the critical alloying elements are generally in solid solution.
[0041] In one embodiment, the corrosion potential difference between the 2XXX core layer and the 6XXX series aluminum alloy clad layer, i.e., at the final temper, is in the range of 30-100 mV to provide sufficient corrosion protection from the anodic clad layer to the core layer.
[0042] In one embodiment, the 2XXX series core layer comprises, in weight percent: Cu 1.9% to 7.0%, preferably 3.0% to 6.8%, more preferably 3.2% to 4.95%, Mg 0.30% to 1.8%, preferably 0.35% to 1.8%, Mn: maximum 1.2%, preferably 0.2% to 1.2%, more preferably 0.2% to 0.9%, Si max 0.40%, preferably max 0.25%, Fe max 0.40%, preferably max 0.25%, Cr max 0.35%, preferably max 0.10%, Zn max 1.0%, Ti max 0.15%, preferably 0.01% to 0.10%, Zr max 0.25%, preferably max 0.12%, V max 0.25%, Li up to 2.0% Ag up to 0.80%, Ni up to 2.5% The balance is derived from an aluminum alloy having a composition including aluminum and impurities, typically <0.05% each and <0.15% total.
[0043] In another embodiment, the 2XXX series core layer comprises, in weight percent: Cu 1.9% to 7.0%, preferably 3.0% to 6.8%, more preferably 3.2% to 4.95%, Mg 0.30% to 1.8%, preferably 0.8% to 1.8%, Mn: maximum 1.2%, preferably 0.2% to 1.2%, more preferably 0.2% to 0.9%, Si max 0.40%, preferably max 0.25%, Fe max 0.40%, preferably max 0.25%, Cr max 0.35%, preferably max 0.10%, Zn max 0.4%, Ti max 0.15%, preferably 0.01% to 0.10%, Zr max 0.25, preferably max 0.12%, V max 0.25%, The balance is derived from an aluminum alloy having a composition including aluminum and impurities, typically <0.05% each and <0.15% total.
[0044] In a preferred embodiment, the 2XXX series core layer is derived from an AA2X24 series aluminum alloy, where X is equal to 0, 1, 2, 3, 4, 5, 6, 7, or 8. Particularly preferred aluminum alloys are within the ranges AA2024, AA2524, and AA2624.
[0045] In one embodiment, the 2XXX series core layer is provided in a T3, T351, T39, T8 or T851 temper.
[0046] The 2XXX series core layers may be provided to the user in a non-solution heat treated temper, e.g., "F" temper or an annealed "O" temper, and then formed, solution heat treated, and aged by the user to the required temper, e.g., T3, T351, T39, T8 or T851 temper.
[0047] The present invention also provides a method for producing the rolled composite aerospace product of the present invention, comprising the steps of: (a) providing an ingot or rolled stock of a 2XXX series aluminum alloy for forming a core layer of a composite aerospace product; (b) homogenizing the 2XXX series aluminum alloy ingot at a temperature in the range of 400°C to 505°C for at least 2 hours; (c) providing an ingot or rolled clad liner of a 6XXX series aluminum alloy for forming an outer clad layer on the 2XXX series core aluminum alloy, optionally wherein two ingots or two rolled clad liners of a 6XXX series aluminum alloy are provided for forming a clad layer on each side of the 6XXX series core aluminum alloy; (d) homogenizing the 6XXX series aluminum alloy ingot(s) at a temperature in the range of at least 480°C for at least 0.5 hours, preferably at a temperature in the range of 500°C to 590°C, prior to hot rolling into a rolled clad; (e) roll bonding the 6XXX series aluminum alloy layer(s) to the 2XXX series core alloy layer, preferably by hot rolling and optionally subsequent cold rolling, to form a roll bonded product; (f) solution heat treating the roll-bonded product at a temperature in the range of 450°C to 505°C; (g) cooling the solution heat treated roll bonded product to less than 100° C., preferably to ambient temperature; (h) optionally stretching the solution heat treated roll bonded product by cold stretching, preferably in the range of 0.5% to 8% of its original length, preferably in the range of 0.5% to 6%, more preferably 0.5% to 4%, and most preferably 0.5% to 3%; (i) ageing the cooled roll bonded product by natural and / or artificial aging. In a preferred embodiment, the 2XXX series core layer is aged to a T3, T351, T39, T8 or T851 temper, and the 6XXX series alloy clad layer is aged to a T4 temper if naturally aged and to a T6 temper if artificially aged.
