Battery protection plate
Patent Information
- Application Number
- CN202420245726.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2034-01-31
Smart Images

Figure CN221900105U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of new energy, in particular to a battery protection plate. Background Art
[0002] The protective plate is installed at the bottom of the car body. It is the bearing part of the power battery box of new energy vehicles and is used to protect the battery box from damage when it is hit or squeezed by the outside world. At present, the protective plate of the car is mainly made of metal alloy materials, but it is heavy and greatly reduces the battery's mileage. In addition, the chassis is often in contact with rain, oil, etc., which will cause continuous corrosion of metal parts and bring safety hazards. Pure thermoplastic composite materials have poor ductility when facing the impact of stones and sharp objects, and cannot protect the battery well.
[0003] Patent CN217788632 U discloses a battery protection bottom plate, including an upper fiber reinforced resin layer, a metal plate and a lower fiber reinforced resin layer. It combines thermoplastic composite materials with metal materials to give full play to their respective advantages, making its application in the protection plate of power battery vehicles an innovation in the industry, but its impact resistance still needs to be improved.
[0004] Patent CN108545159A discloses a gradient pressure-resistant, impact-resistant and energy-absorbing covering layer, comprising an energy-absorbing layer unit; the energy-absorbing layer unit comprises a rubber box body, a plastic foam energy-absorbing body and an intermediate panel, wherein the material composition includes a nylon composite layer with a thickness of 2 to 3 mm, a rubber skin with a thickness of 3 to 4 mm, and the plastic foam energy-absorbing body comprises metal foam or polymer foam. The combined composite material achieves the effect of pressure-resistant, impact-resistant and energy-absorbing, but it cannot meet the lightweight design requirements.
[0005] In view of this, this application is filed. Utility Model Content
[0006] The utility model aims to overcome the shortcomings of the prior art and provide a battery protection plate, which has the advantages of light weight, collision resistance and impact resistance.
[0007] In order to achieve the above purpose, the technical solution adopted by the utility model is:
[0008] A battery protection plate comprises a first continuous fiber reinforced resin layer, a fiber reinforced resin layer and a second continuous fiber reinforced resin layer which are stacked in sequence;
[0009] The first continuous fiber reinforced resin layer and the fiber reinforced resin layer include a metal plate and a foam layer between them;
[0010] The fiber-reinforced resin layer is a short fiber-reinforced resin layer or a fiber felt-reinforced resin layer;
[0011] The thickness ratio of the metal plate, the foam layer and the fiber-reinforced resin layer is (0.3-6): (0.6-8): (1-12). Preferably, the thickness of the first continuous fiber-reinforced resin layer is 0.1-1.5 mm.
[0012] Preferably, the thickness of the second continuous fiber reinforced resin layer is 0.1-1.5 mm.
[0013] Preferably, the fiber-reinforced resin layer has a thickness of 1 to 12 mm and a gram weight of 400 to 1600 g / m 2 .
[0014] Preferably, the length of the short fibers in the short fiber reinforced resin layer is 10 to 70 mm.
[0015] Preferably, the foam layer has a thickness of 0.8 to 6 mm.
[0016] Preferably, the fiber reinforced resin layer is made of GMT material.
[0017] Preferably, the metal plate is adjacent to the first continuous fiber reinforced resin layer, and the foam layer is adjacent to the fiber reinforced resin layer.
[0018] Preferably, the metal plate is adjacent to the fiber reinforced resin layer, and the foam layer is adjacent to the first continuous fiber reinforced resin layer.
[0019] Preferably, the metal plate comprises a substrate and a coating located on at least one surface of the substrate; the substrate is selected from iron and its alloys, aluminum and its alloys, magnesium and its alloys, copper and its alloys, titanium and its alloys or nickel and its alloys, and the coating is a zinc coating, a zinc-iron alloy coating or a zinc-magnesium alloy coating.
[0020] Preferably, the thickness of the substrate is 0.25-5 mm, and the roughness of the surface of the substrate is 0.3-1.2.
[0021] Preferably, the thickness of the coating is 0.05-0.5 mm.
[0022] Preferably, a resin film is provided between the second continuous fiber reinforced resin layer and the fiber reinforced resin layer, and the thickness of the resin film is 0.08-1 mm.
[0023] Preferably, it further comprises a buffer layer, which is a rubber polymer, a thermoplastic elastomer or a resin polymer, and is arranged on a side of the first continuous fiber reinforced resin layer away from the metal plate.
[0024] Preferably, the buffer layer is made of TPV material.
[0025] Preferably, the thickness of the buffer layer is 0.4-2.5 mm.
[0026] Preferably, the total thickness of the battery protection plate is 2.1 to 33.6 mm.
[0027] The beneficial effects of the utility model are as follows: (1) The utility model uses the first continuous fiber reinforced resin layer and the second continuous fiber reinforced resin layer as the upper and lower layers of the protective plate, wherein the first continuous fiber reinforced resin layer and the second continuous fiber reinforced resin layer are used as the inner and outer protective layers of the protective plate respectively, which can effectively improve the impact resistance and corrosion resistance of the protective plate, and at the same time can effectively reduce weight, achieve light weight and high strength, and avoid the bottom of the protective plate from being punctured. The setting of the metal plate further ensures the rigidity and strength of the protective plate, and further improves the impact resistance of the protective plate. (2) The utility model can play an excellent buffering and energy absorption role by setting the fiber reinforced resin layer, the foam layer and the metal plate, further improve the impact resistance of the protective plate, so that the stress of the protective plate can be evenly dispersed when it is used, and will not cause excessive local impact force or excessive local impact force, thereby preventing the protective plate from breaking and failing. At the same time, the setting of the fiber reinforced resin layer and the foam layer can hinder air circulation and achieve excellent noise reduction effect. The setting of the fiber reinforced resin layer and the foam layer can also play a weight reduction effect and achieve light weight and high strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a structural schematic diagram of an embodiment of the utility model.
[0029] Figure 2 It is a structural schematic diagram of another embodiment of the utility model.
[0030] Figure 3 Schematic diagram of the structure of the metal plate.
[0031] Figure 4 Another structural schematic diagram of a metal plate.
[0032] Figure 5 Another structural schematic diagram of a metal plate.
[0033] Figure 6 It is a structural schematic diagram of another embodiment of the utility model.
[0034] Figure 7 It is a structural schematic diagram of another embodiment of the utility model.
[0035] Figure 8 It is a structural schematic diagram of another embodiment of the utility model.
[0036] Markings in the figure: 1, first continuous fiber reinforced resin layer; 2, metal plate; 21, substrate; 22, coating; 3, foam layer; 4, fiber reinforced resin layer; 5, second continuous fiber reinforced resin layer; 6, resin film; 7, buffer layer. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0038] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0039] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.
[0040] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present utility model, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0041] See also Figure 1 The utility model provides a battery protection plate, comprising a first continuous fiber reinforced resin layer 1, a fiber reinforced resin layer 4 and a second continuous fiber reinforced resin layer 5 which are stacked in sequence;
[0042] The metal plate 2 and the foam layer 3 are included between the first continuous fiber reinforced resin layer 1 and the fiber reinforced resin layer 4;
[0043] The fiber-reinforced resin layer 4 is a short fiber-reinforced resin layer or a fiber felt-reinforced resin layer;
[0044] The thickness ratio of the metal plate 2, the foam layer 3, and the fiber-reinforced resin layer 4 is (0.3-6): (0.6-8): (1-12).
[0045] The utility model uses the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 as the upper and lower layers of the protective plate, wherein the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 respectively serve as the inner and outer protective layers of the protective plate, thereby effectively improving the impact resistance and corrosion resistance of the protective plate, and at the same time effectively reducing the weight to achieve light weight and high strength, thereby avoiding the bottom of the protective plate from being punctured. The provision of the metal plate 2 further ensures the rigidity and strength of the protective plate, and further improves the impact resistance of the protective plate.