[0048] In one embodiment of the method according to the invention, in a subsequent processing step, the rolled composite aerospace product is formed in a forming process at ambient or elevated temperature into a product of predetermined shape having at least one of uniaxial or biaxial bending.
[0049] In an alternative embodiment of the method, after roll bonding the 6XXX series aluminum alloy(s) to the 2XXX series core alloy in step (f) to form a roll bonded product, preferably by hot rolling and optionally subsequent cold rolling, the roll bonded product aerospace product of the present invention is formed into a predetermined shaped product having at least one of uniaxial or biaxial bending at ambient or elevated temperature in a forming process, followed by solution heat treatment and then aging to final temper.
[0050] The forming can be by a forming operation from the group of bending operations, roll forming, stretch forming, aged creep forming, deep drawing, and high energy hydroforming, in particular by explosive forming or electric discharge forming. The 6XXX series aluminum alloys used in the rolled composite aerospace products of the present invention provide the necessary bendability even after natural and / or artificial aging. They also have the necessary tensile formability for these forming operations.
[0051] In one embodiment, the forming operation at elevated temperature is carried out at a temperature in the range of 140°C to 200°C, and preferably the aerospace product is maintained at the forming temperature for a time in the range of 1 to 50 hours. To optimize the strength of the 6XXX series cladding layers, forming temperatures in the range of 150°C to 170°C are preferred. In a preferred embodiment, the forming at elevated temperature is an age creep forming operation. Age creep forming is a process or operation that constrains a component into a particular shape during an age heat treatment, allowing the component to release stress and deform, for example to form a fuselage shell having a single or double bend.
[0052] In one embodiment, as disclosed in patent document US-2014 / 036699-A1, incorporated herein, the rolled composite aerospace product according to the invention after undergoing solution heat treatment (SHT) and before forming into a predetermined shape is subjected to a post-SHT cold working step inducing at least 25% cold working in the rolled composite aerospace product, in particular the cold working of cold rolling the rolled aerospace product to a final gauge is excluded from the present invention.
[0053] In one aspect of the invention, it relates to the use of a 6XXX series aluminum alloy as described and claimed herein as a cladding layer on one or both surfaces of a 2XXX series aluminum alloy rolled aerospace product.
[0054] In a further aspect of the invention there is provided a welded structure comprising a rolled composite aerospace product according to the invention and at least one aluminium alloy hardened element joined to the rolled composite aerospace product by a riveting or welding operation.
[0055] In yet another aspect, the invention relates to a welded structural member of an aircraft comprising a rolled composite aerospace product according to the invention and at least one aluminum alloy hardened element, preferably a stringer, joined to the rolled composite aerospace product by a riveting or welding operation, for example by laser beam welding or friction stir welding. It also relates to a welded fuselage structure in which fuselage panels are joined together by laser beam welding ("LBW") or friction stir welding ("FSW"), for example by butt welding.
[0056] The present invention also includes an aircraft or spacecraft whose fuselage is constructed, in whole or in part, from rolled composite aerospace products according to the present invention, which may be incorporated into various structural portions of the aircraft. For example, the various disclosed embodiments may be used to form structural portions in a wing assembly and / or in a tail assembly (tail section). The aircraft are typically representative of commercial passenger aircraft or cargo aircraft. In alternative embodiments, the present invention may be incorporated into other types of air vehicles. Examples of such air vehicles include manned or unmanned military aircraft, rotorcraft, or even suborbital vehicles.
[0057] The rolled composite aerospace products of the invention can be formed into components, such as fuselage parts or panels, or wing parts or panels, for airplanes that can take advantage of the advantages of the invention described. The shaping referred to can include bending, stretch forming, machining and other forming operations known in the art to form panels or other components for aircraft, aerospace or other vehicles. Forming, including bending or other plastic deformation, can be performed at room temperature or at elevated temperatures.
[0058] The present invention will also be described with reference to the accompanying drawings. [Brief description of the drawings]
[0059] [Figure 1] FIG. 1 is a schematic diagram illustrating an embodiment of the present invention. [Diagram 2] 1 is a schematic flow schedule of several embodiments of a process for producing a rolled composite aerospace product in accordance with the present invention.
[0060] FIG. 1 illustrates an embodiment of a rolled composite aerospace product 10 having a three-layer construction of a 2XXX series core alloy layer 20 with a cladding layer 30 of a 6XXX series aluminum alloy on each side as shown and claimed herein.