[0046] The utility model creatively arranges a continuous fiber reinforced resin layer 4, a foam layer 3 and a metal plate 2, and controls the thickness ratio of the continuous fiber reinforced resin layer 4, the foam layer 3 and the metal plate 2, which can play an excellent role in buffering and absorbing energy, further improving the impact resistance of the protective plate, so that the stress applied to the protective plate when in use can be evenly dispersed, and will not cause excessive local impact force or excessively low local impact force, thereby preventing the protective plate from breaking and failing. At the same time, the arrangement of the fiber reinforced resin layer 4 and the foam layer 3 can hinder air circulation and achieve an excellent noise reduction effect. The arrangement of the fiber reinforced resin layer 4 and the foam layer 3 can also reduce weight and achieve light weight and high strength.
[0047] In one embodiment, the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 are both composited by continuous fibers and resin through a melt impregnation process, wherein the mass percentage of the continuous fibers is 30-80%, for example, it can be 30%, 35%, 40%, 50%, 60%, 70%, 75%, 80% or a range consisting of any two values therein. Preferably, it is 35-75%. By limiting the content of fiber material and resin in the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5, the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 have the advantages of light weight, collision resistance and impact resistance.
[0048] In one embodiment, the thickness of the first continuous fiber reinforced resin layer 1 is 0.1-1.5 mm, for example, 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm, 1.5 mm or a range consisting of any two of these values.
[0049] In one embodiment, the thickness of the first continuous fiber reinforced resin layer 1 is 0.15-1.2 mm. In one embodiment, the width of the first continuous fiber reinforced resin layer 1 is cut according to actual product requirements, preferably 20-1500 mm, for example, 20 mm, 25 mm, 30 mm, 50 mm, 100 mm, 200 mm, 400 mm, 800 mm, 1000 mm, 1200 mm, 1400 mm, 1470 mm, 1500 mm or a range consisting of any two of the values. In one embodiment, the width of the first continuous fiber reinforced resin layer 1 is 25-1470 mm.
[0050] In one embodiment, the thickness of the second continuous fiber reinforced resin layer 5 is 0.1-1.5 mm, for example, 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm, 1.5 mm or a range consisting of any two of these values.
[0051] In one embodiment, the thickness of the first continuous fiber reinforced resin layer 1 is 0.15-1.2 mm.
[0052] In one embodiment, the width of the second continuous fiber reinforced resin layer 5 is cut according to actual product requirements, and is preferably 20 to 1500 mm, for example, it can be 20 mm, 25 mm, 30 mm, 50 mm, 100 mm, 200 mm, 400 mm, 800 mm, 1000 mm, 1200 mm, 1400 mm, 1470 mm, 1500 mm or a range consisting of any two of these values.
[0053] In one embodiment, the width of the second continuous fiber reinforced resin layer 5 is 25 to 1470 mm.
[0054] The utility model controls the thickness and width of the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 so that the protective plate has excellent anti-collision and anti-impact performance and also has the advantage of being lightweight.
[0055] In one embodiment, the resins in the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 are independently modified or unmodified polyethylene, modified or unmodified polypropylene, modified or unmodified polystyrene, modified or unmodified polycarbonate, modified or unmodified polyamide, modified or unmodified polyethylene recycled material, modified or unmodified polypropylene recycled material, modified or unmodified polystyrene recycled material, modified or unmodified polycarbonate recycled material, modified or unmodified polyamide recycled material.
[0056] In one embodiment, the continuous fibers in the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 are independently continuous glass fibers, continuous carbon fibers, continuous aramid fibers, continuous basalt fibers or continuous silicon carbide fibers.
[0057] In one embodiment, the types of resin and continuous fibers in the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 may be the same or different.
[0058] In one embodiment, the first continuous fiber reinforced resin layer 1 and the second continuous fiber reinforced resin layer 5 are made of the same resin material. Using the same resin material can effectively improve the overall compatibility and further improve the impact resistance of the protective plate.
[0059] In one embodiment, the fiber reinforced resin layer 4 has a thickness of 1 to 12 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 12 mm or a range consisting of any two of these values.
[0060] In one embodiment, the fiber reinforced resin layer 4 has a thickness of 2 to 10 mm.
[0061] In one embodiment, the fiber-reinforced resin layer 4 has a gram weight of 400 to 1600 g / m 2 , for example, it can be 400g / m 2 , 500g / m 2 , 600g / m 2 , 800g / m 2 1000g / m 2 , 1200g / m 2 , 1400g / m 2 , 1500g / m 2 , 1600g / m 2 Or a range consisting of any two values.
[0062] The fiber-reinforced resin layer 4 with such grammage and thickness can play an excellent role in buffering and absorbing energy, further improving the impact resistance of the protective plate, so that the stress applied to the protective plate can be evenly dispersed when the protective plate is in use, without causing excessive local impact force or excessive local impact force, thereby preventing the protective plate from breaking and failing.
[0063] In one embodiment, the resin in the fiber-reinforced resin layer 4 and the second continuous fiber-reinforced resin layer 5 can be the same resin material or different resin materials.
[0064] In one embodiment, the fiber-reinforced resin layer 4 and the second continuous fiber-reinforced resin layer 5 are made of the same resin material. Using the same resin material can effectively improve the overall compatibility and further improve the impact resistance of the protective plate.
[0065] In one embodiment, the short fiber reinforced resin layer consists of short fibers and resin, wherein the mass percentage of the short fibers is 30-60%, for example, 30%, 40%, 50%, 60% or a range consisting of any two values therein.
[0066] In one embodiment, the length of the short fibers in the short fiber reinforced resin layer is 10 to 70 mm, for example, 10 mm, 20 mm, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm or a range consisting of any two values therein.
[0067] In one embodiment, the short fibers in the short fiber reinforced resin layer are short glass fibers.
[0068] The molding process of the short fiber reinforced resin layer is as follows: prepare two layers of resin films, evenly place the short fibers between the two layers of resin films, and perform composite molding by hot pressing with a molding machine to obtain the short fiber reinforced resin layer.
[0069] In one embodiment, the resin in the short fiber reinforced resin layer is modified or unmodified polyethylene, modified or unmodified polypropylene, modified or unmodified polystyrene, modified or unmodified polycarbonate, modified or unmodified polyamide, modified or unmodified polyethylene recycled material, modified or unmodified polypropylene recycled material, modified or unmodified polystyrene recycled material, modified or unmodified polycarbonate recycled material, modified or unmodified polyamide recycled material.
[0070] In one embodiment, the fiber mat reinforced resin layer consists of fiber mat and resin, wherein the mass percentage of the fiber mat is 30-60%, for example, 30%, 40%, 50%, 60%, 70% or a range consisting of any two values therein.
[0071] In one embodiment, the fiber mat in the fiber mat reinforced resin layer is glass fiber mat, carbon fiber mat or basalt fiber mat.
[0072] The molding process of the fiber felt reinforced resin layer is as follows: prepare two layers of resin films, evenly place the fiber felt between the two layers of resin films, and perform composite molding by hot pressing with a molding machine to obtain a short fiber reinforced resin layer.
[0073] In one embodiment, the resin in the fiber felt reinforced resin layer is modified or unmodified polyethylene, modified or unmodified polypropylene, modified or unmodified polystyrene, modified or unmodified polycarbonate, modified or unmodified polyamide, modified or unmodified polyethylene recycled material, modified or unmodified polypropylene recycled material, modified or unmodified polystyrene recycled material, modified or unmodified polycarbonate recycled material, modified or unmodified polyamide recycled material.
[0074] By limiting the content of the fiber material and the resin in the fiber-reinforced resin layer 4 , the fiber-reinforced resin layer 4 has the advantages of being light, collision-resistant and impact-resistant.
[0075] In one embodiment, the foam layer has a thickness of 0.8-6 mm, for example, 0.8 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm or a range consisting of any two values therein.