[0061] FIG. 2 is a schematic flow schedule of some embodiments of the process of the present invention for manufacturing a rolled composite aerospace product. In process step 1, an ingot is cast of a 2XXX series alloy that forms the core alloy of the composite aerospace product, which may optionally be stripped in step 2 to remove segregation areas close to the as-cast surface of the rolled ingot and increase the flatness of the product. In process step 3, the rolled ingot is homogenized. In parallel, in process step 4, an ingot is cast of a 6XXX series alloy to form at least one cladding layer on the surface of the core alloy of the composite aerospace product, and optionally on both sides of the core alloy. This ingot may also be optionally stripped in step 5. In process step 6, the 6XXX series alloy is homogenized and then hot rolled in process step 7 to form the liner plate(s) since the cladding layers are usually much thinner than the core. In process step 8, the 2XXX core alloy and the 6XXX liner plate on one or both sides of the core alloy are roll bonded, preferably by hot rolling. Depending on the final gauge desired, the roll bonded product may be cold rolled to the final gauge, e.g., a sheet product or a thin gauge plate product, in process step 9. In process step 10, the rolled aerospace product is solution heat treated, then cooled in process step 11 and preferably stretched in process step 12.
[0062] In one embodiment, the cooled product is formed in a forming process 13 and aged, ie, naturally or artificially aged, in process step 14 to a final temper, for example a T3 or T8 temper.
[0063] In one embodiment, the forming process 13 and the aging of process step 14 may be combined, for example, the forming operation is carried out at a temperature in the range of 140° C. to 200° C., preferably for a time in the range of 1 to 50 hours, to also artificially age both the 2XXX series core and the 6XXX series cladding layer(s).
[0064] In one embodiment, the cooled product is aged in process step 14, i.e., natural or artificial aging, to a desired temper, and then formed in forming process 13 into a shaped product of a predetermined shape.
[0065] In an alternative embodiment, after roll bonding the 2XXX series core and 6XXX series cladding layer(s) to final gauge, the rolled product is formed to a predetermined shape in forming process 13, solution heat treating the formed product in process step 15, cooling in process step 11, and subsequently aging to a final temper, e.g., a T3 or T8 temper, i.e., naturally or artificially aged, in process step 14.
[0066] The invention is not limited to the embodiments described above but can be widely varied within the scope of the invention as defined by the appended claims. Some of the embodiments of the present disclosure are described in [Item 1] to [Item 20] below. [Item 1] 1. A rolled composite aerospace product comprising a 2XXX series core layer and a 6XXX series aluminum alloy clad layer bonded to at least one surface of the 2XXX series core layer, the 6XXX series aluminum alloy containing, by weight, 0.3%-1.0% Si, 0.3%-1.1% Mg, 0.04%-1.0% Mn, 0.03%-0.4% Fe, max 0.10% Cu, max 0.25% Cr, max 0.2% V, max 0.2% Zr, max 0.5% Zn, max 0.1% Ti, unavoidable impurities each <0.05% and total <0.15%, and the balance being aluminum. [Item 2] 2. The rolled composite aerospace product according to item 1, wherein the 6XXX series aluminum alloy has a Si content in the range of 0.4% to 0.9%. [Item 3] 3. The rolled composite aerospace product according to any one of items 1 to 2, wherein the 6XXX series aluminum alloy has a Mg content in the range of 0.40% to 0.90%. [Item 4] 4. The rolled composite aerospace product according to any one of items 1 to 3, wherein the 6XXX series aluminum alloy has a Mn content in the range of 0.25% to 1.0%, preferably in the range of 0.30% to 0.90%. [Item 5] 5. The rolled composite aerospace product according to any one of items 1 to 4, wherein the 6XXX series aluminum alloy clad layer is joined to the at least one surface of the 2XXX series core layer by roll bonding. [Item 6] 6. The rolled composite aerospace product according to any one of items 1 to 5, wherein the 6XXX series aluminum alloy clad layer has a thickness in the range of 1% to 20%, preferably 1% to 10% of the total thickness of the rolled composite aerospace product. [Item 7] 7. The rolled composite aerospace product according to any one of items 1 to 6, comprising a 2XXX series core layer and a 6XXX series aluminum alloy clad layer bonded to one surface of the 2XXX series core layer. [Item 8] 7. The rolled composite aerospace product according to any one of items 1 to 6, comprising a 2XXX series core layer and