[0076] In one embodiment, the thickness of the foam layer is 1-5 mm, which ensures the cushioning performance of the foam layer while not affecting the assembly of the protective plate due to the excessive thickness of the foam layer.
[0077] In one embodiment, the foam layer is made of polyethylene foam plastic, polystyrene foam plastic, polyurethane foam plastic, polyvinyl chloride foam material or polyethylene terephthalate foam material.
[0078] In one embodiment, the fiber-reinforced resin layer is a GMT material.
[0079] The GMT material is a composite material with a thermoplastic resin as a matrix and glass fiber mat or glass fiber as a reinforcing skeleton, which can replace traditional metal parts, reduce the weight of the vehicle body, reduce costs, and has the advantages of light weight, collision resistance, and impact resistance, and can evenly transmit and disperse the stress on the material to all parts. In one embodiment, the mass percentage of the glass fiber mat or glass fiber in the thermoplastic resin is 30-60%, for example, it can be 30%, 40%, 50%, 60%, 70% or a range consisting of any two values therein.
[0080] In one embodiment, the thermoplastic resin in the GMT material is modified or unmodified polyethylene, modified or unmodified polypropylene, modified or unmodified polystyrene, modified or unmodified polycarbonate, modified or unmodified polyamide, modified or unmodified polyethylene recycled material, modified or unmodified polypropylene recycled material, modified or unmodified polystyrene recycled material, modified or unmodified polycarbonate recycled material, modified or unmodified polyamide recycled material.
[0081] In one embodiment, the length of the glass fiber in the GMT material is 10-70 mm, for example, 10 mm, 20 mm, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm or a range consisting of any two values therein.
[0082] In one embodiment, the metal plate 2 is adjacent to the first continuous fiber reinforced resin layer 1 , and the foam layer 3 is adjacent to the fiber reinforced resin layer 4 .
[0083] like Figure 2 As shown, the metal plate 2 is adjacent to the fiber reinforced resin layer 4 , and the foam layer 3 is adjacent to the first continuous fiber reinforced resin layer 1 .
[0084] The above arrangement indicates that, in the present invention, the positional relationship between the metal plate 2 and the foam layer 3 can be interchangeable, that is, the metal plate 2 can be located above the foam layer 3 or below the foam layer 3 .
[0085] The features of the present invention are further described below by assuming that the metal plate 2 is located below the foam layer 3 .
[0086] See also Figure 3 to Figure 5 As shown, the metal plate 2 includes a substrate 21 and a coating 22 located on at least one surface of the substrate; the substrate 21 is selected from iron and its alloys, aluminum and its alloys, magnesium and its alloys, copper and its alloys, titanium and its alloys or nickel and its alloys, and the coating 22 is a zinc coating, a zinc-iron alloy coating or a zinc-magnesium alloy coating.
[0087] It should be noted that the substrate 21 includes two opposite first surfaces and a second surface in the thickness direction, and the coating 22 is disposed on at least one surface of the substrate 21. It should be understood by those skilled in the art that the coating 22 can be disposed on the first surface, or on the second surface, or on both the first surface and the second surface. Those skilled in the art can make a selection according to actual needs. It should be noted that the above-mentioned "surface" can be the entire area of the first surface and / or the second surface, or a partial area of the first surface and / or the second surface. This application has no special restrictions, as long as the purpose of this application can be achieved.
[0088] In one embodiment, the substrate 21 is a steel plate, a steel strip or an aluminum plate.
[0089] In one embodiment, the mass percentage of zinc in the coating is 10-100%, for example, it can be 10%, 20%, 50%, 80%, 100% or a range consisting of any two values therein.
[0090] In one embodiment, the thickness of the substrate 21 is 0.25-5 mm, for example, 0.25 mm, 0.28 mm, 0.4 mm, 0.5 mm, 0.8 mm, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm or a range consisting of any two of these values.
[0091] In one embodiment, the thickness of the substrate 21 is 0.28-4 mm.