a 6XXX series aluminum alloy clad layer bonded to both surfaces of the 2XXX series core layer. [Item 9] The 2XXX series alloy of the core layer comprises, in weight percent: Cu 1.9% to 7.0%, preferably 3.0% to 6.8%, more preferably 3.2% to 4.95%, Mg 0.30% to 1.8%, preferably 0.35% to 1.8%, Mn: Maximum 1.2%, preferably 0.2% to 1.2%, Si max 0.40%, Fe max 0.40%, Cr max 0.35% Zn max 1.0%, Ti max. 0.15%, Zr max 0.25% V max 0.25%, Li up to 2.0% Ag up to 0.80%, Ni up to 2.5% 9. The rolled composite aerospace product according to any one of items 1 to 8, having a composition of the remainder being aluminum and impurities. [Item 10] 10. The rolled composite aerospace product according to any one of claims 1 to 9, wherein the 2XXX series core layer is derived from a 2x24 series alloy. [Item 11] 11. The rolled composite aerospace product according to any one of the preceding claims, wherein the 2XXX series core layer is of T3, T351, T39, T8 or T851 temper. [Item 12] 12. The rolled composite aerospace product according to any one of the preceding claims, wherein the 6XXX series cladding layer is T4 or T6 temper. [Item 13] 13. The rolled composite aerospace product according to any one of items 1 to 12, wherein the rolled composite aerospace product has a total thickness of 0.8 mm to 50.8 mm, more preferably 0.8 mm to 25.4 mm. [Item 14] 14. The rolled composite aerospace product according to any one of items 1 to 13, wherein the rolled composite aerospace product is a plate product. [Item 15] 14. The rolled composite aerospace product according to any one of items 1 to 13, wherein the rolled composite aerospace product is a sheet product. [Item 16] 16. The rolled composite aerospace product according to any one of items 1 to 15, wherein the rolled composite aerospace product is an aerospace structural part, preferably an aircraft fuselage. [Item 17] A method for producing a rolled composite aerospace product according to any one of items 1 to 16, (a) providing an ingot of a 2XXX series aluminum alloy for forming said core layer of said composite aerospace product; (b) homogenizing the 2XXX series aluminum alloy ingot at a temperature in the range of 400°C to 505°C for at least 2 hours; (c) providing an ingot or rolled clad liner of a 6XXX series aluminum alloy for forming an outer clad layer on said 2XXX series core aluminum alloy; (d) homogenizing said ingot of said 6XXX series aluminum alloy at a temperature of at least 480°C, preferably in the range of 500°C to 590°C, for at least 0.5 hours; (e) roll bonding the 6XXX series aluminum alloy to a 2XXX series core alloy, preferably by hot rolling and optionally subsequent cold rolling, to form a roll bonded product; (f) solution heat treating the roll-bonded product at a temperature in the range of 450°C to 505°C; (g) cooling the solution heat treated roll bonded product to less than 100° C., preferably to ambient temperature; (h) optionally stretching the solution heat treated and cooled roll bonded product; and (i) aging the 2XXX series core alloy of the cooled roll bonded product, preferably to a T3, T351, T39, T8 or T851 temper. [Item 18] 18. The method according to claim 17, further comprising forming the solution heat treated, cooled and optionally further stretched roll bonded product into a product of a predetermined shape in a forming process. [Item 19] 19. The method according to items 17 and 18, wherein a forming step (j) is carried out after the ageing step (i). [Item 20] Item 19. The method according to item 18, wherein the forming step (j) and the ageing step (i) are combined in a forming step at elevated temperature, preferably at a temperature in the range of 140° C. to 200° C., for a time preferably in the range of 1 to 50 hours.
Claims
1. 1. A rolled composite aerospace product comprising a 2xxx series core layer and a 6xxx series aluminum alloy clad layer bonded to at least one surface of the 2xxx series core layer, the 6xxx series aluminum alloy consisting, by weight, of 0.3%-1.0% Si, 0.3%-1.1% Mg, 0.04%-1.0% Mn, 0.03%-0.4% Fe, 0.10% max Cu, 0.25% max Cr, 0.2% max V, 0.2% max Zr, 0.5% max Zn, 0.1% max Ti, unavoidable impurities each <0.05% and total <0.15%, and the balance Aluminum; The rolled composite aerospace product, wherein the corrosion potential difference between the 2xxx series core layer and the 6xxx series aluminum alloy clad layer is in the range of 30mV to 100mV.
2. 2. The rolled composite aerospace product of claim 1, wherein the 6xxx series aluminum alloy has a Si content in the range of 0.4% to 0.9%.
3. The rolled composite aerospace product according to any one of claims 1 to 2, wherein the 6xxx series aluminum alloy has a Mg content in the range of 0.40% to 0.90%.
4. The rolled composite aerospace product according to any one of claims 1 to 3, wherein the 6xxx series aluminum alloy has a Mn content in the range of 0.25% to 1.0%.
5. 5. The rolled composite aerospace product of any one of claims 1 to 4, wherein the 6xxx series aluminum alloy clad layer is joined to the at least one surface of the 2xxx series core layer by roll bonding.
6. 6. The rolled composite aerospace product of claim 1, wherein the 6xxx series aluminum alloy clad layer has a thickness in the range of 1% to 20% of the total thickness of the rolled composite aerospace product.
7. 7. The rolled composite aerospace product of any one of claims 1 to 6, comprising a 2XXX series core layer and a 6XXX series aluminum alloy clad layer bonded to one surface of the 2XXX series core layer.
8. 7. The rolled composite aerospace product of any one of claims 1 to 6, comprising a 2XXX series core layer and a 6XXX series aluminum alloy clad layer bonded to both surfaces of the 2XXX series core layer.
9. The 2xxx series alloy of the core layer comprises, by weight percent: Cu 1.9% to 7.0%, Mg 0.30% to 1.8%, Mn max 1.2%, Si max 0.40% Fe max 0.40% Cr max 0.35%, Zn max 1.0% Ti maximum 0.15%, Zr max 0.25%, V max 0.25%, Li up to 2.0%, Ag max 0.80%, Ni max 2.5%, The rolled composite aerospace product of any one of claims 1 to 8, having a composition of balance aluminum and impurities.
10. The rolled composite aerospace product according to any one of claims 1 to 9, wherein said 2XXX series core layer is derived from a 2x24 series alloy.
11. The rolled composite aerospace product of any one of claims 1 to 10, wherein the 2XXX series core layer is a T3, T351, T39, T8 or T851 temper.
12. The rolled composite aerospace product of any one of claims 1 to 11, wherein the 6xxx series aluminium alloy clad layer is in a T4 or T6 temper.
13. The rolled composite aerospace product of any one of claims 1 to 12, wherein the rolled composite aerospace product has a total thickness of 0.8 mm to 50.8 mm.
14. The rolled composite aerospace product according to any one of claims 1 to 13, wherein the rolled composite aerospace product is a plate product.
15. The rolled composite aerospace product according to any one of claims 1 to 13, wherein the rolled composite aerospace product is a sheet product.
16. The rolled composite aerospace product according to any one of claims 1 to 15, wherein the rolled composite aerospace product is an aerospace structural part.
17. A method for producing a rolled composite aerospace product according to any one of claims 1 to 16, comprising the steps of: (a) providing an ingot of a 2xxx series aluminum alloy for forming said core layer of said rolled composite aerospace product; (b) homogenizing said 2xxx series aluminum alloy ingot at a temperature in the range of 400°C to 505°C for at least two hours; (c) providing an ingot or rolled clad liner of a 6xxx series aluminum alloy for forming an outer clad layer on said 2xxx series core aluminum alloy; (d) homogenizing said ingot of said 6xxx series aluminum alloy at a temperature of at least 480° C. for at least 0.5 hours; (e) roll bonding the 6xxx series aluminum alloy to a 2xxx series core alloy by hot rolling and optionally subsequent cold rolling to form a roll bonded product; (f) solution heat treating the roll bonded product at a temperature in the range of 450°C to 505°C; (g) cooling the solution heat treated roll bonded product to less than 100°C; (h) optionally stretching the solution heat treated and cooled roll bonded product; and (i) aging the 2xxx series core alloy in the cooled roll bonded product to a T3, T351, T39, T8 or T851 temper.
18. 20. The method of claim 17, further comprising forming the solution heat treated, cooled, and optionally further stretched roll bonded article into a product of a predetermined shape having at least one of uniaxial or biaxial bending in a forming process.
19. 19. The method according to claim 17 or 18, wherein a forming step (j) is carried out after the ageing step (i).
20. 20. The method of claim 19, wherein the forming step (j) and the ageing step (i) are combined in a forming step at elevated temperature, at a temperature in the range of 140° C. to 200° C., for a time in the range of 1 to 50 hours.
Citation Information
Patent Citations
Aluminum alloy clad plate with excellent molding workability, corrosive resistance and hardening property
JP1994278243A
Aluminum thin sheet product having improved fatigue crack growing resistance and its production method
JP2002053925A
Damage-resistant aluminum alloy products, especially for aerospace applications
JP2006527303A
aluminum composite sheet material
JP2009535508A
Aluminium alloy material, method for manufacturing the same, and aluminium alloy clad material using aluminium alloy material