[0092] In one embodiment, the surface roughness of the substrate 21 is 0.3-1.2 μm, for example, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2 or a range consisting of any two of these values.
[0093] In one embodiment, the mass percentage of zinc in the zinc-iron alloy coating and the zinc-magnesium alloy coating is 10-90%, for example, it can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or a range consisting of any two of these values.
[0094] In one embodiment, the thickness of the coating layer 22 is 0.05-0.5 mm, for example, 0.05 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm or a range consisting of any two values therein.
[0095] In one embodiment, the steel plate / steel strip has a yield strength of 100 MPa to 1200 MPa, a tensile strength of 200 MPa to 1400 MPa, and an elongation at break of 1% to 40%.
[0096] The use of the metal plate 2 with the above-mentioned structure further ensures the rigidity and strength of the protective plate, and further improves the impact resistance of the protective plate. At the same time, the setting of the metal plate 2 can achieve excellent buffering and noise reduction effects.
[0097] See also Figure 6 In one embodiment, a resin film 6 is provided between the second continuous fiber reinforced resin layer 5 and the fiber reinforced resin layer 4, and the thickness of the resin film 6 is 0.08-1 mm. For example, it can be 0.08 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.5 mm, 0.6 mm, 0.8 mm, 1 mm, or a range consisting of any two values therein. By providing the resin film 6 between the second continuous fiber reinforced resin layer 5 and the fiber reinforced resin layer 4, the adhesion between the fiber reinforced resin layer 4 and the second continuous fiber reinforced resin layer 5 is effectively improved.
[0098] In one embodiment, the resin material of the resin film 6 is modified or unmodified polyethylene, modified or unmodified polypropylene, modified or unmodified polystyrene, modified or unmodified polycarbonate, modified or unmodified polyamide, modified or unmodified polyethylene recycled material, modified or unmodified polypropylene recycled material, modified or unmodified polystyrene recycled material, modified or unmodified polycarbonate recycled material, modified or unmodified polyamide recycled material.
[0099] In one embodiment, the resin material of the resin film 6 and the resin materials of the fiber-reinforced resin layer 4 and the second continuous fiber-reinforced resin layer 5 may be the same as or different from each other.
[0100] In one embodiment, the resin film 6, the fiber-reinforced resin layer 4 and the second continuous fiber-reinforced resin layer 5 are made of the same resin material. Using the same resin material can effectively improve the overall compatibility and further improve the impact resistance of the protective plate.
[0101] like Figure 7 As shown, in Figure 1 Based on the protective plate shown, the protective plate may further include a buffer layer 7, which is a rubber polymer, a thermoplastic elastomer or a resin polymer, and the buffer layer 7 is arranged on the side of the first continuous fiber reinforced resin layer 1 away from the metal plate 2.
[0102] like Figure 8 As shown, in Figure 6 Based on the protective plate shown, the protective plate may further include a buffer layer 7, which is a rubber polymer, a thermoplastic elastomer or a resin polymer, and the buffer layer 7 is arranged on the side of the first continuous fiber reinforced resin layer 1 away from the metal plate 2.
[0103] The buffer layer 7 is set up so that when the protective plate is subjected to external force, it absorbs energy by deformation and rupture to achieve a better stress transfer effect. At the same time, it can effectively protect the first continuous fiber reinforced resin layer 1, and can effectively improve the impact resistance and corrosion resistance of the protective plate. At the same time, it can effectively reduce the weight, achieve light weight and high strength, and avoid the bottom of the protective plate from being punctured.
[0104] In one embodiment, the rubber polymer is styrene-butadiene rubber, nitrile rubber, chlorinated nitrile rubber, butadiene rubber, chloroprene rubber, butyl rubber, isoprene rubber, acrylic rubber, fluororubber, EPDM rubber, EPDM rubber, chlorosulfonated polyethylene rubber, thermoplastic vulcanized rubber or polyester rubber.
[0105] In one embodiment, the thermoplastic elastomer is a styrene-butylene-styrene block copolymer, a hydrogenated styrene-butylene-styrene block copolymer, a styrene-isoprene-styrene block copolymer, or a hydrogenated ethylene-isoprene-styrene block copolymer.
[0106] In one embodiment, the resin polymer is polyethylene-olefin copolymer, polyurethane, silicone, polystyrene, polyvinylidene fluoride, polyvinyl fluoride, polytetrafluoroethylene, polychlorotrifluoroethylene, polyhexafluoropropylene, polyperfluoroethylene propylene, polyhexafluoropropylene, poly(vinylidene fluoride-hexafluoropropylene), polyethylene, polypropylene, polyvinyl alcohol, polyvinyl butyral, polybutene, polyisobutylene, polyisoprene, polyphenylene ether, polyvinyl chloride or ethylene vinyl acetate.
[0107] In one embodiment, the buffer layer is a TPV material.
[0108] It should be noted that the TPV material mentioned is composed of PP resin and vulcanized rubber particles, where the size of the rubber particles is required to be 1-70 microns, and the hardness of TPV is within the range of 50-85A, and the thickness is within 0.5-2mm. In order to achieve the gradient buffer effect, TPV single-layer sheets of different hardness are compounded together to form a multi-interface.
[0109] In one embodiment, the thickness of the buffer layer 7 is 0.4-2.5 mm, for example, 0.4 mm, 0.5 mm, 0.8 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm or a range consisting of any two values therein.
[0110] In one embodiment, the buffer layer 7 has a thickness of 0.5-2 mm.
[0111] In one embodiment, the layers of the protection plate are formed by hot pressing.
[0112] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.
[0113] Example to Comparative Example
[0114] The structures and thicknesses of the battery protection plates of the embodiments and comparative examples are shown in Table 1, respectively.
[0115] Among them, the structural diagrams of embodiments 1 to 4 are as follows Figure 1 shown.
[0116] Among them, the structural diagram of Example 5 is as follows Figure 6 shown.
[0117] Among them, the structural diagrams of Examples 6 to 8 are as follows Figure 7 shown.
[0118] Comparative Example 1 is based on Example 1, but does not include the foam layer 3 and the fiber-reinforced resin layer 4.
[0119] Comparative Example 2 is based on Example 1, but no foam layer 3 is provided.
[0120] Comparative Example 3 is based on Example 1, but no fiber-reinforced resin layer 4 is provided.
[0121] Comparative Example 4 is based on Example 6, but does not include the foam layer 3, the fiber-reinforced resin layer 4, and the resin film 6.
[0122] The difference between the embodiment and the comparative example is only the thickness, and the types and proportions of materials used in each layer are the same.
[0123] The first continuous fiber reinforced resin layers 1 of Examples 1 to 8 and Comparative Examples 1 to 4 are all continuous glass fiber reinforced polypropylene, and the content of continuous glass fibers in the continuous glass fiber reinforced polypropylene layer is 65 wt %.
[0124] The substrates of the metal plates 2 in Examples 1 to 8 and Comparative Examples 1 to 4 are all steel plates, and the coatings are all zinc coatings.
[0125] The foam layers 3 of Examples 1 to 8 and Comparative Example 3 are all made of polyurethane foam plastic.
[0126] The fiber-reinforced resin layers 4 of Examples 1 to 8 and Comparative Example 2 are all made of GMT material, the mass percentage of glass fiber in the GMT material is 40%, and the length of the glass fiber in the GMT is 40 mm.
[0127] The second continuous fiber reinforced resin layers 5 of Examples 1 to 8 and Comparative Examples 1 to 5 are all made of continuous glass fiber reinforced polypropylene, and the content of continuous glass fibers in the continuous glass fiber reinforced polypropylene is 65 wt %.
[0128] The resin films 6 of Examples 5 to 8 are all made of polypropylene.
[0129] Among them, the buffer layers 7 of Examples 6 to 8 and Comparative Example 4 are all made of TPV materials.
[0130] Table 1
[0131]
[0132] Performance Testing
[0133] The drop hammer impact force E of the embodiment and the comparative example was tested by referring to ASTM D7136 "Standard Test Method for Measuring Damage Resistance of Fiber Reinforced Polymer Matrix Composite Materials to Drop Hammer Impact Events". The diameter of the impact head is 16 mm. According to E = H * m * g, H is the drop height of the impact head, m is the weight of the impact head, m = 30 kg, and g is the acceleration of gravity, g = 9.8 m / s 2 , the test results are shown in Table 2.
[0134] Table 2
[0135]
[0136]
[0137] It can be seen from Table 1 that the utility model effectively improves the impact resistance of the battery protection plate by configuring the continuous fiber reinforced resin layer 4, the foam layer 3 and the metal plate 2, and the configuration of the buffer layer 7 further improves the impact resistance.
[0138] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the utility model rather than to limit the protection scope of the utility model. Although the utility model is described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the utility model can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the utility model.
Claims
1. A battery protection plate, characterized in that: It comprises a first continuous fiber reinforced resin layer, a fiber reinforced resin layer and a second continuous fiber reinforced resin layer which are sequentially stacked; The first continuous fiber reinforced resin layer and the fiber reinforced resin layer include a metal plate and a foam layer between them; The fiber-reinforced resin layer is a short fiber-reinforced resin layer or a fiber felt-reinforced resin layer; The thickness ratio of the metal plate, the foam layer and the fiber-reinforced resin layer is (0.3-6): (0.6-8): (1-12).
2. The battery protection plate according to claim 1, characterized in that: The thickness of the first continuous fiber reinforced resin layer is 0.1 to 1.5 mm; and / or The thickness of the second continuous fiber reinforced resin layer is 0.1-1.5 mm.
3. The battery protection plate according to claim 1, characterized in that: The fiber-reinforced resin layer has a thickness of 1 to 12 mm and a gram weight of 400 to 1600 g / m 2 ; and / or The length of the short fibers in the short fiber reinforced resin layer is 10 to 70 mm; and / or The thickness of the foam layer is 0.8-6 mm.
4. The battery protection plate according to claim 1, characterized in that: The fiber-reinforced resin layer is made of GMT material.
5. The battery protection plate according to claim 1, characterized in that: The metal plate is adjacent to the first continuous fiber reinforced resin layer, and the foam layer is adjacent to the fiber reinforced resin layer; or The metal plate is adjacent to the fiber reinforced resin layer, and the foam layer is adjacent to the first continuous fiber reinforced resin layer.
6. The battery protection plate according to claim 1, characterized in that: The metal plate includes a substrate and a coating located on at least one surface of the substrate; the substrate is selected from iron and its alloys, aluminum and its alloys, magnesium and its alloys, copper and its alloys, titanium and its alloys or nickel and its alloys, and the coating is a zinc coating, a zinc-iron alloy coating or a zinc-magnesium alloy coating.
7. The battery protection plate according to claim 6, characterized in that: The thickness of the substrate is 0.25-5 mm, and the roughness of the surface of the substrate is 0.3-1.2; and / or The thickness of the coating is 0.05-0.5 mm.
8. The battery protection plate according to claim 1, characterized in that: A resin film is provided between the second continuous fiber reinforced resin layer and the fiber reinforced resin layer, and the thickness of the resin film is 0.08-1.0 mm.
9. The battery protection plate according to claim 1, characterized in that: It also includes a buffer layer, which is a rubber polymer, a thermoplastic elastomer or a resin polymer. The buffer layer is arranged on a side of the first continuous fiber reinforced resin layer away from the metal plate.
10. The battery protection plate according to claim 9, characterized in that: The buffer layer is made of TPV material.
Citation Information
Cited By
Bottom protection plate, battery and electric equipment
CN121332061A
Battery protection plate, battery pack, and vehicle
EP4793035A1
Battery protection plate
WO2025162335A1
Buffer plate configured for connecting to battery bottom protective plate, and battery pack
WO2026153395A1
Battery device and electric device
WO2026199132A1